A LiMO2 positive electrode material and its chemical coating modification method and application
Through the bonding of the conductive polymer coating layer and the LiMO2 cathode material, the problem of poor structural stability of the lithium-ion battery cathode material is solved, the cycle performance and capacity retention rate are improved, and economical and environmentally friendly production is achieved.
Patent Information
- Application Number
- CN202110121635.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-01-28
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2041-01-28
AI Technical Summary
Existing lithium-ion battery cathode materials have poor structural stability, and lattice mismatch will occur during long-term cycling, resulting in poor interface stability, affecting the cycle performance of the battery, and posing safety risks.
The conductive polymer coating layer is used to bond the metal ions of the LiMO2 cathode material through -CN, and is connected through the coordination of N-Li and/or N-M to form a surface cyclized PAN transition layer, inducing a phase change in some regions, from The lamellar phase transforms into a rock salt phase, forming a conductive polymer coating that optimizes lattice matching.
It improves the structural stability and electrochemical activity of the cathode material, enhances the cycle performance and capacity retention rate of lithium-ion batteries, reduces production costs, and enables simple and convenient mass production.
Smart Images

Figure CN114824246B_ABST
Abstract
Description
[0001] The present invention belongs to the technical field of electrochemical energy storage, and relates to a LiMO2 positive electrode material and a chemical coating modification method and application thereof, and specifically relates to a lithium secondary battery LiMO2 (M = Ni, Co, Mn, Cr, Fe, Al, Mg, Cu, Zn, etc.) positive electrode material and a chemical coating modification method and application thereof. Background Art
[0002] As the most promising secondary battery, lithium-ion batteries are widely used in small portable electronic products and electric vehicles. The "Action Plan for Promoting the Development of Automotive Power Batteries" jointly issued by the Ministry of Industry and Information Technology and other four ministries in 2017 requires that by 2020, the single-cell specific energy of new lithium-ion power batteries must exceed 300Wh / kg, the system specific energy must strive to reach 260Wh / kg, and the cost must be reduced to less than 1 yuan / Wh; and strive to achieve the goal of 500wh / kg for the single-cell specific energy of lithium-ion power batteries by 2025. The positive electrode material of lithium-ion batteries is the main factor restricting the energy density of lithium-ion power batteries. At present, positive electrode materials such as LiNiO2, LiCoO2, and NCM have been commercialized. However, the above-mentioned positive electrode materials perform poorly in terms of structural stability, and during long-term cycling, the LiMO2-type positive electrode material will transform from a layered structure to a spinel phase or a rock salt phase, and will form a SEI passivation film at the positive electrode-electrolyte interface; on the other hand, the surface reconstruction of the positive electrode material will directly hinder the transmission of lithium ions; in addition, along with the occurrence of phase change, the gas production problem of lithium-ion batteries under high voltage also poses a safety hazard.
[0003] At present, although there have been reports on using coating methods to improve the structural stability of LiMO2 positive electrode materials. However, in the prior art, there is a widespread problem of lattice mismatch between the coating layer and the main LiMO2 material. Lattice mismatch will lead to poor interface stability between the coating layer and the LiMO2 material, thereby affecting its long-term cycle performance. Therefore, how to prepare a LiMO2 positive electrode material with good lattice matching and stable structure between the coating layer and the main LiMO2 material, so as to avoid the problem of interface lattice mismatch, good structural stability, and improve the capacity retention rate after secondary battery cycling, while the preparation method is simple and convenient, the raw materials are abundant, the cost is low, the universality is strong, and it is economical and environmentally friendly, and easy to mass produce has become a technical problem to be solved urgently. Summary of the invention
[0004] In order to improve the above technical problems, the present invention provides a positive electrode composite material, which includes a positive electrode material with a chemical formula of LiMO2 as a core and a conductive polymer coating layer coated on the surface of the positive electrode material, wherein the conductive polymer coating layer is bonded to the positive electrode material.
[0005] According to an embodiment of the present invention, the conductive polymer coating layer is bonded to the metal ions of the LiMO2 positive electrode material through -CN, for example, through the coordination of N-Li and / or NM.
[0006] According to an embodiment of the present invention, the conductive polymer coating layer includes surface cyclized PAN and a transition layer induced by PAN, and the transition layer is located between the positive electrode material and the conductive polymer coating layer. Preferably, the transition layer is a mixed phase. More preferably, the mixed phase includes a layered phase and a rock salt phase.
[0007] In the present invention, the conductive polymer coating layer interacts with the metal ions of the LiMO2 positive electrode material through -CN, and PAN induces a phase change in a part of the surface of the positive electrode material, thereby transforming a part of the surface of the LiMO2 positive electrode material from a layered phase to a rock salt phase.
[0008] According to an embodiment of the present invention, the thickness of the transition layer is 2-4 nm.
[0009] According to an embodiment of the present invention, the thickness of the conductive polymer coating layer is 3-6 nm.
[0010] According to an embodiment of the present invention, in the composite material, the mass percentage of the conductive polymer coating layer may be 0.5-5wt%.
[0011] According to an embodiment of the present invention, in the composite material, the mass percentage of the LiMO2 positive electrode material may be 95-99.5%.
[0012] According to an embodiment of the present invention, in the LiMO2 positive electrode material, M represents one, two or more of Ni, Co, Mn, Cr, Fe, Al, Mg, Cu and Zn, preferably one, two or more of Ni, Co, Mn and Fe; more preferably two or three of Ni, Co, Mn and Fe. For example, the positive electrode material is a ternary layered transition metal oxide positive electrode material.
[0013] According to an exemplary embodiment of the present invention, the LiMO2 is selected from LiNi 0.6 Co 0.2 Mn 0.2 O2 (NCM622), LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2 (NCM333), LiNi 0.8 Co 0.1 Mn 0.1 At least one of O2 (NCM811) and LiNiO2.
[0014] According to an exemplary embodiment of the present invention, the positive electrode composite material has substantially Figure 1 The X-ray diffraction pattern shown belongs to the R-3m space group, and has significant split peaks at (006) / (012) and (018) / (110).
[0015] According to an embodiment of the present invention, the positive electrode composite material has substantially the following Figure 2 Preferably, the morphology of the composite material of the positive electrode is primary particles and / or secondary microspheres.
[0016] According to an embodiment of the present invention, the positive electrode composite material is prepared by subjecting raw materials including a LiMO2 positive electrode material and a -CN-based polymer to a low-temperature calcination treatment.
[0017] According to an embodiment of the present invention, the polymer containing a -CN group may be selected from at least one of polyacrylonitrile (PAN), acrylonitrile (AN), methacrylonitrile (MAN) and polymethacrylonitrile (PMAN), preferably polyacrylonitrile (PAN).
[0018] According to an embodiment of the present invention, the weight average molecular weight of PAN is 50,000-250,000 g / mol, preferably 80,000-200,000 g / mol, exemplified by 50,000 g / mol, 80,000 g / mol, 150,000 g / mol, 200,000 g / mol, and 250,000 g / mol.
[0019] According to an embodiment of the present invention, the amount of the -CN group-containing polymer is 0.5~5wt% of the mass of the LiMO2 positive electrode material, preferably 1~3wt%, and exemplified by 0.5wt%, 1wt%, 1.5wt%, 2wt%, 3wt%, 4wt%, and 5wt%.
[0020] The present invention also provides a coating modification method for the above-mentioned positive electrode composite material, comprising the following steps:
[0021] The positive electrode composite material is prepared by using LiMO2 positive electrode material and a polymer containing -CN group as raw materials through low temperature calcination treatment.
[0022] According to an embodiment of the present invention, the LiMO2 cathode material and the -CN group-containing polymer have the meanings as described above.
[0023] According to an embodiment of the present invention, the LiMO2 cathode material and the -CN group-containing polymer react in a solvent system. Preferably, the -CN group-containing polymer is first dissolved in a solvent and then mixed with the LiMO2 cathode material to obtain a mixed solution. Preferably, the solvent may be dimethylformamide (DMF), acetone, N-methylpyrrolidone (NMP), chloroform, toluene or tetrahydrofuran.
[0024] According to an embodiment of the present invention, the coating modification method further comprises the step of heating and stirring the mixed solution to completely dissolve the polymer containing -CN groups. For example, the temperature of the heating and stirring is 40-80°C, exemplified by 40°C, 60°C, and 80°C.
[0025] According to an embodiment of the present invention, the coating modification method further comprises the step of drying the mixed solution. Preferably, the mixed solution is dried in a vacuum. For example, the drying temperature may be 40 to 80°C, exemplified by 40°C, 50°C, 60°C, 70°C, 80°C, and preferably 60°C.
[0026] According to an embodiment of the present invention, the temperature of the calcination treatment is 200-500°C, exemplified by 200°C, 300°C, 350°C, 400°C, 500°C, and preferably 300°C.
[0027] According to an embodiment of the present invention, the calcination treatment time is 1 to 5 hours, exemplified by 1 hour, 2 hours, 3 hours, 4 hours, 5 hours, and preferably 4 hours.
[0028] According to an embodiment of the present invention, the low-temperature calcination treatment can be carried out in a specific atmosphere, such as air, hydrogen / argon mixed gas, nitrogen or argon, preferably in an argon atmosphere, more preferably argon with a purity of >99%.
[0029] According to an embodiment of the present invention, the coating modification method comprises the following steps:
[0030] (1) Dissolve the polymer containing -CN groups in a solvent and stir to dissolve it;
[0031] (2) adding LiMO2 positive electrode material to the solution of step (1), stirring to mix, and vacuum drying to obtain a mixture;
[0032] (3) Under an inert atmosphere, the mixture obtained in step (2) is subjected to low-temperature calcination to obtain a coated positive electrode composite material.
[0033] The present invention also provides the use of the composite material as a positive electrode material, preferably used as a positive electrode material for a secondary battery, and more preferably used as a positive electrode material for a lithium secondary battery.
[0034] The present invention also provides a positive electrode material, which contains the coated positive electrode composite material. Preferably, the positive electrode material is a positive electrode material for a secondary battery. More preferably, the positive electrode material is a positive electrode material for a lithium secondary battery.
[0035] The present invention also provides the use of the coated positive electrode composite material and / or the positive electrode material in a secondary battery. Preferably, the secondary battery is a lithium secondary battery.
[0036] The present invention also provides a secondary battery, which comprises the coated positive electrode composite material and / or the positive electrode material.
[0037] Beneficial effects of the present invention:
[0038] (1) The present invention provides a coating method for a lithium secondary battery LiMO2 positive electrode material, wherein a strong chemical bond is formed between CN- in a cyano polymer and Li ions or M metal ions in LiMO2, thereby realizing a process of cyclization of the cyano polymer to generate a conductive polymer coating layer, thereby overcoming the structural degradation problem of the LiMO2 positive electrode material during the cycle. The LiMO2 positive electrode composite conductive material prepared by the method of the present invention has high electrical conductivity and a stable chemical structure, and the lithium ion battery electrode prepared based on the excellent characteristics of the LiMO2 positive electrode composite conductive material of the present invention has a layered phase-mixed phase coupling structure, thereby overcoming the defect of poor interface stability caused by the mismatch between the polymer coating layer and the positive electrode material lattice, and the composite material prepared by the present invention has good electrochemical activity and a stable electrode surface.
[0039] (2) The present invention provides a coating method for a lithium secondary battery LiMO2 positive electrode material, wherein PAN is cyclized on the surface of LiMO2 by low-temperature treatment to form an electron path, thereby significantly improving the electrochemical activity of the positive electrode material.
[0040] (3) The present invention provides a coating method for a lithium secondary battery LiMO2 positive electrode material. The method can be implemented under a specific atmosphere, is simple and convenient, has abundant raw materials, is low-cost, has strong universality, is economical and environmentally friendly, and is easy to mass produce. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] Figure 1 1 and 2 are XRD diagrams of the positive electrode materials prepared in Example 1 and Comparative Example 1.
[0042] Figure 2 TEM and FFT images of the corresponding areas of the positive electrode material prepared in Example 1.
[0043] Figure 3The graph is a cycle performance graph of CR2025 button batteries assembled with the positive electrode materials prepared in Comparative Example 1, Comparative Example 2 and Examples 1-4. DETAILED DESCRIPTION
[0044] The technical scheme of the present invention will be further described in detail below in conjunction with specific embodiments. It should be understood that the following embodiments are only exemplary descriptions and explanations of the present invention and should not be construed as limiting the scope of protection of the present invention. All technologies implemented based on the above content of the present invention are included in the scope that the present invention is intended to protect.
[0045] Unless otherwise specified, the raw materials and reagents used in the following examples are commercially available or can be prepared by known methods.
[0046] In the following embodiments of the present invention:
[0047] X-ray diffraction (XRD) test: X-ray diffractometer, instrument model: Rigaku Ultima IV, Japan.
[0048] Transmission electron microscopy (TEM) test: Transmission electron microscope, instrument model: JEOL JEM 3000F, Japan.
[0049] Assembly method of CR2025 button battery:
[0050] The positive electrode material (the final product prepared in Examples 1-4 and Comparative Examples 1 and 2), acetylene black, and polyvinylidene fluoride (PVDF) were made into a slurry in a mass ratio of 8:1:1 and coated on an aluminum foil and dried. The dried aluminum foil was cut into small discs with a diameter of about 1 cm using a cutting machine as the positive electrode. A metal lithium sheet was used as the negative electrode, Celgard2500 was used as the diaphragm, and a 1M carbonate solution was used as the electrolyte (wherein the solvent was a mixed solution of ethylene carbonate and dimethyl carbonate in a volume ratio of 1:1, and the solute was LiPF6), and a CR2025 button battery was assembled in a glove box with an argon atmosphere.
[0051] The electrochemical performance of the assembled CR2025 button cells was tested using a LANDCT 2001A tester (Wuhan Landian Electronics Co., Ltd.) at a temperature of 25 °C and a voltage range of 2.8–4.35 V. During the test, charge and discharge were performed at 0.2 C (1 C = 190 mAh / g).
[0052] Example 1
[0053] A chemical coating modification method for a lithium secondary battery LiMO2 positive electrode material comprises the following steps:
[0054] (1) Weigh 0.01 g of PAN with a molecular weight of 150,000 g / mol and dissolve it in 4 mL of DMF solvent to form a transparent solution;
[0055] (2) Add 1 g of NCM811 to the solution of step (1), heat and stir at 60°C to mix evenly, then transfer to a 60°C oven and vacuum dry for 2 h to obtain a mixture;
[0056] (3) The mixture obtained in step (2) is placed in a tubular furnace protected by an argon atmosphere, calcined at 300° C. for 4 h, and then cooled to room temperature to obtain a coated LiMO2 positive electrode material.
[0057] Example 2
[0058] A chemical coating modification method for a lithium secondary battery LiMO2 positive electrode material comprises the following steps:
[0059] (1) Weigh 0.005 g of PAN with a molecular weight of 150,000 g / mol and dissolve it in 4 mL of DMF solvent to form a transparent solution;
[0060] (2) Add 1 g of NCM811 to the solution of step (1), heat and stir to mix evenly, then transfer to a 60°C oven and vacuum dry for 2 h to obtain a mixture;
[0061] (3) The mixture obtained in step (2) is placed in a tubular furnace protected by an argon atmosphere, calcined at 350° C. for 4 h, and then cooled to room temperature to obtain a coated positive electrode material.
[0062] Example 3
[0063] A chemical coating modification method for a lithium secondary battery LiMO2 positive electrode material comprises the following steps:
[0064] (1) Weigh 0.01 g of PAN with a molecular weight of 150,000 g / mol and dissolve it in 4 mL of DMF solvent to form a transparent solution;
[0065] (2) Add 1 g of NCM811 to the solution of step (1), heat and stir to mix evenly, then transfer to a 60°C oven and vacuum dry for 2 h to obtain a mixture;
[0066] (3) The mixture obtained in step (2) is placed in a muffle furnace, heated to 300° C. in an air atmosphere and maintained for 1 hour, and then cooled to room temperature and ground to obtain a coated positive electrode material.
[0067] Example 4
[0068] A chemical coating modification method for a lithium secondary battery LiMO2 positive electrode material comprises the following steps:
[0069] (1) Weigh 0.015 g of PAN with a molecular weight of 150,000 g / mol and dissolve it in 4 mL of DMF solvent to form a transparent solution;
[0070] (2) Add 1 g of NCM811 to the solution of step (1), heat and stir to mix evenly, then transfer to a 60°C oven and vacuum dry for 2 h to obtain a mixture;
[0071] (3) The mixture obtained in step (2) is placed in a muffle furnace, heated to 300° C. in an air atmosphere and maintained for 1 hour, and then cooled to room temperature and ground to obtain a coated positive electrode material.
[0072] Comparative Example 1
[0073] (1) Weigh 0.01 g of PAN with a molecular weight of 150,000 g / mol and dissolve it in 4 mL of DMF solvent to form a transparent solution;
[0074] (2) Add 1 g of NCM811 to the solution of step (1), heat and stir at 60°C to mix evenly, and then transfer to a 60°C oven and vacuum dry for 2 h. The resulting powder is comparative sample 1.
[0075] Comparative Example 2
[0076] (1) Add 1 g of NCM811 to 4 mL of DMF, heat and stir to mix evenly, then transfer to a 60 °C oven and vacuum dry for 2 h to obtain a mixture;
[0077] (2) The mixture obtained in step (1) was placed in a tubular furnace protected by an argon atmosphere, calcined at 300° C. for 4 h, and the powder obtained after cooling to room temperature was referred to as comparative sample 2.
[0078] Figure 1 The XRD diagrams of the positive electrode materials prepared in Example 1 and Comparative Example 1 show that the positive electrode material prepared in Example 1 has substantially the same crystal structure as that in Comparative Example 1, with only a slight change in the ratio of the I (003) / I (104) peaks. The I (003) / I (104) peak ratio of the positive electrode material prepared in Comparative Example 1 is 2.15, while the I (003) / I (104) peak ratio of the composite positive electrode material prepared in Example 1 is 1.73. The decrease in the I (003) / I (104) ratio indicates that a partial phase change has occurred on the surface of the NCM811 positive electrode material, that is, there is a mixed phase of a layered phase and a rock salt phase.
[0079] Figure 2The TEM and FFT images of the positive electrode material of Example 1 show that the main particle body (A) in the composite positive electrode material still retains the R-3m configuration, and a transition layer (a mixed phase layer composed of a layered phase and a rock salt phase) (B) and a polymer coating layer (C) exist on the surface of the NCM811 positive electrode material after PAN coating modification.
[0080] Figure 3 The figure is a cycle performance diagram of CR2025 button batteries assembled with the positive electrode materials prepared in Comparative Example 1, Comparative Example 2 and Examples 1-4. Figure 3 It can be seen that after 50 cycles at 0.2C (1C=190mA / g), the capacity retention rates of the CR2025 button cells assembled from the positive electrode materials prepared in Comparative Examples 1 and 2 are 95.8% and 94.7%, respectively, while the capacity retention rates of the CR2025 button cells assembled from the positive electrode materials prepared in Examples 1, 2, 3, and 4 are increased to 98.8%, 96.8%, 97.3%, and 97.6%, respectively. This indicates that the positive electrode materials prepared in the present invention all have good capacity retention rates.
[0081] The above is an explanation of the embodiments of the present invention. However, the present invention is not limited to the above embodiments. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A positive electrode composite material, characterized in that: The positive electrode composite material comprises a positive electrode material with a chemical formula of LiMO2 as a core and a conductive polymer coating layer coated on the surface of the positive electrode material, wherein the conductive polymer coating layer is bonded to the metal ions of the LiMO2 positive electrode material through -CN; the conductive polymer coating layer comprises surface cyclized PAN and a transition layer induced by PAN, wherein the transition layer is located between the positive electrode material and the conductive polymer coating layer, wherein the transition layer is a mixed phase, wherein the mixed phase comprises a layered phase and a rock salt phase, and wherein the thickness of the transition layer is 2-4 nm; The positive electrode composite material is prepared by low-temperature calcination of raw materials including LiMO2 positive electrode material and -CN-based polymer; the calcination temperature is 200-350° C., and the calcination time is 1-5 hours; The LiMO2 cathode material is selected from LiNi 0.6 Co 0.2 Mn 0.2 O2 (NCM622), LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2 (NCM333), LiNi 0.8 Co 0.1 Mn 0.1 At least one of O2 (NCM811).
2. The positive electrode composite material according to claim 1, characterized in that The thickness of the conductive polymer coating layer is 3-6 nm; And / or, in the composite material, the mass percentage of the conductive polymer coating layer is 0.5-5wt%; And / or, in the composite material, the mass percentage of LiMO2 positive electrode material is 95-99.5%.
3. The positive electrode composite material according to claim 1 or 2, characterized in that: The positive electrode composite material has the morphology of primary particles and / or secondary micron spheres.
4. The positive electrode composite material according to any one of claims 1 to 2, characterized in that: The polymer containing -CN groups is selected from at least one of polyacrylonitrile (PAN) and polymethacrylonitrile (PMAN); And / or, the weight average molecular weight of PAN is 50000-250000 g / mol; And / or, the amount of the polymer containing -CN group is 0.5~5wt% of the mass of LiMO2 positive electrode material.
5. The coating modification method of the positive electrode composite material according to any one of claims 1 to 4, characterized in that: The coating modification method comprises the following steps: The positive electrode composite material is prepared by using LiMO2 positive electrode material and a polymer containing -CN group as raw materials through low temperature calcination treatment.
6. The coating modification method according to claim 5, characterized in that: The LiMO2 positive electrode material and the -CN group-containing polymer react in a solvent system, the -CN group-containing polymer is first dissolved in a solvent, and then mixed with the LiMO2 positive electrode material to obtain a mixed solution, the solvent is dimethylformamide (DMF), acetone, N-methylpyrrolidone (NMP), chloroform, toluene or tetrahydrofuran; And / or, the coating modification method further comprises the step of heating and stirring the mixed solution to completely dissolve the polymer containing -CN groups, and the heating and stirring temperature is 40-80°C; And / or, the coating modification method further comprises the step of drying the mixed solution, wherein the drying temperature is 40-80° C.; And / or, the low-temperature calcination treatment is carried out in air, a hydrogen / argon mixed gas, nitrogen or argon.
7. The coating modification method according to claim 5, characterized in that: The coating modification method comprises the following steps: (1) Dissolve the polymer containing -CN groups in a solvent and stir to dissolve it; (2) adding LiMO2 positive electrode material to the solution of step (1), stirring to mix, and vacuum drying to obtain a mixture; (3) Under an inert atmosphere, the mixture obtained in step (2) is subjected to low-temperature calcination to obtain a coated positive electrode composite material.
8. Use of the positive electrode composite material according to any one of claims 1 to 4 and / or the composite material obtained by the coating modification method according to any one of claims 5 to 7 as a positive electrode material.
9. The use according to claim 8, characterized in that The positive electrode composite material is used as a positive electrode material for a secondary battery.
10. The use according to claim 9, characterized in that The positive electrode composite material is used as a positive electrode material for a lithium secondary battery.
11. A positive electrode material, comprising the positive electrode composite material according to any one of claims 1 to 4 and / or the positive electrode composite material obtained by the coating modification method according to any one of claims 5 to 7.
12. Use of the positive electrode composite material according to any one of claims 1 to 4 and / or the positive electrode composite material obtained by the coating modification method according to any one of claims 5 to 7 and / or the positive electrode material according to claim 11 in a secondary battery.
13. A secondary battery, comprising the positive electrode composite material according to any one of claims 1 to 4 and / or the positive electrode composite material obtained by the coating modification method according to any one of claims 5 to 7 and / or the positive electrode material according to claim 11.