Binder composition for non-aqueous secondary battery electrode, slurry composition for non-aqueous secondary battery electrode, electrode for non-aqueous secondary battery, and non-aqueous secondary battery

By using a binder composition of specific polymers α and β in lithium-ion secondary battery electrodes, combined with plasticizers and organic solvents, the problem of balancing electrode softness and uniformity is solved, and the rate of secondary batteries is significantly improved. and cycle characteristics, improving battery performance.

CN114830380BActive Publication Date: 2024-10-11ZEON CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080087106.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-12-27
Filing Date
2020-12-16
Publication Date
2024-10-11
Estimated Expiration
2040-12-16

AI Technical Summary

Technical Problem

It is difficult to achieve both softness and uniformity in lithium-ion secondary battery electrodes while improving rate characteristics and cycle characteristics with the existing technology.

Method used

A binder composition for non-aqueous secondary battery electrodes containing specific polymers α and β as binder components is used, combined with plasticizers and organic solvents, and the composition and proportion of the polymers are optimized to form an efficient electrode composite material layer.

Benefits of technology

It achieves high flexibility and uniformity of the electrode, while significantly improving the rate characteristics and cycle characteristics of the secondary battery, and improving the overall performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003695153340000431
    Figure BDA0003695153340000431
Patent Text Reader

Abstract

A binder composition for non-aqueous secondary battery electrodes, comprising a prescribed binder component, a plasticizer, and an organic solvent. The binder component comprises an insoluble polymer and a readily soluble polymer, wherein the insoluble polymer comprises a (meth)acrylate monomer unit and an ethylenically unsaturated acid monomer unit, and the readily soluble polymer comprises an amide group-containing monomer unit and at least one of a (meth)acrylate monomer unit having an alkyl chain with carbon atoms of 1 or more and 6 or less, and a nitrile group-containing monomer unit at a prescribed content ratio.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a binder composition for a non-aqueous secondary battery electrode, a slurry composition for a non-aqueous secondary battery electrode, an electrode for a non-aqueous secondary battery, and a non-aqueous secondary battery. Background Art

[0002] Non-aqueous secondary batteries such as lithium-ion secondary batteries are small, lightweight, have high energy density, and can be repeatedly charged and discharged, and are used in a wide range of applications. Therefore, in recent years, the improvement of battery components such as electrodes has been studied for the purpose of further improving the performance of non-aqueous secondary batteries.

[0003] Here, the electrode for a non-aqueous secondary battery such as a lithium ion secondary battery (hereinafter, sometimes simply referred to as a "secondary battery") generally has a current collector and an electrode composite material layer (a positive electrode composite material layer or a negative electrode composite material layer) formed on the current collector. Moreover, the electrode composite material layer is formed, for example, by applying a slurry composition to the current collector and drying the applied slurry composition, wherein the slurry composition includes an electrode active material and a binder composition, and the binder composition includes a binding material.

[0004] Therefore, in recent years, attempts have been made to improve the slurry composition for forming an electrode composite material layer in order to further improve the performance of secondary batteries.

[0005] For example, Patent Document 1 states that, in order to improve the flexibility of the electrode, a plasticizer can be added to a binder resin for a secondary battery electrode comprising the following polymer, wherein the polymer contains 50 to 99.99 mol % of vinyl cyanide units and 0.01 to 10 mol % of units having an acidic group as structural units and has a mass average molecular weight of more than 200,000 and less than 2,000,000.

[0006] In addition, Patent Document 2 states that in order to improve the flexibility of the electrode, a plasticizer can be added to a binder resin for a non-aqueous secondary battery electrode, wherein the binder resin for a non-aqueous secondary battery electrode contains a polymer having an acidic group and a polymer containing a vinyl cyanide monomer unit as a branch polymer grafted onto a polyolefin backbone polymer.

[0007] Furthermore, Patent Documents 3 and 4 propose to use a plasticizer and polyvinylidene fluoride as a binder in combination when preparing a positive electrode slurry or a positive electrode paste.

[0008] Prior art literature

[0009] Patent Literature

[0010] Patent Document 1: Japanese Patent Application Publication No. 2015-213049;

[0011] Patent Document 2: Japanese Patent Application Publication No. 2017-16890;

[0012] Patent document 3: Chinese patent application publication No. 109841835;

[0013] Patent document 4: Chinese Patent Application Publication No. 108321360. Summary of the invention

[0014] Problem that the invention aims to solve

[0015] In recent years, secondary batteries are required to have further improved battery characteristics such as rate characteristics and cycle characteristics (hereinafter sometimes simply referred to as "battery characteristics"). In order to produce a secondary battery with excellent battery characteristics, it is important that the electrodes used have high flexibility and uniformity.

[0016] However, the above-mentioned conventional binder resins, positive electrode slurries, and positive electrode pastes cannot achieve both high-level compatibility in forming an electrode having excellent flexibility and uniformity and improving rate characteristics and cycle characteristics of a secondary battery having the obtained electrode.

[0017] Therefore, an object of the present invention is to provide a non-aqueous secondary battery electrode binder composition and a non-aqueous secondary battery electrode slurry composition, which can form an electrode with excellent flexibility and uniformity at a high level and improve the rate characteristics and cycle characteristics of a secondary battery having the obtained electrode.

[0018] Another object of the present invention is to provide an electrode for a non-aqueous secondary battery which has excellent flexibility and uniformity and can improve the rate characteristics and cycle characteristics of a secondary battery.

[0019] Furthermore, an object of the present invention is to provide a non-aqueous secondary battery having excellent rate characteristics and cycle characteristics.

[0020] Solutions for solving problems

[0021] The present inventors have conducted in-depth research for the purpose of solving the above problems. Then, the present inventors have found that if a non-aqueous secondary battery electrode binder composition comprising a binder component, a plasticizer and an organic solvent is used, the binder component comprising two polymers satisfying a prescribed composition, the above problems can be advantageously solved, and the present invention has been completed.

[0022] That is, the purpose of the present invention is to advantageously solve the above-mentioned problems. The non-aqueous secondary battery electrode binder composition of the present invention is characterized in that it contains polymer α and polymer β as binder components, a plasticizer, and an organic solvent, wherein the polymer α is an insoluble polymer containing a (meth) acrylate monomer unit and an ethylenically unsaturated acid monomer unit, and the polymer β is an easily soluble polymer containing an amide-containing monomer unit and at least one of a (meth) acrylate monomer unit having an alkyl chain with a carbon number of 1 or more and 6 or less, and a nitrile-containing monomer unit, and the total of all monomer units constituting the polymer β is 100% by mass, the content ratio of the nitrile-containing monomer unit is 70% by mass or more and 95% by mass or less, and the total content ratio of the amide-containing monomer unit and the (meth) acrylate monomer unit is 0.1% by mass or more and 20% by mass or less. As such, according to the binder composition containing the polymers α and β and the plasticizer, it is possible to form an electrode having excellent flexibility and uniformity at a high level and to improve the rate characteristics and cycle characteristics of a secondary battery having the obtained electrode.

[0023] Here, in this specification, "(meth)acrylic acid" means acrylic acid or methacrylic acid. In addition, the types of monomer units contained in a certain polymer and the "ratio of monomer units" in a certain polymer can be expressed as follows: 1 H-NMR or other nuclear magnetic resonance (NMR) method for identification or measurement. In addition, "comprising monomer units" means "a polymer obtained using a monomer contains repeating units derived from the monomer". In addition, whether a certain polymer is "insoluble" or "easily soluble" can be determined by the method described in the examples.

[0024] Here, the non-aqueous secondary battery electrode binder composition of the present invention preferably has the total mass of the above-mentioned binder component as 100 mass%, the content a of the above-mentioned polymer α is 5 mass% or more and 60 mass% or less, and the content b of the above-mentioned polymer β is 20 mass% or more and 94 mass% or less. By making the content of polymer α and β respectively within the above range, the peel strength of the obtained electrode can be improved, and the cycle characteristics of the obtained secondary battery can be further improved.

[0025] In addition, the non-aqueous secondary battery electrode binder composition of the present invention preferably comprises the polymer α and the polymer β as polymers that satisfy the requirement that, in the case of preparing a N-methyl-2-pyrrolidone mixed solution containing the polymer α at the above content rate a and the polymer β at the above content rate b as solid components with a solid content concentration of 8% by mass, the ratio of the insoluble component in the mixed solution is 30% by mass or more and 80% by mass or less. If the amount of insoluble components of the mixture of polymers α and β in N-methyl-2-pyrrolidone is within the above range, the peel strength of the obtained electrode can be improved, and the cycle characteristics of the obtained secondary battery can be further improved.

[0026] In addition, the above-mentioned "ratio of the amount of insoluble components" can be measured by the method described in Examples.

[0027] In addition, the non-aqueous secondary battery electrode binder composition of the present invention preferably has a total mass of the above-mentioned plasticizer and the above-mentioned binder component as 100 mass%, and the content of the above-mentioned plasticizer is 0.1 mass % or more and 30 mass % or less. If the content of the plasticizer relative to the total mass of the plasticizer and the binder component is above the above-mentioned lower limit, the flexibility of the obtained electrode can be further improved. In addition, if the content of the plasticizer is below the above-mentioned upper limit, the peel strength of the obtained electrode can be improved, and the cycle characteristics of the secondary battery with the electrode can be further improved.

[0028] In addition, the non-aqueous secondary battery electrode binder composition of the present invention preferably has a molecular weight of the plasticizer of 1000 or less and a decomposition potential of 3.5 V or more. If the molecular weight of the plasticizer is 1000 or less and the decomposition potential is 3.5 V or more, the flexibility of the obtained electrode can be further improved, and the rate characteristics and cycle characteristics of the obtained secondary battery can be further improved.

[0029] The molecular weight and decomposition potential of the plasticizer can be measured by the method described in the Examples.

[0030] In addition, the non-aqueous secondary battery electrode binder composition of the present invention preferably further comprises polymer γ as the above-mentioned binder component, and the above-mentioned polymer γ is an easily soluble polymer having an iodine value of more than 5g / 100g and less than 100g / 100g. If the non-aqueous secondary battery electrode binder composition of the present invention further comprises polymer γ as an easily soluble polymer having an iodine value within the above range as a binder component, the softness and uniformity of the obtained electrode can be further improved. In addition, if polymer γ is included as a binder component, the peel strength of the obtained electrode can be improved.

[0031] In addition, the "iodine value" of the polymer γ can be measured by the method described in the Examples.

[0032] In addition, the non-aqueous secondary battery electrode binder composition of the present invention preferably has a content of the above-mentioned binder component as 100 mass %, and a content c of the above-mentioned polymer γ of 0.1 mass % or more and 50 mass % or less. If the content of polymer γ in the binder component is within the above range, the flexibility and uniformity of the obtained electrode can be further improved.

[0033] In addition, the object of the present invention is to advantageously solve the above-mentioned problems, and the non-aqueous secondary battery electrode slurry composition of the present invention is characterized in that it comprises any one of the above-mentioned non-aqueous secondary battery electrode binder compositions, an electrode active material, and a conductive material. Like this, according to a slurry composition comprising a non-aqueous secondary battery electrode binder composition, an electrode active material, and a conductive material, and the above-mentioned non-aqueous secondary battery electrode binder composition comprises a binder component, a plasticizer, and an organic solvent, and the above-mentioned binder component comprises two polymers satisfying a specified composition, It is possible to form an electrode with excellent flexibility and uniformity at a high level and improve the rate characteristics and cycle characteristics of a secondary battery having the obtained electrode.

[0034] Here, in the slurry composition for non-aqueous secondary battery electrodes of the present invention, it is preferred that the conductive material includes carbon nanotubes. By adding carbon nanotubes to the slurry composition of the present invention, the rate characteristics of the obtained secondary battery can be further improved.

[0035] In addition, the purpose of the present invention is to advantageously solve the above-mentioned problems. The electrode for a non-aqueous secondary battery of the present invention is characterized in that it has an electrode composite material layer comprising a polymer α and a polymer β as a binder component, a plasticizer, an electrode active material, and a conductive material, the above-mentioned polymer α is a granular polymer comprising a (meth)acrylate monomer unit and an ethylenically unsaturated acid monomer unit, the above-mentioned polymer β is an easily soluble polymer comprising an amide group-containing monomer unit and at least one of a (meth)acrylate monomer unit having an alkyl chain with a carbon number of 1 or more and 6 or less, and a nitrile group-containing monomer unit, and the total of all monomer units constituting the above-mentioned polymer β is 100 mass%, the content ratio of the above-mentioned nitrile group-containing monomer unit is 70 mass% or more and 95 mass% or less, and the total content ratio of the above-mentioned amide group-containing monomer unit and the above-mentioned (meth)acrylate monomer unit is 0.1 mass% or more and 20 mass% or less. An electrode for a non-aqueous secondary battery comprising a binder component, a plasticizer, an electrode active material and a conductive material, wherein the binder component comprises two polymers satisfying a prescribed composition, has excellent flexibility and uniformity, and can improve the rate characteristics and cycle characteristics of the secondary battery.

[0036] Here, the non-aqueous secondary battery electrode of the present invention preferably further comprises polymer γ as the above-mentioned binder component, and the above-mentioned polymer γ is a soluble polymer having an iodine value of 5 g / 100 g or more and 100 g / 100 g or less. If the non-aqueous secondary battery electrode further comprises polymer γ as a soluble polymer having an iodine value within the above-mentioned range as a binder component, the rate characteristics of the secondary battery having the electrode can be further improved.

[0037] Furthermore, the object of the present invention is to advantageously solve the above-mentioned problems, and the non-aqueous secondary battery of the present invention is characterized in that it has an electrode for a non-aqueous secondary battery, and the non-aqueous secondary battery electrode has an electrode composite material layer formed using any of the above-mentioned non-aqueous secondary battery electrode slurry compositions. Alternatively, the non-aqueous secondary battery of the present invention is characterized in that it has any of the above-mentioned non-aqueous secondary battery electrodes. Like this, if a non-aqueous secondary battery electrode having an electrode composite material layer formed using any of the above-mentioned non-aqueous secondary battery electrode slurry compositions or any of the above-mentioned non-aqueous secondary battery electrodes is used, a non-aqueous secondary battery with excellent rate characteristics and cycle characteristics can be provided.

[0038] Effects of the Invention

[0039] According to the present invention, a nonaqueous secondary battery electrode binder composition and a nonaqueous secondary battery electrode slurry composition can be provided that can form an electrode having both high flexibility and excellent uniformity and improve the rate characteristics and cycle characteristics of a secondary battery having the obtained electrode.

[0040] Furthermore, according to the present invention, it is possible to provide a non-aqueous secondary battery electrode which has excellent flexibility and uniformity and can improve the rate characteristics and cycle characteristics of the secondary battery.

[0041] Furthermore, according to the present invention, it is possible to provide a non-aqueous secondary battery having excellent rate characteristics and cycle characteristics. DETAILED DESCRIPTION

[0042] Hereinafter, embodiments of the present invention will be described in detail.

[0043] Here, the non-aqueous secondary battery electrode binder composition of the present invention can be used when preparing a non-aqueous secondary battery electrode slurry composition. In addition, the non-aqueous secondary battery electrode slurry composition prepared using the non-aqueous secondary battery electrode binder composition of the present invention can be preferably used when forming an electrode of a non-aqueous secondary battery such as a lithium ion secondary battery. Furthermore, the non-aqueous secondary battery of the present invention is characterized in that the non-aqueous secondary battery electrode of the present invention is used.

[0044] Furthermore, the binder composition for nonaqueous secondary battery electrodes and the slurry composition for nonaqueous secondary battery electrodes of the present invention can be particularly preferably used when forming a positive electrode of a nonaqueous secondary battery.

[0045] (Binder composition for secondary battery electrodes)

[0046] The non-aqueous secondary battery electrode binder composition of the present invention is a non-aqueous secondary battery electrode binder composition comprising polymer α and polymer β as binder components, a plasticizer, and an organic solvent. Moreover, the non-aqueous secondary battery electrode binder composition of the present invention is characterized in that polymer α is an insoluble polymer comprising a (meth) acrylate monomer unit and an ethylenically unsaturated acid monomer unit, and polymer β is an easily soluble polymer comprising an amide-containing monomer unit and at least one of a (meth) acrylate monomer unit having an alkyl chain with a carbon number of 1 or more and 6 or less, and a nitrile-containing monomer unit, and the total of all monomer units constituting polymer β is 100% by mass, the content ratio of the nitrile-containing monomer unit is 70% by mass or more and 95% by mass or less, and the total content ratio of the amide-containing monomer unit and the (meth) acrylate monomer unit is 0.1% by mass or more and 20% by mass or less. Furthermore, the binder composition for non-aqueous secondary battery electrodes of the present invention preferably contains polymer γ as a binder component in addition to the above-mentioned polymers α and β as binder components, and the above-mentioned polymer γ is a polymer having a specified property. Furthermore, the binder composition for non-aqueous secondary battery electrodes of the present invention may also contain other binder components different from the components contained in the above-mentioned binder component. Polymers that can correspond to polymers α to γ ​​are not included in other binder components.

[0047] Here, the non-aqueous secondary battery electrode binder composition of the present invention (hereinafter, also referred to as "binder composition" only) contains polymers α and β and a plasticizer that satisfy the above-mentioned composition and properties, so it is possible to form an electrode with excellent flexibility and uniformity, and it is possible to improve the rate characteristics and cycle characteristics of the secondary battery having the obtained electrode. The reason is not clear, but it is speculated to be the following reasons.

[0048] First, polymer α, which is a polymer that is insoluble in organic solvents, in other words, exists in an organic solvent and in a granular state in the formed electrode, can be bonded to the bonded components such as electrode active materials in the electrode composite material layer, so that it can play a role in maintaining the flexibility of the electrode while effectively bonding the bonded components to each other. Therefore, polymer α helps to improve the flexibility of the formed electrode composite layer. In addition, polymer β helps to give the slurry composition a moderate viscosity when preparing a slurry composition. Therefore, polymer β can help to improve the uniformity and peel strength of the electrode obtained using the slurry composition, and play a role in relieving the concentration of stress and resistance in the electrode, resulting in the ability to improve the rate characteristics and cycle characteristics of the secondary battery obtained. Furthermore, in addition, the plasticizer can play a role in improving the flexibility of the obtained electrode, and therefore play a role in improving the rate characteristics and cycle characteristics of the secondary battery. This is believed to be because the plasticizer plays a role in reducing the crystallinity and glass transition temperature of polymer α and polymer β. Here, in the case of replacing polymer β with an existing binder component such as polyvinylidene fluoride and combining it with a plasticizer, degradation of the active material sometimes occurs, and degradation of battery characteristics such as cycle characteristics and rate characteristics occurs. However, in the present invention, when polymers α and β satisfying the prescribed composition and properties are combined with a plasticizer, an electrode with high flexibility and uniformity can be obtained, and battery characteristics such as rate characteristics and cycle characteristics can be effectively improved.

[0049] <Polymer α>

[0050] Polymer α is a component that keeps the components contained in the electrode composite layer from being separated from the electrode composite layer (i.e., acting as a binder) in an electrode manufactured by forming an electrode composite layer on a current collector using a slurry composition containing a binder composition. Moreover, polymer α is an insoluble polymer that is insoluble in an organic solvent, and is a granular polymer that exists in an organic solvent and in a granular state in the electrode formed. Whether polymer α is insoluble in an organic solvent and is "granular" in an electrode can be confirmed according to the method described in the embodiment. In addition, polymer α is "insoluble" in an organic solvent, which means that the dried polymer α is placed in N-methyl-2-pyrrolidone at a temperature of 60°C for 72 hours, and the dry mass of the insoluble component obtained by filtering with 200 meshes is 70% by mass or more relative to the total mass of the dried polymer α used. Polymer α is a component that exerts bonding ability by point bonding with an adherend in an electrode. Therefore, polymer α can improve the flexibility of the electrode while exerting bonding ability in the electrode.

[0051] [Composition of polymer α]

[0052] The polymer α needs to contain a (meth)acrylic acid ester monomer unit and an ethylenically unsaturated acid monomer unit as repeating units. Furthermore, the polymer α may optionally contain a crosslinking monomer unit and other monomer units other than the above as repeating units.

[0053] [(Meth)acrylate monomer unit]

[0054] The (meth)acrylate monomer unit is a repeating unit derived from a (meth)acrylate monomer. If the polymer α contains the (meth)acrylate monomer unit, the peel strength of the obtained electrode composite material layer can be improved, and the rate characteristics of the obtained secondary battery can be improved.

[0055] Examples of the (meth)acrylic acid ester monomer include (meth)acrylic acid alkyl ester monomers having 1 ethylenically unsaturated bond. Examples of the (meth)acrylic acid alkyl ester monomer include (meth)acrylic acid alkyl ester monomers having a linear alkyl group and (meth)acrylic acid alkyl ester monomers having a branched alkyl group. For example, as (meth) acrylic acid ester monomers, methyl acrylate, ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate, tert-butyl acrylate, amyl acrylate, hexyl acrylate, heptyl acrylate, octyl acrylate, 2-ethylhexyl acrylate, nonyl acrylate, decyl acrylate, lauryl acrylate, n-tetradecyl acrylate, stearyl acrylate and other alkyl acrylates; methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, tert-butyl methacrylate, amyl methacrylate, hexyl methacrylate, heptyl methacrylate, octyl methacrylate, 2-ethylhexyl methacrylate, nonyl methacrylate, decyl methacrylate, lauryl methacrylate, n-tetradecyl methacrylate, stearyl methacrylate and other alkyl methacrylates, etc. Among them, from the viewpoint of imparting appropriate affinity to the electrolyte to the obtained electrode composite material layer, preferably the alkyl (meth) acrylic acid ester whose alkyl chain is a straight chain, more preferably butyl acrylate and methyl methacrylate. These may be used alone or in combination of two or more.

[0056] Moreover, with all repeating units contained in polymer α as 100.0 mass %, the content ratio of the (meth) acrylate monomer unit in polymer α is preferably 30.0 mass % or more, more preferably 40.0 mass % or more, further preferably 50.0 mass % or more, preferably 98.0 mass % or less, more preferably 95.0 mass % or less. By making the content ratio of the (meth) acrylate monomer unit in polymer α within the above range, the obtained electrode composite material layer can be given a moderate affinity with the electrolyte, and the rate characteristics of the secondary battery having the electrode composite material layer can be improved.

[0057] [Ethylenically unsaturated acid monomer unit]

[0058] The ethylenically unsaturated acid monomer unit is a repeating unit from an ethylenically unsaturated acid monomer. Moreover, polymer α can exert excellent bonding strength due to the ethylenically unsaturated acid monomer unit. Therefore, the electrode composite material layer formed using the slurry composition comprising the binder composition of the present invention can exert more excellent peel strength. In addition, in this specification, "ethylenically unsaturated acid monomer unit" refers to a unit from a monomer comprising an ethylenically unsaturated bond and an acidic group.

[0059] Here, examples of the ethylenically unsaturated acid monomer that can form the ethylenically unsaturated acid monomer unit include monomers having a carboxylic acid group, monomers having a sulfonic acid group, and monomers having a phosphoric acid group in addition to an ethylenically unsaturated bond.

[0060] Examples of the carboxylic acid group-containing monomer include monocarboxylic acids and derivatives thereof, dicarboxylic acids and anhydrides thereof, and derivatives thereof.

[0061] Examples of the monocarboxylic acid include acrylic acid, methacrylic acid, and crotonic acid.

[0062] Examples of the monocarboxylic acid derivative include 2-ethylacrylic acid, isocrotonic acid, α-acetoxyacrylic acid, β-trans-aryloxyacrylic acid, and α-chloro-β-E-methoxyacrylic acid.

[0063] Examples of the dicarboxylic acid include maleic acid, fumaric acid, and itaconic acid.

[0064] Examples of the dicarboxylic acid derivatives include maleic acid monoesters such as methylmaleic acid, dimethylmaleic acid, phenylmaleic acid, chloromaleic acid, dichloromaleic acid, and fluoromaleic acid; and nonyl maleate, decyl maleate, dodecyl maleate, octadecyl maleate, and fluoroalkyl maleate.

[0065] Examples of the anhydride of dicarboxylic acid include maleic anhydride, acrylic anhydride, methylmaleic anhydride, and dimethylmaleic anhydride.

[0066] Furthermore, as the carboxylic acid group-containing monomer, an acid anhydride that generates a carboxyl group by hydrolysis can also be used.

[0067] Examples of the sulfonic acid group-containing monomer include styrene sulfonic acid, vinyl sulfonic acid, methyl vinyl sulfonic acid, (meth)allyl sulfonic acid, 3-allyloxy-2-hydroxypropanesulfonic acid, and 2-acrylamido-2-methylpropanesulfonic acid.

[0068] In the present invention, "(meth)allyl group" means an allyl group and / or a methallyl group.

[0069] Furthermore, examples of the phosphoric acid group-containing monomer include 2-(meth)acryloyloxyethyl phosphate, methyl-2-(meth)acryloyloxyethyl phosphate, and ethyl-(meth)acryloyloxyethyl phosphate.

[0070] In addition, in the present invention, "(meth)acryloyl group" means an acryloyl group and / or a methacryloyl group.

[0071] These ethylenically unsaturated acid monomers can be used alone or in combination of two or more. Moreover, among these ethylenically unsaturated acid monomers, acrylic acid, methacrylic acid, itaconic acid, maleic acid and fumaric acid are preferred from the viewpoint of further improving the peel strength of the obtained electrode composite material layer, and acrylic acid and methacrylic acid are more preferred.

[0072] Moreover, in the case of 100.0 mass % of all repeating units in polymer α, the content ratio of the ethylenically unsaturated acid monomer unit in polymer α is preferably more than 1.0 mass %, more preferably more than 1.5 mass %, more preferably more than 2.0 mass %, more preferably more than 3.0 mass %, preferably less than 10.0 mass %, more preferably less than 8.0 mass %, more preferably less than 6.0 mass %, more preferably less than 5.0 mass %. By making the content ratio of the ethylenically unsaturated acid monomer unit more than the above lower limit, the peel strength of the electrode composite material layer formed using the slurry composition comprising the binder composition can be improved. In particular, by making the content ratio of the ethylenically unsaturated acid monomer unit less than the above upper limit, the flexibility of the polymer α can be improved, so that the peel strength of the electrode composite material layer obtained can be further improved.

[0073] [Crosslinking monomer unit]

[0074] The crosslinkable monomer unit is a repeating unit from a crosslinkable monomer. A crosslinkable monomer refers to a monomer that can form a crosslinked structure when polymerized. Moreover, if the polymer α contains a crosslinkable monomer unit, the peel strength of the obtained electrode composite material layer can be further improved. As an example of a crosslinkable monomer, a monomer having two or more reactive groups per molecule can be cited.

[0075] More specifically, as the crosslinkable monomer, there can be mentioned a polyfunctional ethylenically unsaturated carboxylic acid ester monomer having two or more ethylenically unsaturated bonds.

[0076] Examples of the difunctional ethylenically unsaturated carboxylic acid ester monomer having two ethylenically unsaturated bonds in the molecule include allyl acrylate, allyl methacrylate, ethylene glycol diacrylate, ethylene glycol dimethacrylate, 2-hydroxy-3-acryloxypropyl methacrylate, polyethylene glycol diacrylate, ethoxylated propoxylated bisphenol A diacrylate, ethoxylated bisphenol A diacrylate, 9,9-bis[4-(2-acryloxyethoxy)phenyl]fluorene, propoxylated bisphenol A diacrylate, tricyclodecane dimethanol diacrylate, 1,10-decanediol diacrylate, 1,6-hexanediol Dimethacrylate, 1,9-nonanediol diacrylate, polypropylene glycol diacrylate, polypropylene glycol dimethacrylate, polybutylene glycol diacrylate, ethylene glycol dimethacrylate, diethylene glycol dimethacrylate, polyethylene glycol dimethacrylate, ethoxylated bisphenol A dimethacrylate, tricyclodecane dimethanol dimethacrylate, 1,10-decanediol dimethacrylate, 1,6-hexanediol dimethacrylate, 1,9-nonanediol dimethacrylate, neopentyl glycol dimethacrylate, ethoxylated polypropylene glycol dimethacrylate and glycerol dimethacrylate, etc.

[0077] Examples of the trifunctional ethylenically unsaturated carboxylic acid ester monomer having three ethylenically unsaturated bonds in the molecule include ethoxylated isocyanuric acid triacrylate, ε-caprolactone-modified tris(2-acryloyloxyethyl)isocyanurate, ethoxylated glycerol triacrylate, pentaerythritol triacrylate, trimethylolpropane triacrylate, and trimethylolpropane trimethacrylate.

[0078] Examples of the tetrafunctional or higher-functional ethylenically unsaturated carboxylic acid ester monomer having four or more ethylenically unsaturated bonds in the molecule include ditrimethylolpropane tetraacrylate, ethoxylated pentaerythritol tetraacrylate, pentaerythritol tetraacrylate, dipentaerythritol polyacrylate, and dipentaerythritol hexaacrylate.

[0079] Among them, from the viewpoint of improving the peel strength and flexibility of the obtained electrode composite material layer, preferred are allyl methacrylate (2-functional), ethylene glycol dimethacrylate (2-functional), trimethylolpropane triacrylate (3-functional) and ethoxylated pentaerythritol tetraacrylate (4-functional).

[0080] Moreover, with all repeating units contained in polymer α as 100.0% by mass, the content ratio of the crosslinking monomer unit in polymer α is preferably 0.01% by mass or more, more preferably 0.05% by mass or more, further preferably 0.1% by mass or more, preferably 5.0% by mass or less, more preferably 2.0% by mass or less, and further preferably 1.5% by mass or less. By making the content ratio of the crosslinking monomer unit in polymer α above the above lower limit, the peel strength of the obtained electrode composite material layer can be further improved. In addition, by making the content ratio of the crosslinking monomer unit in polymer α below the above upper limit, the flexibility of the obtained electrode composite material layer can be improved, so that the peel strength of the obtained electrode composite material layer can be further improved.

[0081] [Other monomer units]

[0082] Furthermore, polymer α may also include other monomer units from other monomers that can copolymerize with various monomers as described above. As other monomers that can form such other monomer units, known monomers that can be used to manufacture the adhesive component in the electrode binder composition of the non-aqueous secondary battery can be used. More specifically, for example, as other monomers, nitrile-containing monomers and amide-containing monomers described in detail in the project of <Polymer β> and aromatic vinyl monomers described in detail in the project of <Polymer γ> can be cited. They can be used alone or in combination of two or more.

[0083] Furthermore, when all repeating units in the polymer α are taken as 100.0% by mass, the content ratio of other monomer units in the polymer α is preferably 50.0% by mass or less, and may be 0.0% by mass.

[0084] [NMP insoluble content]

[0085] Here, the amount of insoluble components when polymer α is mixed with N-methyl-2-pyrrolidone at a concentration of 8% by mass needs to be 70% by mass or more, preferably 80% by mass or more, more preferably 90% by mass or more, and can also be 100% by mass, that is, polymer α is completely insoluble in N-methyl-2-pyrrolidone (hereinafter, sometimes abbreviated as "NMP".). If the amount of NMP insoluble components is 70% by mass or more, the battery characteristics of the secondary battery having the obtained electrode composite material layer can be further improved. In addition, the amount of NMP insoluble components can be controlled by adjusting the amount of crosslinking monomers in the monomer composition for preparing polymer α. The amount of NMP insoluble components of polymer α can be measured by the method described in the examples.

[0086] [Method for preparing polymer α]

[0087] The preparation method of the above-mentioned polymer α is not particularly limited. The polymerization method when preparing the polymer α is not particularly limited, and any method of solution polymerization, suspension polymerization, bulk polymerization, emulsion polymerization, etc. can be used. In addition, as the polymerization reaction, any reaction such as ion polymerization, free radical polymerization, and living free radical polymerization can be used. Moreover, the emulsifier, dispersant, polymerization initiator, chain transfer agent, etc. that can be used for polymerization can use those commonly used.

[0088] <Polymer β>

[0089] Polymer β is a component that can impart moderate viscosity to the slurry composition when preparing a slurry composition. In addition, polymer β is a component that can act as a binder in the electrode composite material layer together with polymer α. In addition, polymer β is a component that is easily soluble in the organic solvent constituting the binder composition. In addition, polymer β is "easily soluble" in an organic solvent, meaning that the dried polymer β is placed in N-methyl-2-pyrrolidone at a temperature of 60°C for 72 hours, and the dry mass of the insoluble component obtained by filtering with 200 meshes is 50% by mass or less relative to the total mass of the dried polymer β used. Polymer β is a component that plays a role in improving the uniformity and peel strength of the obtained electrode, and plays a role in improving the rate characteristics and cycle characteristics of the obtained secondary battery.

[0090] As described above, with all repeating units contained in polymer β as 100 mass %, polymer β needs to contain nitrile-containing monomer units in a ratio of more than 70.0 mass % and less than 95.0 mass %. Furthermore, polymer β preferably contains nitrile-containing monomer units of more than 80.0 mass %. If the ratio of nitrile-containing monomer units in polymer β is above the above lower limit, polymer β becomes easy to be adsorbed on electrode active material in the case of preparing slurry composition, and film coating electrode active material can be well. Thus, the battery characteristics of the secondary battery obtained can be improved. In addition, if the ratio of nitrile-containing monomer units in polymer β is below the above upper limit, the flexibility of the electrode obtained can be further improved.

[0091] As nitrile-containing monomers that can be used to form nitrile-containing monomer units, α, β-ethylenically unsaturated nitrile monomers can be cited. Specifically, as α, β-ethylenically unsaturated nitrile monomers, for example: acrylonitrile; α-halogenated acrylonitriles such as α-chloroacrylonitrile and α-bromoacrylonitrile; α-alkyl acrylonitriles such as methacrylonitrile and α-ethylacrylonitrile, etc. They can be used alone or in combination of two or more. Among them, from the viewpoint of increasing the adhesive force exerted by polymer β and thus increasing the peel strength of the obtained electrode, acrylonitrile and methacrylonitrile are preferred, and acrylonitrile is more preferred. They can be used alone or in combination of two or more.

[0092] Furthermore, as described above, in addition to the nitrile-containing monomer unit, the polymer β also needs to include at least one of an amide-containing monomer unit and a (meth)acrylate monomer unit having an alkyl chain with a carbon number of 1 or more and 6 or less. Among them, it is preferred that the polymer β includes both an amide-containing monomer unit and a (meth)acrylate monomer unit having an alkyl chain with a carbon number of 1 or more and 6 or less. Moreover, taking all repeating units in the polymer β as 100% by mass, the total content ratio of the amide-containing monomer unit and the (meth)acrylate monomer unit needs to be 0.1% by mass or more and 20% by mass or less, preferably 0.5% by mass or more, more preferably 1% by mass or more, and preferably 15% by mass or less.

[0093] The amide-containing monomer unit can be formed using an amide-containing monomer. As an amide-containing monomer, it is not particularly limited, and N-vinylacetamide, (methyl) acrylamide, N-methylol (methyl) acrylamide, dimethyl (methyl) acrylamide, diethyl (methyl) acrylamide, N-methoxymethyl (methyl) acrylamide, dimethylaminopropyl (methyl) acrylamide, etc. can be cited. Among them, as an amide-containing monomer for forming polymer β, preferably (methyl) acrylamide, more preferably acrylamide. With all repeating units in polymer β as 100% by mass, the content ratio of the amide-containing monomer unit can be 0% by mass, preferably 0.05% by mass or more, more preferably 0.1% by mass or more, further preferably 0.5% by mass or more, further preferably 1.0% by mass or more, preferably 5% by mass or less, more preferably 2% by mass or less. If the content ratio of the amide-containing monomer unit is above the above lower limit, the flexibility and peel strength of the obtained electrode can be further improved.

[0094] The (meth)acrylate monomer unit having an alkyl chain with a carbon number of 1 or more and 6 or less can be formed using a (meth)acrylate monomer having an alkyl chain with a carbon number of 1 or more and 6 or less. As a (meth)acrylate monomer having an alkyl chain with a carbon number of 1 or more and 6 or less, a (meth)acrylate monomer having an alkyl chain with a carbon number of 1 or more and 6 or less can be cited, that is, methyl acrylate, ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate, tert-butyl acrylate, pentyl acrylate, hexyl acrylate and other alkyl acrylates; methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, tert-butyl methacrylate, pentyl methacrylate, hexyl methacrylate and other alkyl methacrylates, etc. Among them, from the viewpoint of imparting a moderate affinity to the electrolyte to the obtained electrode composite material layer, it is preferred that the alkyl (meth)acrylate having a linear alkyl chain is more preferably butyl acrylate. In addition, these can be used only one, or two or more can be used in combination. Moreover, with all repeating units in polymer β being 100 mass %, the content ratio of the (methyl) acrylate monomer unit having a carbon number of 1 or more and 6 or less can be 0 mass %, preferably 0.05 mass % or more, more preferably 0.1 mass % or more, further preferably 1 mass % or more, preferably 20 mass % or less, more preferably 15 mass % or less. If the content ratio of the (methyl) acrylate monomer unit having a carbon number of 1 or more and 6 or less is above the above lower limit, the flexibility and peel strength of the obtained electrode can be further improved.

[0095] And then, except above-mentioned monomeric unit, polymer β can also comprise other monomeric units such as ethylenically unsaturated acid monomeric unit.As the monomer that can be used to form ethylenically unsaturated acid monomeric unit, it is not particularly limited, and can use the various monomers listed in the item of <polymer α>.And, for example, with all repeating units in polymer β as 100 mass %, the containing ratio of ethylenically unsaturated acid monomeric unit is preferably more than 0.1 mass %, more preferably more than 1 mass %, preferably less than 10 mass %, more preferably less than 5 mass %.

[0096] Moreover, the weight average molecular weight of polymer β is preferably more than 200000, more preferably more than 400000, further preferably more than 600000, preferably less than 2000000, more preferably less than 1500000, and more preferably less than 1300000. If the weight average molecular weight of polymer β is more than the above lower limit, the peel strength of the obtained electrode can be further improved. In addition, if the weight average molecular weight of polymer β is less than the above upper limit, the rate characteristics and cycle characteristics of the obtained secondary battery can be improved.

[0097] The polymer β can be produced by, for example, a known method as described in the section [Method for producing polymer α], and is not particularly limited.

[0098] <Polymer γ>

[0099] Polymer γ is a component that can play a role in further improving the softness and uniformity of the obtained electrode. In addition, polymer γ is a component that can act as a binder in the electrode composite material layer together with polymer α and polymer β. In addition, polymer γ is a component that is easily soluble in the organic solvent that constitutes the binder composition. In addition, polymer γ is "easily soluble" in an organic solvent, which means that the dried polymer γ is placed in N-methyl-2-pyrrolidone at a temperature of 60°C for 72 hours, and the dry mass of the insoluble component obtained by filtering with 200 meshes is 50% by mass or less relative to the total mass of the dried polymer γ used. If the binder composition contains polymer γ as a binder component, the softness and uniformity of the obtained electrode can be further improved. In addition, if the binder composition contains polymer γ as a binder component, the peel strength of the obtained electrode can be improved.

[0100] The iodine value of polymer γ is 5 g / 100 g or more and 100 g / 100 g or less, preferably 10 g / 100 g or more, and more preferably 20 g / 100 g or more. If the iodine value of polymer γ is above the above lower limit, the flexibility of the obtained electrode can be further improved. In addition, if the iodine value of polymer γ is below the above upper limit, the uniformity and peel strength of the obtained electrode can be further improved.

[0101] Moreover, the weight average molecular weight of polymer γ is preferably more than 5000, more preferably more than 70000, further preferably more than 100000, preferably less than 500000, more preferably less than 400000, and further preferably less than 350000. If the weight average molecular weight of polymer γ is above the above lower limit, the peel strength of the obtained electrode can be further improved. In addition, if the weight average molecular weight of polymer γ is below the above upper limit, the rate characteristics and cycle characteristics of the obtained secondary battery can be improved.

[0102] The composition of polymer γ is not particularly limited as long as it satisfies the above iodine value range, and may be any composition. Preferably, polymer γ contains aromatic vinyl monomer units, nitrile group-containing monomer units, ethylenically unsaturated acid monomer units, and linear alkylene structural units having 4 or more carbon atoms.

[0103] As monomers that can be used to form aromatic vinyl monomer units, aromatic vinyl monomers such as styrene, α-methylstyrene, butoxystyrene, vinyltoluene, and vinylnaphthalene can be cited. In addition, aromatic vinyl monomers do not contain acidic groups. They can be used alone or in combination of two or more. Among them, from the viewpoint of good copolymerizability, styrene is preferred. When all repeating units (the total of structural units and monomer units) of polymer γ are 100% by mass, the content ratio of aromatic vinyl monomer units of polymer γ is preferably 30% by mass or more, more preferably 35% by mass or more, further preferably 40% by mass or more, preferably 55% by mass or less, more preferably 50% by mass or less, and further preferably 45% by mass or less.

[0104] In addition, as a monomer that can be used to form a nitrile-containing monomer unit, the same monomers as the various monomers listed in the above-mentioned <polymer β> item can be cited. They can be used alone or in combination of two or more. Among them, from the viewpoint of improving the bonding force that can be exerted by polymer γ, acrylonitrile and methacrylonitrile are preferred, and acrylonitrile is more preferred. They can be used alone or in combination of two or more. In the case of taking all repeating units of polymer γ as 100% by mass, the content ratio of the nitrile-containing monomer unit is preferably 10% by mass or more, more preferably 13% by mass or more, further preferably 18% by mass or more, preferably 40% by mass or less, more preferably 33% by mass or less, and further preferably 28% by mass or less.

[0105] In addition, as a monomer that can be used to form an ethylenically unsaturated acid monomer unit, it is possible to use the same monomers as the various monomers listed in the item [ethylenically unsaturated acid monomer unit] of the above-mentioned <polymer α>. Among them, from the viewpoint of being particularly efficient in capturing transition metal ions that are sometimes dissolved from the positive electrode active material, acrylic acid and methacrylic acid are preferred, and methacrylic acid is more preferred. In the case where all repeating units of polymer γ are 100% by mass, the content ratio of the ethylenically unsaturated acid monomer unit is preferably 0.1% by mass or more, more preferably 1% by mass or more, preferably 10% by mass or less, and more preferably 6% by mass or less.

[0106] Here, the linear alkylene structural unit having 4 or more carbon atoms refers to a linear alkylene structural unit having 4 or more carbon atoms (hereinafter, also simply referred to as an "alkylene structural unit") consisting only of the general formula: n H 2n -[wherein n is an integer of 4 or more] is a repeating unit composed of a linear alkylene structure having 4 or more carbon atoms. The method for introducing the linear alkylene structural unit having 4 or more carbon atoms into the polymer γ is not particularly limited, and examples thereof include the following method (1) or (2):

[0107] (1) a method of preparing a polymer from a monomer composition containing a conjugated diene monomer, and hydrogenating the polymer to convert the conjugated diene monomer unit into a linear alkylene structural unit having 4 or more carbon atoms;

[0108] (2) A method for producing a polymer from a monomer composition containing a 1-olefin monomer having 4 or more carbon atoms, such as 1-butene and 1-hexene. These conjugated diene monomers and 1-olefin monomers can be used alone or in combination of two or more.

[0109] Among them, the method (1) is preferred because it is easy to produce a polymer.

[0110] In addition, as conjugated diene monomers that can be used in the method of (1) above, for example, conjugated diene compounds having carbon atoms of 4 or more, such as 1,3-butadiene, isoprene, 2,3-dimethyl-1,3-butadiene, and 1,3-pentadiene, can be cited. They can be used alone or in combination of two or more. Among them, 1,3-butadiene is preferred. That is, the straight-chain alkylene structural unit having carbon atoms of 4 or more is preferably a structural unit (conjugated diene hydride unit) obtained by hydrogenating a conjugated diene monomer unit, and more preferably a structural unit (1,3-butadiene hydride unit) obtained by hydrogenating a 1,3-butadiene unit. Moreover, the selective hydrogenation of the conjugated diene monomer unit can be carried out using known methods such as an oil layer hydrogenation method and an aqueous layer hydrogenation method.

[0111] The polymer γ can be prepared, for example, by polymerizing a monomer composition containing the above-mentioned monomers to obtain a copolymer and then hydrogenating (adding hydrogen) the obtained copolymer as necessary, and is not particularly limited.

[0112] Moreover, when all repeating units in polymer γ are 100 mass %, the content ratio of the straight-chain alkylene structural units having 4 or more carbon atoms is preferably 15 mass % or more, more preferably 20 mass % or more, further preferably 25 mass % or more, preferably 50 mass % or less, more preferably 45 mass % or less, further preferably 40 mass % or less.

[0113] In addition, when the linear alkylene structural units having 4 or more carbon atoms contained in the polymer γ are formed by preparing a polymer from a monomer composition containing a conjugated diene monomer and hydrogenating the polymer, it is preferred that the total content ratio of the linear alkylene structural units having 4 or more carbon atoms contained in the polymer γ and the conjugated diene monomer units remaining in the polymer γ without being hydrogenated satisfies the above range.

[0114] <Content ratio of polymers α to γ>

[0115] Here, the content of the polymers α to γ ​​satisfying the above-mentioned properties and / or composition conditions in the adhesive composition is preferably within the following ranges, respectively, based on 100 mass % of the content of the adhesive component in the adhesive composition.

[0116] First, the content a of the above-mentioned polymer α is preferably more than 5% by mass, more preferably more than 10% by mass, preferably less than 60% by mass, more preferably less than 50% by mass, further preferably less than 40% by mass, and particularly preferably less than 30% by mass. If the content a of polymer α is more than the above-mentioned lower limit, the flexibility of the electrode formed using the binder composition can be fully improved. In addition, if the content a of polymer α is less than the above-mentioned upper limit, the peel strength of the obtained electrode can be improved.

[0117] Furthermore, the content b of the above-mentioned polymer β is preferably 20% by mass or more, more preferably 30% by mass or more, further preferably 35% by mass or more, further preferably 40% by mass or more, and preferably 94% by mass or less. If the content b of polymer β is above the above lower limit, the uniformity of the obtained electrode can be improved, and the cycle characteristics of the secondary battery having the electrode can be improved. In addition, if the content b of polymer β is below the above upper limit, the rate characteristics of the obtained secondary battery can be improved.

[0118] In addition, the content c of the above-mentioned polymer γ is preferably 0.1% by mass or more, more preferably 1% by mass or more, preferably 50% by mass or less, more preferably 40% by mass or less, further preferably 30% by mass or less, and particularly preferably 20% by mass or less. If the content c of polymer γ is above the above lower limit, the flexibility, uniformity and peel strength of the obtained electrode can be further improved. In addition, if the content c of polymer γ is below the above upper limit, the battery characteristics of the obtained secondary battery can be further improved.

[0119] <Relationship between content ratios a to c>

[0120] With respect to the content a of polymer α and the content b of polymer β, the value of the ratio (%) of polymer α in the total content of polymer α and β represented by the formula: a / (a+b)×100 preferably satisfies 10≤a / (a+b)×100≤50, more preferably satisfies 10≤a / (a+b)×100≤40, and further preferably satisfies 10≤a / (a+b)×100≤35. If the value of the above formula: a / (a+b)×100 is 10 or more, the adhered components can be bonded to each other at a sufficient frequency point by polymer α, and the softness of the obtained electrode composite material layer can be further improved. In addition, if the value of the above formula: a / (a+b)×100 is 50 or less, the uniformity of the obtained electrode can be improved, and the rate characteristics and cycle characteristics of the obtained secondary battery can be further improved.

[0121] In addition, with respect to the content a of polymer α and the content c of polymer γ, the value of the ratio (%) of polymer α in the total content of polymer α and γ represented by the formula: a / (a+c)×100 preferably satisfies 20≤a / (a+c)×100≤90, and more preferably satisfies 50≤a / (a+c)×100≤90. If the value of the above formula: a / (a+c)×100 is 20 or more, the peel strength of the obtained electrode composite material layer can be further improved. In addition, if the value of the above formula: a / (a+c)×100 is 90 or less, the rate characteristics of the obtained secondary battery can be further improved.

[0122] <NMP Solubility of Polymers α and β>

[0123] The above-mentioned polymer α and β are preferably a polymer that satisfies the solid content concentration of 8% by mass of N-methyl-2-pyrrolidone mixed solution prepared by containing polymer α with a content rate a and polymer β with a content rate b as solid components, and the ratio of the insoluble component amount in the mixed solution becomes 30% by mass or more and 80% by mass or less. Moreover, the ratio of the above-mentioned insoluble component amount of polymer α and β is preferably 35% by mass or more and 75% by mass or less. If the ratio of the above-mentioned insoluble component amount is more than 30% by mass, the flexibility of the obtained electrode composite material layer can be further improved. In addition, if the ratio of the above-mentioned insoluble component amount is less than 80% by mass, the rate characteristics and cycle characteristics of the obtained secondary battery can be improved.

[0124] <Other adhesive materials>

[0125] In addition to the above-mentioned polymer α~γ, the adhesive composition of the present invention may also contain other adhesive materials different from them as other adhesive components. As such adhesive materials, fluorine-based polymer adhesive materials such as polyvinylidene fluoride, polyvinyl acetate-based adhesive materials, polyacrylic acid-based adhesive materials, polyvinyl alcohol-based adhesive materials, etc. can be cited. In addition, when the adhesive composition of the present invention contains other adhesive components, the mass of all adhesive components contained in the adhesive composition is 100 mass %, and the content ratio of the other adhesive components is preferably less than 50 mass %, more preferably less than 40 mass %, further preferably less than 30 mass %, and may also be 0 mass %, that is, the adhesive composition of the present invention is an adhesive composition containing only the above-mentioned polymer α~γ as an adhesive component.

[0126] <Plasticizer>

[0127] Plasticizer is a component that improves the flexibility of the obtained electrode by acting on the polymer contained as a binder component, and then can play a role in improving the rate characteristics and cycle characteristics of the secondary battery. In addition, the plasticizer is a component that can play a role in protecting the surface of the electrode active material in the obtained electrode. From this point of view, the plasticizer is also a component that can play a role in improving the battery characteristics of the secondary battery.

[0128] There are no particular limitations on the plasticizers used in the adhesive composition of the present invention, and various compounds can be used. More specifically, the plasticizers that can be used include: phosphate plasticizers such as diphenyl octyl phosphate, tributyl phosphate, trimethyl phosphate, tricresyl phosphate, triphenyl phosphate, tri(xylene) phosphate, tri(2-ethylhexyl) phosphate, 2-ethylhexyl diphenyl phosphate, triisopropylphenyl phosphate, resorcinol bis(diphenyl phosphate), bisphenol A bisdiphenyl phosphate, bisphenol A biscresyl phosphate, and 2-ethylhexyl diphenyl phosphate; citric acid ester plasticizers such as tributyl citrate and acetylcitrate tributyl ester; epoxy plasticizers such as epoxidized soybean oil and epoxidized linseed oil, di(butoxyethoxyethyl) phthalate, isophthalic acid esters such as bis(diphenyl phosphate) and bis(bis(diphenyl phosphate)). dibutyloxyethyl phthalate, di(butoxyethoxyethyl) isophthalate, dimethoxyethyl phthalate, dibutyl phthalate, dioctyl phthalate, diisononyl phthalate, diisodecyl phthalate, diundecyl phthalate, butyl benzyl phthalate, dimethoxyethyl phthalate, diethoxyethyl phthalate, dibutoxyethyl phthalate, di(2-ethylhexyl) phthalate, diisobutyl phthalate, diheptyl phthalate, dicyclohexyl phthalate, diphenyl phthalate, butyl benzyl phthalate, di(2-ethylhexyl) isophthalate, isophthalic acid Phthalate plasticizers such as diisooctyl ester; tetrahydrophthalate plasticizers such as di(2-ethylhexyl)tetrahydrophthalate, di-n-octyl tetrahydrophthalate, and diisodecyl tetrahydrophthalate; adipate plasticizers such as dibutoxyethyl adipate, di(butoxyethoxyethyl) adipate, di-2-hexyl adipate, di(2-ethylhexyl) adipate, diisodecyl adipate, diisononyl adipate, and dibutyl adipate; sebacic acid plasticizers such as dibutoxyethyl sebacate, di(butoxyethoxyethyl) sebacate, di-n-butyl sebacate, di(2-ethylhexyl) sebacate, and di-2-ethylhexyl sebacate Ester plasticizers; azelaic acid ester plasticizers such as dibutoxyethyl azelate, di(butoxyethoxyethyl) azelate, di(2-ethylhexyl) azelate, diisooctyl azelate, di-n-hexyl azelate, and di-2-hexyl azelate; trimellitic acid ester plasticizers such as tri(2-ethylhexyl) trimellitic acid ester; fumaric acid ester plasticizers such as dibutyl fumarate; oleic acid ester plasticizers such as butyl oleate; polyester plasticizers; trimellitic acid derivatives such as tri(2-ethylhexyl) trimellitic acid ester, tri-n-octyl trimellitic acid, tri-isodecyl trimellitic acid, tri-isooctyl trimellitic acid, tri-n-hexyl trimellitic acid, tri-isononyl trimellitic acid, and tri-isodecyl trimellitic acid.

[0129] In addition, as a plasticizer, a compound obtained by esterifying an alkane dicarboxylic acid such as succinic acid, glutaric acid, adipic acid, suberic acid, azelaic acid and an alcohol having an ether bond in the molecule such as methoxytriethoxyethanol, methoxytetraethoxyethanol, butoxytriethoxyethanol, pentyloxytetraethoxyethanol, ethoxytripropoxypropanol, ethoxytetrapentyloxypentanol, etc., can be cited as a plasticizer containing an alkyl chain with a carbon number of more than 4. Among them, as a preferred plasticizer, a compound containing an alkyl chain with a carbon number of more than 4 and containing at least one polar group selected from a phosphate group, a carbonyl group and a hydroxyl group can be cited. In particular, as a plasticizer, a phosphate ester plasticizer is preferred, and 2-ethylhexyl diphenyl phosphate is more preferred. In addition, the carbon number of the alkyl chain contained in the plasticizer is not particularly limited and can be less than 10.

[0130] Due to the high affinity with the (meth) acrylate monomer units contained in the above-mentioned polymer α, the (meth) acrylate monomer units contained in the polymer β, the nitrile-containing monomer units contained in the polymer β, and the nitrile-containing monomer units contained in the polymer γ as an optional component, and having polar groups, it can be preferably contained as a plasticizer, an alkyl chain containing more than 4 carbon atoms and a compound containing at least one polar group selected from a phosphate group, a carbonyl group, and a structure represented by the general formula R-OH (R is a saturated or unsaturated hydrocarbon chain) There is a tendency to accompany the side of the binder components such as polymers α and β in a binder composition with an organic solvent as a dispersion medium. Therefore, in the case of using a binder composition to form an electrode composite material layer, the plasticizer is uniformly dispersed in the electrode composite material layer and well maintained in the electrode composite material layer. Furthermore, it can be considered that in the case of using an electrode with the electrode composite material layer to form a secondary battery, there is a tendency that the plasticizer is not easy to move to the electrolyte side. Therefore, by combining a compound containing an alkyl chain having more than 4 carbon atoms and containing at least one polar group selected from a phosphate group, a carbonyl group and a structure represented by the general formula R-OH (R is a saturated or unsaturated hydrocarbon chain) as a plasticizer with the binder composition, the flexibility of the obtained electrode can be greatly improved, and the degradation of battery characteristics such as the rate characteristics and cycle characteristics of the obtained secondary battery can be effectively suppressed.

[0131] In addition, the molecular weight of the plasticizer is preferably less than 1000, more preferably less than 900, preferably more than 100, more preferably more than 200. If the molecular weight of the plasticizer is below the above upper limit, the flexibility of the electrode obtained can be further improved. In addition, if the molecular weight of the plasticizer is above the above lower limit, the peel strength of the electrode obtained can be further improved.

[0132] The decomposition potential of the plasticizer is preferably 3.5 V or more, more preferably 4.0 V or more. The decomposition potential is usually 10 V or less. If the decomposition potential of the plasticizer is equal to or more than the above lower limit, the rate characteristics and cycle characteristics of the obtained secondary battery can be further improved.

[0133] In addition, the boiling point of the plasticizer is preferably higher than the boiling point of the organic solvent contained in the binder composition. In addition, the boiling point of the plasticizer refers to the boiling point of 1atm. If the boiling point of the plasticizer is higher than the boiling point of the organic solvent, it is possible to suppress the volatilization of the plasticizer when heating and drying is performed when manufacturing the electrode, so that the plasticizer remains well in the electrode composite material layer. Furthermore, the plasticizer is preferably a liquid substance at room temperature (25°C).

[0134] And then, with the total content of binder component and plasticizer as 100 mass %, the content of plasticizer in binder composition is preferably 0.1 mass % or more, more preferably 0.5 mass % or more, more preferably 1.2 mass % or more, preferably 30 mass % or less, more preferably 15 mass % or less, more preferably 12 mass % or less. If the content of plasticizer is above the lower limit, the flexibility of the electrode obtained can be further improved. In addition, if the content of plasticizer is below the upper limit, the peel strength of the electrode obtained can be improved. And then, if the content of plasticizer is below the upper limit, the rate characteristics and cycle characteristics of the secondary battery obtained can be further improved.

[0135] <Organic Solvents>

[0136] In addition, examples of the organic solvent of the adhesive composition of the present invention include alcohols such as methanol, ethanol, n-propanol, isopropanol, n-butanol, isobutanol, tert-butanol, pentanol, hexanol, heptanol, octanol, nonanol, decanol, and amyl alcohol; ketones such as acetone, methyl ethyl ketone, and cyclohexanone; esters such as ethyl acetate and butyl acetate; diethyl ether, diethyl ether, dimethicone ... Ethers such as alkane and tetrahydrofuran; amide-based polar organic solvents such as N,N-dimethylformamide and N-methyl-2-pyrrolidone (NMP); aromatic hydrocarbons such as toluene, xylene, chlorobenzene, o-dichlorobenzene, and p-dichlorobenzene, etc. These may be used alone or in combination of two or more.

[0137] Among them, NMP is preferred as the organic solvent.

[0138] <Other ingredients>

[0139] In addition to the above-mentioned components, the binder composition of the present invention may also contain components such as reinforcing materials, leveling agents, viscosity modifiers, electrolyte additives, etc. These are not particularly limited as long as they do not affect the battery reaction, and known ones such as those described in International Publication No. 2012 / 115096 can be used. In addition, these components can be used alone or in combination of two or more in any ratio.

[0140] <Preparation of Adhesive Composition>

[0141] Moreover, the binder composition of the present invention can be prepared by mixing the above-mentioned polymer α and β as the binder component, a plasticizer, an organic solvent, and other optional components by a known method. Specifically, the binder composition can be prepared by mixing the above-mentioned components using a mixer such as a ball mill, a sand mill, a bead mill, a pigment disperser, a grinder, an ultrasonic disperser, a homogenizer, a planetary mixer, Filmix, etc. In addition, the solid content concentration of the binder composition is not particularly limited, and can be, for example, more than 5% by mass and less than 60% by mass.

[0142] (Slurry composition for non-aqueous secondary battery electrodes)

[0143] The non-aqueous secondary battery electrode slurry composition of the present invention comprises an electrode active material, a conductive material and the above-mentioned binder composition, and optionally comprises other components. That is, the slurry composition of the present invention comprises an electrode active material, a conductive material, the above-mentioned polymers α and β, a plasticizer and an organic solvent, and optionally comprises other components. Moreover, the slurry composition of the present invention, because it comprises the above-mentioned binder composition, can form an electrode with excellent flexibility and uniformity at a high level and improve the rate characteristics and cycle characteristics of the secondary battery comprising the obtained electrode.

[0144] In addition, below, although the case where the slurry composition for secondary battery electrodes is a slurry composition for lithium ion secondary battery positive electrodes is described as an example, the present invention is not limited to the following one example.

[0145] <Electrode Active Material>

[0146] The electrode active material is a material that transfers electrons in the electrode of the secondary battery. In addition, as the positive electrode active material for lithium ion secondary batteries, a material that can insert and release lithium is generally used.

[0147] Specifically, as the positive electrode active material for the lithium ion secondary battery, there is no particular limitation, and examples thereof include lithium cobalt oxide (LiCoO2), lithium manganate (LiMn2O4), lithium nickel oxide (LiNiO2), lithium-containing composite oxide of Co-Ni-Mn (Li(CoMnNi)O2), lithium-containing composite oxide of Ni-Mn-Al, lithium-containing composite oxide of Ni-Co-Al, olivine-type lithium iron phosphate (LiFePO4), olivine-type lithium manganese phosphate (LiMnPO4), Li2MnO3-LiNiO2-based solid solution, Li 1+x Mn 2-x spinel compound with excess lithium represented by O4 (0 < X < 2), Li[Ni 0.17 Li 0.2 Co 0.07 Mn 0.56 O2, LiNi 0.5 Mn 1.5 O4 and other known positive electrode active materials.

[0148] In addition, the particle size of the positive electrode active material is not particularly limited and can be the same as that of the positive electrode active material used in the past. In addition, based on 100% by mass of all the solid components in the slurry composition, the content ratio of the positive electrode active material in the slurry composition can be, for example, 90% by mass or more and 99% by mass or less.

[0149] <Conductive material>

[0150] The conductive material is a material for ensuring electrical contact between the electrode active materials. Moreover, the slurry composition of the present invention preferably contains carbon nanotubes (CNT) as a fibrous carbon material as the conductive material. This is because the CNT can be well dispersed in the slurry composition by the binder composition of the present invention described above. As a result, the dispersibility of other solid components such as the electrode active material in the slurry composition can also be improved. As the CNT, single-walled or multi-walled carbon nanotubes (including stacked cup type in multi-walled carbon nanotubes) can be cited. Moreover, the specific surface area of the CNT is preferably 50 m 2 / g or more, more preferably 70 m 2 / g or more, further preferably 100 m 2 / g or more, and preferably 400 m 2 / g or less, more preferably 350 m 2 / g or less, further preferably 300 m 2 / g or less. If the specific surface area of the CNT is within the above range, good dispersibility of the CNT in the slurry composition can be ensured, thereby stabilizing the viscosity of the slurry composition. In addition, in the present invention, the "specific surface area" refers to the nitrogen adsorption specific surface area measured by the BET method.

[0151] Furthermore, as a conductive material other than CNT, carbon black (e.g., acetylene black, Ketjen black (registered trademark), furnace black, etc.), carbon nanohorns, ground carbon fibers obtained by sintering and crushing polymer fibers, single-layer or multi-layer graphene, non-woven fabrics formed by polymer fibers, sintered to obtain conductive carbon materials such as carbon non-woven fabric sheets and the like; fibers or foils of various metals, etc. They can be used alone or in combination of two or more. In addition, the particle size of the conductive material is not particularly limited and can be the same as the conductive material used in the past. In addition, taking the total solid content in the slurry composition as 100% by mass, the content ratio of the conductive material in the slurry composition can be, for example, 0.1% by mass or more and 3% by mass or less.

[0152] <Binder Composition>

[0153] As the binder composition, the non-aqueous secondary battery electrode binder composition of the present invention is used. In addition, when the total solid content in the slurry composition is 100% by mass, the content of the binder composition in the slurry composition can be, for example, 0.1% by mass or more and 5% by mass or less.

[0154] <Other ingredients>

[0155] The other components that can be added to the slurry composition are not particularly limited, and examples thereof include the same components as those that can be added to the binder composition of the present invention. The other components may be used alone or in combination of two or more at any ratio.

[0156] <Method for producing slurry composition>

[0157] The above-mentioned slurry composition can be prepared by, for example, dissolving or dispersing the above-mentioned components in an organic solvent. More specifically, the above-mentioned slurry composition of the present invention can be prepared by dividing the operation of adding the above-mentioned components to the organic solvent into multiple stages, or can be prepared by adding the required components to the organic solvent in one operation. When adding the matching components to the organic solvent is carried out in multiple stages, the order of addition and the combination of the added components are not particularly limited.

[0158] The mixing method when adding the compounding components to the organic solvent is not particularly limited, and examples thereof include mixing methods using a mixer such as a ball mill, a sand mill, a bead mill, a pigment disperser, an attritor, an ultrasonic disperser, a homogenizer, a planetary mixer, and Filmix.

[0159] As an organic solvent, an organic solvent identical to an organic solvent that can be coordinated with the binder composition of the present invention can be cited. In addition, as an organic solvent used when manufacturing a slurry composition, an organic solvent contained in the binder composition can be used. In addition, the total amount of various components added when manufacturing a slurry composition is as described in detail in the items of (binder composition for non-aqueous secondary battery electrodes) and (slurry composition for non-aqueous secondary battery electrodes).

[0160] For example, as described in the following item "Method for producing a slurry composition using a binder particle assembly", the slurry composition can be prepared by first preparing a binder particle assembly containing polymers α and β and a plasticizer, and then using the binder particle assembly.

[0161] 《Method for producing a slurry composition using an assembly of binder particles》

[0162] In the method for manufacturing a slurry composition using a binder particle assembly, the slurry composition can be manufactured using the binder particle assembly, which is prepared by spray drying an aqueous dispersion (hereinafter, sometimes referred to as "binder particle slurry") containing at least a plasticizer, a polymer α and a polymer β, and optionally a polymer γ and other components. More specifically, for example, the binder particle assembly prepared as described below can be mixed with an organic solvent, an electrode active material, a conductive material, and other optional components to obtain a slurry composition.

[0163] [Method for producing a binder particle assembly]

[0164] When manufacturing the binder particle assembly, first, the binder particle slurry is sprayed in hot air for drying. Here, as a device for spraying the binder particle slurry, an atomizer can be cited. Moreover, as an atomizer, two methods, a rotating disk method and a pressurized method, can be cited.

[0165] The rotating disc method is to introduce the binder particles into the central part of the disc rotating at high speed, and discharge the binder particles to the outside of the disc by the centrifugal force of the disc, thereby making the binder particles into a mist. In the rotating disc method, the rotation speed of the disc is not particularly limited, preferably more than 5000rpm and less than 30000rpm.

[0166] The pressurization method is a method of pressurizing the binder particle slurry so as to discharge it from the nozzle, thereby making the binder particle slurry into a mist, and examples thereof include a pressurized nozzle method, a pressurized two-fluid nozzle method, etc. In the pressurized two-fluid nozzle method, the air pressure (dispersion air pressure) discharged from the air nozzle for fine-tuning the spray of the binder particle slurry is not particularly limited, but is preferably 0.01 MPa or more and 0.5 MPa or less.

[0167] The temperature of hot air during spray drying is, for example, 80° C. to 250° C. In the spray drying, the method of blowing hot air is not particularly limited, and a known method can be used.

[0168] (Electrode for non-aqueous secondary batteries)

[0169] The electrode for a non-aqueous secondary battery of the present invention has an electrode composite material layer, and the electrode composite material layer includes polymer α and polymer β as binder components, a plasticizer, an electrode active material, and a conductive material. Furthermore, the electrode for a non-aqueous secondary battery of the present invention may be an electrode formed by forming the electrode composite material layer on a current collector. The electrode composite material layer can be formed using the slurry composition of the present invention, or it can be formed according to other methods, as long as it contains the above-mentioned necessary components. In addition, the electrode composite material layer may optionally include polymer γ and other components other than it. The electrode for a non-aqueous secondary battery of the present invention has an electrode composite material layer that satisfies the above-mentioned composition, so it has excellent softness and uniformity, and can improve the rate characteristics and cycle characteristics of the secondary battery.

[0170] In addition, the preferred existence ratio of each component contained in the electrode composite material layer is the same as the preferred existence ratio of each component in the slurry composition. In addition, polymer α is a granular polymer, and when the electrode composite material layer is magnified and observed, the particle shape can be confirmed. In addition, polymer β preferably exists in a manner that covers at least a portion of the surface of solid components such as electrode active materials. Furthermore, polymer γ as an optional component preferably exists in a manner adjacent to CNT. Details about polymers α to γ ​​are described in detail in the item (binder composition).

[0171] <Method for producing electrode>

[0172] In addition, the electrode for the non-aqueous secondary battery of the present invention can be manufactured by, for example, the following steps: a step of coating a slurry composition containing the above-specified components on a current collector (coating step), and a step of drying the slurry composition coated on the current collector to form an electrode composite material layer on the current collector (drying step).

[0173] [Coating process]

[0174] As a method for applying the above-mentioned slurry composition on the current collector, it is not particularly limited, and a known method can be used. Specifically, as a coating method, a doctor blade method, an immersion method, a reverse roller method, a direct roller method, a gravure printing method, an extrusion method, a brush coating method, etc. can be used. At this time, the slurry composition can be applied only on one side of the current collector, or the slurry composition can be applied on both sides of the current collector. The thickness of the slurry film on the current collector before drying after coating can be appropriately set according to the thickness of the electrode composite material layer obtained by drying.

[0175] Here, as the current collector for coating the slurry composition, a material having conductivity and electrochemical durability can be used. Specifically, as the current collector, for example, a current collector formed of iron, copper, aluminum, nickel, stainless steel, titanium, tantalum, gold, platinum, etc. can be used. In addition, the above materials can be used alone or in combination of two or more in any ratio.

[0176] [Drying process]

[0177] The method for drying the slurry composition on the current collector is not particularly limited, and a known method can be used, such as a drying method using warm air, hot air, or low-humidity air; a vacuum drying method; a drying method using irradiation of infrared rays, electron beams, etc. By drying the slurry composition on the current collector in this way, an electrode composite material layer can be formed on the current collector, and an electrode for a secondary battery including the current collector and the electrode composite material layer can be obtained.

[0178] In addition, after the drying process, the electrode composite material layer can be subjected to pressure treatment using mold pressing or roll pressing. By pressure treatment, the adhesion of the electrode composite material layer to the current collector can be improved. In addition, in the case where the electrode composite material layer includes a curable polymer, it is preferred that the above-mentioned polymer is cured after forming the electrode composite material layer.

[0179] (Non-aqueous secondary battery)

[0180] The non-aqueous secondary battery of the present invention has the electrode for the non-aqueous secondary battery of the present invention. More specifically, the non-aqueous secondary battery of the present invention has a positive electrode, a negative electrode, an electrolyte, and a separator, and the electrode for the non-aqueous secondary battery of the present invention is used as at least one of the positive electrode and the negative electrode. Moreover, the non-aqueous secondary battery of the present invention has excellent battery characteristics such as rate characteristics and cycle characteristics because it has the electrode for the non-aqueous secondary battery of the present invention.

[0181] The nonaqueous secondary battery of the present invention preferably uses the nonaqueous secondary battery electrode of the present invention as a positive electrode. In addition, the case where the secondary battery is a lithium ion secondary battery is described below as an example, but the present invention is not limited to the following example.

[0182] <Electrode>

[0183] Here, as an electrode other than the above-mentioned electrode for non-aqueous secondary batteries that can be used in the non-aqueous secondary battery of the present invention, there is no particular limitation, and known electrodes that can be used to manufacture non-aqueous secondary batteries can be used. Specifically, as an electrode other than the above-mentioned electrode for non-aqueous secondary batteries, an electrode formed by forming an electrode composite material layer on a current collector using a known manufacturing method can be used.

[0184] <Electrolyte>

[0185] In addition, as an electrolyte, an organic electrolyte in which a supporting electrolyte is dissolved in an organic solvent can generally be used. As a supporting electrolyte for a lithium ion secondary battery, for example, a lithium salt can be used. As a lithium salt, for example, LiPF6, LiAsF6, LiBF4, LiSbF6, LiAlCl4, LiClO4, CF3SO3Li, C4F9SO3Li, CF3COOLi, (CF3CO)2NLi, (CF3SO2)2NLi, (C2F5SO2)NLi, etc. can be cited. Among them, since it is easily soluble in a solvent and shows a high degree of dissociation, LiPF6, LiClO4, CF3SO3Li are preferred, and LiPF6 is particularly preferred. In addition, the electrolyte can be used alone or in combination of two or more in any ratio. Generally, since there is a tendency that the higher the degree of dissociation, the higher the lithium ion conductivity, the lithium ion conductivity can be adjusted by the type of supporting electrolyte.

[0186] As an organic solvent used in the electrolyte, there is no particular limitation as long as it can dissolve the supporting electrolyte, and preferably carbonates such as dimethyl carbonate (DMC), ethylene carbonate (EC), diethyl carbonate (DEC), propylene carbonate (PC), butylene carbonate (BC), ethyl methyl carbonate (EMC) can be used; esters such as γ-butyrolactone and methyl formate; ethers such as 1,2-dimethoxyethane and tetrahydrofuran; sulfur-containing compounds such as cyclopentane and dimethyl sulfoxide, etc. In addition, a mixed solution of these solvents can also be used. Among them, due to the high dielectric constant and wide stable potential region, carbonates are preferably used, and a mixture of ethylene carbonate and diethyl carbonate is further preferably used.

[0187] In addition, the concentration of the electrolyte in the electrolytic solution can be appropriately adjusted. In addition, a known additive such as vinylene carbonate can be added to the electrolytic solution.

[0188] <Spacer>

[0189] As a separator, there is no particular limitation, and for example, the separators described in Japanese Patent Publication No. 2012-204303 can be used. Among them, from the aspect of being able to make the overall film thickness of the separator thinner, thereby being able to increase the ratio of the electrode active material in the secondary battery and thus increase the capacity per unit volume, a microporous membrane formed of a polyolefin-based (polyethylene, polypropylene, polybutylene, polyvinyl chloride) resin is preferred.

[0190] <Method for producing non-aqueous secondary battery>

[0191] The non-aqueous secondary battery of the present invention can be manufactured by, for example, the following method: overlapping the positive electrode and the negative electrode through a spacer, winding and folding the battery according to the shape of the battery as required, placing the battery container, injecting electrolyte into the battery container, and sealing. In order to prevent the internal pressure of the secondary battery from rising, overcharging and discharging, etc., fuses, PTC elements and other overcurrent protection elements, porous metal mesh, guide plates, etc. can be provided as required. The shape of the secondary battery can be, for example, any one of a coin type, a button type, a sheet type, a cylindrical type, a square type, a flat type, etc.

[0192] Example

[0193] Hereinafter, the present invention will be specifically described based on Examples, but the present invention is not limited to these Examples. In the following description, "%" and "part" indicating an amount are based on mass unless otherwise specified.

[0194] Furthermore, unless otherwise specified, in a polymer produced by copolymerizing a plurality of monomers, the ratio of a monomer unit formed by polymerization of a certain monomer in the polymer generally corresponds to the ratio (charge ratio) of the monomer in all monomers used for polymerization of the polymer.

[0195] Moreover, in the embodiments and comparative examples, various properties of plasticizers, NMP solubility of polymers α to γ, iodine value of polymer γ, weight average molecular weight of polymers β and γ, and ratio of NMP insoluble components of a mixture of polymers α and β are measured or confirmed as follows. In addition, in the embodiments and comparative examples, electrode flexibility, electrode uniformity, peel strength of electrode composite material layer, initial capacity of secondary battery, rate characteristics, and cycle characteristics are evaluated as follows.

[0196] <Various properties of plasticizers>

[0197] The molecular weight of the plasticizer is measured by LC-MS (Liquid Chromatography Mass Spectrometry), and the decomposition potential is measured by CV (Cyclic Voltammetry) as described below.

[0198] A plasticizer was added to a 1M LiPF6 solution (solvent: ethylene carbonate (EC) / ethyl methyl carbonate (EMC) = 3 / 7 (volume ratio)) so that the solid content concentration was 0.2 mass %, thereby obtaining a plasticizer solution. Metallic Li and glassy carbon were placed in the plasticizer solution as reference electrodes, and the starting point of the current value rise when the voltage was changed at an insertion speed of 2 mV / s was taken as the decomposition potential.

[0199] <NMP Solubility of Polymer α (Confirmation of Insoluble Polymer)>

[0200] The polymer α prepared in the examples and comparative examples was vacuum dried for 24 hours at 25°C to obtain a dry polymer (mass: W1g). The obtained dry polymer was placed in NMP at 60°C for 72 hours and then filtered with 200 mesh (75μm) to separate the insoluble components. After washing the insoluble components with methanol, it was dried for 24 hours at 25°C to obtain a dry insoluble component (mass: W2g). The amount of NMP insoluble components of polymer α was calculated from the above W1 and W2 (=W2 / W1×100 (mass %)). Then, for the polymer α prepared in all the examples and comparative examples, it was confirmed that the amount of NMP insoluble components was 70% by mass or more. It was thus confirmed that the polymer α used was an "insoluble polymer".

[0201] <NMP Solubility of Polymers β and γ (Confirmation of Easily Soluble Polymers)>

[0202] The NMP solubility of polymers β and γ was confirmed by the following procedure.

[0203] 25 g of the composition containing polymer β / γ in N-methyl-2-pyrrolidone (NMP) prepared in the examples and comparative examples was added dropwise to 1 L of methanol to precipitate polymer β / γ. The precipitated polymer β / γ was vacuum dried at 25°C for 24 hours to obtain a dry polymer β / γ (mass: W1g). The obtained dry polymer β / γ was placed in NMP at 60°C for 72 hours and then filtered with 200 mesh to separate the insoluble components. After washing the insoluble components with methanol, it was dried at 25°C for 24 hours to obtain a dry insoluble component (mass: W2g). The amount of NMP insoluble components of polymer β / γ was calculated from the above W1 and W2 (=W2 / W1×100 (mass %)). Then, for the polymers β and γ prepared in all the examples, it was confirmed that the amount of NMP insoluble components was 50% by mass or less. In addition, regarding the comparative examples, it was confirmed that the amount of NMP insoluble components in polymers β and γ other than the polymer β prepared in Comparative Example 1 was 50% by mass or less.

[0204] <Iodine value of polymer γ>

[0205] 100 g of the aqueous dispersion of polymer γ prepared in Examples and Comparative Examples (aqueous dispersion before solvent substitution with NMP) was coagulated with 1 liter of methanol and then vacuum dried at 60° C. for 12 hours. The iodine value of the dried readily soluble polymer γ was measured in accordance with JIS K6235 (2006).

[0206] <Weight Average Molecular Weight of Polymers β and γ>

[0207] The weight average molecular weight of polymers β and γ prepared in the examples and comparative examples was measured by gel permeation chromatography (GPC). Specifically, a calibration curve was prepared using polystyrene as a standard substance, and the weight average molecular weight as a standard substance conversion value was calculated. In addition, the measurement conditions were as follows.

[0208] 《Measurement conditions》

[0209] Measuring device

[0210] Column: TSKgelα-M×2 columns ( (Made by Tosoh Corporation)

[0211] Measurement conditions

[0212] Eluent: dimethylformamide (50 mM lithium bromide, 10 mM phosphoric acid)

[0213] Flow rate: 0.5mL / min

[0214] Sample concentration: about 0.5g / L (solid content concentration)

[0215] Injection volume: 200 μL

[0216] Column temperature: 40°C

[0217] Detector: Differential refractive index detector RI (HLC-8320GPC RI detector manufactured by Tosoh Corporation)

[0218] Detector conditions: RI: Pol(+), Res(1.0s)

[0219] Molecular weight marker: Tosoh Corporation polystyrene standard kit PstQuick K

[0220] <Ratio of NMP-insoluble components in a mixture of polymers α and β>

[0221] Under a temperature of 25° C., the polymers α and β prepared or prepared in the examples and comparative examples or components replacing them were added to the NMP solvent at the mixing ratio described in the examples so that the solid content concentration became 8%, thereby preparing 100 g of a (polymer α and β)-NMP mixed solution. The prepared mixed solution was filtered through a metal mesh of 80 mesh (180 μm), and the filtrate was weighed to calculate the ratio (mass %) of the mass of the insoluble components to the total solid content added.

[0222] <Electrode Flexibility>

[0223] The positive electrode composite material layer side of the positive electrode of the lithium ion secondary battery produced in the embodiment and the comparative example is loaded with rods of different diameters, and the positive electrode is wound on the rod to evaluate whether the positive electrode composite material layer is broken. When the positive electrode is wound on the rod, the smaller the diameter of the rod where the positive electrode composite material layer is not broken, the more flexible the positive electrode is, and the better the winding property is. According to the diameter of the thinnest rod where the positive electrode composite material layer is not broken, the flexibility of the electrode (positive electrode) is evaluated using the following benchmarks.

[0224] A: No cracking even when wound around a rod with a diameter of 1.15 mm.

[0225] B: No breakage even when wound around a rod having a diameter of 1.40 mm.

[0226] C: No breakage even when wound around a rod having a diameter of 2.00 mm.

[0227] D: No breakage even when wound around a rod having a diameter of 3.00 mm.

[0228] <Electrode Uniformity>

[0229] The electrode uniformity was evaluated based on the uniformity of the thickness of the electrode composite material layer. 2 The film thickness in the battery was measured at 5 locations, and the film thickness deviation was evaluated. The smaller the film thickness deviation, the easier it is for lithium to move evenly in the battery, and the smaller the impedance.

[0230] A: In-plane deviation is less than 1.5%

[0231] B: In-plane deviation is 1.5% or more and less than 3%

[0232] C: In-plane deviation is 3% or more and less than 5%

[0233] D: In-plane deviation is more than 5%

[0234] <Peel Strength of Electrode Composite Layer>

[0235] The positive electrode for the lithium ion secondary battery made in the embodiment and the comparative example is cut into a rectangle of 100mm in length and 10mm in width as a test piece, the surface with the positive electrode composite material layer is faced down, and a transparent tape (transparent tape specified by JIS Z1522) is pasted on the surface of the positive electrode composite material layer, and one end of the current collector is stretched in the vertical direction, and the stress when stretched at a speed of 100mm / minute is measured (in addition, the transparent tape is fixed on the test bench). 3 measurements are carried out, and the average value is obtained as the peel strength, and it is evaluated according to the following benchmarks. The larger the value of the peel strength, the more firmly the positive electrode composite material layer and the current collector are in close contact, and the higher the peel strength of the electrode (positive electrode) composite material layer.

[0236] A: Peel strength is 30N / m or more

[0237] B: Peel strength is 25 N / m or more and less than 30 N / m

[0238] C: Peel strength is 20 N / m or more and less than 25 N / m

[0239] D: Peel strength less than 20N / m

[0240] <Initial Capacity of Secondary Battery>

[0241] After the electrolyte is injected, the lithium-ion secondary battery prepared in the embodiment and the comparative example is left to stand at a temperature of 25°C for 5 hours. Next, it is charged at a temperature of 25°C and a constant current method of 0.2C until the battery cell voltage is 3.65V, and then an aging treatment is performed at a temperature of 60°C for 12 hours. Then, it is discharged at a temperature of 25°C and a constant current method of 0.2C until the battery cell voltage is 3.00V. Thereafter, CC-CV charging is performed at a constant current of 0.2C (the upper limit battery cell voltage is 4.20V), and CC discharge is performed at a constant current of 0.2C until the battery cell voltage is 3.00V. Repeat the 0.2C charge and discharge three times. The third discharge capacity is taken as the initial capacity, and the value of initial capacity / theoretical capacity is evaluated according to the following benchmark. The larger the value, the higher the initial discharge capacity.

[0242] A: Initial capacity / theoretical capacity is 0.78 or more

[0243] B: Initial capacity / theoretical capacity is greater than 0.75 and less than 0.78

[0244] C: Initial capacity / theoretical capacity is 0.73 or more and less than 0.75

[0245] D: Initial capacity / theoretical capacity is less than 0.73

[0246] <Rate Characteristics of Secondary Batteries>

[0247] After the electrolyte is injected, the lithium-ion secondary battery prepared in the embodiment and the comparative example is left to stand at a temperature of 25°C for 5 hours. Next, it is charged at a temperature of 25°C and a constant current method of 0.2C until the battery cell voltage is 3.65V, and then an aging treatment is performed at a temperature of 60°C for 12 hours. Then, it is discharged at a temperature of 25°C and a constant current method of 0.2C until the battery cell voltage is 3.00V. Thereafter, CC-CV charging is performed at a constant current of 0.2C (the upper limit battery cell voltage is 4.20V), and CC discharge is performed at a constant current of 0.2C until the battery cell voltage is 3.00V. Repeat the 0.2C charge and discharge 3 times.

[0248] Next, at a temperature of 25°C, a constant current charge and discharge of 0.2C is performed between the battery cell voltage of 4.20-3.00V, and the discharge capacity at this time is defined as C0. Thereafter, CC-CV charging is performed at a constant current of 0.2C in the same manner, and CC discharge is performed at a constant current of 2.0C to 3.00V at a temperature of 25°C, and the discharge capacity at this time is defined as C1. Then, the ratio (percentage, capacity retention rate) of the discharge capacity (C1) at 2.0C to the discharge capacity (C0) at 0.2C, expressed as (C1 / C0)×100(%), is obtained as the rate characteristic, and is evaluated according to the following criteria. The larger the value of the capacity retention rate, the less the decrease in the discharge capacity at high current, and the smaller the internal impedance (that is, the rate characteristic is excellent).

[0249] A: Capacity retention rate is more than 75%

[0250] B: Capacity retention rate is 73% or more and less than 75%

[0251] C: Capacity retention rate is 70% or more and less than 73%

[0252] D: Capacity retention rate is less than 70%

[0253] <Cycle characteristics of secondary batteries>

[0254] After the electrolyte is injected, the lithium ion secondary battery prepared in the embodiment and the comparative example is left to stand at a temperature of 25°C for 5 hours. Next, it is charged at a temperature of 25°C and a constant current method of 0.2C until the battery cell voltage is 3.65V, and then an aging treatment is performed at a temperature of 60°C for 12 hours. Then, it is discharged at a temperature of 25°C and a constant current method of 0.2C until the battery cell voltage is 3.00V. Thereafter, CC-CV charging is performed at a constant current of 0.2C (the upper limit battery cell voltage is 4.20V), and CC discharge is performed at a constant current of 0.2C until the battery cell voltage is 3.00V. This 0.2C charge and discharge is repeated 3 times. Thereafter, 100 cycles of charge and discharge are performed at a battery cell voltage of 4.20-3.00V and a charge and discharge rate of 1.0C at a temperature of 35°C. At this time, the discharge capacity of the first cycle is defined as X1, and the discharge capacity of the 100th cycle is defined as X2. The discharge capacity X1 and the discharge capacity X2 were used to obtain the capacity retention rate (the ratio of the discharge capacity at the 100th cycle to the discharge capacity at the 1st cycle) expressed as (X2 / X1)×100(%) as the cycle characteristics, and the evaluation was performed according to the following criteria. The larger the value of the capacity retention rate, the better the cycle characteristics.

[0255] A: Capacity retention rate is more than 93%

[0256] B: Capacity retention rate is 90% or more and less than 93%

[0257] C: Capacity retention rate is 87% or more and less than 90%

[0258] D: Capacity retention rate is less than 87%

[0259] (Example 1)

[0260] <Preparation of Polymer α>

[0261] 100 parts of ion exchange water were added to a 1 L flask with a septum and a stirrer, the gas phase was replaced with nitrogen, the temperature was raised to 80°C, and 0.3 parts of ammonium persulfate (APS) as a polymerization initiator was dissolved in 5.7 parts of ion exchange water and added.

[0262] On the other hand, in another container, 40 parts of ion exchange water, 0.18 parts of sodium polyoxyethylene alkyl ether sulfate (manufactured by Kao Chemical Co., Ltd., "LATEMUL E-118B") as an emulsifier, 55 parts of methyl methacrylate and 39 parts of n-butyl acrylate as (meth)acrylate monomers, 5 parts of methacrylic acid as an ethylenically unsaturated acid monomer, and 1 part of allyl methacrylate as a crosslinking monomer were mixed to obtain a monomer composition. The monomer composition was continuously added to the above-mentioned 1L flask with a diaphragm over 1 hour to perform polymerization. During the addition, the reaction was carried out at 80°C. After the addition was completed, the mixture was further stirred at 80°C for 1 hour to terminate the reaction.

[0263] Next, an appropriate amount of NMP was added to the obtained aqueous dispersion of polymer α to obtain a mixture, and then, water and excess NMP were removed from the mixture by vacuum distillation at 90° C. to obtain an NMP dispersion of polymer α (solid content concentration: 8%).

[0264] The obtained NMP dispersion of polymer α was dried at 120° C. for 1 hour to prepare a film with a thickness of 0.2 mm to 0.5 mm. The polymer α was confirmed to be in a granular form by scanning electron microscopy (SEM), thereby confirming that the granular polymer α was dispersed in the dispersion medium (NMP).

[0265] <Preparation of Polymer β1>

[0266] In a nitrogen atmosphere, 85 parts of ion exchange water and 0.2 parts of sodium dodecylbenzene sulfonate were placed in a reactor A equipped with a mechanical stirrer and a condenser. The contents were heated to 55° C. while being stirred, and 0.3 parts of a 5.0% aqueous solution of potassium persulfate were added to the reactor A. Next, in a nitrogen atmosphere, 92 parts of acrylonitrile as a nitrile group-containing monomer, 1 part of acrylamide as an amide group-containing monomer, 2 parts of methacrylic acid as an ethylenically unsaturated acid monomer, and 5 parts of butyl acrylate as a (meth)acrylate monomer, as well as 0.6 parts of sodium dodecylbenzene sulfonate, 0.035 parts of tert-dodecyl mercaptan, 0.4 parts of polyoxyethylene lauryl ether, and 80 parts of ion exchange water were added to another container B equipped with a mechanical stirrer other than the reactor A, and the mixture was stirred and emulsified to prepare a monomer mixed solution. Then, the monomer mixture was added to the reactor A at a constant rate for 5 hours in a state of stirring and emulsification, and reacted until the polymerization conversion rate reached 95%, thereby obtaining an aqueous dispersion of a nitrile polymer (polymer β1) mainly containing acrylonitrile units (92% by mass). Next, an appropriate amount of NMP was added to the obtained aqueous dispersion of polymer β1 to obtain a mixture. Thereafter, reduced pressure distillation was performed at 90° C. to remove water and excess NMP from the mixture, thereby obtaining an NMP solution of polymer β1 (solid content concentration: 8%).

[0267] <Preparation of Polymer γ1>

[0268] In an autoclave with a stirrer, 240 parts of ion exchange water, 25 parts of sodium alkylbenzene sulfonate as an emulsifier, 24 parts of acrylonitrile as a nitrile-containing monomer, 43 parts of styrene as an aromatic vinyl monomer, and 4 parts of methacrylic acid as an ethylenically unsaturated acid monomer were sequentially placed, and after the interior was replaced with nitrogen, 29 parts of 1,3-butadiene as a conjugated diene monomer was pressed in, and 0.25 parts of ammonium persulfate as a polymerization initiator were added, and a polymerization reaction was carried out at a reaction temperature of 40°C to obtain a copolymer containing a nitrile-containing monomer unit, an aromatic vinyl monomer unit, an ethylenically unsaturated acid monomer unit, and a conjugated diene monomer unit. The iodine value of the obtained copolymer (polymer before hydrogenation) was measured according to the above method, and the result was 140g / 100g. In addition, the polymerization conversion rate was 85%.

[0269] For the polymer before hydrogenation, ion exchange water is added to obtain 400mL of solution (all solid components are 48g) in which the total solid content concentration is adjusted to 12% by mass. The solution is put into an autoclave with a stirrer of 1L in volume, and after circulating nitrogen for 10 minutes to remove dissolved oxygen in the solution, 50mg of palladium acetate as a hydrogenation reaction catalyst is dissolved in 180mL of ion exchange water to which 4 times moles of nitric acid have been added relative to palladium (Pd), and added. After replacing the system twice with hydrogen, the contents of the autoclave are heated to 50°C under the state of being pressurized to 3MPa with hydrogen, and it is subjected to a 6-hour hydrogenation reaction (hydrogenation reaction of the first stage).

[0270] Next, the autoclave was returned to atmospheric pressure, and 25 mg of palladium acetate as a hydrogenation catalyst was further dissolved in 60 ml of water to which 4 times the mole of nitric acid was added relative to Pd. After the system was replaced twice with hydrogen, the contents of the autoclave were heated to 50° C. under a state where the pressure was pressurized to 3 MPa by gauge pressure with hydrogen, and a hydrogenation reaction was carried out for 6 hours (hydrogenation reaction in the second stage).

[0271] Thereafter, the contents were returned to room temperature, the system was placed in a nitrogen atmosphere, and then concentrated using an evaporator until the solid content concentration became 40%, thereby obtaining an aqueous dispersion of polymer γ1 as polymer γ.

[0272] To 100 parts of the aqueous dispersion of the polymer γ1 obtained above was added 320 parts of N-methylpyrrolidone (hereinafter referred to as "NMP") as a solvent, and water was evaporated under reduced pressure to obtain an NMP dispersion of the polymer γ1.

[0273] <Manufacturing of Slurry Composition for Secondary Battery Positive Electrode>

[0274] In this example, a slurry composition was produced according to a slurry composition production method I (indicated as "Production method I" in Table 1) with the following operation.

[0275] [Pre-mixing process]

[0276] One part of CNT (specific surface area measured by BET method: 150 m 2 / g, multilayer type), and a specified amount of polymer γ1, and further add NMP (boiling point: 204°C) as an organic solvent so that the solid content concentration becomes 4% by mass, and stir and mix at a temperature of 25±3°C and a rotation speed of 3000 rpm for 10 minutes to obtain a premix.

[0277] [Main mixing process]

[0278] To the premix obtained in the above step, 97 parts of Co-Ni-Mn lithium composite oxide active material NMC532 (LiNi 5 / 10 Co 2 / 10 Mn 3 / 10 O2), 0.15 parts of 2-ethylhexyl diphenyl phosphate as a plasticizer, and a specified amount of polymer α and polymer β, and further NMP is added as needed, and stirred and mixed at a temperature of 25±3°C and a rotation speed of 50 rpm to obtain a positive electrode slurry composition having a viscosity of 3600 mPa·s measured using a B-type viscometer at 60 rpm (rotor M4) and 25±3°C.

[0279] In the above-mentioned preliminary mixing step and main mixing step, the total amount of the binder component (ie, polymers α to γ) and the plasticizer was 2 parts per 97 parts by mass of the positive electrode active material.

[0280] The blending amount of the binder component and the blending amount of the plasticizer were adjusted so that the blending amount of the plasticizer would be 7.5% by mass, based on the total mass of the plasticizer and the binder component being 100% by mass.

[0281] Furthermore, with regard to the amount of binder component (i.e., polymers α to γ), the amount of each polymer is adjusted as follows: taking the content of the binder component as 100 mass %, the content a of polymer α becomes 19 mass %, the content b of polymer β becomes 78 mass %, and the content c of polymer γ becomes 3 mass %.

[0282] <Manufacturing of positive electrode>

[0283] The positive electrode slurry composition obtained in the above method was applied onto a 20 μm thick aluminum foil as a current collector using a notch wheel coater so that the coating amount became 20±0.5 mg / cm 2 .

[0284] Furthermore, the slurry composition on the aluminum foil was dried by conveying it at a speed of 200 mm / min in an oven at 100°C for 2 minutes and then in an oven at 130°C for 2 minutes to obtain a positive electrode raw material having a positive electrode composite material layer formed on the current collector.

[0285] Thereafter, the positive electrode composite material layer side of the prepared positive electrode raw material was roll-pressed at a temperature of 25±3°C and a linear pressure of 14 t (tons) to obtain a positive electrode composite material layer with a density of 3.50 g / cm 3 For the obtained positive electrode, the peel strength of the positive electrode composite material layer was evaluated according to the above method. The results are shown in Table 1.

[0286] <Preparation of Negative Electrode Binder Composition>

[0287] In a 5MPa pressure-resistant container with a stirrer, 64 parts of styrene, 33 parts of 1,3-butadiene, 2 parts of itaconic acid, 1 part of 2-hydroxyethyl acrylate, 0.3 parts of tert-dodecyl mercaptan as a molecular weight regulator, 5 parts of sodium dodecylbenzenesulfonate as an emulsifier, 150 parts of ion exchange water, and 1 part of potassium persulfate as a polymerization initiator were added, and after sufficient stirring, the mixture was heated to a temperature of 55°C to initiate polymerization. When the monomer consumption reached 95.0%, the reaction was terminated by cooling. A 5% aqueous sodium hydroxide solution was added to the aqueous dispersion containing the polymer thus obtained, and the pH was adjusted to 8. Thereafter, the unreacted monomers were removed by heating and distillation under reduced pressure. Thereafter, the mixture was cooled to a temperature below 30°C, thereby obtaining an aqueous dispersion containing a negative electrode binder.

[0288] <Preparation of Negative Electrode Slurry Composition>

[0289] In a planetary mixer, 48.75 parts of artificial graphite (theoretical capacity: 360 mAh / g) and 48.75 parts of natural graphite (theoretical capacity: 360 mAh / g) as negative electrode active materials and 1 part of carboxymethyl cellulose as a thickener were added. Furthermore, the solid content concentration was diluted with ion exchange water to 60%, and then kneaded at a speed of 45 rpm for 60 minutes. Thereafter, 1.5 parts of the negative electrode binder composition obtained above were added in terms of solid content, and kneaded at a speed of 40 rpm for 40 minutes. Then, ion exchange water was added to make the viscosity 3000 ± 500 mPa·s (B-type viscometer, measured at 25°C and 60 rpm), thereby preparing a negative electrode slurry composition.

[0290] <Manufacturing of negative electrode>

[0291] The negative electrode slurry composition was applied to the surface of a 15 μm thick copper foil as a current collector using a notch wheel coater so that the coating amount was 11±0.5 mg / cm 2 Thereafter, the copper foil coated with the negative electrode slurry composition was transported in an oven at 80°C for 2 minutes and then in an oven at 110°C for 2 minutes at a speed of 400 mm / min, thereby drying the slurry composition on the copper foil to obtain a negative electrode raw material having a negative electrode composite material layer formed on the current collector.

[0292] Thereafter, the negative electrode composite material layer side of the prepared negative electrode raw material was roll-pressed at a temperature of 25±3°C and a linear pressure of 11 t (tons) to obtain a negative electrode composite material layer with a density of 1.60 g / cm 3 of the negative electrode.

[0293] <Preparation of Separator for Secondary Battery>

[0294] A single-layer polypropylene spacer (manufactured by Searge Co., Ltd., “#2500”) was used.

[0295] <Production of non-aqueous secondary batteries>

[0296] The above-mentioned negative electrode, positive electrode and separator are used to make a single-layer laminated battery cell (initial design discharge capacity is equivalent to 40 mAh), which is arranged in an aluminum packaging material. Thereafter, a 1.0 M LiPF6 solution (solvent: a mixed solvent of ethylene carbonate (EC) / diethyl carbonate (DEC) = 3 / 7 (volume ratio), containing an additive: 2 volume % (solvent ratio) of vinyl carbonate) is filled as an electrolyte. Furthermore, in order to seal the opening of the aluminum packaging material, heat sealing at a temperature of 150°C is performed to seal the aluminum packaging material to manufacture a lithium-ion secondary battery.

[0297] The initial capacity, rate characteristics, and cycle characteristics of the lithium ion secondary battery were evaluated according to the above-mentioned methods.

[0298] Furthermore, when the positive electrode composite material layer of the obtained secondary battery was observed by SEM, particulate polymer was confirmed.

[0299] (Example 2)

[0300] In this example, a slurry composition was produced according to a slurry composition production method II (indicated as "Production method II" in Table 1) with the following operation.

[0301] A mixture (slurry for binder particles) in which the aqueous dispersion of polymer α, the aqueous dispersion of polymer β1, the aqueous dispersion of polymer γ1 obtained in Example 1 and 2-ethylhexyl diphenyl phosphate as a plasticizer were mixed in the proportions shown in Table 1 was spray-dried using a spray dryer (manufactured by Niro Corporation, GEA) to prepare a binder particle assembly.

[0302] Two parts of the obtained binder particle aggregate were adjusted with NMP so that the solid content concentration became 6%, and one part of CNT (specific surface area measured by BET method: 150 m 2 / g), 97 parts of Co-Ni-Mn lithium composite oxide active material NMC532 (LiNi 5 / 10 Co 2 / 10 Mn 3 / 10O2) and NMP as an organic solvent were stirred and mixed at a temperature of 25±3°C for 60 minutes to disperse the binder, conductive material and active material. A positive electrode slurry composition having a viscosity of 3600 mPa·s measured using a B-type viscometer at a rotation speed of 60 rpm (rotor M4) and 25±3°C was obtained.

[0303] Then, a positive electrode was produced in the same manner as in Example 1 using the obtained positive electrode slurry composition, and a negative electrode, a separator, and a nonaqueous secondary battery were produced in the same manner as in Example 1, and various evaluations and measurements were performed.

[0304] (Example 3)

[0305] When preparing polymer γ, the hydrogenation reaction conditions were changed so that the iodine value became the value shown in Table 1, thereby obtaining polymer γ2. Except for this point, various operations, measurements, and evaluations were performed in the same manner as in Example 1. The results are shown in Table 1.

[0306] (Example 4)

[0307] The various operations, measurements, and evaluations were performed in the same manner as in Example 1 except that the polymer β2 prepared as described below was blended as the polymer β.

[0308] <Preparation of Polymer β2>

[0309] In the reactor B, the same method as in Example 1 was used, except that the amount of acrylonitrile added was 72 parts, the amount of acrylamide added was 8 parts, the amount of methacrylic acid added was 2 parts, and the amount of n-butyl acrylate added was 18 parts, to obtain an aqueous dispersion of a polyacrylonitrile (PAN) copolymer (polymer β2) having an acrylonitrile unit content of 72% by mass. Then, in the same manner as in Example 1, the solvent was replaced with NMP to obtain an NMP solution of polymer β2 (solid content concentration: 8%).

[0310] (Examples 5-6)

[0311] The various operations, measurements, and evaluations were performed in the same manner as in Example 1 except that the blending amounts of the plasticizers were changed as shown in Table 1. The results are shown in Table 1.

[0312] (Examples 7 to 9)

[0313] The various operations, measurements, and evaluations were performed in the same manner as in Example 1, except that the types of plasticizers to be blended were changed as shown in Table 1. The results are shown in Table 1.

[0314] (Example 10)

[0315] Various operations, measurements, and evaluations were performed in the same manner as in Example 1, except that the component corresponding to the polymer γ was not blended and the content a of the polymer α was changed as shown in Table 1. The results are shown in Table 1.

[0316] (Example 11)

[0317] The various operations, measurements, and evaluations were performed in the same manner as in Example 1, except that polymer β3 was used as polymer β, and the polymer β3 was prepared by using 1 part of methacrylamide instead of 1 part of acrylamide as the amide group-containing monomer.

[0318] (Example 12)

[0319] Various operations, measurements, and evaluations were performed in the same manner as in Example 1, except that the amide group-containing monomer was not used but the polymer β4 was used as the polymer β, and the polymer β4 was prepared to have the composition shown in Table 1. The results are shown in Table 1.

[0320] (Example 13)

[0321] Various operations, measurements, and evaluations were performed in the same manner as in Example 1, except that the (meth)acrylate monomer was not used but the polymer β5 was used as the polymer β, and the polymer β5 was prepared to have the composition shown in Table 1. The results are shown in Table 1.

[0322] (Comparative Example 1)

[0323] The various operations, measurements and evaluations were performed in the same manner as in Example 1 except that a polymer B1 was used instead of a component corresponding to the polymer β, wherein the content ratio of the acrylonitrile unit as the nitrile group-containing monomer unit in the polymer B1 was 40 mass % and the polymer B1 was prepared in a manner to have the composition shown in Table 1. The results are shown in Table 1.

[0324] (Comparative Example 2)

[0325] Various operations, measurements, and evaluations were performed in the same manner as in Example 1, except that the component corresponding to the polymer α was not added and the amounts of the polymers β and γ added were changed as shown in Table 1. The results are shown in Table 1.

[0326] (Comparative Example 3)

[0327] No component equivalent to a plasticizer was added. In addition, regarding polymers α to γ, each amount was changed so that the total amount was 2 parts relative to 97 parts of the electrode active material and the content ratio shown in Table 1 was satisfied. Except for these aspects, various operations, measurements and evaluations were performed in the same manner as in Example 1. The results are shown in Table 1.

[0328] (Comparative Example 4)

[0329] The various operations, measurements, and evaluations were performed in the same manner as in Example 1, except that the component corresponding to the polymer β was not blended and PVdF was blended instead.

[0330] (Comparative Example 5)

[0331] The various operations, measurements and evaluations were performed in the same manner as in Example 1 except that the component corresponding to the polymer β was not blended and the polymer B2 was used instead, the content ratio of the acrylamide unit as the amide group-containing monomer unit in the polymer B2 was 25 mass %, and the polymer B2 was prepared in a manner to have the composition shown in Table 1. The results are shown in Table 1.

[0332] (Comparative Example 6)

[0333] Various operations, measurements, and evaluations were performed in the same manner as in Example 1, except that the component corresponding to the polymer β was not blended and the polymer B3 was used instead. The polymer B3 was prepared to have the composition shown in Table 1. The results are shown in Table 1.

[0334] (Comparative Example 7)

[0335] Various operations, measurements, and evaluations were performed in the same manner as in Example 1, except that the component corresponding to the polymer β was not blended and the polymer B4 was used instead. The polymer B4 was prepared to have the composition shown in Table 1. The results are shown in Table 1.

[0336] In addition, in Table 1 shown below,

[0337] "MMA" means methyl methacrylate,

[0338] "BA" stands for n-butyl acrylate,

[0339] "MAA" means methacrylic acid,

[0340] "AMA" stands for allyl methacrylate,

[0341] "AN" stands for acrylonitrile,

[0342] "AAm" stands for acrylamide,

[0343] "ST" stands for styrene,

[0344] "H-BD" represents 1,3-butadiene hydride unit,

[0345] "CNT" means carbon nanotube.

[0346] [Table 1]

[0347]

[0348] As can be seen from Table 1, in Examples 1 to 13 using a binder composition containing specified polymers α and β, it is possible to form an electrode having excellent flexibility and uniformity at a high level and to improve the rate characteristics and cycle characteristics of a secondary battery having the obtained electrode. In addition, as can be seen from Table 1, in Comparative Examples 1 to 2 and 4 to 7 lacking either polymer α or β and Comparative Example 3 lacking a plasticizer, it is not possible to form an electrode having excellent flexibility and uniformity at a high level and to improve the rate characteristics and cycle characteristics of a secondary battery having the obtained electrode.

[0349] Industrial Applicability

[0350] According to the present invention, a nonaqueous secondary battery electrode binder composition and a nonaqueous secondary battery electrode slurry composition can be provided that can form an electrode having both high flexibility and excellent uniformity and improve the rate characteristics and cycle characteristics of a secondary battery having the obtained electrode.

[0351] Furthermore, according to the present invention, it is possible to provide a non-aqueous secondary battery electrode which has excellent flexibility and uniformity and can improve the rate characteristics and cycle characteristics of the secondary battery.

[0352] Furthermore, according to the present invention, it is possible to provide a non-aqueous secondary battery having excellent rate characteristics and cycle characteristics.

Claims

1. A binder composition for non-aqueous secondary battery electrodes, comprising polymer α and polymer β as binder components, a plasticizer, and an organic solvent, The polymer α is an insoluble polymer comprising a (meth)acrylate monomer unit and an ethylenically unsaturated acid monomer unit. The polymer β is a readily soluble polymer comprising an amide group-containing monomer unit, a (meth)acrylate monomer unit having an alkyl chain with carbon atoms of 1 or more and 6 or less, and a nitrile group-containing monomer unit, and taking the total of all monomer units constituting the polymer β as 100 mass %, the total content ratio of the amide group-containing monomer unit and the (meth)acrylate monomer unit is 0.1 mass % or more and 20 mass % or less, and the content ratio of the nitrile group-containing monomer unit is 70 mass % or more and 95 mass % or less.

2. The binder composition for non-aqueous secondary battery electrodes according to claim 1, in, With the total mass of the binder component being 100 mass %, the content a of the polymer α is 5 mass % or more and 60 mass % or less, and the content b of the polymer β is 20 mass % or more and 94 mass % or less.

3. The binder composition for non-aqueous secondary battery electrodes according to claim 2, in, The polymer α and the polymer β are polymers that satisfy the requirement that, when preparing an N-methyl-2-pyrrolidone mixed liquid having a solid content concentration of 8% by mass and containing the polymer α at the content ratio a and the polymer β at the content ratio b as solid components, the ratio of the insoluble components in the mixed liquid is greater than 30% by mass and less than 80% by mass.

4. The binder composition for non-aqueous secondary battery electrodes according to any one of claims 1 to 3, in, The content of the plasticizer is 0.1% by mass or more and 30% by mass or less, based on the total mass of the plasticizer and the binder component being 100% by mass.

5. The binder composition for non-aqueous secondary battery electrodes according to any one of claims 1 to 3, in, The plasticizer has a molecular weight of 1000 or less and a decomposition potential of 3.5 V or more. 6 . The non-aqueous secondary battery electrode binder composition according to claim 1 , further comprising a polymer γ as the binder component, wherein the polymer γ is a readily soluble polymer having an iodine value of 5 g / 100 g or more and 100 g / 100 g or less.

7. The binder composition for non-aqueous secondary battery electrodes according to claim 6, in, With the content of the binder component being 100 mass %, the content c of the polymer γ is 0.1 mass % or more and 50 mass % or less. 8 . A slurry composition for a non-aqueous secondary battery electrode, comprising an electrode active material, a conductive material, and the binder composition for a non-aqueous secondary battery electrode according to claim 1 .

9. The slurry composition for non-aqueous secondary battery electrodes according to claim 8, in, The conductive material includes carbon nanotubes.

10. An electrode for a non-aqueous secondary battery, comprising an electrode composite material layer, the electrode composite material layer comprising a polymer α and a polymer β as binder components, a plasticizer, an electrode active material, and a conductive material, The polymer α is a granular polymer comprising (meth)acrylate monomer units and ethylenically unsaturated acid monomer units, The polymer β is a readily soluble polymer comprising an amide group-containing monomer unit, a (meth)acrylate monomer unit having an alkyl chain with carbon atoms of 1 or more and 6 or less, and a nitrile group-containing monomer unit, and taking the total of all monomer units constituting the polymer β as 100 mass %, the total content ratio of the amide group-containing monomer unit and the (meth)acrylate monomer unit is 0.1 mass % or more and 20 mass % or less, and the content ratio of the nitrile group-containing monomer unit is 70 mass % or more and 95 mass % or less. 11 . The nonaqueous secondary battery electrode according to claim 10 , further comprising a polymer γ as the binder component, wherein the polymer γ is a readily soluble polymer having an iodine value of 5 g / 100 g or more and 100 g / 100 g or less. 12 . A non-aqueous secondary battery electrode, comprising an electrode composite material layer formed using the slurry composition for a non-aqueous secondary battery electrode according to claim 8 . 13 . A non-aqueous secondary battery comprising the electrode for a non-aqueous secondary battery according to claim 10 or 11.