Method for producing a crystalline film

By using atomized chemical vapor deposition method of gasified metal source and oxygen-containing raw material gas on the surface of the uneven substrate, the film formation speed and quality of α-Ga2O3 film in the prior art was solved, and high-quality α-Ga2O3 crystallization was achieved. Membrane growth.

CN114836833BActive Publication Date: 2024-12-06FLOSFIA +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202210479527.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2017-08-21
Filing Date
2018-08-20
Publication Date
2024-12-06
Estimated Expiration
2038-08-20

AI Technical Summary

Technical Problem

It is difficult to effectively form a metastable α-Ga2O3 crystal film and its mixed crystal film, and there are high-density dislocations and crystal defects, which affect the film formation speed and quality.

Method used

The gasified metal source and oxygen-containing raw material gas are used to form a crystal film on the surface of the uneven substrate by atomizing chemical vapor deposition. The reaction is carried out in the range of 400°C to 700°C by etching gas and hydrogen halide. α-Ga2O3 crystalline film.

Benefits of technology

The film formation speed and quality of the α-Ga2O3 crystal film are improved, crystal defects are reduced, and high-quality crystal film growth is achieved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114836833B_ABST
    Figure CN114836833B_ABST
Patent Text Reader

Abstract

According to aspects of the present invention, a method for manufacturing a crystalline film includes vaporizing a metal source to convert the metal source into a metal-containing raw material gas; supplying the metal-containing raw material gas and an oxygen-containing raw material gas into a reaction chamber onto a substrate; and supplying a reaction gas into the reaction chamber onto the substrate to form a crystalline film under the gas flow of the reaction gas.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Description of the case

[0002] This application is a divisional application of the invention patent application with the application date of August 20, 2018, the national application number of 201810948015.9, and the invention name of “Method for Manufacturing Crystalline Film”.

[0003] CROSS-REFERENCE TO RELATED APPLICATIONS

[0004] This application claims the benefit of priority from Japanese Patent Application No. 2017-158305, filed on August 21, 2017, the disclosure of which is incorporated herein by reference in its entirety. Technical Field

[0005] The present disclosure relates to methods for making crystalline films. Background Art

[0006] As background, gallium oxide (Ga 2 O 3 ) has five different polymorphs, including α, β, γ, δ and ε (see NPL 1: Rustum Roy et al., "Polymorphism of Ga 2 O 3 and the System Ga 2 O 3 -H 2 O". Among these five polymorphs, β-Ga 2 O 3 It is considered to be the most thermodynamically stable, and α-Ga 2 O 3 and ε-Ga 2 O 3 Gallium oxide (Ga 2 O 3 ) exhibit a wide bandgap and have attracted much attention as a potential semiconductor material for semiconductor devices.

[0007] According to NPL 2, gallium oxide (Ga 2 O 3 ) can be controlled by forming a mixed crystal with indium and / or aluminum (see NPL 2: Kentaro KANEKO, "Fabrication and physical properties of corundum-structured alloys based on gallium oxide", paper, Kyoto University, March 2013, overview and contents open to the public on January 31, 2014). X AlY Ga Z O 3 InAlGaO-based semiconductors represented by (0≤X≤2, 0≤Y′≤2, 0≤Z′≤2, X+Y+Z=1.5 to 2.5) are extremely attractive materials (see PCT International Publication No. WO2014 / 050793A1).

[0008] However, since the β phase is the most stable phase of gallium oxide, it is difficult to form a crystalline film of metastable corundum-structured gallium oxide without using a suitable film formation method. In addition, a bulk substrate obtained by melt growth cannot be used for forming a metastable α-GaO film with a corundum structure. 2 O 3 Therefore, α-Ga has the same structure as corundum 2 O 3 The sapphire substrate with the same structure is used to form α-Ga on the sapphire substrate. 2 O 3 However, sapphire and α-Ga 2 O 3 The lattice mismatch of α-Ga2O3 is not small (Δa / a~4.5%, Δc / c~3.3%). Therefore, the heteroepitaxial growth of α-Ga2O3 on the sapphire substrate 2 O 3 Crystalline films tend to include a high density of dislocations. In addition, there are further challenges to accelerate the film formation rate, improve the quality of crystalline films of α-phase gallium oxide and / or crystalline films of mixed crystals of α-phase gallium oxide, and suppress crystal defects (including the occurrence of cracks, abnormal growth, crystal twins, and / or bending of the crystalline film). Under such circumstances, research on crystalline semiconductor films of corundum structure is continuously carried out.

[0009] Disclosed is an oxide crystalline film manufactured by atomizing chemical vapor deposition (CVD) using bromide or iodide of gallium and / or indium (see Japanese Patent Publication No. 5397794). In addition, a multilayer structure including a semiconductor layer of a corundum structure on a substrate of a corundum structure and an insulating layer of a corundum structure is disclosed (see Japanese Patent Publication No. 5343224 and Publication No. 5397795 and unexamined Japanese Patent Publication No. JP2014-72533). In addition, it is disclosed that an ELO substrate is used to form a film and form a gap by atomizing CVD method (see unexamined Japanese Patent Publication No. 2016-100592, Publication No. 2016-98166, Publication No. 2016-100593 and Publication No. 2016-155714). In addition, it is disclosed that a gallium oxide film of a corundum structure is formed by a halide vapor phase epitaxy (HVPE) method. However, there is room for improvement in film formation rate or speed, and a method of manufacturing a crystalline film at a sufficient speed is needed.

[0010] Moreover, considering that α-Ga 2 O 3 is metastable, unlike the stable β-Ga with a stable phase 2 O 3 Compared with the case of suppressing defect density, it is more difficult to form α-Ga 2 O 3 films and crystalline films of crystalline metal oxides containing gallium and one or more metals. Therefore, in order to obtain α-Ga 2 O 3 Various challenges remain to be addressed in the preparation of films and crystalline metal oxides containing gallium and one or more metals. Summary of the invention

[0011] According to a first aspect of the inventive subject matter, a method for manufacturing a crystalline film includes: vaporizing a metal source to convert the metal source into a metal-containing raw material gas; supplying the metal-containing raw material gas and an oxygen-containing raw material gas into a reaction chamber onto a substrate; and supplying a reaction gas into the reaction chamber onto the substrate to form a crystalline film under a gas flow of the reaction gas.

[0012] Furthermore, it is recommended that the reactive gas is an etching gas.

[0013] According to an embodiment of the method for manufacturing a crystalline film of the present inventive subject matter, the reaction gas may contain at least one selected from a hydrogen halide and a group containing halogen and hydrogen.

[0014] It is suggested that the substrate includes an uneven portion arranged on a surface of the substrate.

[0015] According to an embodiment of the method for manufacturing a crystallized film of the present inventive subject matter, the uneven portion may include at least one mask.

[0016] Furthermore, it is suggested that the uneven portion may include at least one opening.

[0017] According to an embodiment of the method for manufacturing a crystalline film of the present inventive subject matter, the substrate may be a patterned sapphire substrate.

[0018] It is recommended to heat the substrate at a temperature in the range of 400°C to 700°C.

[0019] Furthermore, according to an embodiment of the method for producing a crystalline film of the inventive subject matter, the metal source contains gallium.

[0020] It is recommended that the vaporization of the metal source be carried out by halogenating the metal source.

[0021] According to an embodiment of the method for producing a crystalline film of the subject matter of the present invention, the oxygen-containing raw material gas contains oxygen (O 2 ), water (H 2 O) and nitrous oxide (N2 O) at least one.

[0022] Furthermore, it is suggested that the substrate has a corundum structure.

[0023] Furthermore, it is suggested that the crystalline film has a corundum structure.

[0024] According to an embodiment of the method for manufacturing a crystallized film of the present subject matter, the method may include forming a buffer layer on at least one surface of a substrate by using a mist chemical vapor deposition method.

[0025] According to a second aspect of the subject matter of the present invention, a method for manufacturing a crystalline film includes: forming an uneven portion on a surface of a substrate; vaporizing a metal source to convert the metal source into a metal-containing raw material gas; supplying the metal-containing raw material gas and the oxygen-containing raw material gas into a reaction chamber onto the uneven portion on the surface of the substrate; and supplying a reaction gas into the reaction chamber onto the uneven portion on the surface of the substrate to form a crystalline film under the gas flow of the reaction gas.

[0026] It is suggested that the method further includes: forming an uneven portion on the surface of the crystallization film as the first crystallization film; and vaporizing a metal source to convert the metal source into a metal-containing raw material gas; supplying the metal-containing raw material gas and the oxygen-containing raw material gas into a reaction chamber onto the uneven portion on the surface of the substrate; supplying a reaction gas into the reaction chamber onto the uneven portion on the surface of the substrate to form a second crystallization film under the gas flow of the reaction gas.

[0027] According to a third aspect of the subject matter of the present invention, a method for manufacturing a crystalline film includes: forming a buffer layer on at least one surface of a substrate by using an atomized chemical vapor deposition method; forming an uneven portion on the surface of the buffer layer; vaporizing a metal source to convert the metal source into a metal-containing raw material gas; supplying the metal-containing raw material gas and the oxygen-containing raw material gas into a reaction chamber, onto the uneven portion on the surface of the buffer layer of the substrate; supplying a reaction gas into the reaction chamber, onto the uneven portion on the surface of the buffer layer of the substrate, to form a crystalline film under the gas flow of the reaction gas.

[0028] It is suggested that the method may further include: forming an uneven portion on the surface of the crystalline film as the first crystalline film; and vaporizing a metal source to convert the metal source into a metal-containing raw material gas; supplying the metal-containing raw material gas and the oxygen-containing raw material gas into the reaction chamber onto the uneven portion on the surface of the substrate; and supplying a reaction gas into the reaction chamber onto the uneven portion on the surface of the substrate to form a second crystalline film under the gas flow of the reaction gas. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1A schematic perspective view showing a halide vapor phase epitaxy (HVPE) apparatus used in an embodiment of a method of manufacturing a crystalline film according to the present subject matter.

[0030] Figure 2 A schematic perspective view showing a substrate having an uneven portion formed on a surface of the substrate according to an embodiment of the inventive subject matter as an example.

[0031] Figure 3 A schematic top view of a substrate according to the present subject matter is shown as an example, the substrate having an uneven portion formed on a surface of the substrate.

[0032] Figure 4 A schematic perspective view showing a substrate according to the present subject matter, which has an uneven portion formed on a surface of the substrate, as an example.

[0033] Figure 5 A top view of a substrate according to the present subject matter, which has an uneven portion formed on a surface of the substrate, is shown as an example.

[0034] Fig. 6A A schematic perspective view showing a substrate according to the present subject matter, which has an uneven portion formed on a surface of the substrate, as an example.

[0035] Figure 6B Show Fig. 6A Schematic top view of the substrate shown in .

[0036] Fig. 7A A schematic perspective view showing a substrate according to the present subject matter, which has an uneven portion formed on a surface of the substrate, as an example.

[0037] Figure 7B A schematic top view of a substrate according to the present subject matter is shown as an example, the substrate having an uneven portion formed on a surface of the substrate.

[0038] Figure 8 A schematic diagram of an atomized chemical vapor deposition (CVD) apparatus is shown, which is used in an embodiment of a method of making a crystalline film according to the present subject matter.

[0039] Fig. 9 The crystallized film according to the embodiment of the present subject matter is shown Scanning XRD measurement results.

[0040] Fig.10 A surface SEM image of a crystal film according to Example 2 which is an embodiment of the subject matter of the present invention is shown.

[0041] Fig.11A picture showing a crystallized film formed on a substrate according to an embodiment of the inventive subject matter.

[0042] Fig.12 SIMS measurement results of a crystallized film obtained according to an embodiment of the present inventive subject matter are shown. DETAILED DESCRIPTION

[0043] The terms used herein are only used for the purpose of describing specific embodiments and are not intended to limit the present subject matter. As used herein, the singular forms "a", "an" and "the" are also intended to include the plural forms, unless the context clearly indicates otherwise.

[0044] As used herein, the term "and / or" includes any and all combinations of one or more of the associated listed items.

[0045] As illustrated in the drawings filed with this document, for illustrative purposes, the sizes of some structures or parts may be exaggerated relative to other structures or parts. Relative terms such as "below" or "above" or "on" or "under" may be used herein to describe the relationship of one element, layer or region to another element, layer or region as shown in the figures. It should be understood that these terms are intended to cover different orientations of layers, devices and / or systems in addition to the orientations depicted in the figures.

[0046] According to a first aspect of the inventive subject matter, a method for manufacturing a crystalline film includes: vaporizing a metal source to convert the metal source into a metal-containing raw material gas; supplying the metal-containing raw material gas and an oxygen-containing raw material gas into a reaction chamber onto a substrate; and supplying a reaction gas into the reaction chamber onto the substrate to form a crystalline film under a gas flow of the reaction gas.

[0047] (Metal Source)

[0048] The metal source is not particularly limited as long as the metal source contains at least one metal and can be gasified. The metal source may be a metal source of an elemental metal. Moreover, the metal source may be a metal source of a metal compound. Examples of metals contained in the metal source include gallium, aluminum, indium, iron, chromium, vanadium, titanium, rhodium, nickel, cobalt, and iridium. The metal source may contain one or more metals.

[0049] In an embodiment of the method for producing a crystalline film of the subject of the present invention, the metal of the metal source may be at least one selected from gallium, aluminum and indium, but further preferably, the metal of the metal source contains gallium. In an embodiment of the method for producing a crystalline film of the subject of the present invention, the metal source is most preferably a gallium source.

[0050] Furthermore, the metal source may be a gas source, a liquid source, and a solid source, but if the metal of the metal source is gallium, a liquid source of gallium is preferred.

[0051] The gasification of the metal source to convert the metal source into a metal-containing raw material gas is not particularly limited, as long as it does not interfere with the purpose of the subject of the present invention and can be carried out by known methods. In the embodiment of the subject of the present invention, the gasification of the metal source to convert the metal source into a metal-containing raw material gas is preferably carried out by a halogenated metal source. The halogenating agent for the halogenated metal source is not particularly limited, as long as the metal source can be halogenated and can be a known halogenating agent. The halogenating agent can be a halogen and / or a hydrogen halide. Examples of halogens include fluorine, chlorine, bromine and iodine. Moreover, examples of hydrogen halides include hydrogen fluoride, hydrogen chloride, hydrogen bromide and hydrogen iodide. In the embodiment of the subject of the present invention, it is preferred to use a hydrogen halide halogenated metal source, and it is further preferred to use a hydrogen chloride halogenated metal source. In the embodiment of the method for manufacturing a crystalline film, the halogenated metal source is preferably carried out by supplying a halogen or a hydrogen halide as a halogenating agent to the metal source and reacting the metal source and the halogenating agent at a temperature at or above the evaporation temperature of the metal halide. The evaporation temperature is not particularly limited, but in an embodiment where the metal of the metal source is gallium and the halogenating agent is hydrogen chloride, the evaporation temperature is preferably 900°C or lower, more preferably 700°C or lower. The evaporation temperature is most preferably in the range of 400°C to 700°C.

[0052] The metal-containing raw material gas is not particularly limited as long as the metal-containing raw material gas is a gas containing the metal of the metal source. Examples of the metal-containing raw material gas may be halogenating agents such as fluorides, chlorides, bromides, and iodides.

[0053] In an embodiment of the subject matter of the present invention, after gasifying the metal source to convert the metal source into a metal-containing raw material gas, the metal-containing raw material gas and the oxygen-containing raw material gas are supplied into the reaction chamber onto the substrate. Also, in an embodiment of the subject matter of the present invention, the reaction gas is supplied into the reaction chamber onto the substrate. Examples of the oxygen-containing raw material gas include oxygen (O 2 ) gas, carbon dioxide (CO 2 ) gas, nitric oxide (NO) gas, nitrogen dioxide (NO 2 ) gas, nitrous oxide (N 2 O) gas, H 2 O gas and ozone (O 3 In an embodiment of the present invention, the oxygen-containing feed gas is preferably selected from O 2 Gas, H 2 O gas and (N 2 O) gas, and the oxygen-containing raw material gas further preferably contains O 2 According to an embodiment of the method for manufacturing a crystalline film, the oxygen-containing raw material gas may contain CO 2Gas. The reaction gas (usually different from the metal-containing raw material gas and the oxygen-containing raw material gas) does not include an inert gas. The reaction gas is not particularly limited as long as it does not interfere with the purpose of the subject matter of the present invention, but the etching gas is taken as an example. The etching gas is not particularly limited as long as it does not interfere with the purpose of the subject matter of the present invention, and can be a known etching gas. In an embodiment of the method for manufacturing a crystalline film, the reaction gas is preferably a halogen gas, a hydrogen halide gas and / or hydrogen. Examples of halogen gases include fluorine gas, chlorine gas, bromine gas and iodine gas. Examples of hydrogen halide gases include hydrofluoric acid gas, hydrochloric acid gas, hydrogen bromide gas and hydrogen iodide gas.

[0054] The reaction gas may be a mixed gas containing two or more of the above gases, and the reaction gas preferably contains a hydrogen halide gas, and most preferably contains hydrogen chloride.

[0055] Furthermore, the metal-containing raw material gas, the oxygen-containing raw material gas, and the reaction gas may contain a carrier gas, respectively. As an example, the carrier gas may be an inert gas. Examples of the inert gas include nitrogen and argon.

[0056] In addition, the partial pressure of the metal-containing raw material gas is not particularly limited, but in the embodiment of the method of the subject of the present invention, the partial pressure of the metal-containing raw material gas is preferably in the range of 0.5Pa to 1kPa, and further preferably in the range of 5Pa to 0.5kPa. Moreover, the partial pressure of the oxygen-containing raw material gas is not particularly limited, but in the embodiment of the method of the subject of the present invention, the partial pressure of the oxygen-containing raw material gas is preferably in the range of 0.5 to 100 times the partial pressure of the metal-containing raw material gas, and further preferably in the range of 1 to 20 times the partial pressure of the metal-containing raw material gas. In addition, the partial pressure of the reaction gas is not particularly limited, but in the embodiment of the method of the subject of the present invention, the partial pressure of the reaction gas is preferably in the range of 0.1 to 5 times the partial pressure of the metal-containing raw material gas, and further preferably in the range of 0.2 to 3 times.

[0057] In an embodiment of the method of the subject of the present invention, it is further preferred to supply a raw material gas containing a dopant into the reaction chamber onto the substrate. The raw material gas containing a dopant is not particularly limited as long as the raw material gas containing a dopant contains a dopant. The dopant is also not particularly limited, but in an embodiment of the method of the subject of the present invention, the dopant may contain one or more elements selected from germanium, silicon, titanium, zirconium, vanadium, niobium and tin. According to an embodiment of the subject of the present invention, the dopant preferably contains germanium, silicon and / or tin, and most preferably contains germanium. By using a raw material gas containing a dopant in a method for manufacturing a crystalline film, the conductivity of the crystalline film to be obtained can be easily controlled. The raw material gas containing a dopant preferably contains a dopant in the form of a compound. Examples of dopants in the form of compounds include halides and oxides. The raw material gas containing a dopant further preferably contains a halide as a dopant. The partial pressure of the raw material gas containing a dopant is not particularly limited, but in an embodiment of the method of the subject of the present invention, the partial pressure of the raw material gas containing a dopant is preferably between 1×10 -7 to 0.1 times, and more preferably in the range of 2.5×10 -6 to 7.5×10 -2 In addition, in an embodiment of the method of the subject matter of the present invention, the raw material gas containing the dopant is preferably supplied into the reaction chamber onto the substrate together with the reaction gas.

[0058] (Substrate)

[0059] The substrate is not particularly limited as long as the substrate includes an uneven portion on the surface of the substrate and is capable of supporting the crystalline film to be grown on the substrate. The uneven portion on the surface of the substrate may include at least one mask and / or at least one opening. The substrate may be a known substrate. The substrate may be an electrically insulating substrate. The substrate may be a conductive substrate. Moreover, the substrate may be a semiconductor substrate. In an embodiment of the method for manufacturing a crystalline film of the subject matter of the present invention, the substrate is preferably a crystalline substrate.

[0060] (Crystalline Substrate)

[0061] The crystalline substrate is not particularly limited as long as the substrate contains crystals as a main component, and may be a known substrate. The crystalline substrate may be an electrically insulating substrate. Moreover, the crystalline substrate may be a semiconductor substrate. The crystalline substrate may be a single crystal substrate. Moreover, the crystalline substrate may be a polycrystalline substrate. Examples of crystalline substrates include substrates containing crystals of a corundum structure as a main component, substrates containing crystals of a β-gallium oxide structure as a main component, and substrates of a hexagonal structure. The term "main component" herein means that the composition ratio of the crystals in the crystalline substrate is 50% or more, preferably 70% or more, and further preferably 90% or more.

[0062] Examples of substrates containing corundum structure crystals as a main component include sapphire (α-Al 2 O 3 ) substrate and α-phase gallium oxide (α-Ga 2 O 3 ) substrate. Examples of the substrate containing a crystal of a β-gallium oxide structure as a main component include β-phase gallium oxide (β-Ga 2 O 3 ) substrate and containing β-Ga 2 O 3 and α-Al 2 O 3 As a substrate containing β-Ga 2 O 3 and α-Al 2 O 3 The substrate of the mixed crystal contains Al 2 O 3 The mixed crystal substrate is in the range of more than 0% to 60% or less. Moreover, examples of hexagonal structure substrates include silicon carbide (SiC) substrates, zinc oxide (ZnO) substrates, gallium nitride (GaN) substrates. Another example of a crystalline substrate is, for example, a silicon (Si) substrate.

[0063] In an embodiment of the subject matter of the present invention, the crystalline substrate is preferably a sapphire substrate. Examples of sapphire substrates include c-plane sapphire substrates, m-plane sapphire substrates, and a-plane sapphire substrates. The sapphire substrate may include an off-angle. The off-angle of the sapphire substrate is not particularly limited, but is preferably in the range of 0° to 15°. Moreover, the thickness of the crystalline substrate is not particularly limited, but is preferably in the range of 50 μm to 2000 μm, and further preferably in the range of 200 μm to 800 μm.

[0064] In the embodiment of the subject of the present invention, since the substrate includes an uneven portion containing at least one mask and / or two or more openings, a crystalline film can be effectively manufactured. The uneven portion of the substrate is not particularly limited, as long as the uneven portion of the substrate includes at least one selected from a mask and an opening. The uneven portion of the substrate may be two or more masks. Moreover, the uneven portion of the substrate may be two or more openings. In addition, the uneven portion of the substrate may be a combination of a mask and an opening. The uneven portion of the substrate may include a regularly arranged mask and / or opening. Moreover, the uneven portion of the substrate may include an irregularly arranged mask and / or opening. In the embodiment of the subject of the present invention, the mask and / or opening of the uneven portion are arranged at regular intervals. For example, the regular interval may be set to the distance between the center of the first mask and the center of the second mask positioned adjacent to the first mask, or the distance between the center of the first opening and the center of the second opening positioned adjacent to the first opening. In the embodiment of the subject of the present invention, the mask and / or opening of the uneven portion are preferably regularly and repeatedly arranged as a regular pattern. Examples of regular patterns of masks include stripe patterns, dot patterns, and lattice patterns. In an embodiment of the subject matter of the present invention, the mask and / or opening of the uneven portion is preferably arranged in a stripe pattern or a dot pattern, and is further preferably arranged in a dot pattern. Masks and / or openings each having a polygonal shape in a plan view may be arranged. Examples of polygons in a plan view include triangles, quadrilaterals, pentagons, and hexagons. Moreover, examples of quadrilaterals include squares, rectangles, and trapezoids. In addition, the mask and / or opening may be regularly and repeatedly arranged as a pattern. Examples of masks of uneven portions appear to be in a pattern such as Figure 3 The circles are arranged in a grid pattern at regular intervals in the top view shown. Figure 5 Regular squares and triangles at regular intervals in the top view shown.

[0065] The material component of at least one mask is not particularly limited and may be a known material component. The mask of the uneven portion may be electrically insulating. Moreover, the mask of the uneven portion may be conductive. The mask of the uneven portion may be semiconductive. The material component of the mask of the uneven portion may be amorphous. The material component of the mask of the uneven portion may be single crystal. Moreover, the material component of the mask of the uneven portion may be polycrystalline. Examples of the material component of the mask of the uneven portion include oxides, nitrides, carbides, carbon, diamonds, metals, and mixtures of at least two selected from oxides, nitrides, carbides, carbon, diamonds, and metals. Examples of oxides include silicon (Si) oxide, germanium (Ge) oxide, titanium (Ti) oxide, zirconium (Zr) oxide, hafnium (Hf) oxide, tantalum (Ta) oxide, and tin (Sn) oxide. More specifically, the material component of the mask of the uneven portion may be a material containing a material selected from SiO 2, SiN and polysilicon as a main component of a silicon-containing compound, and a metal having a melting point higher than the crystal growth temperature of a crystalline film (which is a crystalline oxide semiconductor film). Examples of metals having a melting point higher than the crystal growth temperature of a crystalline film include platinum, gold, silver, palladium, rhodium, iridium and ruthenium. Moreover, the main component of the mask of the uneven portion accounts for 50% or more, preferably 70% or more, and most preferably 90% or more in terms of composition ratio.

[0066] The mask of the uneven portion can be formed by a known method. Examples of known methods include photolithography, electron beam lithography, laser irradiation and etching (such as dry etching and wet etching). In an embodiment of the subject matter of the present invention, the ridge-shaped masks are preferably arranged in parallel, and the ridge-shaped masks are further preferably arranged in a grid pattern at regular intervals. In an embodiment of the method for manufacturing a crystalline film of the subject matter of the present invention, the crystalline substrate is preferably a patterned sapphire substrate (PSS). The shape of the mask of the uneven portion can be formed into a pattern. The shape of the pattern includes a cone, a hemisphere, a dome, a quadrangular prism and a quadrangular pyramid. Moreover, the distance between each shape of the mask is not particularly limited, but, in an embodiment of the subject matter of the present invention, the distance is preferably 5 μm or less, and further preferably in the range of 1 μm to 3 μm.

[0067] The opening of the uneven portion is not particularly limited, and the surface of the substrate may be exposed in the opening. The surface in the opening of the uneven portion may contain a material component that is the same or similar to the material component of the mask. Moreover, according to an embodiment of the subject matter of the present invention, the opening of the uneven portion is preferably an opening located on the surface of the substrate. Moreover, according to an embodiment of the subject matter of the present invention, the opening of the uneven portion is only the surface of the substrate. In addition, according to an embodiment of the subject matter of the present invention, the opening of the uneven portion may be a through hole formed in the mask. Moreover, according to an embodiment of the subject matter of the present invention, the opening of the uneven portion may be a recessed portion formed in the surface of the substrate. The opening may be formed by a known method. Moreover, the same and similar techniques as the known methods of the above-mentioned mask are applied, including photolithography, electron beam lithography, laser irradiation and etching (such as dry etching and wet etching) to form an opening. The opening of the uneven portion may be a groove. The width and depth of the groove and the size of the upper surface of the flat portion exposed in the groove are not particularly limited, as long as they do not interfere with the purpose of the subject matter of the present invention. The flat portion surrounded by the groove may be the surface of the substrate or the mask. According to an embodiment of the subject matter of the present invention, the crystallized film may include at least one mask having two or more openings. Air or an inert gas may be contained in the opening.

[0068] According to an embodiment of the method for manufacturing a crystal film of the present subject matter, the substrate includes an uneven portion arranged on a surface of the substrate, such as Figure 2In this embodiment, the uneven portion on the surface of the substrate is a mask 2 a arranged on the surface of the substrate 1 . Figure 3 FIG. 1 is a schematic top view of a substrate, wherein an uneven portion is formed on a surface 1a of the substrate 1. Figure 2 and Figure 3 As shown, the masks 2a are arranged at regular intervals "a". The regular interval "a" can be set to the distance between the center of the first mask and the center of the second mask positioned adjacent to the first mask. In this embodiment, multiple masks 2a are spaced apart from each other and separated from each other. The regular interval "a" is not particularly limited, but in the present embodiment, it is preferably in the range of 0.5μm to 10μm. The regular interval "a" in the present embodiment is further preferably in the range of 1μm to 5μm, and most preferably in the range of 1μm to 3μm. Examples of the shape of the mask 2a in the present embodiment are conical and hemispherical. The mask 2a can be formed, for example, by photolithography.

[0069] Figure 4 A schematic perspective view showing a substrate according to the present subject matter, which has an uneven portion formed on a surface of the substrate, as an example. Figure 5 A top view of a substrate having an uneven portion formed on a surface of the substrate is shown. The uneven portion of this embodiment has Figure 2 and Figure 3 The shapes of the uneven portions shown are different shapes. Figure 4 The uneven portion shown is a mask arranged on the surface of the substrate. The shape of the mask 2a in this embodiment is a triangular pyramid. The triangular pyramid masks are arranged at regular intervals, which can be set to a regular distance "a" between the center of the first triangular pyramid and the center of the second triangular pyramid located adjacent to the first triangular pyramid. Figure 5 As shown, the triangular pyramids in this embodiment can be arranged in parallel laterally and obliquely. Moreover, two or more triangular pyramids can be in contact with adjacent triangular pyramids at the vertices of the triangular pyramids. The regular interval "a" is not particularly limited, but in this embodiment, it is preferably in the range of 0.5μm to 10μm. The regular interval in this embodiment is further preferably in the range of 1μm to 5μm, and most preferably in the range of 1μm to 3μm. In this embodiment, the mask has a regular triangular shape in a plan view, and the opening has a regular triangular shape in a plan view.

[0070] Fig. 6A A schematic perspective view showing a substrate according to the inventive subject matter having an uneven portion formed on a surface of the substrate. Figure 6B A schematic top view of a substrate is shown, the substrate having Fig. 6A An uneven portion is formed on the surface of the substrate shown.

[0071] The uneven portion of this embodiment is a sheet-like mask 2a having two or more openings 2b arranged on the surface of the substrate 1. In the openings 2b of the mask 2a, the surface 1a of the substrate is exposed, as shown in FIG. Fig. 6A and Figure 6B In this embodiment, the mask 2a appears as a grid having triangular openings 2b. Examples of the shape of the openings 2b in a plan view include a circle, a triangle, a quadrilateral, a pentagon, and / or a hexagon.

[0072] The mask 2a can be made of the same material as the substrate. Furthermore, the mask can be made of a silicon-containing compound, which can be SiO 2 . In addition, the mask 2a can be formed by photolithography, for example. The regular interval "a" can be set to the distance between the center of the first opening and the center of the second opening located adjacent to the first opening. The regular interval "a" is not particularly limited, but in the present embodiment, it is preferably in the range of 0.5 μm to 10 μm. The regular interval in this embodiment is further preferably in the range of 1 μm to 5 μm, and most preferably in the range of 1 μm to 3 μm.

[0073] Fig. 7A A schematic perspective view of a substrate according to the subject matter of the present invention having an uneven portion formed on a surface of the substrate is shown as an example. In this embodiment, the opening 2b is a recessed portion formed in the substrate 1.

[0074] Figure 7B A schematic top view of a substrate according to the subject matter of the present invention is shown as an example, the substrate having an uneven portion formed on the surface of the substrate. In this embodiment, the uneven portion of the substrate is a triangular-shaped opening 2b surrounding the upper surface of the substrate. For example, the opening 2b can be formed by laser irradiation. The triangular opening in this embodiment can be connected to the adjacent triangular opening at the vertex of the triangular opening, and the vertex can be set to a regular interval a. The regular interval a is not particularly limited, but in the present embodiment, it is preferably in the range of 0.5 μm to 10 μm. The regular interval in this embodiment is further preferably in the range of 1 μm to 5 μm.

[0075] The opening of the uneven portion may be a groove. The width and depth of the groove and the size of the upper surface of the substrate surrounded by the groove are not particularly limited, as long as they do not interfere with the purpose of the subject matter of the present invention. The flat portion surrounded by the groove may be a convex portion or a mask. According to an embodiment of the subject matter of the present invention, the crystalline film may include an uneven portion, the uneven portion including at least one mask and at least one opening. At least one mask may include a plurality of masks. Moreover, at least one opening may include a plurality of openings. The distance between adjacent masks and / or between adjacent openings is not particularly limited, but, according to an embodiment of the subject matter of the present invention, the distance may be, for example, in the range of 10nm to 1mm. In some embodiments of the subject matter of the present invention, the distance between adjacent masks and / or between adjacent openings is preferably in the range of 10nm to 300μm, further preferably in the range of 10nm to 1μm, and most preferably in the range of 100nm to 1μm.

[0076] According to an embodiment of the subject matter of the present invention, the substrate may include a buffer layer on top of the substrate. Moreover, if the substrate includes a buffer layer, the buffer layer on the substrate may include an uneven portion on the surface of the buffer layer. The uneven portion may include at least one mask and at least one opening. The buffer layer may include an uneven portion on the entire surface of the buffer layer. Examples of methods for forming a buffer layer include spraying, atomized chemical vapor deposition (CVD) method, halide vapor phase epitaxy (HVPE) method, molecular beam epitaxy (MBE) method, metal organic chemical vapor deposition (MOCVD) method and sputtering method. The buffer layer may be formed by a known method. In an embodiment of the method for manufacturing a crystalline film of the subject matter of the present invention, the buffer layer is preferably formed by using an atomized CVD method, which can improve the quality of the crystalline film to be formed on the buffer layer having an uneven portion. The buffer layer formed on the substrate by the atomized CVD method can be used to suppress the occurrence of tilt included in the crystal defect. The embodiment of the method for manufacturing a crystalline film on a buffer layer formed by using an atomized CVD method is described in detail below.

[0077] According to an embodiment of forming a buffer layer by using an atomized CVD method, the buffer layer is preferably formed by converting a raw material solution into atomized droplets, carrying the atomized droplets onto a substrate by using a carrier gas, and adjusting the temperature of the air and / or the substrate to cause a thermal reaction of the atomized droplets adjacent to the substrate to form a buffer layer on the substrate.

[0078] <Forming atomized droplets from raw material solution>

[0079] The raw solution is converted into atomized droplets floating in the space of the container of the mist generator. The raw solution can be converted into atomized droplets by a known method, and the method is not particularly limited, but, according to an embodiment of the subject matter of the present invention, the raw solution is preferably converted into atomized droplets by ultrasonic vibration. The initial velocity of the atomized droplets comprising mist particles and obtained by using ultrasonic vibration and floating in the space is zero. Since the atomized droplets floating in the space can be carried as a gas, the atomized droplets floating in the space are preferred to avoid damage caused by collision energy without being blown out like a spray. The size of the droplets is not limited to a specific size and can be several millimeters, but the size of the atomized droplets is preferably 50 μm or less. The size of the droplets is preferably in the range of 0.1 μm to 10 μm.

[0080] (Raw material solution)

[0081] The raw material solution is not particularly limited as long as a buffer layer can be formed from the raw material solution by an atomized CVD method. Examples of raw material solutions include organic metal complex solutions and halide solutions of metals. Examples of organic metal complex solutions include acetylacetone complex solutions. Examples of halide solutions include fluoride solutions, chloride solutions, bromide solutions, and iodide solutions. Examples of metals of organic metal complexes include gallium, indium, and / or aluminum. According to an embodiment of the subject matter of the present invention, the metal of the organic metal complex preferably contains at least gallium. The amount of metal contained in the raw material solution is not particularly limited as long as it does not interfere with the purpose of the subject matter of the present invention, but the amount of metal contained in the raw material solution is preferably 0.001mol% to 50mol%. The amount of metal contained in the raw material solution is further preferably 0.01mol% to 50mol%.

[0082] Moreover, according to an embodiment of the subject matter of the present invention, the raw material solution may contain a dopant. For example, by introducing a dopant into the raw material solution, the conductivity of the crystalline layer or crystalline film can be controlled without ion implantation, thereby forming a semiconductor layer without destroying the crystalline structure of the semiconductor layer. Therefore, the method can be used to form a crystalline film as a semiconductor layer or semiconductor film. Examples of n-type dopants include tin, germanium, silicon, and lead. The n-type dopant is preferably tin or germanium, and most preferably tin. Examples of p-type dopants include magnesium, calcium, and zinc. The dopant concentration can typically be between 1×10 16 / cm 3 Up to 1×10 22 / cm 3 The dopant concentration can be lower, for example, about 1×10 17 / cm 3 or lower, the dopant concentration may also be, for example, 1×10 20 / cm 3According to an embodiment of the present subject matter, the dopant concentration is preferably 1×10 20 / cm 3 or less, and more preferably 5×10 19 / cm 3 or lower.

[0083] According to the embodiment of the present invention, the solvent of the raw material solution is not particularly limited, and can be an inorganic solvent including water. Moreover, according to the embodiment, the solvent of the raw material solution can be an organic solvent including alcohol. In addition, according to the embodiment of the present invention, a mixed solvent of water and alcohol can be used. According to the embodiment of the present invention, the solvent of the raw material solution preferably contains water, and further preferably uses a mixed solvent of water and alcohol, and most preferably, the solvent of the raw material solution is water, which can include, for example, pure water, ultrapure water, tap water, well water, mineral water, hot spring water, spring water, fresh water and seawater. According to the embodiment of the present invention, ultrapure water is preferably used as the solvent of the raw material solution.

[0084] (Carrying atomized droplets into the film forming chamber)

[0085] Atomized droplets floating in the space of the container for forming atomized droplets are carried to the film forming chamber by a carrier gas. The carrier gas is not limited as long as it does not interfere with the purpose of the subject matter of the present invention, therefore, examples of carrier gases can be inert gases, such as nitrogen and argon, can be oxidizing gases, such as oxygen and ozone, and can be reducing gases, such as hydrogen and synthetic gas. One or more carrier gases of the examples can be used, and a dilution gas (e.g., 10 times dilution gas) with a reduced flow rate can be used as a second carrier gas. Moreover, the carrier gas can be supplied from one or more locations. Although the flow rate of the carrier gas is not particularly limited, the flow rate of the carrier gas can be in the range of 0.01 to 20L / min. According to an embodiment of the subject matter of the present invention, the flow rate of the carrier gas can preferably be in the range of 1 to 10L / min. When a dilution gas is used, the flow rate of the dilution gas is preferably in the range of 0.001 to 2L / min, and further preferably in the range of 0.1 to 1L / min.

[0086] (forming a buffer layer)

[0087] In order to form a buffer layer, the atomized droplets carried into the film forming chamber by the carrier gas undergo a thermal reaction (by "thermal reaction") to form a buffer layer on the surface of the substrate. Here, "thermal reaction" covers the range as long as the atomized droplets react by heat, therefore, the term "thermal reaction" herein may include chemical reaction and / or physical reaction. The "thermal reaction" herein may include another reaction, and the reaction conditions are not particularly limited as long as the purpose of the subject matter of the present invention is not interfered with. According to an embodiment of the subject matter of the present invention, the thermal reaction is carried out at a temperature of the evaporation temperature of the solvent of the raw material solution or above the evaporation temperature, but the temperature range of the "thermal reaction" is not too high and, for example, may be less than 1000°C. The thermal reaction is preferably carried out at a temperature of less than 650°C, most preferably at a temperature of 400°C to 650°C. Moreover, the thermal reaction may be carried out in any atmosphere of vacuum, non-oxygen atmosphere, reducing gas atmosphere and oxidizing gas atmosphere. Moreover, the thermal reaction may be carried out under any conditions of atmospheric pressure, supercharging and decompression, but, according to an embodiment of the subject matter of the present invention, the thermal reaction is preferably carried out at atmospheric pressure. Moreover, the thickness of the buffer layer can be set by adjusting the film forming time.

[0088] As described above, the buffer layer can be formed on at least a portion of the surface of the substrate. It is also possible to form the buffer layer on the entire surface of the substrate. The crystalline film formed on the buffer layer formed on the substrate can reduce crystal defects, such as tilting. Therefore, a good quality crystalline film with fewer defects can be obtained.

[0089] The buffer layer is not particularly limited, but, in the embodiment of the present invention, the buffer layer preferably contains a metal oxide as a main component. Examples of metal oxides include aluminum (Al) oxide, gallium (Ga) oxide, indium (In) oxide, iron (Fe) oxide, chromium (Cr) oxide, vanadium (V) oxide, titanium (Ti) oxide, rhodium (Rh) oxide, nickel (Ni) oxide, cobalt (Co) oxide and iridium (Ir) oxide, and at least one of the examples of metal oxides may be included in the buffer layer as a main component. Of course, the buffer layer may contain an oxide of a combination of two or more metals selected from Al, Ga, In, Fe, Cr, V, Ti, Rh, Ni, Co and Ir as a main component. In the embodiment of the present invention, the buffer layer preferably contains at least one selected from In, Al and Ga as a main component. In the embodiment of the present invention, the buffer layer further preferably contains In and / or Ga, and most preferably contains Ga. As an embodiment of the method for manufacturing the crystalline film of the subject of the present invention, the buffer layer may contain a metal oxide as a main component, and the amount of gallium and aluminum contained in the metal oxide is less than the amount of gallium contained in the metal oxide of the crystalline film. Moreover, according to an embodiment of the method for manufacturing a crystalline film of the subject of the present invention, the buffer layer may include a superlattice structure. In the embodiment of the subject of the present invention, the term "main component" means in this article that the metal oxide as the main component accounts for 50% or more of all the components contained in the buffer layer in terms of atomic ratio. In the embodiment of the subject of the present invention, the buffer layer further preferably contains a metal oxide as a main component, which accounts for 70% or more of all the components contained in the buffer layer, more preferably 90% or more. This means that the metal oxide may account for 100% of the buffer layer.

[0090] The crystal structure of the crystalline film is not particularly limited, but in an embodiment of the subject matter of the present invention, the crystalline film preferably has a corundum structure and / or a β-gallium oxide structure. The crystalline film further preferably has a corundum structure. As long as the purpose of the subject matter of the present invention is not interfered with, the main component of the crystalline film may be different from the main component of the buffer layer, but, according to an embodiment of the subject matter of the present invention, the crystalline film preferably contains a metal oxide as a main component, which is the same as the metal oxide as the main component of the buffer layer.

[0091] In an embodiment of the method for manufacturing a crystalline film, the method includes supplying a metal-containing raw material gas, an oxygen-containing raw material gas, and a reaction gas to a substrate. The substrate may include a buffer layer on top of the substrate. Moreover, if necessary, in addition to supplying a metal-containing raw material gas, an oxygen-containing raw material gas, and a reaction gas, the method may also include supplying a dopant-containing raw material gas. In this embodiment, a crystalline film containing a metal oxide as a main component is formed under a gas flow of a reaction gas. Preferably, the crystalline film is formed on a heated substrate or on a buffer layer on a heated substrate. The film forming temperature is not particularly limited as long as it does not hinder the purpose of the subject matter of the present invention, but in an embodiment of the method of the subject matter of the present invention, the film forming temperature is preferably 900°C or less. The film forming temperature is further preferably 700°C or less, and most preferably in the range of 400°C to 700°C. Moreover, film formation can be performed in any atmosphere of a vacuum, a non-vacuum environment, a reducing gas atmosphere, an inert gas atmosphere, and an oxidizing gas atmosphere. Moreover, film formation can be performed under any conditions of atmospheric pressure, supercharging, and decompression. According to an embodiment of the subject matter of the present invention, film formation is preferably performed at atmospheric pressure. Furthermore, the film thickness of the crystalline oxide semiconductor film can be set by adjusting the film formation time.

[0092] According to an embodiment of the crystalline film of the subject of the present invention, the crystalline film contains a crystalline metal oxide as a main component. Examples of crystalline metal oxides include Al oxide, Ga oxide, In oxide, Fe oxide, Cr oxide, V oxide, Ti oxide, Rh oxide, Ni oxide, Co oxide and Ir oxide. Of course, an oxide of a combination of two or more metals selected from Al, Ga, In, Fe, Cr, V, Ti, Rh, Ni, Co and Ir may be included in the crystalline film as a main component. In an embodiment of the subject of the present invention, the crystalline film preferably contains at least one selected from In, Al and Ga as a main component. In an embodiment of the subject of the present invention, the crystalline film further preferably contains In and / or Ga. According to an embodiment of the crystalline film of the subject of the present invention, the crystalline film most preferably contains crystalline gallium oxide as a main component or a mixed crystal of gallium oxide as a main component. In an embodiment of the crystalline film of the subject of the present invention, the term "main component" means in this article that the crystalline metal oxide as the main component accounts for 50% or more of all components contained in the crystalline film in terms of atomic ratio. In an embodiment of the subject matter of the present invention, the crystalline film further preferably contains a metal oxide as a main component, which accounts for 70% or more of all the components contained in the crystalline film in terms of atomic ratio, more preferably 90% or more. This means that the metal oxide may account for 100% of the crystalline film. The crystalline structure of the crystalline film is not particularly limited, but in an embodiment of the subject matter of the present invention, the crystalline film preferably has a corundum structure and / or a β-gallium oxide structure. The crystalline film further preferably has a corundum structure. The crystalline film is most preferably a crystal growth film including a corundum structure. The crystalline metal oxide contained in the crystalline film may be single crystalline. Moreover, the crystalline metal oxide contained in the crystalline film may be polycrystalline. In an embodiment of the crystalline film of the subject matter of the present invention, the crystalline metal oxide is preferably single crystalline. The film thickness of the crystalline film is not particularly limited, but the film thickness of the crystalline film is preferably 3 μm or more. Further preferably, the thickness of the crystalline film is 10 μm or more, most preferably 20 μm or more.

[0093] The crystalline film obtained by the method for manufacturing a crystalline film of an embodiment of the subject matter of the present invention is used for a semiconductor device including a power device. For example, it is expected that the power device using the crystalline film of the subject matter of the present invention is a switching device for realizing a high withstand voltage. Moreover, it is expected that such a device obtains a high thermal resistance. Examples of semiconductor devices include transistors (such as high electron mobility transistors (HEMT)), metal insulator semiconductors (MIS), thin film transistors (TFT), semiconductor devices, Schottky barrier diodes (SBD), pn junction diodes, PIN diodes, light-emitting elements, and photodetector devices. According to an embodiment of the subject matter of the present invention, a crystalline film separated from a substrate can be used in a semiconductor device. Moreover, according to an embodiment of the subject matter of the present invention, a crystalline film formed on a substrate can be used in a semiconductor device.

[0094] The embodiments are explained in more detail.

[0095] (Example 1)

[0096] 1. Form a buffer layer

[0097] 1-1. Atomization CVD equipment

[0098] As an embodiment of a method of forming the crystal layer, a mist chemical vapor deposition (CVD) method may be used. Figure 8 The atomized CVD device 19 used in this embodiment is shown. The atomized CVD device 19 includes a mist generator 24 having a container, a container 25 containing water 25a, and an ultrasonic transducer 26 attached to the bottom of the container 25. The atomized CVD device 19 further includes a carrier gas supply 22a, a flow control valve 23a of the carrier gas. In addition, the atomized CVD device 19 may include a dilution carrier gas supply device 22b and a flow control valve 23b of the dilution carrier gas. The atomized CVD device 19 includes a film forming chamber 27 (which can be a quartz tube with an inner diameter of 40mm), a heater 28, and a support 21 (for supporting an object 20 in the film forming chamber 27). The heater 28 can be arranged around the film forming chamber 27. A film will be formed on the object, and the object can be a substrate. The support 21 is made of quartz and includes an inclined surface, and the object is placed on the inclined surface. The inclined surface of the support 21 can be inclined to the horizontal plane. The film-forming chamber 27 and the stage 21 , both of which are made of quartz, tend to suppress the entry of impurities derived from materials of components and devices into a film to be formed on an object.

[0099] 1-2. Preparation of raw material solution

[0100] A raw material solution was prepared by mixing gallium bromide and tin bromide in ultrapure water so that the atomic ratio of tin to gallium was 1:0.08 and gallium was 0.1 mol / L, and the raw material solution contained hydrobromic acid at a volume ratio of 20%.

[0101] 1-3. Film (layer) formation and preparation

[0102] The raw material solution 24a obtained in the preparation of the raw material solution in 1-2. above is set in the container of the mist generator 24. Moreover, a patterned sapphire substrate (PSS) (which is a c-plane sapphire substrate with a bias angle of 0.2°) and an uneven portion including a mask are placed in a film forming chamber 27. The mask of the uneven portion is a triangular pyramid in which the vertices are arranged at regular intervals of 1 μm in a triangular lattice. The PSS is placed on a bracket 21, and the heater is started to raise the temperature of the film forming chamber to 460°C. The first flow control valve 23a and the second flow control valve 23b are opened to supply a carrier gas from the carrier gas device 22a as a carrier gas source and the dilution carrier gas device 22b into the film forming chamber 27 to fully replace the atmosphere in the film forming chamber 27 with the carrier gas. After the atmosphere in the film forming chamber 27 is sufficiently replaced with the carrier gas, the flow rate of the carrier gas from the carrier gas source 22a is adjusted to 2.0 L / min, and the diluted carrier gas from the diluted carrier gas source 22b is adjusted to 0.1 L / min. In this embodiment, nitrogen is used as the carrier gas.

[0103] 1-4. Membrane formation

[0104] The ultrasonic transducer 26 is then started to vibrate at 2.4 MHz, and the vibration is propagated to the raw material solution 24a through the water 25a in the container to convert the raw material solution 24a into atomized droplets. The atomized droplets are introduced into the film forming chamber 27 with a carrier gas. The film forming chamber 27 is heated to 460° C. by the heater 28, and the atomized droplets are thermally reacted in the film forming chamber 27 to form a film on the object 20. The obtained film is used as a buffer layer. The film forming time is 5 minutes.

[0105] 2. Formation of crystalline film

[0106] 2-1.HVPE equipment

[0107] refer to Figure 1, describes the HVPE apparatus in this embodiment of the method for manufacturing a crystal film. The HVPE apparatus 50 includes a reaction chamber 51, a heater 52a for heating a metal source 57, and a heater 52b for heating an object, which may be a substrate held by a substrate holder 56. In the reaction chamber 51, the HVPE apparatus 50 further includes a supply pipe 55b of an oxygen-containing raw material gas, a supply gas pipe 54b of a reaction gas, and a substrate holder 56 on which the substrate is placed. In addition, a supply pipe 53b of a metal-containing raw material gas is arranged in the supply gas pipe 54b of the reaction gas to have a double-tube structure. The supply pipe 55b of the oxygen-containing raw material gas is connected to the supply device 55a of the oxygen-containing raw material gas to form a flow path of the oxygen-containing raw material gas, so that the oxygen-containing raw material gas is supplied to the substrate held by the substrate holder 56. The supply pipe 53b of the metal-containing raw material gas is connected to the supply device 53a of the halogen-containing raw material gas, so that the halogen-containing raw material gas is supplied to the metal source to form the metal-containing raw material gas. The metal-containing raw material gas is then supplied to the substrate held by the substrate holder 56. The reaction chamber 51 further includes a gas exhaust portion 59 for exhausting a used gas and a protective sheet 58 disposed on an inner surface of the reaction chamber 51.

[0108] 2-2 Film (layer) formation and preparation

[0109] A gallium (Ga) metal source 57 (99.99999% or higher purity) was arranged in a supply pipe 53b for a metal-containing raw material gas, and a PSS substrate having a buffer layer (obtained in 1 above) on its surface was placed on a substrate holder 56 in a reaction chamber 51. Thereafter, heaters 52a and 52b were activated to raise the temperature of the reaction chamber 51 to 510°C.

[0110] 3. Membrane Formation

[0111] Hydrogen chloride (HCl) gas (99.999% or higher purity) is supplied from the halogen-containing raw material gas supply device 53a to the Ga metal source 57 disposed in the metal-containing raw material gas supply pipe 53b to form gallium chloride (GaCl / GaCl) by a chemical reaction of Ga metal and HCl. 3 The obtained gallium chloride (GaCl / GaCl) supplied through the metal-containing raw material gas supply pipe 53b is 3 ) and O supplied through the supply pipe 55b of the oxygen-containing raw gas supply device 55a 2 The gas (99.99995% or higher purity) is supplied to the substrate. Under the HCl gas flow (99.999% or higher purity), gallium chloride (GaCl / GaCl 3 ) and O 2The gas reacts at 510° C. and atmospheric pressure to form a crystalline film on the substrate. The film formation time is 25 minutes. Here, respectively, the gas flow rate of the HCl gas supplied from the halogen-containing raw material gas supply device 53a is maintained at 10 sccm, the gas flow rate of the reaction gas supply device 54a is maintained at 5.0 sccm, and the gas flow rate of the oxygen-containing raw material gas supply device 55a is maintained at 20 sccm.

[0112] 4. Evaluation

[0113] The film obtained at 3. was a crystalline film without cracks and abnormal growth, and was characterized by using X-ray diffraction (XRD) analysis with XRD 2θ / ω scans at angles from 15 to 95 degrees. The measurement was performed using CuKα radiation. The obtained film was found to be α-Ga 2 O 3 membrane. Moreover, Fig. 9 Show The results of the scan. Fig. 9 As shown, the film obtained at 3. is a good quality crystalline film without twins. The thickness of the film is 10 μm. The film obtained at 3. has a thickness of 9 μm. 2 or larger surface area and less than 5×10 6 cm -2 The dislocation density.

[0114] (Example 2)

[0115] A crystalline film was obtained under the same conditions as those of Example 1 except for the following two conditions: a PSS substrate with a regular interval of 3 μm was used instead of the PSS substrate with a buffer layer with a regular interval of 1 μm used in Example 1, and the film formation time of Example 2 was 75 minutes. The film obtained in Example 2 was characterized in a manner similar to that in Example 1, and it was found to be a good quality α-Ga 2+ film similar to that of the crystalline film obtained in Example 1. 2 O 3 The surface of the crystalline film was observed by SEM. Fig.10 The thickness of the crystal film is 30 μm.

[0116] (Example 3)

[0117] A crystalline film was obtained by the same conditions as those of Example 1 except for the following four conditions: a c-plane sapphire substrate was used instead of the PSS substrate with a buffer layer having a regular interval of 1 μm used in Example 1, the flow rate of the HCl gas supplied from the halogen-containing raw material gas supply device 53a was set to 5 sccm, germanium tetrachloride gas was supplied to the substrate at a flow rate of 10 sccm as a dopant-containing raw material gas together with the reaction gas (HCl gas), a crystalline film was formed under the gas flow of HCl gas and germanium tetrachloride gas, the temperature in the film forming chamber was set to 550° C. while the crystalline film was formed, and the film forming time was 7 minutes. The crystalline film obtained in Example 3 had no cracks, as shown in FIG. Fig.11 The crystalline film was identified in a similar manner to the film in Example 1 and was found to be a good quality α-Ga 2 O 3 Crystalline Film. Furthermore, the crystallized film was analyzed by secondary ion mass spectrometry (SIMS), and the analysis was performed using a Cameca SIMS instrument, the primary ions were cesium (Cs) ions, and the first acceleration voltage was 14.5 kV. Fig.12 The results show that germanium is uniformly doped in the crystalline film from the surface of the crystalline film to a depth of 2.0 μm. In addition, the Hall effect of the crystalline film was measured by the Van der Pauw method. As a result, the carrier concentration of the crystalline film was 9.1×10 18 / cm 3 , and the electron mobility is 20cm 2 / Vs.

[0118] (Comparative Example 1)

[0119] A crystal film was obtained by the same conditions as those of Example 1 except for one condition: the reaction gas (HCl gas) was not supplied to the substrate. As a result, the film formation rate became one tenth or less compared to the film formation rates in Examples 1 to 3. Moreover, the film obtained in Comparative Example 1 was inferior in film quality of surface flatness, and the film did not have a mirror surface.

[0120] (Comparative Example 2 and Comparative Example 3)

[0121] A crystallized film was obtained under the same conditions as those of Example 2 except for one condition: the reaction gas (HCl gas) was not supplied to the substrate. As a result, the film formation rate became one tenth or less compared to the film formation rates of Examples 1 to 3. Moreover, the film obtained in Comparative Example 2 was inferior in film quality of surface flatness, and the film did not have a mirror surface.

[0122] Furthermore, a crystallized film was obtained under the same conditions as those of Example 3 except for one condition: the reaction gas (HCl gas) was not supplied to the substrate. As a result, the film formation rate became one tenth or less compared to the film formation rates of Examples 1 to 3. Furthermore, the film obtained in Comparative Example 3 was inferior in film quality of surface flatness, and the film did not have a mirror surface.

[0123] In addition, although certain embodiments of the subject matter of the present invention have been described with reference to a specific combination of elements, various other combinations may also be provided without departing from the teachings of the subject matter of the present invention. Therefore, the subject matter of the present invention should not be interpreted as being limited to the specific exemplary embodiments described herein and illustrated in the accompanying drawings, but may also include combinations of elements of the various illustrated embodiments.

[0124] Without departing from the spirit and scope of the subject matter of the present invention, many changes and modifications may be made by those of ordinary skill in the art, taking into account the benefits of this disclosure. Therefore, it must be understood that the embodiments shown are presented for illustrative purposes only and should not be regarded as limiting the subject matter of the present invention as defined by the claims. Therefore, the claims should be understood to include not only the combination of elements literally stated, but also all equivalent elements for performing substantially the same function in substantially the same manner to obtain substantially the same results. Therefore, the claims should be understood to include the content specifically illustrated and described above, the content that is conceptually equivalent, and the content that incorporates the basic idea of ​​the subject matter of the present invention.

[0125] The method for manufacturing a crystal film according to an embodiment of the inventive subject matter can be applied to a method of manufacturing various devices including a semiconductor device, a power device including an inverter, an electronic device, an optical device, a power supply, and a power system.

[0126] Reference Numbers

[0127] a Regular interval

[0128] 1 substrate

[0129] 1a Surface of substrate 1

[0130] 2a Mask

[0131] 2b Opening

[0132] 3 Crystallized film

[0133] 4 Mask layer

[0134] 5 Buffer layer

[0135] 19 Atomization CVD equipment

[0136] 20 Object on which the film is to be formed

[0137] 21. A support for an object

[0138] 22a Carrier gas supply

[0139] 22b Dilution carrier gas supply device

[0140] 23a Carrier gas flow control valve

[0141] 23b Flow control valve for dilution carrier gas

[0142] 24 Fog Generator

[0143] 24a Raw material solution

[0144] 25 Container

[0145] 25a Water

[0146] 26 Ultrasonic transducer

[0147] 27 Film Forming Room

[0148] 28 Heater

[0149] 50 Halide Vapor Phase Epitaxy (HVPE) Device

[0150] 52a Heater

[0151] 52b Heater

[0152] 53a Supply device for halogen-containing raw material gas

[0153] 53b Supply pipe for metal-containing raw material gas

[0154] 54a Reaction gas supply device

[0155] 54b Reaction gas supply pipe

[0156] 55a Supply device for oxygen-containing raw gas

[0157] 55b Supply pipe for oxygen-containing raw gas

[0158] 56 base plate base

[0159] 57 Metal Source

[0160] 58 Protective film

[0161] 59 Gas Emissions Section

[0162] 60 Crystalline Film

[0163] 60a The first side of the crystal film

[0164] 60b Second side of the crystal film

[0165] 61a First electrode

[0166] 61b Second electrode

[0167] 70 Mask part

[0168] 71 substrate part

[0169] 101 Second Crystalline Film

[0170] 102 Mask

[0171] 103 First Crystalline Film

[0172] 104 substrate

[0173] 550 Mask

[0174] 560 Sapphire Substrate

[0175] 1000 Semiconductor devices

Claims

1. A method for producing a crystalline film, comprising: supplying a metal-containing raw material gas into a reaction chamber onto a substrate via a supply pipe for the metal-containing raw material gas, and supplying an oxygen-containing raw material gas into the reaction chamber onto the substrate via a supply pipe for the oxygen-containing raw material gas, the metal-containing raw material gas being formed by vaporizing a metal source in the supply pipe for the metal-containing raw material gas; and supplying a reaction gas into the reaction chamber onto the substrate via a reaction gas supply pipe to form a crystallized film on the substrate under a gas flow of the reaction gas, The metal includes one or more of gallium, aluminum, indium, iron, chromium, vanadium, titanium, rhodium, nickel, cobalt and iridium, The reaction gas is hydrogen chloride gas.

2. The method of claim 1, wherein: supplying a halogen-containing raw material gas to the metal source from a halogen-containing raw material gas supply device to form a metal-containing raw material gas, wherein a supply pipe for the metal-containing raw material gas is connected to the halogen-containing raw material gas supply device, The reaction gas is supplied from a reaction gas supply device, and a reaction gas supply gas pipe is connected to the reaction gas supply device.

3. The method of claim 1, wherein: The substrate includes an uneven portion arranged on a surface of the substrate.

4. The method of claim 3, wherein: The uneven portion includes at least one mask.

5. The method of claim 4, wherein: The uneven portion includes two or more openings.

6. The method of claim 1, wherein: The substrate is a patterned sapphire substrate.

7. The method of claim 1, wherein: The substrate is heated at a temperature in a range of 400°C to 700°C.

8. The method of claim 1, wherein: The metal source includes gallium.

9. The method of claim 1, wherein: The gasifying of the metal source is performed by halogenating the metal source.

10. The method of claim 1, wherein: The oxygen-containing raw material gas includes at least one selected from oxygen (O2), water (H2O) and nitrous oxide (N2O).

11. The method of claim 1, wherein: The substrate includes a corundum structure.

12. The method of claim 1, wherein: The crystalline film has a corundum structure.

13. An apparatus for producing a crystalline film, comprising: a reaction chamber including a substrate holder; A supply pipe for a metal-containing raw material gas; A supply pipe for a raw gas containing oxygen; Supply gas pipe for reaction gas, wherein the metal-containing raw material gas supply pipe is configured to supply the metal-containing raw material gas into the reaction chamber by gasifying a metal source in the metal-containing raw material gas supply pipe, wherein the supply pipe of the oxygen-containing raw material gas is configured to supply the oxygen-containing raw material gas into the reaction chamber, wherein the reaction gas supply pipe is configured to supply the reaction gas into the reaction chamber, and wherein a crystalline film is formed on the substrate held by the substrate holder by a reaction of a metal-containing raw material gas supplied through a metal-containing raw material gas supply pipe and an oxygen-containing raw material gas supplied through an oxygen-containing raw material gas supply pipe under a flow of the reaction gas supplied through the reaction gas supply pipe, The metal includes one or more of gallium, aluminum, indium, iron, chromium, vanadium, titanium, rhodium, nickel, cobalt and iridium, The reaction gas is hydrogen chloride gas.

Citation Information

Patent Citations

  • α-Ga2O3 SINGLE CRYSTAL, PRODUCTION METHOD OF α-Ga2O3, AND SEMICONDUCTOR DEVICE USING THE SAME

    JP2016155714A

  • Switching power supply circuit

    JP2017158305A

  • Semiconductor device or crystal, and method for producing semiconductor device or crystal

    WO2014050793A1

  • Method for growing beta-Ga2O3-based single crystal film, and crystalline layered structure

    CN105992841A

  • Crystalline laminate structure and method for manufacturing the same

    JP2016100592A