A bismuth oxybromide-lignin-based activated carbon composite photocatalyst and its preparation method and application

Through the preparation of bismuth bromine oxide-lignin-based activated carbon composite photocatalyst, the problems of poor adsorption performance and low quantum efficiency of BiOBr photocatalyst are solved, the photocatalytic reaction performance and pollutant adsorption effect are improved, and the pulp and paper wastewater is realized Efficient processing and sustainable use of resources.

CN114832842BActive Publication Date: 2024-12-06INST OF CHEM IND OF FOREST PROD CHINESE ACAD OF FORESTRY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210493179.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-05-07
Publication Date
2024-12-06
Estimated Expiration
2042-05-07

AI Technical Summary

Technical Problem

In the prior art, BiOBr photocatalysts have the disadvantages of poor adsorption performance, low quantum efficiency, rapid recombination of electron-hole pairs and small specific surface area, making it difficult to effectively treat pulp and paper industry wastewater.

Method used

The photocatalyst of the bismuth bromine oxide-lignin-based activated carbon composite photocatalyst is used to form a [Bi2O2] layered structure and lignin-based activated carbon composite to enhance the photogenerated electron-hole separation efficiency and pollutants of the photocatalyst. Adsorption capacity.

Benefits of technology

The photocatalytic reaction performance of the catalyst is improved, the adsorption effect of pollutants is enhanced, the efficient treatment of pulp and paper wastewater is achieved, and the sustainable utilization of resources is achieved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114832842B_ABST
    Figure CN114832842B_ABST
Patent Text Reader

Abstract

The invention discloses a bismuth oxybromide-lignin-based activated carbon composite photocatalyst and its preparation method and application. The composite photocatalyst includes lignin-based activated carbon and bismuth oxybromide loaded on the lignin-based activated carbon. The preparation method is as follows: bromine salt and lignin are dispersed in a dispersant to obtain a dispersion, bismuth salt is dissolved in an alcohol reagent to obtain a bismuth salt solution; the bismuth salt solution is added to the dispersion and mixed evenly to obtain a reaction solution; the reaction solution is poured into a hydrothermal kettle, and the hydrothermal kettle is heated to cause the reaction solution to undergo a hydrothermal reaction to obtain a bismuth oxybromide-biochar composite; the bismuth oxybromide-biochar composite is calcined to obtain a bismuth oxybromide-lignin-based activated carbon composite photocatalyst. The composite photocatalyst has good photocatalytic reaction performance, effectively utilizes lignin, a byproduct of the pulping and papermaking industry, to treat wastewater in the pulping and papermaking industry, and realizes sustainable utilization of resources.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of environmental materials, in particular to industrial wastewater such as printing and dyeing and pulping and papermaking, and specifically to a bismuth oxybromide-lignin-based activated carbon composite photocatalyst and a preparation method and application thereof. Background Art

[0002] The rapid population growth and the development of industrialization have led to the widespread distribution of organic and inorganic pollutants in aquatic ecosystems, especially in the pulp and paper industry. During the pulp and papermaking process, the physicochemical properties and toxicity of wastewater are affected by the process flow (such as pulping and bleaching of raw materials). In 2019, the global pulp and paper market was valued at approximately US$518.83 billion and grew at an annual rate of 3.45%. Although a large amount of water (5-100 cubic meters per ton of paper) and various lignocellulosic biomass are consumed in the actual production process, 85% of the consumed water is returned to the environment without deep treatment, causing serious impacts on the environment. These discharged wastewaters usually have the following characteristics: chemical oxygen demand (COD) (500-115000 mg / L), lignin (11000-25000 mg / L), tannic acid (2730 mg / L), resin acid (3.2-550 mg / L), phenols (17-800 mg / L) and chlorides (13.9-38.5 mg / L).

[0003] Advanced oxidation processes (AOPs) have attracted extensive attention as effective measures to degrade various recalcitrant and toxic organic pollutants. AOPs can induce the generation of reactive oxygen species (ROS) (especially hydroxyl (·OH) radicals, whose oxidation potential is +2.80 V) in the presence of external energy (e.g., electricity, ultraviolet (UV) light, and sound waves) or chemical oxidants (O3 and H2O2). Photocatalytic technology using clean and renewable solar energy is one of the effective ways to solve environmental problems such as water pollution. BiOBr is a typical ternary p-type semiconductor with a conduction band minimum (CBM) and valence band maximum (VBM) located at different positions and a bandgap width of 2.7-2.9 eV. It is a narrow bandgap semiconductor with good visible light response and high photogenerated electron-hole separation efficiency. However, BiOBr has some disadvantages such as poor adsorption performance, low quantum efficiency, rapid recombination of electron-hole pairs, and small specific surface area, which weaken the catalytic degradation performance. Building composite materials is an effective way to improve the separation efficiency of photogenerated electron-hole pairs in photocatalysts. Using activated carbon doping can improve the separation efficiency of photogenerated electron-hole pairs in BiOBr, and at the same time increase the concentration of pollutants around the catalyst and accelerate the reaction rate. Lignin, as a byproduct of the pulp and paper industry, is cheap, easy to degrade and has low toxicity, and can be used to produce activated carbon. There is no report on combining BiOBr and lignin-based activated carbon to prepare bismuth oxybromide-lignin-based activated carbon composite photocatalyst. Summary of the invention

[0004] In view of the problems in the prior art, the purpose of the present invention is to provide a bismuth oxybromide-lignin-based activated carbon composite photocatalyst and its preparation method and application, so as to enhance the photocatalytic effect of bismuth oxybromide (BiOBr), recover the by-products of pulping and papermaking, realize the effective utilization of resources, and apply it to actual wastewater treatment.

[0005] To achieve the above object, the technical solution adopted by the present invention is:

[0006] The first object of the present invention is to provide a method for preparing the above-mentioned bismuth oxybromide-lignin-based activated carbon composite photocatalyst, comprising the following steps:

[0007] The bromine salt and lignin are dispersed in a dispersant to obtain a dispersion, and the bismuth salt is dissolved in an alcohol reagent to obtain a bismuth salt solution; the bismuth salt solution is added to the dispersion and mixed evenly to obtain a reaction solution; the reaction solution is poured into a hydrothermal kettle, and the hydrothermal kettle is heated to allow the reaction solution to undergo a hydrothermal reaction. After the reaction is completed, the reaction solution is cooled to room temperature, and the obtained product is successively separated, washed, and vacuum dried at a temperature of 50-60°C to obtain a bismuth oxybromide-biochar complex; the main chemical reactions involved in the above hydrothermal reaction process are as follows: Bi and O in the reaction solution are linked by covalent bonds to form a [Bi2O2] layered structure, and then form a BiOBr layered structure with a double Br layer, and the lignin is converted into biochar (biochar) through a hydrothermal reaction, and BiOBr grows on the biochar to obtain a bismuth oxybromide-biochar complex.

[0008] The bismuth oxybromide-biochar composite is placed in a tubular furnace and nitrogen is introduced for calcination, so that the biochar is further carbonized into activated carbon (AC), thereby obtaining a bismuth oxybromide-lignin-based activated carbon (BiOBr / Lignin-AC) composite photocatalyst. It should be noted that the nitrogen gas can also be replaced by inert gases such as helium and argon, which have the same effect as nitrogen, that is, to carbonize the reactants in an oxygen-free environment.

[0009] Preferably, the molar ratio of the bismuth salt to the bromide salt is 1:1 to 1:2.

[0010] Preferably, the dispersant is water, nitric acid or sulfuric acid; the alcohol reagent is anhydrous ethanol, ethylene glycol or isopropanol.

[0011] Preferably, the temperature of the hydrothermal reaction is 130-230° C. and the time is 24-48 hours.

[0012] Preferably, the gas environment of the calcination treatment is nitrogen, the temperature is 400-700° C., and the time is 1-5 hours.

[0013] Preferably, the lignin is at least one of alkali lignin and lignin sulfonate; the bismuth salt is any one of bismuth nitrate, bismuth sulfate, bismuth chloride or bismuth acetate; and the bromide salt is any one of potassium bromide and sodium bromide.

[0014] Preferably, the mass of lignin in the bismuth oxybromide-biochar composite is 1 wt% to 10 wt% of the mass of bismuth oxybromide.

[0015] The second object of the present invention is to provide a bismuth oxybromide-lignin-based activated carbon composite photocatalyst, wherein the bismuth oxybromide-lignin-based activated carbon composite photocatalyst is prepared by the preparation method described in the first object.

[0016] The third object of the present invention is to provide the use of bismuth oxybromide-lignin-based activated carbon composite photocatalyst in treating wastewater under visible light as in the second object. Further preferably, the wastewater is printing and dyeing wastewater or pulping and papermaking wastewater.

[0017] Compared with the prior art, the present invention has the following advantages:

[0018] (1) The BiOBr / Lignin-AC composite photocatalyst prepared by the present invention effectively utilizes lignin, a by-product of the pulp and paper industry, to treat wastewater from the pulp and paper industry, thereby achieving sustainable utilization of resources.

[0019] (2) The BiOBr / Lignin-AC composite photocatalyst prepared by the method of the present invention overcomes the shortcomings of BiOBr such as poor adsorption performance, low quantum efficiency, rapid recombination of electron-hole pairs and small specific surface area, and increases the concentration of pollutants around the catalyst, thereby enhancing the photocatalytic reaction performance of the catalyst.

[0020] (3) The activated carbon formed by calcining lignin through a hydrothermal method has a large specific surface area and many pores, and has a significant adsorption effect on pollutants. It can quickly enrich the pollutants around the catalyst, and the composite catalyst formed after calcination has better stability and recyclability. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 XRD patterns of BiOBr and BiOBr / Lignin-AC;

[0022] Figure 2 Scanning electron micrographs of BiOBr (a), AC (b), and F-BiOBr / 1wt% Lignin (cd).

[0023] Figure 3 It is the X-ray energy spectrum (EDS) of BiOBr / 2wt%Lignin;

[0024] Figure 4 High-resolution XPS spectra of Br, Bi, O and C elements of F-BiOBr / 1wt% Lignin (ad). DETAILED DESCRIPTION

[0025] The present invention is further described below in conjunction with the examples so that those skilled in the art can better understand the present invention and implement it, but the examples are not intended to limit the present invention. The raw materials or reagents used in the following examples are all commercially available products.

[0026] Embodiment 1:

[0027] 1g of alkaline lignin was placed in a beaker and dried in an oven at 40°C for 30 minutes for later use; 4mmol Bi(NO3)3·5H2O was dissolved in 30mL of anhydrous ethanol and stirred evenly by ultrasonication to obtain a Bi(NO3)3·5H2O solution; 4mmol KBr and 0.0122g of lignin were added to 20ml of distilled water respectively and stirred evenly to obtain a dispersion; then the Bi(NO3)3·5H2O solution was added to the dispersion containing KBr and lignin, ultrasonicated for 30min, and then vigorously stirred for 30min to obtain a reaction solution; the reaction solution was poured into a 100mL stainless steel hydrothermal autoclave lined with polytetrafluoroethylene, and placed in an oven and heated at 160°C for 24h to perform a hydrothermal reaction; after the reaction was completed, the obtained product was separated, washed, and dried in sequence to obtain bromine oxide Bismuth-biochar composite; placing the bismuth oxybromide-biochar composite into a tubular furnace, heating the tubular furnace at a rate of 5°C / min in a nitrogen environment to raise its temperature to 550°C, keeping the bismuth oxybromide-biochar composite at 550°C for 3 hours, and then cooling it naturally to obtain a F-BiOBr / 1wt% Lignin-AC composite photocatalyst, denoted as F-BL1, wherein 1wt% represents the mass percentage of lignin raw material used in the preparation of F-BL1 to the mass percentage of BiOBr in the target product (the same below).

[0028] Comparative Example 1

[0029] Compared with Example 1, in Comparative Example 1, when preparing the dispersion, the amount of lignin added was 0 g, that is, no lignin was added, and no tubular furnace calcination was performed to obtain the BiOBr photocatalyst, which was recorded as F-BiOBr.

[0030] Comparative Example 2

[0031] 0.0122 g of lignin was added to 20 ml of distilled water and stirred evenly to obtain a dispersion; the dispersion was first ultrasonicated for 30 min and then vigorously stirred for 30 min, then poured into a 100 mL stainless steel hydrothermal autoclave lined with polytetrafluoroethylene, and placed in an oven and heated at 160 ° C for 24 h for hydrothermal reaction; after the reaction was completed, the obtained product was separated, washed, and dried in sequence to obtain biochar; the biochar was placed in a tubular furnace, and the tubular furnace was heated to 550 ° C at a rate of 5 ° C / min in a nitrogen environment, and the biochar was kept at 550 ° C for 3 hours, and then naturally cooled to obtain lignin-based activated carbon (AC).

[0032] Example 2 to Example 4

[0033] Compared with Example 1, the difference between Examples 2 to 4 is that the amount of lignin added is different, and the other processes are the same as Example 1. The amounts of lignin added in Examples 2 to 4 are: 0.0244 g, 0.0488 g, and 0.0976 g, respectively; the products obtained in Examples 2 to 4 are respectively recorded as F-BiOBr / 2wt%Lignin-AC (F-BL2), F-BiOBr / 4wt%Lignin-AC (F-BL4), and F-BiOBr / 8wt%Lignin-AC (F-BL8).

[0034] Photocatalytic performance test

[0035] The photocatalytic performance of the photocatalysts prepared in Examples 1-4 and the comparative example was tested respectively, and the method was as follows: 50 mg of the photocatalyst was added to 250 mL of a 30 mg / L rhodamine B solution, irradiated with a 300w Xe lamp (a 420 nm cutoff filter was installed at the outlet of the light source), and the degradation rate of rhodamine B was tested after 1 hour. The results are shown in Table 1 below.

[0036] Table 1 Degradation rate of rhodamine B by photocatalysts prepared in Examples 1-4 and Comparative Examples

[0037]

[0038] It can be seen from Table 1 that the catalytic performance of the composite catalysts is improved after calcination. With the increase of the lignin doping amount, the catalytic effect first increases and then weakens, among which F-BL1 has the strongest catalytic effect.

[0039] The F-BiOBr / 1wt% Lignin-AC which had been tested for catalytic performance was centrifuged and taken out from the Rhodamine B solution. After washing and drying, the same environment was repeated three times to treat 250mL of 30mg / L Rhodamine B solution. It was irradiated with a 300wXe lamp (a 420nm cutoff filter was installed at the outlet of the light source). The degradation rate of Rhodamine B after 1 hour is shown in Table 2 below:

[0040] Table 2 Degradation rate of Rhodamine B after F-BiOBr / 1wt%Lignin-Biochar was reused three times

[0041]

[0042] It can be seen from Table 2 that after three cycles, the catalytic effect is still significant, indicating that the catalyst has good stability and repeatability.

[0043] Example 5

[0044] Put 1 g of lignin sulfonate into a beaker and dry it in an oven at 40°C for 30 minutes to obtain lignin. 4mmol BiCl3 was dissolved in 30mL anhydrous ethanol and stirred evenly by ultrasonication to obtain BiCl3 solution; 4mmol KBr and 0.122g lignin were added to 20ml distilled water and stirred evenly to obtain a dispersion; then the BiCl3 solution was added to the dispersion containing NaBr and lignin, ultrasonicated for 30min, and then vigorously stirred for 30min to obtain a reaction solution; the reaction solution was poured into a 100mL stainless steel hydrothermal autoclave lined with polytetrafluoroethylene, and placed in an oven and heated at 230°C for 48h to perform a hydrothermal reaction; after the reaction was completed, the obtained product was separated, washed, and dried in sequence to obtain a bismuth oxybromide-biochar composite; the bismuth oxybromide-biochar composite was placed in a tubular furnace, and the tubular furnace was heated to 400°C at a rate of 5°C / min in a nitrogen environment, and the bismuth oxybromide-biochar composite was kept at 400°C for 3 hours, and then naturally cooled to obtain a F-BiOBr / 10wt% Lignin-AC composite photocatalyst, recorded as F-BL10.

[0045] 50 mg of F-BiOBr / 10 wt% Lignin-AC composite photocatalyst was added to 250 mL of 30 mg / L Rhodamine B solution and irradiated with a 300 w Xe lamp (a 420 nm cutoff filter was installed at the outlet of the light source). After 1 hour, the degradation rate of Rhodamine B was 49.13%.

[0046] Example 6

[0047] The preparation method of lignin is the same as that of Example 1. 2 mmol Bi2(SO4)3 was dissolved in 30 mL of anhydrous ethanol and stirred with ultrasonic to obtain Bi2(SO4)3 solution; 4 mmol NaBr and 0.0488 gg of lignin are added to 20 ml of distilled water and stirred evenly to obtain a dispersion; then a Bi2(SO4)3 solution is added to the dispersion containing NaBr and lignin, first ultrasonicated for 30 minutes, and then vigorously stirred for 30 minutes to obtain a reaction solution; the reaction solution is poured into a 100 mL stainless steel hydrothermal autoclave lined with polytetrafluoroethylene, and placed in an oven and heated at 160°C for 48 hours for a hydrothermal reaction; after the reaction is completed, the resulting product is separated, washed, and dried in sequence to obtain a bismuth oxybromide-biochar composite; the bismuth oxybromide-biochar composite is placed in a tubular furnace, and the tubular furnace is heated to 400°C at a rate of 5°C / min in a nitrogen environment, and the bismuth oxybromide-biochar composite is kept at 400°C for 1 hour, and then naturally cooled to obtain a F-BiOBr / 4wt% Lignin-AC composite photocatalyst.

[0048] 50 mg of F-BiOBr / 4 wt% Lignin-AC composite catalyst was added to 250 mL of 30 mg / L Rhodamine B solution and irradiated with a 300 w Xe lamp (a 420 nm cutoff filter was installed at the outlet of the light source). After 1 hour, the degradation rate of Rhodamine B was 64.78%.

[0049] Example 7

[0050] The preparation method of lignin is the same as that of Example 1. 4 mmol Bi(NO3)3·5H2O was dissolved in 30 mL nitric acid and stirred evenly by ultrasonic to obtain Bi(NO3)3·5H2O solution; 4 mmol KBr and 0.0976g of lignin are added to 20ml of distilled water and stirred evenly to obtain a dispersion; then Bi(NO3)3·5H2O solution is added to the dispersion containing KBr and lignin, first ultrasonicated for 30min, and then vigorously stirred for 30min to obtain a reaction solution; the reaction solution is poured into a 100mL stainless steel hydrothermal autoclave lined with polytetrafluoroethylene, and placed in an oven and heated at 160°C for 12h to perform a hydrothermal reaction; after the reaction is completed, the resulting product is separated, washed, and dried in sequence to obtain a bismuth oxybromide-biochar composite; the bismuth oxybromide-biochar composite is placed in a tubular furnace, and the tubular furnace is heated to 550°C at a rate of 5°C / min in a nitrogen environment, and the bismuth oxybromide-biochar composite is kept at 550°C for 3 hours, and then naturally cooled to obtain a F-BiOBr / 8wt% Lignin-AC composite photocatalyst.

[0051] 50 mg of F-BiOBr / 8 wt% Lignin-AC composite catalyst was added to 250 mL of 30 mg / L Rhodamine B solution and irradiated with a 300 w Xe lamp (a 420 nm cutoff filter was installed at the outlet of the light source). After 1 hour, the degradation rate of Rhodamine B was 56.34%.

[0052] Material characterization

[0053] like Figure 1 As shown, in order to study the crystal phase and structure of BiOBr and its composites, we carried out XRD characterization of the catalysts. Figure 1It shows that all samples show similar diffraction peaks in the X-ray diffraction spectrum, indicating that all samples are high-purity crystals without impurity peaks. All diffraction peaks of the samples obtained by hydrothermal reaction and calcination treatment match those of tetragonal crystal JCPDF No.09-0393. At 10.90°, 21.93°, 25.16°, 31.69°, 32.22°, 39.38°, 44.69°, 46.21°, 50.67°, 53.38°, 57.12°, 61.90°, 67.40°, 71.00° and 76.70°, the diffraction peaks correspond to the crystal planes of (001), (002), (101), (102), (110), (112), (004), (200), (104), (211), (212), (105), (220), (214) and (310), respectively. Figure 1 The diffraction peak intensities of all composite catalysts prepared in Examples 1 to 5 are significantly reduced compared to the pure BiOBr prepared in the comparative example, indicating that the addition of lignin-based activated carbon may have led to lattice defects in BiOBr. Several new diffraction peaks appeared between 30° and 40° in the XRD patterns of F-BL10 and F-BL8, indicating that lignin was converted into activated carbon with a graphite structure. The other samples did not have these diffraction peaks, which may be due to the low content of lignin in the composite material. This also shows that there is some interaction between the BiOBr crystals and the lignin-based activated carbon structure.

[0054] Figure 2 Scanning electron micrographs of BiOBr (a), AC (b), and F-BiOBr / 1wt% Lignin (cd). Figure 2 a and 2b are SEM images of pure BiOBr and AC, respectively. It can be seen that BiOBr is a layered structure with a relatively smooth surface and a size distribution between 500nm and 1μm. Lignin-based activated carbon (AC) is a block structure with a very rough surface. Figure 2 c and 2d are SEM images of the F-BiOBr / 1wt%Lignin-AC composite photocatalyst at different magnifications. It can be seen that BiOBr is evenly dispersed on the lignin-based activated carbon and grows in all directions to form a three-dimensional layered structure. The thickness of each layer of BiOBr in the composite catalyst is reduced, which makes BiOBr expose more active points and increase the contact opportunities between it and the reactant molecules. At the same time, EDS energy spectrum analysis was performed on F-BiOBr / 1wt%Lignin (F-BL1), such as Figure 3 As shown, from Figure 3 It can be seen that F-BL1 contains Br, Bi, O and C elements, which further proves that BiOBr is successfully and evenly dispersed and grown on the surface of lignin-based activated carbon.

[0055] In order to analyze the elemental composition and valence state of each element in F-BiOBr / 1wt%Lignin (F-BL1), X-ray photoelectrochemical spectroscopy was used to characterize it. Figure 4 The XPS spectra of each element of F-BL1 are shown in Figure 2. Figure 4 From the spectrum of Br 3d in a, we can find two strong spin-orbit splitting energy peaks at 68.39 eV and 69.41 eV, which are respectively related to the Br 3d 5 / 2 and Br 3d 3 / 2 The Bi 4f spectrum of 4b shows two independent symmetrical peaks at 159.37 and 16468 eV, which belong to Bi 4f 7 / 2 and Bi 4f 5 / 2 The O1s peak of F-BL1 ( Figure 4 c) There are two peaks at 530.06 and 530.55 eV, which are related to the lattice O atoms (Bi-O bonds) and the surface -OH, respectively. The peak at 530.85 eV may be caused by the physical absorption of carbon dioxide and water molecules. Figure 4 d) The binding energies at 284.84, 286.64, and 289.11 eV match the CC, CO, and C=O bonds, respectively. The peak at 294.64 eV may be due to satellite jitter caused by vacuum contamination. Due to the low amount of lignin doping, the peak of C1s is very uneven.

[0056] In summary, the BiOBr / Lignin-AC photocatalyst prepared by the method of the present invention can accelerate the separation of photogenerated electrons and holes, improve the absorption of visible light and the concentration of pollutants around the catalyst, enhance the photocatalytic reaction performance, and has stable properties and high recycling efficiency, and has a good effect on the treatment of industrial wastewater such as printing and dyeing and pulp and paper making.

Claims

1. A method for preparing a bismuth oxybromide-lignin-based activated carbon composite photocatalyst, characterized in that: The method comprises the following steps: dispersing a bromine salt and lignin in a dispersant to obtain a dispersion, dissolving a bismuth salt in an alcohol reagent to obtain a bismuth salt solution; adding the bismuth salt solution to the dispersion and mixing them evenly to obtain a reaction solution; pouring the reaction solution into a hydrothermal kettle, and heating the hydrothermal kettle to allow the reaction solution to undergo a hydrothermal reaction, and after the reaction is completed, cooling the reaction solution to room temperature, and separating, washing, and drying the obtained product in sequence to obtain a bismuth oxybromide-biochar composite; placing the bismuth oxybromide-biochar composite in a protective gas for calcination treatment, i.e., a bismuth oxybromide-lignin-based activated carbon composite photocatalyst; The dispersant is water, nitric acid or sulfuric acid; The alcohol reagent is anhydrous ethanol, ethylene glycol or isopropanol; The temperature of the hydrothermal reaction is 130-230°C and the time is 24-48h; The calcination temperature is 400-700°C and the time is 1-5h; The lignin is alkali lignin; The mass of lignin in the bismuth oxybromide-biochar composite is 1wt% to 4wt% of the mass of bismuth oxybromide.

2. The method for preparing the bismuth oxybromide-lignin-based activated carbon composite photocatalyst according to claim 1, characterized in that: The molar ratio of the bismuth salt to the bromine salt is 1:1 to 1:

2.

3. The method for preparing the bismuth oxybromide-lignin-based activated carbon composite photocatalyst according to claim 1, characterized in that: The protective gas is nitrogen or an inert gas.

4. The method for preparing the bismuth oxybromide-lignin-based activated carbon composite photocatalyst according to claim 1, characterized in that: The bismuth salt is any one of bismuth nitrate, bismuth sulfate, bismuth chloride or bismuth acetate; the bromide salt is any one of potassium bromide and sodium bromide.

5. A bismuth oxybromide-lignin-based activated carbon composite photocatalyst, characterized in that: The bismuth oxybromide-lignin-based activated carbon composite photocatalyst is prepared by the preparation method described in any one of claims 1 to 4.

6. Use of the bismuth oxybromide-lignin-based activated carbon composite photocatalyst as claimed in claim 5 in treating wastewater under visible light.

7. The use according to claim 6, characterized in that: The wastewater is printing and dyeing wastewater or pulping and papermaking wastewater.