Bipolar current collector and preparation method thereof, lithium ion battery, and vehicle

By adopting a bipolar current collector design in lithium-ion batteries, the technology of energy density and mechanical strength of lithium-ion batteries is solved by using a removable carrier layer to improve mechanical strength in the production stage and reducing the current collector layer thickness during the use stage. Challenge, achieving more efficient energy density and mechanical properties.

CN114784289BActive Publication Date: 2024-12-03NIO TECH ANHUI CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210406436.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-04-18
Publication Date
2024-12-03
Estimated Expiration
2042-04-18

AI Technical Summary

Technical Problem

The current collectors of existing lithium-ion batteries are difficult to maintain electrical conductivity and mechanical strength while increasing energy density, reducing foil weight and reducing foil thickness, resulting in technical challenges in the production and use of lithium-ion batteries.

Method used

Design of bipolar current collectors, including an insulating layer, a removable carrier layer and a positive or negative current collector layer, improves mechanical strength during the production process through the carrier layer and is removed during the use phase to reduce the current collector layer Thickness, thereby increasing the energy density of lithium-ion batteries.

Benefits of technology

It realizes the advantages of increasing the energy density in the lithium-ion battery while maintaining sufficient mechanical strength, reducing the thickness of the current collecting layer, extending the service life of the battery, and saving material costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114784289B_ABST
    Figure CN114784289B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of lithium-ion batteries, and specifically provides a bipolar current collector for lithium-ion batteries and a preparation method thereof, a lithium-ion battery, and a vehicle, wherein the bipolar current collector comprises: an insulating layer; a positive current collecting layer, which is arranged on the first side of the insulating layer; and a negative current collecting layer, which is arranged on the second side of the insulating layer; wherein the positive current collecting layer and / or the negative current collecting layer are provided with a carrier layer on a side away from or close to the insulating layer, and the carrier layer is removably arranged on the positive current collecting layer and / or the negative current collecting layer, so that: during the production of the bipolar current collector, the mechanical strength of the positive current collecting layer and / or the negative current collecting layer attached thereto is improved by the carrier layer. Through such a structure, the energy density of the lithium-ion battery is improved under the premise of ensuring that the bipolar current collector has sufficient mechanical strength / capability to collect current.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium ion batteries, and specifically provides a bipolar current collector for a lithium ion battery and a preparation method thereof, a lithium ion battery, and a vehicle. Background Art

[0002] As a secondary battery, the main working principle of lithium-ion batteries is to work by means of the movement of lithium ions between the positive and negative electrodes of the battery. Specifically, during the charging process, lithium ions are deintercalated from the positive electrode and embedded in the negative electrode through the electrolyte, so the negative electrode is in a lithium-rich state. Correspondingly, during the discharge process, lithium ions are deintercalated from the negative electrode and embedded in the positive electrode through the electrolyte, so the positive electrode is in a lithium-rich state. As a high-voltage, high-energy-density, and long-cycle-life energy storage device, lithium-ion batteries have been widely used in consumer electronics, power tools, new energy vehicles, and energy storage.

[0003] As one of the indispensable components of lithium-ion batteries, current collectors are mainly used to collect current from positive and negative active materials during the charging and discharging process. At present, the current collectors widely used in the production of lithium-ion battery cells are positive metal aluminum foil current collectors (positive current collector layer) and negative metal copper foil current collectors (negative current collector layer). In order to continuously improve the energy density of lithium-ion batteries, reducing the weight and thickness of foil materials and ensuring conductivity / tensile strength / flexibility are the directions in which the industry continues to work hard.

[0004] Accordingly, the art needs a new technical solution to solve the above problems. Summary of the invention

[0005] Technical issues

[0006] The present invention is proposed to solve the above technical problems at least to a certain extent, or to solve at least a part of the above technical problems.

[0007] Technical Solution

[0008] In view of this, the first aspect of the present invention provides a bipolar current collector for a lithium-ion battery, the bipolar current collector comprising: an insulating layer; a positive current collecting layer, which is arranged on a first side of the insulating layer; and a negative current collecting layer, which is arranged on a second side of the insulating layer; wherein the positive current collecting layer and / or the negative current collecting layer is provided with a carrier layer on a side away from or close to the insulating layer, and the carrier layer is removably arranged on the positive current collecting layer and / or the negative current collecting layer, so that: during the production of the bipolar current collector, the mechanical strength of the positive current collecting layer and / or the negative current collecting layer attached thereto is improved by the carrier layer.

[0009] With such a configuration, it is possible to ensure that the bipolar current collector has sufficient mechanical strength by providing the carrier layer.

[0010] Specifically, due to the addition of the carrier layer, the electrode containing the bipolar current collector can have the necessary mechanical strength during the coating, drying, rolling and other processes (production stage) because the carrier layer is not removed. In this way, due to the addition of the first / second carrier layer, the thickness of the positive and negative current collecting layers in the bipolar current collector in the use stage can be reduced under the premise of sufficient strength, so it is expected to increase the energy density of the lithium-ion battery.

[0011] It is understandable that those skilled in the art can determine the material, number of layers, thickness, etc. of the carrier layer according to actual needs, as well as whether it is specifically configured on the positive current collecting layer or the negative current collecting layer, the way in which the positive / negative current collecting layer is mounted thereon, and the way in which it is removed from the positive / negative current collecting layer. Exemplarily, the carrier layer corresponding to the positive current collecting layer includes stacked layers A and B, and the carrier layer corresponding to the negative current collecting layer includes layer A. The thickness of the two layers may be the same or different. For example, the thickness of the two layers A is the same, so the thickness of the carrier layer corresponding to the positive current collecting layer is greater than the thickness of the carrier layer corresponding to the negative current collecting layer.

[0012] For the above-mentioned bipolar current collector for lithium-ion batteries, in one possible implementation, the carrier layer includes: a first carrier layer, which is removably disposed on the positive electrode current collecting layer; and a second carrier layer, which is removably disposed on the negative electrode current collecting layer; wherein the first carrier layer and the second carrier layer are the same or different.

[0013] Such a configuration provides a specific structural form of the carrier layer.

[0014] For the above-mentioned bipolar current collector for lithium-ion batteries, in a possible implementation manner, the thickness of the positive electrode current collecting layer is 0.1-10 μm; and / or the thickness of the negative electrode current collecting layer is 0.1-10 μm.

[0015] With such a configuration, the thickness of the positive / negative electrode current collecting layer is quantitatively determined.

[0016] Specifically, due to the provision of the carrier layer, the thickness of the positive / negative electrode current collecting layer can be reduced, and on this basis it is expected to improve the energy density of the lithium-ion battery.

[0017] For the above-mentioned bipolar current collector for lithium-ion batteries, in a possible implementation manner, the carrier layer is a metal foil layer, a plastic film layer or a release paper.

[0018] Such a configuration provides possible material / structural forms for the carrier layer.

[0019] Taking the carrier layer as release paper as an example, after completing the process flow requiring it, the release paper can be removed from the corresponding positive / negative electrode current collecting layer by peeling.

[0020] For example, the plastic film layer may include but is not limited to PET, PE, OPP, BOPET, BOPP, BOPA, PVC, CPP, nylon, etc.

[0021] For the above-mentioned bipolar current collector for lithium-ion batteries, in one possible implementation, the thickness of the carrier layer is 10-200 μm.

[0022] This configuration provides a possible thickness range for the carrier layer. By way of example, the carrier layer is a 150 μm metal aluminum foil layer.

[0023] For the above-mentioned bipolar current collector for lithium-ion batteries, in a possible implementation, the positive electrode current collecting layer and / or the negative electrode current collecting layer are attached to the carrier layer by electroplating, chemical plating or magnetron sputtering.

[0024] This configuration provides a possible way to attach the positive / negative current collecting layer to the carrier layer.

[0025] For the above-mentioned bipolar current collector for lithium-ion batteries, in a possible implementation manner, the thickness of the insulating layer is 0.1-10 μm.

[0026] This configuration provides a possible thickness range for the insulating layer.

[0027] For example, the insulating layer may use a thermosetting insulating adhesive, and the thermosetting insulating adhesive may be one or more of polyester, epoxy, polyurethane, polybutadiene acid, silicone, polyester imide, polyimide or polyacrylic acid.

[0028] For the above-mentioned bipolar current collector for lithium-ion batteries, in a possible implementation, the positive electrode current collecting layer is an aluminum layer, and the negative electrode current collecting layer is a copper layer.

[0029] This structure provides possible materials for the positive / negative electrode current collecting layers.

[0030] A second aspect of the present invention provides a method for preparing a bipolar current collector for a lithium-ion battery, the bipolar current collector comprising: an insulating layer; a positive current collecting layer, which is arranged on a first side of the insulating layer; and a negative current collecting layer, which is arranged on a second side of the insulating layer; wherein the preparation method comprises: providing a carrier layer, and attaching the positive current collecting layer and / or the negative current collecting layer thereto; removing the carrier layer from the positive current collecting layer and / or the negative current collecting layer attached thereto, so as to: during the production of the bipolar current collector, improve the mechanical strength of the positive current collecting layer and / or the negative current collecting layer attached thereto by the carrier layer.

[0031] It can be understood that the method for preparing the bipolar current collector for a lithium ion battery has all the technical effects of any of the aforementioned bipolar current collectors for a lithium ion battery, which will not be described in detail herein.

[0032] For the above-mentioned preparation method, in a possible embodiment, the "removing the carrier layer from the positive electrode current collecting layer and / or the negative electrode current collecting layer attached thereto" includes: before introducing the insulating layer, the carrier layer is removed from the positive electrode current collecting layer and / or the negative electrode current collecting layer attached thereto.

[0033] This configuration provides a specific relationship between the introduction of the insulating layer and the removal of the carrier layer.

[0034] For the above-mentioned preparation method, in a possible embodiment, the "removing the carrier layer from the positive electrode current collecting layer and / or the negative electrode current collecting layer attached thereto" includes: after introducing the insulating layer, the carrier layer is removed from the positive electrode current collecting layer and / or the negative electrode current collecting layer attached thereto.

[0035] This configuration provides another specific relationship between the introduction of the insulating layer and the removal of the carrier layer.

[0036] For the above preparation method, in a possible implementation manner, the thickness of the positive electrode current collecting layer is 0.1-10 μm; and / or the thickness of the negative electrode current collecting layer is 0.1-10 μm.

[0037] Through such a structure, a specific form of the positive / negative electrode current collecting layer is given.

[0038] A third aspect of the present invention provides a lithium ion battery, the lithium ion battery comprising any of the above-mentioned bipolar current collectors for lithium ion batteries.

[0039] It is understandable that the lithium-ion battery has all the technical effects of the lithium-ion battery described in any of the above items, which will not be described in detail here.

[0040] A fourth aspect of the present invention provides a vehicle equipped with the aforementioned lithium-ion battery.

[0041] It can be understood that the vehicle has all the technical effects of the lithium-ion battery described in any of the above items, which will not be repeated here.

[0042] Proposal 1. A bipolar current collector for a lithium-ion battery, characterized in that the bipolar current collector comprises:

[0043] Insulation layer;

[0044] a positive electrode current collecting layer, which is disposed on a first side of the insulating layer; and

[0045] a negative electrode current collecting layer, which is disposed on the second side of the insulating layer;

[0046] Wherein, the positive electrode current collecting layer and / or the negative electrode current collecting layer is provided with a carrier layer on a side away from or close to the insulating layer, and

[0047] The carrier layer is disposed on the positive electrode current collecting layer and / or the negative electrode current collecting layer in a removable manner so as to:

[0048] During production of the bipolar current collector, the mechanical strength of the positive electrode current collecting layer and / or the negative electrode current collecting layer attached thereto is improved by the support layer.

[0049] Proposal 2. The bipolar current collector for a lithium-ion battery according to Proposal 1, characterized in that the carrier layer comprises:

[0050] A first carrier layer is disposed on the positive electrode current collecting layer in a removable manner; and

[0051] A second carrier layer, which is removably disposed on the negative electrode current collecting layer;

[0052] The first carrier layer and the second carrier layer are the same or different.

[0053] Proposal 3. A bipolar current collector for a lithium-ion battery according to Proposal 1 or 2, characterized in that the thickness of the positive electrode current collector layer is 0.1-10 μm; and / or

[0054] The thickness of the negative electrode current collecting layer is 0.1-10 μm.

[0055] Proposal 4. The bipolar current collector for lithium-ion batteries according to Proposal 1 is characterized in that the carrier layer is a metal foil layer, a plastic film layer or a release paper.

[0056] Proposal 5. The bipolar current collector for lithium-ion batteries according to Proposal 4 is characterized in that the thickness of the carrier layer is 10-200 μm.

[0057] Proposal 6. The bipolar current collector for lithium-ion batteries according to Proposal 4 is characterized in that the positive electrode current collecting layer and / or the negative electrode current collecting layer are attached to the carrier layer by electroplating, chemical plating or magnetron sputtering.

[0058] Proposal 7. The bipolar current collector for lithium-ion batteries according to Proposal 1 is characterized in that the thickness of the insulating layer is 0.1-10 μm.

[0059] Proposal 8. The bipolar current collector for a lithium-ion battery according to Proposal 1 is characterized in that the positive electrode current collecting layer is an aluminum layer and the negative electrode current collecting layer is a copper layer.

[0060] Proposal 9. A method for preparing a bipolar current collector for a lithium-ion battery, characterized in that the bipolar current collector comprises:

[0061] Insulation layer;

[0062] a positive electrode current collecting layer, which is disposed on a first side of the insulating layer; and

[0063] a negative electrode current collecting layer, which is disposed on the second side of the insulating layer;

[0064] Wherein, the preparation method comprises:

[0065] Providing a carrier layer, and attaching the positive electrode current collecting layer and / or the negative electrode current collecting layer thereon;

[0066] The carrier layer is removed from the positive electrode current collecting layer and / or the negative electrode current collecting layer attached thereto, so as to:

[0067] During production of the bipolar current collector, the mechanical strength of the positive electrode current collecting layer and / or the negative electrode current collecting layer attached thereto is improved by the support layer.

[0068] Proposal 10. The preparation method according to Proposal 9 is characterized in that the “removing the carrier layer from the positive electrode current collecting layer and / or the negative electrode current collecting layer attached thereto” comprises:

[0069] Prior to the introduction of the insulating layer, the carrier layer is removed from the positive electrode current collecting layer and / or the negative electrode current collecting layer attached thereto.

[0070] Proposal 11. The preparation method according to Proposal 9 is characterized in that the “removing the carrier layer from the positive electrode current collecting layer and / or the negative electrode current collecting layer attached thereto” comprises:

[0071] After the insulating layer is introduced, the carrier layer is removed from the positive electrode current collecting layer and / or the negative electrode current collecting layer attached thereto.

[0072] Proposal 12. The preparation method according to any one of Proposals 9 to 11, characterized in that the thickness of the positive electrode current collecting layer is 0.1-10 μm; and / or

[0073] The thickness of the negative electrode current collecting layer is 0.1-10 μm.

[0074] Proposal 13. A lithium ion battery, characterized in that the lithium ion battery comprises the bipolar current collector for a lithium ion battery according to any one of Proposals 1 to 8.

[0075] Proposal 14. A vehicle, characterized in that the vehicle is equipped with the lithium-ion battery described in Proposal 13. BRIEF DESCRIPTION OF THE DRAWINGS

[0076] The present invention is described below with reference to the accompanying drawings. In the accompanying drawings:

[0077] Figure 1 A schematic diagram showing the structure of a bipolar current collector according to an embodiment of the present invention;

[0078] Figure 2 A schematic diagram showing the structure of a bipolar electrode according to an embodiment of the present invention;

[0079] Figure 3 A schematic diagram showing the structure of a lithium-ion battery according to an embodiment of the present invention;

[0080] Figure 4 A schematic diagram showing a process of preparing a bipolar current collector according to an embodiment of the present invention; and

[0081] Figure 5 A schematic flow chart of a method for preparing a bipolar current collector (bipolar electrode) comprising positive and negative electrode active coatings according to an embodiment of the present invention is shown.

[0082] List of reference numerals:

[0083] 100, bipolar current collector; 200, bipolar electrode; 300, winding core; 1, insulating layer; 21, positive electrode current collecting layer; 22, negative electrode current collecting layer; 31, first carrier layer; 32, second carrier layer; 41, positive electrode active coating; 42, negative electrode active coating. DETAILED DESCRIPTION

[0084] The preferred embodiments of the present invention are described below with reference to the accompanying drawings. It should be understood by those skilled in the art that these embodiments are only used to explain the technical principles of the present invention and are not intended to limit the scope of protection of the present invention. For example, although the embodiments are described in conjunction with the case where both the positive current collecting layer and the negative current collecting layer are configured with a carrier layer and the structures of the two are substantially the same, it is obvious that the scheme of the present invention can also be configured with a carrier layer for only one of the positive current collecting layer and the negative current collecting layer, or the positive current collecting layer and the negative current collecting layer are respectively configured with a carrier layer but the two carrier layers are different, etc.

[0085] It should be noted that in the description of the present invention, the terms "center", "up", "down", "left", "right", "vertical", "horizontal", "inside", "outside" and the like indicating directions or positional relationships are based on the directions or positional relationships shown in the drawings, which are merely for the convenience of description, and do not indicate or imply that the device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first", "second", and "third" are used for descriptive purposes only, and cannot be understood as indicating or implying relative importance. The singular terms "one" and "the" may also include plural forms.

[0086] In addition, it should be noted that in the description of the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For those skilled in the art, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0087] In addition, in order to better illustrate the present invention, many specific details are given in the following specific embodiments. It should be understood by those skilled in the art that the present invention can also be implemented without certain specific details. In some examples, the working principle of lithium-ion batteries and the specific process of magnetron sputtering, which are well known to those skilled in the art, are not described in detail in order to highlight the main purpose of the present invention.

[0088] Reference Figures 1 to 3 , Figure 1 A schematic diagram showing the structure of a bipolar current collector according to an embodiment of the present invention is shown. Figure 2 A schematic diagram showing the structure of a bipolar electrode according to an embodiment of the present invention is shown. Figure 3 FIG. 2 is a schematic diagram showing the structure of a lithium-ion battery according to an embodiment of the present invention. Figures 1 to 3As shown, the bipolar current collector 100 mainly includes an insulating layer 1, a positive current collecting layer 21 disposed on the first side of the insulating layer, and a negative current collecting layer 22 disposed on the second side of the insulating layer. By coating the positive active coating 41 and the negative active coating 42 on the positive current collecting layer and the negative current collecting layer of the bipolar current collector, respectively, a bipolar electrode 200 can be formed. Then, by introducing a separator or a structure with the same function as the separator, a winding core 300 as a basic winding unit of a lithium-ion battery can be formed.

[0089] By adding a positive / negative current collecting layer to the first / second carrier layer (31, 32), and then making the first / second carrier layer removably disposed on the positive / negative current collecting layer, the composition mode of the bipolar current collector / electrode in the production stage and the finished product stage can be changed. Specifically, in the stages of coating, drying, rolling and other stages of producing the bipolar current collector / electrode, the mechanical strength of the positive / negative current collecting layer can be ensured by the support of the first / second carrier layer. In the finished product stage, the thickness of the positive / negative current collecting layer can be reduced by removing the first / second carrier layer, thereby improving the energy density of the lithium-ion battery containing the positive / negative current collecting layer. Specifically, during the processing of the electrode containing the bipolar current collector, the positive / negative current collecting layer needs to have sufficient tensile strength to ensure the smooth progress of the production process, otherwise, the foil of the positive and negative current collecting layer will break, resulting in the inability to smoothly proceed with the production. Taking the currently common 6μm copper foil as an example, its tensile strength is 250-300Mpa. Taking the currently common 12μm aluminum foil as an example, its tensile strength is 200-250Mpa. In fact, due to the excellent conductivity of copper / aluminum, a thickness of 1-2μm can meet the basic function of the current collector to collect current, and the reduction in thickness means an increase in energy density. However, since the tensile strength of the foil will decrease with the reduction in thickness, the thinning of copper / aluminum foil is obviously necessary from the perspective of energy density, but there are great technical challenges from the perspective of mechanical strength.

[0090] Based on the bipolar current collector of the present invention, in the later stage, it is only necessary to remove the first / second carrier layer from the positive / negative current collecting layer (such as tearing the film, peeling, etc. mentioned below). Based on this, the thickness of the positive / negative current collecting layer in the bipolar current collector can be reduced, thereby reducing the total thickness of the bipolar current collector and improving the energy density of the lithium-ion battery. In addition, the first / second carrier layer removed from the positive / negative current collecting layer has the possibility of being reused, so the present invention also has a certain advantage of saving material costs.

[0091] by Figure 1 For example, in a possible implementation manner, the insulating layer 1 mainly includes a main body portion, and the main body portion is along one side of the width direction of the positive electrode current collecting layer ( Figure 1The left side of the figure) is in the direction toward the positive electrode current collector ( Figure 1 The main part and the first flange form the arrangement area of ​​the first carrier layer of the positive electrode current collector. The main part is formed along one side of the width direction of the negative electrode current collector ( Figure 1 The right side of the figure) is in the direction toward the negative electrode current collector ( Figure 1 The main body and the second flange form a setting area of ​​the second carrier layer corresponding to the negative electrode current collecting layer. The first / second flange is set to ensure the insulation of the ends of the positive / negative electrode current collecting layer.

[0092] In a possible implementation, the insulating layer 1 uses a thermosetting insulating adhesive, such as polyurethane, and the thickness of the insulating layer is 0.1-10 μm. After the thermosetting insulating adhesive is introduced, it is cured to form a stable insulating layer. For example, the curing method can be: in a drying tunnel of a curing machine, curing at 150° C. for about 30 minutes. The material of the positive electrode current collecting layer 21 is aluminum, and the thickness is 0.1-10 μm. The material of the negative electrode current collecting layer 22 is copper, and the thickness is 0.1-10 μm.

[0093] In the two embodiments described below, for the same embodiment, it is assumed that the material, thickness, introduction method of the first / second carrier layer into the positive / negative current collecting layer, and removal method of the first / second carrier layer from the positive / negative current collecting layer are substantially the same.

[0094] Among them, Figure 1 In the illustrated embodiment, the positive electrode current collecting layer 21 is provided with a first carrier layer 31 on a side (lower side) away from the insulating layer, and the first carrier layer 31 is removably provided on the positive electrode current collecting layer. The negative electrode current collecting layer 22 is provided with a second carrier layer 32 on a side (upper side) away from the insulating layer, and the second carrier layer 32 is removably provided on the negative electrode current collecting layer.

[0095] It can be seen that for this form of bipolar current collector, the first / second carrier layer and the insulating layer are located on both sides of the positive / negative current collecting layer, so there is no interference between the removal of the first / second carrier layer and the introduction of the insulating layer. In view of this, the following processing method can be adopted: the removal of the first / second carrier layer can be before, at the same time or after the addition of the insulating layer.

[0096] Corresponds to Figure 1 The arrangement position of the first / second carrier layer shown is shown in FIG. Figure 4 , Figure 4 FIG. 1 is a schematic flow chart showing a method for preparing a bipolar current collector according to an embodiment of the present invention. Figure 4 As shown, in a possible embodiment, the method for preparing the bipolar current collector includes the following steps:

[0097] S401, provision of the first / second carrier layer (introduction of the positive / negative current collecting layer): a metal foil (such as copper foil) layer with a thickness of 10-200 μm (such as 100 μm) is selected as the substrate of the first / second carrier layer corresponding to the positive / negative current collecting layer. The metal foil layer is respectively released outward by belt drive through the unwinding mechanism corresponding to the positive / negative current collecting layer, and a metal aluminum / copper layer of about 0.2 μm is plated on the surface of the substrate by vacuum plating or other plating methods, that is, the positive / negative current collecting layer is plated on the first / second carrier layer.

[0098] S403, introduction of insulating layer: coating the surface of the positive current collecting layer with an insulating adhesive (e.g., flame-retardant thermosetting epoxy resin solid glue with a coating thickness of about 1 μm), and forming a composite component by rolling the positive current collecting layer (metal foil layer plated with aluminum) and the negative current collecting layer (metal foil layer plated with copper) with the aid of the insulating adhesive. The insulating adhesive in the composite component is cured, so that the composite component forms a stable insulating layer of the bipolar current collector at the location where the insulating adhesive is coated.

[0099] S405, removal of the first / second carrier layer: the two metal foil layers as the first / second carrier layer are torn off from the surface of the positive / negative current collector layer. Afterwards, the composite assembly with the first / second carrier layer torn off is cleaned by a cleaning method such as plasma, so as to obtain an ultra-thin bipolar current collector that meets the quality standards.

[0100] It can be seen that in this embodiment, the first / second carrier layer is first provided and the positive / negative current collecting layer is introduced thereon, and then the insulating layer is introduced, and finally the first / second carrier layer is torn off.

[0101] For example, if, on the basis of preparing a bipolar current collector, a positive / negative active coating is coated on the side of the positive / negative current collecting layer away from the insulating layer, an ultra-thin bipolar electrode that meets the quality standards can be obtained.

[0102] Among them, Figure 2 In the illustrated embodiment, the positive electrode current collecting layer 21 is provided with a first carrier layer 31 on a side (upper side) close to the insulating layer, and the first carrier layer 31 is removably provided on the positive electrode current collecting layer. The negative electrode current collecting layer 22 is provided with a second carrier layer 32 on a side (lower side) close to the insulating layer, and the second carrier layer 32 is removably provided on the negative electrode current collecting layer.

[0103] It can be seen that for this form of bipolar current collector, the first / second carrier layer and the insulating layer are on the same side of the positive / negative current collector layer, so there must be a sequence between the removal of the first / second carrier layer and the introduction of the insulating layer, and since the insulating layer belongs to the functional layer of the finished bipolar current collector, it is necessary to introduce the insulating layer after the first / second carrier layer is removed. In view of this, the following processing method can be adopted: first remove the first / second carrier layer, and then add an insulating layer between the positive / negative current collector. Among them, since the side where the positive / negative active coating needs to be coated and the side where the insulating layer / first carrier layer / second carrier layer is located belong to different sides of the positive / negative current collector layer, the positive / negative active coating can be coated on the side of the positive / negative current collector layer away from the insulating layer at any time according to the actual situation.

[0104] exist Figure 2 In the figure, the first / second carrier layer is shown by a dotted line. It should be noted that the meaning of such a representation is that after the first / second carrier layer is removed from the two composite components respectively consisting of "the first carrier layer, the positive electrode current collector, and the positive electrode active coating" and "the second carrier layer, the negative electrode current collector, and the negative electrode active coating", the insulating layer is introduced. Therefore, the first / second carrier layer appears in the process of producing the bipolar electrode but does not appear in the product of the bipolar electrode.

[0105] Corresponds to Figure 2 The arrangement position of the first / second carrier layer shown is shown in FIG. Figure 5 , Figure 5 FIG. 1 is a schematic flow chart showing a method for preparing a bipolar electrode according to an embodiment of the present invention. Figure 5 As shown, in a possible implementation, the method for preparing a bipolar electrode includes the following steps:

[0106] S501, introduction of the first / second carrier layer (introduction of the positive / negative current collecting layer), introduction of the positive / negative active coating, specifically: select a PET coil with a thickness of 10-200μm (such as 100μm) as the substrate of the first / second carrier layer corresponding to the positive / negative current collecting layer. After coating the surface of the base layer with a release agent of 0.2-0.6μm, rewind the PET film with the release agent on the unwinding roller of the vacuum coating equipment to complete the loading of the substrate. Afterwards, start the vacuum coating equipment to unwind the PET film, and use magnetron sputtering to coat the surface of the PET film close to the side coated with the release agent. Among them, the target material for coating is high-purity aluminum wire / copper with a purity of 99.999%. By controlling the working pressure, temperature, time and other process parameters in the vacuum chamber of the coating equipment, a metal aluminum / copper film with a thickness of about 2μm is finally deposited on the surface of the PET film close to the side coated with the release agent, that is, the positive / negative current collecting layer is deposited on the first / second carrier layer. After that, the positive / negative active coating is coated on the positive / negative current collecting layer to form a positive / negative electrode assembly corresponding to the positive / negative current collecting layer and including the first / second carrier layer.

[0107] S503, removal of the first / second carrier layer, specifically: peeling off the PET film on the positive / negative electrode assembly to obtain an ultra-thin positive electrode current collecting layer (aluminum coating) and negative electrode current collecting layer (copper coating). For example, the peel strength between the positive / negative electrode current collecting layer and the first / second carrier layer is ≤0.5N / mm (such as preferably 0.1-0.2N / mm). Afterwards, the PET film release agent on the aluminum coating and the copper coating is cleaned off by a cleaning method such as plasma, and then the positive / negative electrode assembly with a total thickness of about 5μm without the first / second carrier layer is obtained by winding.

[0108] S505, introduction of the insulating layer, specifically: take a PET coil with aluminum film deposited (excluding the positive electrode component of the first carrier layer) as the basis for the introduction of the insulating layer, and apply a layer of flame-retardant thermosetting epoxy resin solid glue as an insulating layer on the surface of the PET coil (on the same side as the previous first carrier layer), with a coating thickness of 1μm. Then, the PET coil with copper film deposited (excluding the negative electrode component of the second carrier layer) is unrolled through the unwinding mechanism, and the surface of the PET coil (on the same side as the previous second carrier layer) is brought close to the thermosetting epoxy resin solid glue, so as to achieve bonding between the positive electrode component and the negative electrode component. For example, after bonding is completed, the aforementioned curing treatment method can be used to ensure that a stable insulating layer is obtained, thereby obtaining an ultra-thin bipolar electrode that meets the quality standards.

[0109] It can be seen that in this embodiment, the first / second carrier layer is first provided and the positive / negative current collecting layer is introduced thereon, then the first / second carrier layer is peeled off from the positive / negative current collecting layer, and finally the insulating layer is introduced. Obviously, the above two preparation methods are only an exemplary description and are not intended to limit the scope of protection of the present invention. For example, those skilled in the art can also adjust the material, structural form, thickness, etc. of the first / second carrier layer according to the product form involved, and flexibly select the equipment used to implement the corresponding steps. For example, according to actual conditions, electroplating, chemical plating, vacuum sputtering, etc. can be used to complete the introduction of the positive / negative current collecting layer. In addition, without violating the core invention point, the steps can be changed according to the actual situation. For example, for the corresponding Figure 2 In the embodiment, the introduction of the positive / negative electrode active coating can be adjusted to be introduced last.

[0110] It can be seen that in the bipolar current collector of the present invention, since the first / second carrier layer that can be removed is respectively added to the positive / negative current collector layer during the production stage, the bipolar current collector has sufficient mechanical strength during the production stage when the first / second carrier layer is not removed. Under this premise, the positive / negative current collector layer after removing the first / second carrier layer can provide sufficient capacity for collecting current during the charge and discharge process of the positive / negative active coating during the use stage. Since the thickness of the positive / negative current collector layer is reduced, it is expected to increase the energy density of the lithium-ion battery containing the bipolar current collector.

[0111] So far, the technical solutions of the present invention have been described in conjunction with the preferred embodiments shown in the accompanying drawings. However, it is easy for those skilled in the art to understand that the protection scope of the present invention is obviously not limited to these specific embodiments. Without departing from the principle of the present invention, those skilled in the art can make equivalent changes or substitutions to the relevant technical features, and the technical solutions after these changes or substitutions will fall within the protection scope of the present invention.

Claims

1. A bipolar current collector for a lithium ion battery, characterized in that: The bipolar current collector comprises: Insulation layer; a positive electrode current collecting layer, which is disposed on a first side of the insulating layer; and a negative electrode current collecting layer, which is disposed on the second side of the insulating layer; Wherein, the positive electrode current collecting layer and / or the negative electrode current collecting layer is provided with a carrier layer on a side away from or close to the insulating layer, and The carrier layer is disposed on the positive electrode current collecting layer and / or the negative electrode current collecting layer in a removable manner, During the coating, drying, and rolling processes of producing the bipolar current collector, the mechanical strength of the positive electrode current collector layer and / or the negative electrode current collector layer attached thereto is improved by the carrier layer; Wherein, the “the carrier layer is disposed on the positive electrode current collecting layer and / or the negative electrode current collecting layer in a removable manner” includes: Before the insulating layer is introduced, the carrier layer can be removed from the positive electrode current collecting layer and / or the negative electrode current collecting layer attached thereto; or After the insulating layer is introduced, the carrier layer can be removed from the positive electrode current collecting layer and / or the negative electrode current collecting layer attached thereto; Wherein, the carrier layer comprises: A first carrier layer is disposed on the positive electrode current collecting layer in a removable manner; and / or A second carrier layer, which is removably disposed on the negative electrode current collecting layer; Wherein, the first carrier layer and the second carrier layer are the same or different; The positive electrode current collecting layer and / or the negative electrode current collecting layer are attached to the carrier layer by electroplating, chemical plating or magnetron sputtering, and The peel strength between the positive electrode current collecting layer and / or the negative electrode current collecting layer and the first carrier layer and / or the second carrier layer is ≤0.5 N / mm.

2. The bipolar current collector for a lithium ion battery according to claim 1, characterized in that: The thickness of the positive electrode current collecting layer is 0.1-10 μm; and / or The thickness of the negative electrode current collecting layer is 0.1-10 μm.

3. The bipolar current collector for a lithium ion battery according to claim 1, characterized in that: The carrier layer is a metal foil layer, a plastic film layer or a release paper.

4. The bipolar current collector for a lithium ion battery according to claim 3, characterized in that: The thickness of the carrier layer is 10-200 μm.

5. The bipolar current collector for a lithium ion battery according to claim 1, characterized in that: The thickness of the insulating layer is 0.1-10 μm.

6. The bipolar current collector for a lithium ion battery according to claim 1, characterized in that: The positive electrode current collecting layer is an aluminum layer, and the negative electrode current collecting layer is a copper layer.

7. A method for preparing a bipolar current collector for a lithium ion battery, characterized in that: The bipolar current collector comprises: Insulation layer; a positive electrode current collecting layer, which is disposed on a first side of the insulating layer; and a negative electrode current collecting layer, which is disposed on the second side of the insulating layer; Wherein, the preparation method comprises: Providing a carrier layer, and attaching the positive electrode current collecting layer and / or the negative electrode current collecting layer thereon; removing the support layer from the positive electrode current collecting layer and / or the negative electrode current collecting layer attached thereto, During the coating, drying, and rolling processes of producing the bipolar current collector, the mechanical strength of the positive electrode current collector layer and / or the negative electrode current collector layer attached thereto is improved by the carrier layer; Wherein, the “removing the carrier layer from the positive electrode current collecting layer and / or the negative electrode current collecting layer attached thereto” includes: Before introducing the insulating layer, removing the carrier layer from the positive electrode current collecting layer and / or the negative electrode current collecting layer attached thereto; or After the insulating layer is introduced, removing the carrier layer from the positive electrode current collecting layer and / or the negative electrode current collecting layer attached thereto; Wherein, the carrier layer comprises: A first carrier layer is disposed on the positive electrode current collecting layer in a removable manner; and / or A second carrier layer, which is removably disposed on the negative electrode current collecting layer; Wherein, the first carrier layer and the second carrier layer are the same or different; The positive electrode current collecting layer and / or the negative electrode current collecting layer are attached to the carrier layer by electroplating, chemical plating or magnetron sputtering, and The peel strength between the positive electrode current collecting layer and / or the negative electrode current collecting layer and the first carrier layer and / or the second carrier layer is ≤0.5 N / mm.

8. The preparation method according to claim 7, characterized in that: The thickness of the positive electrode current collecting layer is 0.1-10 μm; and / or The thickness of the negative electrode current collecting layer is 0.1-10 μm.

9. A lithium ion battery, characterized in that: The lithium ion battery comprises the bipolar current collector for a lithium ion battery according to any one of claims 1 to 6, The bipolar current collector is prepared by the preparation method of the bipolar current collector for lithium ion battery according to claim 7 or 8.

10. A vehicle, characterized in that: The vehicle is equipped with the lithium-ion battery according to claim 9.