Positive electrode sheet, electrochemical device and electronic device
By using high-specific-capacity positive electrode plates and fluorinated vinyl carbonate-improved electrolyte in lithium-ion secondary batteries, the problem of irreversible loss of active lithium in lithium-ion secondary batteries is solved, and the energy density and cycle of the battery are improved. performance.
Patent Information
- Application Number
- CN202180006723.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-25
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2041-10-25
AI Technical Summary
During the charge and discharge process of lithium-ion secondary batteries, the solid electrolyte interface (SEI) film formed on the surface of the negative active material causes irreversible loss of active lithium, reducing the energy density and cycle life of the battery.
A cathode plate including a first cathode active material and a second cathode active material with high specific capacity is used, doped with Cu and Ti to form a Li-Ni-Cu-Ti-O solid solution, and combined with fluorinated ethylene carbonate in the electrolyte , optimize the structure of the cathode plate and the composition of the electrolyte to reduce the irreversible loss of active lithium.
It effectively compensates for the irreversible loss of active lithium caused by the SEI film, improves the energy density and cycle performance of lithium-ion secondary batteries, and improves the rate performance and long cycle life.
Smart Images

Figure CN114766067B_ABST
Abstract
Description
[0001] Citation of Related Applications
[0002] This application claims priority to international application PCT / CN2021 / 126213, filed on October 25, 2021, entitled “Positive Electrode Plate, Electrochemical Device and Electronic Device”, the entire contents of which are incorporated herein by reference. Technical Field
[0003] The present application belongs to the field of electrochemical technology, and specifically relates to a positive electrode sheet, an electrochemical device and an electronic device. Background Art
[0004] During the first cycle of charge and discharge of lithium-ion secondary batteries, a solid electrolyte interface (SEI) film will form on the surface of the negative electrode active material, causing irreversible loss of active lithium, thereby reducing the energy density of lithium-ion secondary batteries. For example, when graphite is used as the negative electrode active material, about 10% of the active lithium will be consumed during the first cycle of charge and discharge of lithium-ion secondary batteries; when using negative electrode active materials with higher specific capacity, such as alloy negative electrode active materials (silicon, tin, etc.), oxide negative electrode active materials (silicon oxide, tin oxide, etc.), and amorphous carbon negative electrode active materials, the irreversible loss of active lithium will further increase. Therefore, supplementing the irreversible loss of active lithium during the first cycle of charge and discharge by appropriate methods is of great significance to improving the energy density of lithium-ion secondary batteries. Summary of the invention
[0005] The purpose of the present application is to provide a positive electrode sheet, an electrochemical device and an electronic device, aiming to improve the processing performance of the positive electrode sheet, compensate for the irreversible loss of active lithium during the first cycle of charging and discharging, and enable the electrochemical device to have high energy density, long cycle life and good rate performance.
[0006] In a first aspect, the present application provides a positive electrode plate, which includes a positive electrode film layer, wherein the positive electrode film layer includes a first positive electrode active material shown in Chemical Formula 1 and a second positive electrode active material shown in Chemical Formula 2.
[0007] Li 1+x Co y M1 1-y O 2-z A z Chemical formula 1
[0008] Li 2+r Ni p Cu q Ti u M2 v O 2-s B s Chemical formula 2
[0009] -0.1 ≤ x ≤ 0.2, 0.8 ≤ y ≤ 1, 0 ≤ z ≤ 0.2, M1 includes at least one of Ni, Mn, Al, Mg, Ti, Zr, La, Y, Fe, Cr, V, Zn, Ru, Rh, Ga, Pd, Pt, Mo, W, Sb, Nb, Se, Te, Ce, and A includes at least one of S, N, P, F, Cl, Br.
[0010] -0.2 ≤ r ≤ 0.2, 0 < p < 1, 0 < q < 1, 0 < u ≤ 0.01, 0 ≤ v ≤ 0.2, 0 < p + q + u + v ≤ 1, 0 ≤ s < 0.2, M2 includes at least one of Mn, Fe, Co, Al, V, Cr, Nb, Mg, Zr, La, Y, Zn, Ru, Rh, Ga, Pd, Pt, Mo, W, Sb, Nb, Se, Te, Ce, and B includes at least one of S, N, P, F, Cl, Br.
[0011] The specific capacity of the first positive electrode active material is relatively high, and the volume change during charge and discharge is relatively small. Therefore, the electrochemical device can have relatively high cycle stability and relatively high initial Coulomb efficiency. The positive electrode sheet of this application can fully exert the synergistic effect between the first positive electrode active material and the second positive electrode active material. During the first charge process of the electrochemical device, due to the characteristics of the second positive electrode active material having a high first charge specific capacity and a low first Coulomb efficiency, it can effectively compensate for the irreversible loss of active lithium caused by the formation of the SEI film on the surface of the negative electrode active material. At the same time, during the first discharge process of the electrochemical device, there is still enough active lithium intercalated back into the first positive electrode active material, thereby effectively improving the energy density and cycle performance of the electrochemical device.
[0012] The second positive electrode active material simultaneously performs Cu, Ti, and optionally M2 cation doping on the Li2NiO2 lithium supplement material and forms a Li-Ni-Cu-Ti-O (or Li-Ni-Cu-Ti-M2-O) solid solution. Compared with Li2NiO2, the Li-Ni-Cu-Ti-O (or Li-Ni-Cu-Ti-M2-O) solid solution has a lower phase formation potential barrier, higher purity and specific capacity, and a lower first Coulomb efficiency, so it can better compensate for the irreversible loss of active lithium caused by the formation of the SEI film on the surface of the negative electrode active material, and further improve the energy density and cycle performance of the electrochemical device. In addition, the second positive electrode active material contains a small amount of Ti element, and the affinity between the Ti element and free lithium (such as LiOH, Li2CO3, etc.) is higher. Therefore, the second positive electrode active material also has a lower surface free lithium content, which can significantly improve the gel problem of the positive electrode slurry and improve the processing performance of the positive electrode sheet.
[0013] In any implementation manner of this application, -0.05 ≤ x ≤ 0.1.
[0014] In any embodiment of the present application, 0.8≤y<1.
[0015] In any embodiment of the present application, 0 <z≤0.2。
[0016] In any embodiment of the present application, M1 includes at least one of Ni, Mn, Al, Mg, Ti, Zr, La, Y, Fe, Cr, V, Zn, and Rh.
[0017] In any embodiment of the present application, A includes at least one of S and F.
[0018] In any embodiment of the present application, -0.1≤r≤0.1.
[0019] In any embodiment of the present application, 0.39≤p<0.5.
[0020] In any embodiment of the present application, 0.39≤q<0.5.
[0021] In any embodiment of the present application, 0 <u≤0.005。
[0022] In any embodiment of the present application, 0 <v≤0.2。
[0023] In any embodiment of the present application, 0 <s≤0.2。
[0024] In any embodiment of the present application, M2 includes at least one of Mn, Fe, Co, Al, V, Cr, Nb, Mg, Zr, and Zn.
[0025] In any embodiment of the present application, B includes at least one of S and F.
[0026] In any embodiment of the present application, the mass ratio of the first positive electrode active material to the second positive electrode active material is 5:1 to 99:1. Optionally, the mass ratio of the first positive electrode active material to the second positive electrode active material is 9:1 to 99:1. The positive electrode sheet of the present application contains a higher content of the first positive electrode active material with higher structural stability, which can reduce the loss of active lithium and the increase in impedance caused by structural damage, so that the electrochemical device has higher cycle stability and better kinetic performance.
[0027] In any embodiment of the present application, based on the total mass of the positive electrode film layer, the mass percentage of the first positive electrode active material is 80% to 98%. Optionally, the mass percentage of the first positive electrode active material is 85% to 98%.
[0028] In any embodiment of the present application, the positive electrode sheet satisfies 2≤R×P / Q≤36, RΩ is the single-sided resistance of the positive electrode sheet, P g / cm 3is the compaction density of the positive electrode, Q g / 1540.25mm 2 is the single-surface density of the positive electrode sheet. Optionally, the positive electrode sheet satisfies 5≤R×P / Q≤32.
[0029] By rationally designing the single-surface resistance, compaction density, and single-surface surface density of the positive electrode plate, the energy density, rate performance, and cycle performance of the electrochemical device can be further improved, so that the electrochemical device using the positive electrode plate of the present application can simultaneously have high energy density, long cycle life, and good rate performance.
[0030] In any embodiment of the present application, the single-surface resistance of the positive electrode sheet is RΩ, R≤3. Optionally, R≤1.5. When the single-surface resistance of the positive electrode sheet is within a suitable range, it is beneficial to further improve the cycle performance and rate performance of the electrochemical device.
[0031] In any embodiment of the present application, the compaction density of the positive electrode sheet is P g / cm 3 , 4.0≤P≤4.3. When the compaction density of the positive electrode sheet is within a suitable range, it is beneficial to the migration of electrons and lithium ions, thereby further improving the cycle performance of the electrochemical device, and the electrochemical device also has a high energy density.
[0032] In any embodiment of the present application, the single-sided surface density of the positive electrode sheet is Q g / 1540.25 mm 2 , 0.16≤Q≤0.38. When the single-surface density of the positive electrode sheet is within an appropriate range, the electrochemical device can have a high charge and discharge capacity while also having further improved cycle performance and rate performance.
[0033] In any embodiment of the present application, the second positive electrode active material belongs to the Immm space group.
[0034] In any embodiment of the present application, in the X-ray diffraction spectrum measured after the first cycle of charging of the second positive electrode active material, there are characteristic diffraction peaks at 2θ values of 36° to 38°, 42° to 44°, and 62° to 64°.
[0035] A second aspect of the present application provides an electrochemical device, which includes the positive electrode sheet of the first aspect of the present application.
[0036] In any embodiment of the present application, the electrochemical device includes an electrolyte, the electrolyte includes a negative electrode film-forming additive, and the mass percentage of the additive is 0% to 15% based on the total mass of the electrolyte. Optionally, the mass percentage of the additive is 0.5% to 15%.
[0037] In any embodiment of the present application, the additive includes at least one of fluoroethylene carbonate, vinylene carbonate, vinyl carbonate, vinyl sulfate, propylene sulfate, vinyl sulfite, 1,3-propane sultone, 1,3-propylene sultone, sulfonate cyclic quaternary ammonium salt, succinic anhydride, succinonitrile, adiponitrile, tris(trimethylsilane)phosphate, and tris(trimethylsilane)borate.
[0038] In any embodiment of the present application, the additive includes at least fluoroethylene carbonate.
[0039] When the electrolyte of the present application contains fluoroethylene carbonate, it is conducive to forming a more uniform, dense and thin SEI film after the first cycle of charge and discharge of the electrochemical device, preventing the organic solvent from continuously undergoing reduction reaction at the negative electrode, thereby compensating for the irreversible loss of active lithium caused by the formation of the SEI film, while also forming a more uniform and dense SEI film on the surface of the negative electrode active material, reducing the continuous loss of active lithium. Therefore, the electrochemical device of the present application can have high energy density, long cycle life and good rate performance at the same time.
[0040] A third aspect of the present application provides an electronic device, which includes the electrochemical device of the second aspect of the present application. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] Figure 1 This is the X-ray diffraction spectrum of the second positive electrode active material of Example 1 measured after the first cycle of charging. DETAILED DESCRIPTION
[0042] In order to make the purpose, technical scheme and advantages of the present application clearer, the technical scheme of the present application will be clearly and completely described in conjunction with the embodiments below. Obviously, the described embodiments are part of the embodiments of the present application, rather than all of the embodiments. The relevant embodiments described herein are illustrative in nature and are used to provide a basic understanding of the present application. The embodiments of the present application should not be interpreted as limiting the present application. Based on the technical scheme provided by the present application and the embodiments given, all other embodiments obtained by those skilled in the art without making creative work are within the scope of protection of the present application.
[0043] For simplicity, only some numerical ranges are specifically disclosed herein. However, any lower limit can be combined with any upper limit to form an unspecified range; and any lower limit can be combined with other lower limits to form an unspecified range, and any upper limit can be combined with any other upper limit to form an unspecified range. In addition, each separately disclosed point or single value can itself be combined as a lower limit or upper limit with any other point or single value or with other lower limits or upper limits to form an unspecified range.
[0044] In the description herein, unless otherwise specified, “above” and “below” include the number.
[0045] Unless otherwise specified, the terms used in this application have the commonly known meanings generally understood by those skilled in the art. Unless otherwise specified, the numerical values of the various parameters mentioned in this application can be measured using various measurement methods commonly used in the art (for example, they can be tested according to the methods given in the examples of this application).
[0046] The term "about" is used to describe and illustrate small changes. When used in conjunction with an event or situation, the term may refer to an example in which the event or situation occurs precisely and an example in which the event or situation occurs very approximately. For example, when used in conjunction with a numerical value, the term may refer to a range of variation of less than or equal to ±10% of the numerical value, such as less than or equal to ±5%, less than or equal to ±4%, less than or equal to ±3%, less than or equal to ±2%, less than or equal to ±1%, less than or equal to ±0.5%, less than or equal to ±0.1%, or less than or equal to ±0.05%. In addition, amounts, ratios, and other numerical values are sometimes presented in this article in a range format. It should be understood that such a range format is for convenience and simplicity, and should be flexibly understood to include not only numerical values explicitly designated as range limits, but also all individual numerical values or subranges encompassed within the range, as if each numerical value and subrange were explicitly designated.
[0047] A list of items connected by the terms "at least one of," "at least one of," "at least one of," or other similar terms may mean any combination of the listed items. For example, if items A and B are listed, the phrase "at least one of A and B" means only A; only B; or A and B. In another example, if items A, B, and C are listed, the phrase "at least one of A, B, and C" means only A; or only B; only C; A and B (excluding C); A and C (excluding B); B and C (excluding A); or all of A, B, and C. Item A may contain a single component or multiple components. Item B may contain a single component or multiple components. Item C may contain a single component or multiple components.
[0048] In order to improve the energy density of lithium-ion secondary batteries, lithium replenishment technology can be used to increase the active lithium content and compensate for the irreversible loss of active lithium during the first cycle of charge and discharge of lithium-ion secondary batteries. The main and more mature technology is the negative electrode lithium replenishment process, such as covering the surface of the negative electrode with a layer of lithium metal by lithium powder or lithium foil. However, the chemical properties of metallic lithium are very active and easily react with moisture in the air. Therefore, the requirements for the environment (air humidity, oxygen content, etc.) and equipment during the lithium replenishment process are relatively high, which increases the difficulty of the process; in addition, lithium powder easily floats in the air, resulting in a higher safety risk during the lithium replenishment process.
[0049] Compared with the negative electrode lithium replenishment process, the positive electrode lithium replenishment process has higher safety and reduces the requirements for the environment and equipment. The positive electrode lithium replenishment process can be to add lithium replenishment materials to the positive electrode slurry to prepare lithium-rich positive electrode plates. During the first cycle of charge and discharge of the lithium-ion secondary battery (for example, during formation or initial cycle), the lithium replenishment material releases active lithium to compensate for the irreversible loss of active lithium caused by the formation of SEI film. The prior art discloses the use of Li2NiO2 as a lithium replenishment material to compensate for the irreversible loss of active lithium caused by the formation of SEI film. Li2NiO2 has a high specific capacity and a simple preparation method, which can greatly improve the energy density of lithium-ion secondary batteries. However, the content of free lithium (for example, LiOH, Li2CO3, etc.) on the surface of Li2NiO2 is also high, which is very easy to cause gelation during the preparation of the positive electrode slurry, seriously affecting the processing performance of the positive electrode plate.
[0050] In order to solve the above problems, the inventors have proposed a positive electrode plate through extensive research that can effectively improve the energy density and has good processing performance.
[0051] Positive electrode
[0052] A first aspect of an embodiment of the present application provides a positive electrode plate, which includes a positive electrode collector and a positive electrode film layer arranged on at least one surface of the positive electrode collector, wherein the positive electrode film layer includes a first positive electrode active material shown in Chemical Formula 1 and a second positive electrode active material shown in Chemical Formula 2.
[0053] Li 1+x Co y M1 1-y O 2-z A z Chemical formula 1
[0054] Li 2+r Ni p Cu q Ti u M2 v O 2-s B s Chemical formula 2
[0055] -0.1≤x≤0.2, 0.8≤y≤1, 0≤z≤0.2, M1 includes at least one of Ni, Mn, Al, Mg, Ti, Zr, La, Y, Fe, Cr, V, Zn, Ru, Rh, Ga, Pd, Pt, Mo, W, Sb, Nb, Se, Te, Ce, and A includes at least one of S, N, P, F, Cl, and Br.
[0056] -0.2 ≤ r ≤ 0.2, 0 < p < 1, 0 < q < 1, 0 < u ≤ 0.01, 0 ≤ v ≤ 0.2, 0 < p + q + u + v ≤ 1, 0 ≤ s < 0.2, M2 includes at least one of Mn, Fe, Co, Al, V, Cr, Nb, Mg, Zr, La, Y, Zn, Ru, Rh, Ga, Pd, Pt, Mo, W, Sb, Nb, Se, Te, Ce, and B includes at least one of S, N, P, F, Cl, Br.
[0057] The specific capacity of the first positive electrode active material is relatively high and the volume change during charge and discharge is relatively small. Therefore, the electrochemical device can have relatively high cycle stability and relatively high initial Coulomb efficiency. The positive electrode sheet of this application can give full play to the synergistic effect between the first positive electrode active material and the second positive electrode active material. During the first charge process of the electrochemical device, due to the characteristics of the second positive electrode active material having a high first charge specific capacity and a low first Coulomb efficiency, it can effectively compensate for the irreversible loss of active lithium caused by the formation of the SEI film on the surface of the negative electrode active material. At the same time, during the first discharge process of the electrochemical device, there is still enough active lithium intercalated back into the first positive electrode active material, thereby effectively improving the energy density and cycle performance of the electrochemical device.
[0058] The second positive electrode active material simultaneously dopes Cu, Ti, and optionally M2 cations into the Li2NiO2 lithium supplement material and forms a Li-Ni-Cu-Ti-O (or Li-Ni-Cu-Ti-M2-O) solid solution. Compared with Li2NiO2, the Li-Ni-Cu-Ti-O (or Li-Ni-Cu-Ti-M2-O) solid solution has a lower phase formation energy barrier, higher purity and specific capacity, and a lower first Coulomb efficiency, so it can better compensate for the irreversible loss of active lithium caused by the formation of the SEI film on the surface of the negative electrode active material and further improve the energy density and cycle performance of the electrochemical device. In addition, the second positive electrode active material contains a small amount of Ti element, and the affinity between the Ti element and free lithium (such as LiOH, Li2CO3, etc.) is higher. Therefore, the second positive electrode active material also has a lower surface free lithium content, which can significantly improve the gel problem of the positive electrode slurry and improve the processing performance of the positive electrode sheet.
[0059] In the positive electrode sheet of this application, the first positive electrode active material and the second positive electrode active material may also optionally include doped anions. After the anions and cations are doped and modified simultaneously, the structures of the first positive electrode active material and the second positive electrode active material are more stable, thereby enabling the electrochemical device to maintain better comprehensive performance.
[0060] In some embodiments, -0.05 ≤ x ≤ 0.1.
[0061] In some embodiments, y = 1.
[0062] In some embodiments, 0.8 ≤ y < 1. Optionally, 0.9 ≤ y < 1.
[0063] In some embodiments, z = 0.
[0064] In some embodiments, 0 < z ≤ 0.2. Optionally, 0 < z ≤ 0.1. Further, 0 < z ≤ 0.05.
[0065] In some embodiments, M1 includes at least one of Ni, Mn, Al, Mg, Ti, Zr, La, Y, Fe, Cr, V, Zn, Rh.
[0066] In some embodiments, M1 is selected from at least one of Ni, Mn, Al, Mg, Ti, Zr, La, Y, Fe, Cr, V, Zn, Rh.
[0067] In some embodiments, A includes at least one of S, F. Optionally, A includes F.
[0068] In some embodiments, A is selected from S, F, or a combination thereof. Optionally, A is selected from F.
[0069] In some embodiments, -0.05 ≤ x ≤ 0.1, 0.9 ≤ y < 1, z = 0, and M1 includes at least one of Ni, Mn, Al, Mg, Ti, Zr, La, Y, Fe, Cr, V, Zn, Rh.
[0070] In embodiments, -0.05 ≤ x ≤ 0.1, 0.9 ≤ y < 1, z = 0, and M1 is selected from at least one of Ni, Mn, Al, Mg, Ti, Zr, La, Y, Fe, Cr, V, Zn, Rh.
[0071] In some embodiments, -0.05 ≤ x ≤ 0.1, 0.9 ≤ y < 1, 0 < z ≤ 0.1, M1 includes at least one of Ni, Mn, Al, Mg, Ti, Zr, La, Y, Fe, Cr, V, Zn, Rh, and A includes at least one of S, F.
[0072] In some embodiments, -0.05 ≤ x ≤ 0.1, 0.9 ≤ y < 1, 0 < z ≤ 0.1, M1 is selected from at least one of Ni, Mn, Al, Mg, Ti, Zr, La, Y, Fe, Cr, V, Zn, Rh, and A is selected from S, F, or a combination thereof.
[0073] In some embodiments, x = 1, y = 1, z = 0.
[0074] In some embodiments, x = 1, y = 1, 0 < z ≤ 0.1, and A includes at least one of S, F.
[0075] In some embodiments, x = 1, y = 1, 0 < z ≤ 0.1, and A is selected from S, F, or a combination thereof.
[0076] In some embodiments, -0.1 ≤ r ≤ 0.1.
[0077] In some embodiments, 0.39 ≤ p < 0.5. Optionally, 0.44 ≤ p < 0.5. Further, 0.49 ≤ p < 0.5.
[0078] In some embodiments, 0.39 ≤ q < 0.5. Optionally, 0.44 ≤ q < 0.5. Further, 0.49 ≤ q < 0.5.
[0079] In some embodiments, 0 < u ≤ 0.005.
[0080] In some embodiments, v = 0.
[0081] In some embodiments, 0 < v ≤ 0.2. Optionally, 0 < v ≤ 0.1.
[0082] In some embodiments, 0 < p + q + u + v < 1.
[0083] In some embodiments, s = 0.
[0084] In some embodiments, 0 < s ≤ 0.2. Optionally, 0 < s ≤ 0.1.
[0085] In some embodiments, M2 includes at least one of Mn, Fe, Co, Al, V, Cr, Nb, Mg, Zr, Zn.
[0086] In some embodiments, M2 is selected from at least one of Mn, Fe, Co, Al, V, Cr, Nb, Mg, Zr, Zn.
[0087] In some embodiments, B includes at least one of S, F. Optionally, B includes F.
[0088] In some embodiments, B is selected from S, F, or a combination thereof. Optionally, B is selected from F.
[0089] In some embodiments, -0.1 ≤ r ≤ 0.1, 0.49 ≤ p < 0.5, 0.49 ≤ q < 0.5, 0 < u ≤ 0.01, v = 0, 0 < s ≤ 0.1, and B includes at least one of S, F.
[0090] In some embodiments, -0.1 ≤ r ≤ 0.1, 0.49 ≤ p < 0.5, 0.49 ≤ q < 0.5, 0 < u ≤ 0.01, v = 0, 0 < s ≤ 0.1, and B is selected from S, F, or a combination thereof.
[0091] In some embodiments, -0.1 ≤ r ≤ 0.1, 0.49 ≤ p < 0.5, 0.49 ≤ q < 0.5, 0 < u ≤ 0.01, v = 0, s = 0.
[0092] In some embodiments, -0.1 ≤ r ≤ 0.1, 0.44 ≤ p < 0.5, 0.44 ≤ q < 0.5, 0 < u ≤ 0.01, 0 < v ≤ 0.1, s = 0, and M2 includes at least one of Mn, Fe, Co, Al, V, Cr, Nb, Mg, Zr, Zn.
[0093] In some embodiments, -0.1 ≤ r ≤ 0.1, 0.44 ≤ p < 0.5, 0.44 ≤ q < 0.5, 0 < u ≤ 0.01, 0 < v ≤ 0.1, s = 0, and M2 is selected from at least one of Mn, Fe, Co, Al, V, Cr, Nb, Mg, Zr, Zn.
[0094] In some embodiments, -0.1 ≤ r ≤ 0.1, 0.44 ≤ p < 0.5, 0.44 ≤ q < 0.5, 0 < u ≤ 0.01, 0 < v ≤ 0.1, 0 < s ≤ 0.1, M2 includes at least one of Mn, Fe, Co, Al, V, Cr, Nb, Mg, Zr, Zn, and B includes at least one of S, F.
[0095] In some embodiments, -0.1 ≤ r ≤ 0.1, 0.44 ≤ p < 0.5, 0.44 ≤ q < 0.5, 0 < u ≤ 0.01, 0 < v ≤ 0.1, 0 < s ≤ 0.1, M2 is selected from at least one of Mn, Fe, Co, Al, V, Cr, Nb, Mg, Zr, Zn, and B is selected from S, F, or a combination thereof.
[0096] The second positive electrode active material of the present application has more excellent performance than Li2NiO2, but its crystal structure is similar to that of Li2NiO2. In some embodiments, the second positive electrode active material belongs to the Immm space group.
[0097] In some embodiments, in the X-ray diffraction spectrum measured after the first charge of the second positive electrode active material, characteristic diffraction peaks are present at positions where the 2θ value is 36° to 38°, 42° to 44°, and 62° to 64°.
[0098] In some embodiments, the mass ratio of the first positive electrode active material to the second positive electrode active material is 5:1 to 99:1. For example, the mass ratio of the first positive electrode active material to the second positive electrode active material is 5:1, 10:1, 15:1, 20:1, 25:1, 30:1, 35:1, 40:1, 45:1, 50:1, 55:1, 60:1, 65:1, 70:1, 75:1, 80:1, 85:1, 90:1, 95:1, 99:1 or any range thereof. Optionally, the mass ratio of the first positive electrode active material to the second positive electrode active material is 9:1 to 99:1.
[0099] The positive electrode plate of the present application contains a higher content of the first positive electrode active material with higher structural stability, which can reduce the loss of active lithium and the increase in impedance caused by structural damage, so that the electrochemical device has higher cycle stability and better kinetic performance.
[0100] In some embodiments, based on the total mass of the positive electrode film layer, the mass percentage of the first positive electrode active material is 80% to 98%. For example, the mass percentage of the first positive electrode active material is 80%, 81%, 82%, 83%, 84%, 85%, 86%, 87%, 88%, 89%, 90%, 91%, 92%, 93%, 94%, 95%, 96%, 97%, 98% or any range consisting of the above values. Optionally, the mass percentage of the first positive electrode active material is 85% to 98%.
[0101] In some embodiments, the mass percentage of the second positive electrode active material can be adjusted according to the type of negative electrode active material used. For example, when graphite is used as the negative electrode active material, the mass percentage of the second positive electrode active material can be maintained in a relatively low range; while when alloy negative electrode active materials (silicon, tin, etc.), oxide negative electrode active materials (silicon oxide, tin oxide, etc.), and amorphous carbon negative electrode active materials are used, the mass percentage of the second positive electrode active material can be maintained in a relatively high range to better compensate for the irreversible loss of active lithium caused by the formation of SEI film on the surface of the negative electrode active material.
[0102] The inventors further discovered that the single-surface resistance, compaction density and single-surface density of the positive electrode sheet are key parameters in the design and preparation process of the electrochemical device. If the single-surface resistance of the positive electrode sheet is too large, the cycle performance and rate performance of the electrochemical device will deteriorate; if the compaction density of the positive electrode sheet is too large or too small, the cycle performance and rate performance of the electrochemical device will deteriorate; if the single-surface density of the positive electrode sheet is too large, the electrolyte wettability will deteriorate, and the cycle performance and rate performance of the electrochemical device will deteriorate, especially the discharge capacity of the electrochemical device at a high rate will be significantly reduced; if the single-surface density of the positive electrode sheet is too small, the length of the positive current collector and the separator will increase at the same capacity, the ohmic internal resistance of the electrochemical device will increase, and the cycle performance and rate performance will also deteriorate. Therefore, it is necessary to reasonably design the above parameters of the electrochemical device to ensure that the electrochemical performance of the positive electrode sheet and the electrochemical device can achieve the expected effect.
[0103] In some embodiments, the positive electrode sheet satisfies 2≤R×P / Q≤36, RΩ is the single-sided resistance of the positive electrode sheet, P g / cm 3 is the compaction density of the positive electrode sheet, Q g / 1540.25mm 2 is the single-surface density of the positive electrode sheet. For example, R×P / Q is 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, 31, 32, 33, 34, 35, 36 or any range thereof.
[0104] Optionally, the positive electrode sheet satisfies 3≤R×P / Q≤36, 4≤R×P / Q≤36, 5≤R×P / Q≤36, 6≤R×P / Q≤36, 7≤R×P / Q≤36, 8≤R×P / Q≤36, 2≤R×P / Q≤32, 3≤R×P / Q≤32, 4≤R×P / Q≤32, 5≤R×P / Q≤32, 6≤R×P / Q≤32, 7≤R×P / Q≤32, 8≤R×P / Q≤32, 2≤R×P / Q≤28, 3≤R×P / Q≤28, 4≤R×P / Q≤28, 5≤R×P / Q≤28, 6≤R×P / Q≤28, 7≤R×P / Q≤28, 8≤R×P / Q≤28, 2≤R×P / Q≤24, 3≤R×P / Q≤24, 4≤R×P / Q≤24, 5≤R×P / Q≤24, 6≤R×P / Q≤24, 7≤R×P / Q≤24, 8≤R×P / Q≤24, 2≤R×P / Q≤20, 3≤R×P / Q≤20, 4≤R×P / Q≤20, 5≤R×P / Q≤20, 6≤R×P / Q≤20, 7≤R×P / Q≤20, or 8≤R×P / Q≤20.
[0105] By reasonably designing the single-sided resistance, compaction density, and single-sided surface density of the positive electrode sheet, the energy density, rate performance, and cycle performance of the electrochemical device can be further improved. Therefore, the electrochemical device using the positive electrode sheet of this application can simultaneously have a high energy density, a long cycle life, and good rate performance.
[0106] It should be noted that the calculation of R×P / Q only involves numerical calculations. For example, the single-sided resistance RΩ of the positive electrode sheet is 1.0Ω, and the compaction density P g / cm 3 is 4.2 g / cm 3 , and the single-sided surface density Q g / 1540.25mm 2 is 0.26 g / 1540.25mm 2 , then R×P / Q = 1.0×4.2 / 0.26 = 16.15.
[0107] In some embodiments, the single-sided resistance of the positive electrode sheet is RΩ, and R≤3. For example, R≤2.5, ≤2.0, ≤1.5, or ≤1.0. When the single-sided resistance of the positive electrode sheet is within a suitable range, it is beneficial to further improve the cycle performance and rate performance of the electrochemical device.
[0108] In some embodiments, the compaction density of the positive electrode sheet is P g / cm 3 , and 4.0≤P≤4.3. When the compaction density of the positive electrode sheet is within a suitable range, it is beneficial to the migration of electrons and lithium ions, thereby further improving the cycle performance of the electrochemical device, and at the same time, the electrochemical device also has a high energy density.
[0109] In some embodiments, the single-sided surface density of the positive electrode sheet is Q g / 1540.25mm 2 , and 0.16≤Q≤0.38. For example, Q is a range composed of 0.16, 0.18, 0.20, 0.22, 0.24, 0.26, 0.28, 0.30, 0.32, 0.34, 0.36, 0.38 or any value above. Optionally, 0.16 < Q < 0.38. When the single-sided surface density of the positive electrode sheet is within a suitable range, the electrochemical device can have further improved cycle performance and rate performance on the premise of having a high charge-discharge capacity.
[0110] In some embodiments, the positive electrode film layer may further include a conductive agent and a binder. The specific types of the conductive agent and the binder are not subject to specific restrictions and can be selected according to demand. As an example, the conductive agent includes but is not limited to at least one of conductive graphite, superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene and carbon nanofibers. As an example, the binder includes but is not limited to at least one of styrene-butadiene rubber (SBR), water-based acrylic resin (Water basedacrylic resin), carboxymethyl cellulose (CMC), polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), polyvinyl butyral (PVB), ethylene-vinyl acetate copolymer (EVA) and polyvinyl alcohol (PVA).
[0111] In some embodiments, based on the total mass of the positive electrode film layer, the mass percentage of the conductive agent is ≥0.5%. For example, the mass percentage of the conductive agent is 0.5%, 1.0%, 1.5%, 2.0%, 2.5%, 3.0%, 3.5%, 4.0%, 4.5%, 5.0%, 6.0%, 7.0%, 8.0%, 9.0%, 10.0%, 11.0%, 12.0%, 13.0%, 14.0%, 15.0%, 16.0%, 17.0%, 18.0% or any range consisting of the above values. Optionally, the mass percentage of the conductive agent is 0.5% to 18%. Further, the mass percentage of the conductive agent is 0.5% to 5%. When the mass percentage of the conductive agent is within a suitable range, it is beneficial to obtain a lower single-sided resistance of the positive electrode sheet.
[0112] In some embodiments, based on the total mass of the positive electrode film layer, the mass percentage of the binder is ≤2.0%. When the mass percentage of the binder is within a suitable range, it is beneficial to obtain a lower single-surface resistance of the positive electrode sheet.
[0113] In some embodiments, the positive electrode current collector may be a metal foil or a porous metal plate, such as a foil or a porous plate made of a metal such as aluminum, copper, nickel, titanium, silver, or an alloy thereof. As an example, the positive electrode current collector is aluminum foil.
[0114] In some embodiments, the thickness of the positive electrode current collector is 5 μm to 20 μm. For example, the thickness of the positive electrode current collector is 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, 11 μm, 12 μm, 13 μm, 14 μm, 15 μm, 16 μm, 17 μm, 18 μm, 19 μm, 20 μm or any range consisting of the above values. Optionally, the thickness of the positive electrode current collector is 6 μm to 18 μm. Further, the thickness of the positive electrode current collector is 8 μm to 16 μm.
[0115] In some embodiments, the positive electrode current collector has two surfaces opposite to each other in the thickness direction thereof, and the positive electrode film layer is disposed on any one or both of the two opposite surfaces of the positive electrode current collector. When the positive electrode film layer is disposed on both surfaces of the positive electrode current collector, the parameters of the positive electrode film layer on any one of the surfaces satisfy the parameter range of the present application, that is, it is considered to fall within the protection scope of the present application.
[0116] The first positive electrode active material can be prepared according to conventional methods in the art. An exemplary test method is as follows: a lithium source, a cobalt source, an M1 element precursor, and an A element precursor are mixed and sintered to obtain a first positive electrode active material. The sintering atmosphere may be an oxygen-containing atmosphere, for example, an air atmosphere or an oxygen atmosphere. The O2 concentration of the sintering atmosphere is, for example, 70% to 100%. The sintering temperature and sintering time can be adjusted according to actual conditions, for example, the sintering temperature is 700°C to 1000°C, and the sintering time is 8h to 24h.
[0117] As an example, the lithium source includes but is not limited to at least one of lithium oxide (Li2O), lithium phosphate (Li3PO4), lithium dihydrogen phosphate (LiH2PO4), lithium acetate (CH3COOLi), lithium hydroxide (LiOH), lithium carbonate (Li2CO3) and lithium nitrate (LiNO3). As an example, the cobalt source includes but is not limited to at least one of cobalt sulfate, cobalt nitrate, cobalt chloride, cobalt oxalate and cobalt acetate. As an example, the M1 element precursor includes but is not limited to at least one of the oxide, nitrate compound, carbonate compound, hydroxide and acetate compound of the M1 element. As an example, the A element precursor includes but is not limited to at least one of ammonium fluoride, lithium fluoride, hydrogen fluoride, ammonium chloride, lithium chloride, hydrogen chloride, ammonium bromide, lithium bromide, hydrogen bromide, ammonium nitrate, ammonium nitrite, ammonium carbonate, ammonium bicarbonate, ammonium sulfate, ammonium bisulfate, ammonium bisulfite, ammonium sulfite, ammonium hydrogen sulfide, hydrogen sulfide, lithium sulfide, ammonium sulfide and elemental sulfur.
[0118] The second positive electrode active material can be prepared according to conventional methods in the art. An exemplary test method is as follows: a lithium source, a nickel source, a copper source, a titanium source, an M2 element precursor, and a B element precursor are mixed and sintered to obtain a second positive electrode active material. The sintering atmosphere may be an inert atmosphere, for example, a nitrogen atmosphere or an argon atmosphere. The sintering temperature and sintering time may be adjusted according to actual conditions, for example, the sintering temperature is 500°C to 800°C, and the sintering time is 8h to 24h.
[0119] As an example, the lithium source includes but is not limited to at least one of lithium oxide (Li2O), lithium phosphate (Li3PO4), lithium dihydrogen phosphate (LiH2PO4), lithium acetate (CH3COOLi), lithium hydroxide (LiOH), lithium carbonate (Li2CO3) and lithium nitrate (LiNO3). As an example, the nickel source includes but is not limited to at least one of nickel sulfate, nickel nitrate, nickel chloride, nickel oxalate and nickel acetate. As an example, the copper source includes but is not limited to at least one of copper sulfate, copper nitrate, copper chloride, copper oxalate and copper acetate. As an example, the titanium source includes but is not limited to at least one of titanium sulfate, titanium nitrate, titanium chloride, titanium oxalate and titanium acetate. As an example, the M2 element precursor includes but is not limited to at least one of the oxide, nitric acid compound, carbonate compound, hydroxide and acetate compound of the M2 element. As an example, the precursor of element B includes but is not limited to at least one of ammonium fluoride, lithium fluoride, hydrogen fluoride, ammonium chloride, lithium chloride, hydrogen chloride, ammonium bromide, lithium bromide, hydrogen bromide, ammonium nitrate, ammonium nitrite, ammonium carbonate, ammonium bicarbonate, ammonium sulfate, ammonium bisulfate, ammonium bisulfite, ammonium sulfite, ammonium bisulfide, hydrogen sulfide, lithium sulfide, ammonium sulfide and elemental sulfur.
[0120] The positive electrode sheet can be prepared according to conventional methods in the art. Usually, the first positive electrode active material, the second positive electrode active material, and the optional conductive agent and binder are dispersed in a solvent, and the solvent can be N-methylpyrrolidone (NMP) to form a uniform positive electrode slurry, and the positive electrode slurry is coated on the positive electrode current collector, and the positive electrode sheet is obtained through drying, cold pressing and other processes.
[0121] The positive electrode sheet of the present application does not exclude other positive electrode active materials in addition to the first positive electrode active material and the second positive electrode active material. The specific types of other positive electrode active materials are not subject to specific restrictions and can be selected according to needs. As an example, other positive electrode active materials include but are not limited to lithium iron phosphate, a composite material of lithium iron phosphate and carbon, lithium manganese phosphate, a composite material of lithium manganese phosphate and carbon, lithium iron manganese phosphate, a composite material of lithium iron manganese phosphate and carbon, and at least one of their respective modified compounds.
[0122] The positive electrode sheet of the present application does not exclude other additional functional layers in addition to the positive electrode film layer. For example, in some embodiments, the positive electrode sheet of the present application also includes a conductive primer layer (for example, composed of a conductive agent and a binder) sandwiched between the positive electrode collector and the positive electrode film layer and disposed on the surface of the positive electrode collector. In other embodiments, the positive electrode sheet of the present application also includes a protective layer covering the surface of the positive electrode film layer.
[0123] The single-sided resistance of the positive electrode sheet is a well-known meaning in the art and can be measured using instruments and methods known in the art. For example, the single-sided resistance of the positive electrode sheet is tested using a DC two-probe method. An exemplary test method is as follows: Take a single-sided coated and cold-pressed positive electrode sheet (if it is a double-sided coated positive electrode sheet, the positive electrode film layer on one side can be wiped off first) and clamp it in parallel between the two conductive terminals of an internal resistance tester (for example, Hioki BT23562 internal resistance tester), apply a certain pressure to fix it, and obtain the single-sided resistance of the positive electrode sheet. The diameter of the conductive terminal can be 14 mm, and the applied pressure can be 15 MPa to 27 MPa.
[0124] During the test, the positive electrode sheet can be cut into a certain area (for example, 10 cm×10 cm) before the test.
[0125] During the test, the positive electrode film layer on one side of the positive electrode plate can be wiped off by using water or other solvents.
[0126] The compaction density of the positive electrode sheet is well known in the art and can be measured using instruments and methods known in the art. For example, it can be calculated using the formula P = m / v, P (g / cm 3 ) is the compaction density of the positive electrode sheet, m (g) is the mass of the positive electrode film, v (cm 3 ) is the volume of the positive electrode film layer. The volume of the positive electrode film layer = the area of the positive electrode film layer × the thickness of the positive electrode film layer.
[0127] The single-surface density of the positive electrode sheet is well known in the art and can be measured using instruments and methods known in the art. For example, it can be calculated using the formula Q = 1540.25 × m / Ar, Q (g / 1540.25 mm 2 ) is the single-surface density of the positive electrode sheet, m (g) is the mass of the positive electrode film, Ar (mm 2 ) is the area of the positive electrode film layer.
[0128] As an example, the quality test method of the positive electrode film layer is as follows: take a single-sided coated and cold-pressed positive electrode sheet (if it is a double-sided coated positive electrode sheet, the positive electrode film layer on one side can be wiped off first), weigh its mass, and record it as m1 (g); wipe off the positive electrode film layer of the above-weighed positive electrode sheet, weigh the mass of the positive electrode current collector, and record it as m0 (g); the mass of the positive electrode film layer is calculated by the formula m=m1-m0.
[0129] It should be noted that when the parameters of the positive electrode sheet of the present application (including the single-sided resistance, compaction density and single-sided surface density of the positive electrode sheet, etc.) are tested, the positive electrode sheet can be directly taken from a freshly prepared cold-pressed positive electrode sheet, or a positive electrode sheet can be obtained from an electrochemical device. If it is a double-sided coated positive electrode sheet, the positive electrode film layer on one side can be wiped off first, for example, by using water or other solvents to wipe off the positive electrode film layer on one side of the positive electrode sheet.
[0130] An exemplary method for obtaining a positive electrode sheet from an electrochemical device is as follows: disassemble the positive electrode sheet after fully discharging the electrochemical device, soak the positive electrode sheet in an organic solvent (e.g., dimethyl carbonate) for a period of time (e.g., 30 minutes), and then take out the positive electrode sheet and dry it at a certain temperature and time (e.g., 80°C, 6 hours).
[0131] Electrochemical Devices
[0132] The second aspect of the embodiment of the present application provides an electrochemical device, including any device in which an electrochemical reaction occurs to convert chemical energy into electrical energy, and its specific examples include all kinds of lithium primary batteries or lithium secondary batteries. In particular, lithium secondary batteries include lithium metal secondary batteries, lithium ion secondary batteries, lithium polymer secondary batteries or lithium ion polymer secondary batteries.
[0133] In some embodiments, the electrochemical device of the present application includes a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte.
[0134] In some embodiments, the positive electrode sheet, the negative electrode sheet, and the separator may be formed into an electrode assembly by a winding process or a lamination process.
[0135] The electrochemical device of the present application also includes an outer package for packaging the electrode assembly and the electrolyte. In some embodiments, the outer package can be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc., or a soft package, such as a bag-type soft package. The material of the soft package can be plastic, such as at least one of polypropylene (PP), polybutylene terephthalate (PBT), and polybutylene succinate (PBS).
[0136] [Positive electrode]
[0137] The positive electrode sheet used in the electrochemical device of the present application is the positive electrode sheet of the first aspect of the embodiment of the present application.
[0138] [Negative electrode]
[0139] The material, composition and manufacturing method of the negative electrode sheet used in the electrochemical device of the present application may include any technology known in the prior art.
[0140] The negative electrode sheet can be a metal lithium sheet, or an electrode sheet including a negative electrode current collector and a negative electrode film layer disposed on at least one surface of the negative electrode current collector. The negative electrode film layer generally includes a negative electrode active material and optional conductive agent, binder and thickener.
[0141] The specific type of the negative electrode active material is not subject to specific restrictions and can be selected according to needs. As an example, the negative electrode active material includes but is not limited to natural graphite, artificial graphite, mesophase microcarbon beads (MCMB), hard carbon, soft carbon, silicon, silicon-carbon composite, SiO, Li-Sn alloy, Li-Sn-O alloy, Sn, SnO, SnO2, spinel structured Li4Ti5O 12 , Li-Al alloy.
[0142] The specific type of the conductive agent is not subject to specific restrictions and can be selected according to needs. As an example, the conductive agent includes but is not limited to at least one of conductive graphite, superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene and carbon nanofibers.
[0143] The specific type of the binder is not subject to specific restrictions and can be selected according to needs. As an example, the binder includes but is not limited to at least one of styrene-butadiene rubber (SBR), polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), polyvinyl butyral (PVB), water-based acrylic resin and carboxymethyl cellulose.
[0144] The specific type of thickener is not subject to specific restrictions and can be selected according to needs. As an example, the thickener includes but is not limited to sodium carboxymethylcellulose (CMC).
[0145] However, the present application is not limited to the above materials, and the negative electrode plate of the present application may also use other known materials that can be used as negative electrode active materials, conductive agents, binders and thickeners.
[0146] In some embodiments, the negative electrode current collector has two surfaces opposite to each other in the thickness direction thereof, and the negative electrode film layer is disposed on any one or both of the two opposite surfaces of the negative electrode current collector.
[0147] The negative electrode current collector may be made of a metal foil or a porous metal plate, for example, a foil or a porous plate made of a metal such as copper, nickel, titanium, iron, or an alloy thereof. As an example, the negative electrode current collector is a copper foil.
[0148] The negative electrode sheet can be prepared according to conventional methods in the art. Usually, the negative electrode active material and optional conductive agent, binder and thickener are dispersed in a solvent, and the solvent can be N-methylpyrrolidone (NMP) or deionized water to form a uniform negative electrode slurry, and the negative electrode slurry is coated on the negative electrode current collector, and the negative electrode sheet is obtained through drying, cold pressing and other processes.
[0149] The negative electrode plate of the present application does not exclude other additional functional layers besides the negative electrode film layer. For example, in some embodiments, the negative electrode plate of the present application also includes a conductive primer layer (e.g., composed of a conductive agent and a binder) sandwiched between the negative electrode current collector and the negative electrode film layer and disposed on the surface of the negative electrode current collector. In other embodiments, the negative electrode plate of the present application also includes a protective layer covering the surface of the negative electrode film layer.
[0150] [Electrolyte]
[0151] The electrolyte plays a role in conducting active ions between the positive electrode plate and the negative electrode plate. The electrolyte that can be used in the electrochemical device of the present application can be an electrolyte known in the prior art.
[0152] In some embodiments, the electrolyte includes an organic solvent, a lithium salt, and optional additives. The types of the organic solvent, the lithium salt, and the additives are not subject to specific restrictions and can be selected according to requirements.
[0153] In some embodiments, as an example, the lithium salt includes but is not limited to at least one of LiPF6 (lithium hexafluorophosphate), LiBF4 (lithium tetrafluoroborate), LiClO4 (lithium perchlorate), LiAsF6 (lithium hexafluoroarsenate), LiFSI (lithium bisfluorosulfonyl imide), LiTFSI (lithium bistrifluoromethanesulfonyl imide), LiTFS (lithium trifluoromethanesulfonate), LiDFOB (lithium difluorooxalate borate), LiBOB (lithium dioxalate borate), LiPO2F2 (lithium difluorophosphate), LiDFOP (lithium difluorobisoxalate phosphate) and LiTFOP (lithium tetrafluorooxalate phosphate). The above lithium salts can be used alone or in combination of two or more.
[0154] In some embodiments, as an example, the organic solvent includes but is not limited to ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butylene carbonate (BC), fluoroethylene carbonate (FEC), methyl formate (MF), methyl acetate (MA), ethyl acetate (EA), propyl acetate (PA), methyl propionate (MP), ethyl propionate (EP), propyl propionate (PP), methyl butyrate (MB), ethyl butyrate (EB), 1,4-butyrolactone (GBL), cyclopentane (SF), dimethyl sulfone (MSM), methyl ethyl sulfone (EMS) and diethyl sulfone (ESE) At least one. The above organic solvents can be used alone or in combination. Alternatively, two or more of the above organic solvents are used in combination.
[0155] In some embodiments, the additive includes but is not limited to anode film-forming additives. As an example, the additive includes but is not limited to at least one of fluoroethylene carbonate (FEC), vinylene carbonate (VC), vinyl carbonate (VEC), diethylene sulfate (DTD), propylene sulfate, vinyl sulfite (ES), 1,3-propane sultone (PS), 1,3-propylene sultone (PST), sulfonate cyclic quaternary ammonium salt, succinic anhydride, succinonitrile (SN), adiponitrile (AND), tris(trimethylsilyl) phosphate (TMSP), and tris(trimethylsilyl) borate (TMSB).
[0156] Based on the total mass of the electrolyte, the total mass percentage of the additives is 0% to 15%. Optionally, the total mass percentage of the additives is 0.5% to 15%.
[0157] In some embodiments, the additive includes at least fluoroethylene carbonate (FEC).
[0158] During the first cycle of charge and discharge of the electrochemical device, a large amount of active lithium released from the second positive electrode material is embedded in the negative electrode active material, which further reduces the real potential of the negative electrode. The organic solvent in the electrolyte is more likely to undergo a reduction reaction at the negative electrode, causing the SEI film thickness on the surface of the negative electrode active material to continue to increase and the negative electrode impedance to continue to grow, thereby affecting the cycle performance of the electrochemical device. Fluoroethylene carbonate can undergo a reduction reaction at the negative electrode in priority to the organic solvent and form a uniform and dense SEI film, inhibiting the organic solvent from continuously undergoing a reduction reaction at the negative electrode, inhibiting the SEI film thickness on the surface of the negative electrode active material to continue to increase and the negative electrode impedance to continue to grow; fluoroethylene carbonate can also form a synergistic effect with the second positive electrode active material, which is beneficial to the formation of a LiF-rich and uniform and dense SEI film on the surface of the negative electrode active material after the first cycle of charge and discharge of the electrochemical device, thereby reducing the continuous loss of active lithium. At the same time, fluoroethylene carbonate is more resistant to high-voltage oxidation at the positive electrode, which is beneficial to matching high-voltage positive electrode active materials, thereby further improving the energy density and cycle performance of the electrochemical device, especially the cycle performance under high voltage.
[0159] Therefore, when the electrolyte of the present application contains fluoroethylene carbonate, it is conducive to the formation of a more uniform, dense and thin SEI film after the first cycle of charge and discharge of the electrochemical device, preventing the organic solvent from continuously undergoing reduction reaction at the negative electrode, thereby compensating for the irreversible loss of active lithium caused by the formation of the SEI film, while also forming a more uniform and dense SEI film on the surface of the negative electrode active material, reducing the continuous loss of active lithium. Therefore, the electrochemical device of the present application can have high energy density, long cycle life and good rate performance at the same time.
[0160] Based on the gross mass of described electrolyte, the mass percentage composition of fluoroethylene carbonate is 0% to 15%.For example, the mass percentage composition of fluoroethylene carbonate is 0%, 0.1%, 0.2%, 0.5%, 1.0%, 1.5%, 2.0%, 2.5%, 3.0%, 3.5%, 4.0%, 4.5%, 5.0%, 6.0%, 7.0%, 8.0%, 9.0%, 10%, 11%, 12%, 13%, 14%, 15% or the scope that any above numerical value forms.Alternatively, the mass percentage composition of fluoroethylene carbonate is 0.5% to 15%.Further, the mass percentage composition of fluoroethylene carbonate is 0.5% to 5%.
[0161] The electrolyte can be prepared according to conventional methods in the art. For example, an organic solvent, a lithium salt, and an optional additive can be mixed evenly to obtain an electrolyte. There is no particular restriction on the order of adding the materials. For example, a lithium salt and an optional additive are added to an organic solvent and mixed evenly to obtain an electrolyte; or, a lithium salt is first added to an organic solvent, and then the optional additive is added to the organic solvent and mixed evenly to obtain an electrolyte.
[0162] [Isolation film]
[0163] The separator is disposed between the positive electrode and the negative electrode, and mainly plays the role of preventing the positive and negative electrodes from short-circuiting, while allowing active ions to pass through. The present application has no particular restrictions on the type of separator, and any known porous structure separator with good chemical stability and mechanical stability can be selected. The separator can be a single-layer film or a multi-layer composite film. When the separator is a multi-layer composite film, the materials of each layer can be the same or different.
[0164] In some embodiments, the isolation film includes a polymer or an inorganic substance formed of a material that is stable to the electrolyte of the present application.
[0165] For example, the isolation film may include a substrate layer and an optional surface treatment layer. The substrate layer is a non-woven fabric, a film or a composite film having a porous structure, and the material of the substrate layer includes at least one of polyethylene, polypropylene, polyethylene terephthalate and polyimide. As an example, a polypropylene porous film, a polyethylene porous film, a polypropylene non-woven fabric, a polyethylene non-woven fabric or a polypropylene-polyethylene-polypropylene porous composite film may be used.
[0166] The surface of the substrate layer may or may not be provided with a surface treatment layer. In some embodiments, at least one surface of the substrate layer is provided with a surface treatment layer, which may be a polymer layer or an inorganic layer, or a layer formed by a mixed polymer and an inorganic material.
[0167] The inorganic layer includes inorganic particles and a binder, wherein the inorganic particles include at least one of aluminum oxide, silicon oxide, magnesium oxide, titanium oxide, hafnium dioxide, tin oxide, cerium dioxide, nickel oxide, zinc oxide, calcium oxide, zirconium oxide, yttrium oxide, silicon carbide, boehmite, aluminum hydroxide, magnesium hydroxide, calcium hydroxide, and barium sulfate. The binder includes at least one of polyvinylidene fluoride, a copolymer of vinylidene fluoride and hexafluoropropylene, polyamide, polyacrylonitrile, polyacrylate, polyacrylic acid, polyacrylate, polyvinylpyrrolidone, polyvinyl ether, polymethyl methacrylate, polytetrafluoroethylene, and polyhexafluoropropylene.
[0168] The polymer layer contains polymers, and the polymer material includes at least one of polyamide, polyacrylonitrile, acrylate polymer, polyacrylic acid, polyacrylate, polyvinylpyrrolidone, polyvinyl ether, polyvinylidene fluoride, and poly(vinylidene fluoride-hexafluoropropylene).
[0169] Electronic Devices
[0170] A third aspect of the embodiments of the present application provides an electronic device, which includes the electrochemical device of the second aspect of the embodiments of the present application.
[0171] The electronic device of the present application is not particularly limited, and it can be used for any electronic device known in the prior art. In some embodiments, the electronic device can include, but is not limited to, a laptop computer, a pen-input computer, a mobile computer, an electronic book player, a portable phone, a portable fax machine, a portable copier, a portable printer, a head-mounted stereo headset, a video recorder, an LCD television, a portable cleaner, a portable CD player, a mini-disc, a transceiver, an electronic notepad, a calculator, a memory card, a portable recorder, a radio, a backup power supply, a motor, a car, a motorcycle, a power-assisted bicycle, a bicycle, a lighting fixture, a toy, a game console, a clock, an electric tool, a flashlight, a camera, a large household battery and a lithium-ion capacitor, etc.
[0172] Example
[0173] The following examples describe the disclosure of the present invention in more detail, and these examples are intended for illustrative purposes only, as various modifications and variations within the scope of the disclosure of the present invention are apparent to those skilled in the art. Unless otherwise stated, all parts, percentages, and ratios reported in the following examples are by mass, and all reagents used in the examples are commercially available or synthesized according to conventional methods and can be used directly without further processing, and the instruments used in the examples are commercially available.
[0174] Example 1
[0175] Preparation of positive electrode
[0176] The first positive electrode active material LiCoO2 and the second positive electrode active material Li2Ni 0.498 Cu 0.498 Ti 0.002 O2, binder PVDF, and conductive agent carbon black are mixed in a mass ratio of 92.6:5.0:1.3:1.1, and an appropriate amount of solvent NMP is added, and the positive electrode slurry is obtained under the action of a vacuum mixer; the positive electrode slurry is evenly coated on the two surfaces of the positive electrode current collector aluminum foil; and then dried in a 120°C oven, cold pressed, cut, etc. to obtain the positive electrode sheet.
[0177] Preparation of negative electrode
[0178] The negative electrode active materials artificial graphite and silicon oxide, the binder polyacrylic acid (PAA), and the conductive agent carbon black are mixed in a mass ratio of 85.9:10.0:2.8:1.3, and an appropriate amount of solvent deionized water is added to obtain the negative electrode slurry under the action of a vacuum mixer; the negative electrode slurry is evenly coated on the two surfaces of the negative electrode collector copper foil; and then dried in a 120°C oven, cold pressed, cut, etc. to obtain the negative electrode sheet.
[0179] Preparation of electrolyte
[0180] Ethylene carbonate (EC), ethyl methyl carbonate (EMC) and diethyl carbonate (DEC) are mixed in a volume ratio of 1:1:1 to obtain an organic solvent; LiPF6 is dissolved in the organic solvent, and then fluoroethylene carbonate (FEC) is added and mixed evenly to obtain an electrolyte. The concentration of LiPF6 is 1 mol / L, and the mass percentage of fluoroethylene carbonate is 5% based on the total mass of the electrolyte.
[0181] Preparation of isolation membrane
[0182] A porous polypropylene film (from Celgard Corporation) having a thickness of 14 μm was used as a separator.
[0183] Preparation of lithium-ion secondary batteries
[0184] The positive electrode sheet, the separator, and the negative electrode sheet are stacked and wound in order to obtain an electrode assembly, the electrode assembly is placed in an outer package, the above-mentioned electrolyte is added, and after packaging, standing, forming, shaping and other processes, a lithium-ion secondary battery is obtained.
[0185] Examples 2 to 28 and Comparative Examples 1 to 5
[0186] The preparation method of the lithium ion secondary battery is similar to that of Example 1, except that the relevant parameters in the preparation of the positive electrode plate and the electrolyte are adjusted. The specific parameters are shown in Table 1, and “ / ” indicates that the corresponding component is not added.
[0187] Table 1
[0188]
[0189]
[0190] Test Section
[0191] The single-sided resistance of the positive electrode sheet, the compaction density of the positive electrode sheet and the single-sided surface density test of the positive electrode sheet can be tested according to the method described above in this specification.
[0192] (1) High temperature cycle performance test of lithium-ion secondary batteries
[0193] At 45°C, charge the lithium-ion secondary battery to 4.5V at a constant current of 1.5C, and continue to charge at a constant voltage until the current is less than or equal to 0.05C. At this time, the lithium-ion secondary battery is fully charged. Record the charging capacity at this time, which is the charging capacity of the first cycle; after the lithium-ion secondary battery is left to stand for 5 minutes, discharge it to 3.0V at a constant current of 1C. This is a cyclic charge and discharge process. Record the discharge capacity at this time, which is the discharge capacity of the first cycle. Perform a cyclic charge and discharge test on the lithium-ion secondary battery according to the above method, and record the discharge capacity after each cycle until the discharge capacity of the lithium-ion secondary battery decays to 80% of the discharge capacity of the first cycle. The number of cycles at this time is used to characterize the cycle performance of the lithium-ion secondary battery. The higher the number of cycles of the lithium-ion secondary battery, the better the cycle performance.
[0194] (2) Rate performance test of lithium-ion secondary batteries
[0195] At 25°C, the lithium-ion secondary battery was charged at a constant current of 0.2C to 4.5V, and then continued to be charged at a constant voltage until the current was less than or equal to 0.05C. After the lithium-ion secondary battery was allowed to stand for 5 minutes, it was discharged at a constant current of 0.2C to 3.0V, and the discharge capacity at the 0.2C rate was recorded.
[0196] At 25°C, the lithium-ion secondary battery was charged at a constant current of 0.2C to 4.5V, and then continued to be charged at a constant voltage until the current was less than or equal to 0.05C. After the lithium-ion secondary battery was allowed to stand for 5 minutes, it was discharged at a constant current of 2C to 3.0V, and the discharge capacity at the 2C rate was recorded.
[0197] Lithium ion secondary battery 2C / 0.2C discharge capacity retention rate (%)=2C rate discharge capacity / 0.2C rate discharge capacity×100%.
[0198] Table 2 gives the performance test results of Examples 1 to 28 and Comparative Examples 1 to 5.
[0199] Table 2
[0200]
[0201]
[0202] Figure 1 is the X-ray diffraction spectrum of the second positive electrode active material of Example 1 measured after the first cycle of charging, referring to Figure 1, the second positive electrode active material has a lower first cycle coulombic efficiency, and the second positive electrode active material has characteristic diffraction peaks at 2θ values of 36° to 38°, 42° to 44°, and 62° to 64° after the first cycle of charging. From the test results in Table 2, it can be seen that the positive electrode sheet of the present application can give full play to the synergistic effect between the first positive electrode active material and the second positive electrode active material, and effectively compensate for the irreversible loss of active lithium caused by the formation of SEI film on the surface of the negative electrode active material, thereby improving the energy density of the lithium ion secondary battery and improving the cycle performance of the lithium ion secondary battery.
[0203] It can also be seen from the test results in Table 2 that by reasonably designing the single-sided resistance, compaction density and single-sided surface density of the positive electrode sheet, so that the positive electrode sheet satisfies 2≤R×P / Q≤36, the rate performance and cycle performance of the lithium-ion secondary battery can be further improved, so that the lithium-ion secondary battery can have high energy density, long cycle life and good rate performance at the same time.
[0204] It can also be seen from the test results in Table 2 that when the electrolyte contains fluoroethylene carbonate, it is beneficial to form a more uniform, dense and thin SEI film after the first cycle of charge and discharge of the lithium-ion secondary battery, preventing the organic solvent from continuously undergoing reduction reaction at the negative electrode, thereby further improving the cycle performance of the lithium-ion secondary battery.
[0205] The above is only a specific implementation of the present application, but the protection scope of the present application is not limited thereto. Any technician familiar with the technical field can easily think of various equivalent modifications or replacements within the technical scope disclosed in the present application, and these modifications or replacements should be included in the protection scope of the present application. Therefore, the protection scope of the present application shall be based on the protection scope of the claims.
Claims
1. A positive electrode sheet, characterized in that: Comprising: A positive electrode film layer, the positive electrode film layer comprising a first positive electrode active material represented by Chemical Formula 1 and a second positive electrode active material represented by Chemical Formula 2. Based on the total mass of the positive electrode film layer, the mass percentage of the first positive electrode active material is 80% to 98%. Li 1+x Co y M1 1-y O 2-z A z Chemical formula 1 Li 2+r Ni p Cu q Ti u M2 v O 2-s B s Chemical formula 2 Wherein, -0.1 ≤ x ≤ 0.2, 0.8 ≤ y ≤ 1, 0 ≤ z ≤ 0.2, M1 comprises at least one of Ni, Mn, Al, Mg, Ti, Zr, La, Y, Fe, Cr, V, Zn, Ru, Rh, Ga, Pd, Pt, Mo, W, Sb, Nb, Se, Te, Ce, A comprises at least one of S, N, P, F, Cl, Br. -0.2 ≤ r ≤ 0.2, 0 < p < 1, 0 < q < 1, 0 < u ≤ 0.01, 0 ≤ v ≤ 0.2, 0 < p + q + u + v ≤ 1, 0 ≤ s < 0.2, M2 comprises at least one of Mn, Fe, Co, Al, V, Cr, Nb, Mg, Zr, La, Y, Zn, Ru, Rh, Ga, Pd, Pt, Mo, W, Sb, Nb, Se, Te, Ce, B comprises at least one of S, N, P, F, Cl, Br.
2. The positive electrode sheet according to claim 1, characterized in that: The first positive electrode active material satisfies at least one of conditions (1) to (5): (1)-0.05≤x≤0.1, (2)0.8≤y<1, (3)0<z≤0.2, (4) M1 comprises at least one of Ni, Mn, Al, Mg, Ti, Zr, La, Y, Fe, Cr, V, Zn, Rh. (5) A comprises at least one of S, F.
3. The positive electrode sheet according to claim 1 or 2, characterized in that: The second positive electrode active material satisfies at least one of conditions (6) to (13): (6)-0.1≤r≤0.1, (7)0.39≤p<0.5, (8)0.39≤q<0.5, (9)0<u≤0.005, (10)0<v≤0.2, (11)0<s<0.2, (12) M2 comprises at least one of Mn, Fe, Co, Al, V, Cr, Nb, Mg, Zr, Zn. (13) B comprises at least one of S, F.
4. The positive electrode sheet according to claim 1, characterized in that: The mass ratio of the first positive electrode active material to the second positive electrode active material is 5:1 to 99:
1.
5. The positive electrode sheet according to claim 4, characterized in that: The mass ratio of the first positive electrode active material to the second positive electrode active material is 9:1 to 99:
1.
6. The positive electrode sheet according to claim 4, characterized in that: Based on the total mass of the positive electrode film layer, the mass percentage of the first positive electrode active material is 85% to 98%.
7. The positive electrode sheet according to claim 1, characterized in that: The positive electrode sheet satisfies 2≤R×P / Q≤36, RΩ is the single-sided resistance of the positive electrode sheet, P g / cm 3 is the compaction density of the positive electrode sheet, Q g / 1540.25mm 2 is the single-sided surface density of the positive electrode plate.
8. The positive electrode sheet according to claim 7, characterized in that: 5 ≤ R × P / Q ≤ 32.
9. The positive electrode sheet according to claim 1, characterized in that: The single-sided resistance of the positive electrode tab is R Ω, R ≤ 3.
10. The positive electrode sheet according to claim 9, characterized in that: R≤1.5。 11. The positive electrode sheet according to claim 1, characterized in that: The compaction density of the positive electrode sheet is P g / cm 3 , 4.0≤P≤4.
3.
12. The positive electrode sheet according to claim 1, characterized in that: The single-sided surface density of the positive electrode sheet is Q g / 1540.25 mm 2 , 0.16≤Q≤0.
38.
13. The positive electrode sheet according to claim 1, characterized in that: The second positive electrode active material belongs to the Immm space group.
14. The positive electrode sheet according to claim 1, characterized in that: In the X-ray diffraction spectrum measured after the first charge of the second positive electrode active material, characteristic diffraction peaks are present at positions where 2θ values are 36° to 38°, 42° to 44°, and 62° to 64°.
15. An electrochemical device, characterized in that: Comprising: The positive electrode tab according to any one of claims 1 to 14.
16. The electrochemical device according to claim 15, characterized in that Further comprising an electrolytic solution, the electrolytic solution comprising a negative electrode film-forming additive. Based on the total mass of the electrolytic solution, the mass percentage of the additive is 0% to 15%.
17. The electrochemical device according to claim 16, characterized in that The mass percentage of the additive is 0.5% to 15%.
18. The electrochemical device according to claim 16, characterized in that The additive includes at least one of fluoroethylene carbonate, vinylene carbonate, vinyl carbonate, vinyl sulfate, propylene sulfate, vinyl sulfite, 1,3-propane sultone, 1,3-propylene sultone, sulfonate cyclic quaternary ammonium salt, succinic anhydride, succinonitrile, adiponitrile, tris(trimethylsilyl)phosphate, and tris(trimethylsilyl)borate.
19. The electrochemical device according to claim 18, characterized in that The additive includes at least fluoroethylene carbonate.
20. An electronic device, characterized in that: Comprising an electrochemical device according to any one of claims 15 to 19.
Citation Information
Patent Citations
Lithium ion secondary battery, positive electrode active material, positive electrode, and electrical tool
CN102569878A
Ti-doped nickel-cobalt-aluminum ternary lithium ion battery positive pole material and preparation method and use thereof
CN108321381A
High energy density lithium ion secondary battery
CN109860584A
Positive electrode piece and lithium ion secondary battery
CN110265627A
Positive electrode material, positive electrode sheet containing same and lithium ion battery
CN110459736A