Single-ion polymer electrolyte containing benzimidazole, preparation method and application thereof

By using a cross-linked network structure containing benzimidazole functional groups, cyclotriphosphazene derivatives and lithium salt monomers in single-ion polymer electrolytes, combined with plasticizers, the problems of lithium dendrite growth and safety in lithium batteries are solved , achieving high room temperature ionic conductivity and improved flame retardant performance.

CN114865071BActive Publication Date: 2024-10-01JILIN UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210423592.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-04-21
Publication Date
2024-10-01
Estimated Expiration
2042-04-21

AI Technical Summary

Technical Problem

It is difficult for existing single-ion polymer electrolytes to achieve high room temperature ionic conductivity, high lithium ion migration number, wide electrochemical window and suppression of lithium dendrites while maintaining high safety and flame retardant properties in lithium batteries.

Method used

Cross-linking agents containing benzimidazole functional groups, multi-functional cyclotriphosphazene derivatives and lithium salt monomers containing double bonds are used for cross-linking to form a cross-linked network structure, combined with plasticizers, to prepare high room temperature Single-ion polymer gel electrolyte with ionic conductivity, wide electrochemical window and flame retardant properties.

Benefits of technology

It achieves the synergistic improvement of high room temperature ionic conductivity, wide electrochemical window, lithium ion migration number and flame retardant performance, significantly inhibits the growth of lithium dendrites, and improves the safety and cycle performance of lithium batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114865071B_ABST
    Figure CN114865071B_ABST
Patent Text Reader

Abstract

The present invention provides a single-ion polymer electrolyte containing benzimidazole, a preparation method and its application. First, a novel cross-linking agent containing benzimidazole functional groups is synthesized, and then mixed with a lithium salt monomer containing a double bond, an initiator, and a derivative of a multifunctional cyclotriphosphazene, and a single-ion polymer solid electrolyte with a cross-linked network structure is generated in situ by free radical polymerization, and then soaked in a plasticizer to obtain a single-ion polymer gel electrolyte. The single-ion polymer gel electrolyte prepared by the present invention has high room temperature ionic conductivity, high lithium ion migration number, wide electrochemical window, excellent flame retardant performance, and effectively inhibits the growth of lithium dendrites, and is widely used in the field of lithium batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of lithium batteries, and in particular relates to a single-ion polymer electrolyte containing benzimidazole, a preparation method and an application thereof. Background Art

[0002] With the rapid development of electric vehicles, smart grids and the upgrading of portable electronic products, people are committed to developing a high energy density (≥500Wh / kg) and high safety energy storage technology. Although traditional lithium-ion batteries are widely used due to their advantages such as high output voltage, no memory effect, and low self-discharge, they still cannot meet people's needs for high energy density and high power density energy storage batteries. Lithium metal has the advantages of the lowest redox potential, the highest theoretical specific capacity, and low density. It is crucial to use it as an anode material to develop lithium metal batteries with higher energy density, longer service life, and better safety.

[0003] As we all know, lithium metal has high chemical activity and will react with the electrolyte to produce lithium dendrites that pierce the diaphragm, causing the battery to short-circuit, causing the battery to have a series of problems such as thermal runaway, combustion, and explosion. To solve the problem of lithium dendrites, there are several main solutions in current research: one is to modify the surface of lithium metal to construct a solid artificial solid electrolyte interface (SEI) layer (J.Mater.Chem.A, 2019, 7, 13113), hindering the nucleation of lithium dendrites and inhibiting the growth of lithium dendrites; the other is the optimization design of the electrolyte (CN 108630992 B, CN 110416615 A), and the film-forming additives in the electrolyte will promote the formation of a stable SEI film on the surface of lithium metal, thereby inhibiting the growth of lithium dendrites; there is also the preparation of single-ion polymer electrolytes to achieve uniform lithium ion flux for inhibiting the growth of lithium dendrites. Due to the complexity of polymer structures and the diversity of types, researchers have gradually set off a wave of research on single-ion polymer electrolytes.

[0004] Chinese patent CN 112164824 B prepares an anion receptor type single ion conductor flame retardant polymer gel electrolyte, which uses an electrospun PVDF membrane as a substrate. Although the mechanical strength of the polymer gel electrolyte can be improved, the PVDF membrane will affect the ionic conductivity of the gel electrolyte to a certain extent, and it is difficult to control the uniformity of the gel electrolyte membrane.

[0005] As mentioned in the review, how to rationally design the chemical structure of the polymer, utilize the synergistic effect of each component, simplify the preparation process, and ultimately obtain a single-ion polymer electrolyte with high room temperature ionic conductivity, high lithium ion migration number, wide electrochemical window, high dimensional stability and the ability to inhibit lithium dendrites is one of the problems that need to be solved urgently. Summary of the invention

[0006] In order to solve the above technical problems, the present invention provides a single-ion polymer gel electrolyte containing benzimidazole, and its preparation method comprises the following steps:

[0007] (1) adding a cross-linking agent containing a benzimidazole functional group, a multifunctional cyclotriphosphazene derivative, a double-bond-containing lithium salt monomer, and an initiator to a solvent in sequence to obtain a uniform and transparent casting solution, wherein the initiator is a thermal initiator or a photoinitiator;

[0008] (2) after passing an inert gas into the casting solution obtained in step (1), casting it on a clean substrate, reacting it at 60-100° C. for 8-12 hours, and then drying it at 100-140° C. for 24-36 hours to obtain a single-ion polymer solid electrolyte, and then soaking it in a plasticizer to obtain a single-ion polymer gel electrolyte; the single-ion polymer gel electrolyte contains a cross-linked network structure of benzimidazole;

[0009] Furthermore, in step (1), the mass percentage of the cross-linking agent containing benzimidazole functional groups is 10-30%; the mass percentage of the multifunctional cyclotriphosphazene derivative is 20-45%; the mass percentage of the lithium salt monomer containing double bonds is 40-60%; the mass percentage of the initiator to the total mass of the cross-linking agent, the cyclotriphosphazene derivative and the lithium salt monomer is 1-5%;

[0010] Furthermore, the structure of the cross-linking agent containing a benzimidazole functional group in step (1) is as follows:

[0011]

[0012] R1 is any of the following structures:

[0013]

[0014] Further, the multifunctional cyclotriphosphazene derivative described in step (1) is any one of hexa-(eugenol)cyclotriphosphazene or hexa-(2-allylphenoxy)cyclotriphosphazene, and their structures are as follows:

[0015]

[0016] Further, the double bond-containing lithium salt monomer in step (1) is any one of (trifluoromethanesulfonyl)-(vinylsulfonyl)imide lithium, 1-[3-(methacryloyloxy)propylsulfonyl]-1-(trifluoromethanesulfonyl)imide lithium or (4-styrenesulfonyl)-(trifluoromethanesulfonyl)imide lithium, and their structures are as follows:

[0017]

[0018] R2 is any of the following structures:

[0019]

[0020] Furthermore, the inert gas in step (2) is any one of nitrogen or argon.

[0021] The crosslinking agent containing benzimidazole functional groups is any one of 2,2'-bis(propylene)-5,5'-bibenzimidazole, 2,2'-bis(chloromethyl)-5,5'-bibenzimidazole, 2,2'-bis(vinyl)-5,5'-bibenzimidazole or 2,2'-bis(phenylvinyl)-5,5'-bibenzimidazole.

[0022] Furthermore, the 2,2'-bis(propylene)-5,5'-bibenzimidazole is prepared by the following method: α-methylacrylic acid and 3,3'-diaminobenzidine are dissolved in a mixed solution of polyphosphoric acid and phosphoric acid in a volume ratio of 1:4, the mass ratio of α-methylacrylic acid to 3,3'-diaminobenzidine is 1:1-1:3, under the protection of inert gas, mechanically stirred at 160-185°C for 5-10 hours, poured into distilled water, and then sodium bicarbonate is added to adjust the solution pH to 7-9 to obtain a precipitate, and then filtered, washed with water, recrystallized, and vacuum dried to obtain 2,2'-bis(propylene)-5,5'-bibenzimidazole.

[0023] Furthermore, the 2,2'-bis(chloromethyl)-5,5'-bibenzimidazole is prepared by the following method: chloroacetic acid and 3,3'-diaminobenzidine are mixed and dissolved in a 3M-6M hydrochloric acid solution, wherein the mass ratio of the chloroacetic acid to the 3,3'-diaminobenzidine is 1:1-3:1; under the protection of an inert gas, the reaction solution is mechanically stirred at 100-130°C for 8-10 hours, then the reaction solution is cooled to 60-90°C, filtered, the filtrate is poured into water, sodium hydroxide is added and stirred, the pH value of the solution is adjusted to 7-9, and then 2,2'-bis(chloromethyl)-5,5'-bibenzimidazole is obtained after suction filtration, washing, and freeze-drying.

[0024] Furthermore, the photoinitiator in step (1) is any one of 2-hydroxy-2-methyl-1-phenylpropanone, 1-hydroxycyclohexyl phenyl ketone or benzoin dimethyl ether; and the thermal initiator is any one of azobisisobutyronitrile, dibenzoyl peroxide or potassium persulfate.

[0025] Furthermore, the solvent in step (1) is any one of dimethyl sulfoxide, N,N-dimethylformamide, N,N-dimethylacetamide, acetone, tetrahydrofuran or N-methylpyrrolidone.

[0026] Furthermore, the multifunctional cyclotriphosphazene derivative described in step (1) is hexa-(eugenol) cyclotriphosphazene, which is prepared by the following method: dissolving eugenol and anhydrous potassium carbonate in anhydrous acetonitrile, stirring magnetically for 1-4 hours, and then adding an acetonitrile solution of hexachlorocyclotriphosphazene under N2 protection, wherein the mass ratio of eugenol, anhydrous potassium carbonate and hexachlorocyclotriphosphazene is 4:3:1-6:5:1, reacting at 85-120°C for 24-48 hours, filtering, and recrystallizing to obtain hexa-(eugenol) cyclotriphosphazene.

[0027] Furthermore, the substrate in step (2) is any one of a glass plate, a polytetrafluoroethylene plate, a steel plate or a silica gel plate; the plasticizer is any one of cyclopentane sulfone, ethylene carbonate, propylene carbonate, polyethylene glycol monomethyl ether, diethyl carbonate, a mixture of ethylene carbonate and propylene carbonate in a volume ratio of 1:1, a mixture of ethylene carbonate and dimethyl carbonate in a volume ratio of 1:1, or a mixture of ethylene carbonate and diethyl carbonate in a volume ratio of 1:1.

[0028] The present invention also provides an application of a single-ion polymer electrolyte containing benzimidazole in the field of lithium batteries. The single-ion polymer electrolyte containing benzimidazole can effectively inhibit the growth of lithium dendrites and has good flame retardancy and a room temperature ionic conductivity of 4.7×10 -3 -7.4×10 -2 S / cm, lithium ion migration number ≈1, electrochemical window ≥5.7V.

[0029] The advantages of the present invention are:

[0030] The present invention obtains a single-ion polymer gel electrolyte with high room temperature ion conductivity, high lithium ion migration number, wide electrochemical window, high dimensional stability, and the ability to inhibit lithium dendrites. The single-ion polymer gel electrolyte combines the advantages of liquid electrolytes and solid electrolytes, and has higher safety than liquid electrolytes; it has higher ion conductivity than solid electrolytes. In addition, due to the presence of plasticizers, the problem of poor interface contact between the electrolyte and the electrode material in solid electrolytes can be solved, providing more excellent performance, and is applied to the field of lithium batteries.

[0031] The present invention adopts a cross-linking agent containing a benzimidazole functional group, a multifunctional cyclotriphosphazene derivative and a double-bond-containing lithium salt monomer for cross-linking to obtain a single-ion polymer gel electrolyte, so that anions are fixed in the cross-linking network and are difficult to move. Only lithium ions can move freely in the system, which can increase the lithium ion migration number and inhibit the growth of lithium dendrites.

[0032] The present invention promotes ( ) structure, increasing the concentration of free lithium ions; at the same time, there are highly electronegative heteroatoms in the cross-linked network, and the plasticizer is also a polar molecule, which will produce a "coordination-dissociation-recoordination" interaction with lithium ions, promoting the migration of lithium ions and improving the conductivity of lithium ions. The room temperature ionic conductivity of the single-ion polymer gel electrolyte is the result of the synergistic effect of multiple factors such as the content of free lithium ions, migration rate, benzimidazole functional groups in the cross-linked structure, plasticizers, and preparation process.

[0033] The present invention utilizes a cross-linking network structure generated by a cross-linking agent containing a benzimidazole functional group, a multifunctional cyclotriphosphazene derivative, and a double-bond-containing lithium salt monomer to improve the dimensional stability of a single-ion polymer gel electrolyte, thereby improving the cycle performance of a battery. In addition, the flame retardant properties of the cyclotriphosphazene derivative itself are utilized to introduce a flame retardant group into the cross-linking network structure to prepare a single-ion polymer gel electrolyte with excellent flame retardant performance, thereby improving the safety performance of the battery.

[0034] The present invention adopts a "one-pot method" to in-situ generate a cross-linked network structure with excellent dimensional stability, which simplifies the production process and improves the mechanical properties of the electrolyte. The cross-linking agent containing benzimidazole functional groups has the dual effects of "self-polymerization" and "cross-linking", which is of great significance for improving the mechanical and battery properties of single-ion polymer gel electrolytes. In addition, the derivative of cyclotriphosphazene with flame retardant properties also participates in the cross-linking reaction and will be fixed in the cross-linked network structure, rather than being simply added to the liquid electrolyte or polymer electrolyte, which can avoid the adverse effects of incompatibility with electrode materials and low mechanical properties caused by simple blending.

[0035] The present invention prepares a single-ion polymer electrolyte containing benzimidazole, more specifically, a single-ion polymer gel electrolyte, which can be applied to the field of lithium batteries. The performance of the single-ion polymer gel electrolyte is: the room temperature ion conductivity is 4.7×10 -3 -7.4×10 -2 S / cm, lithium ion migration number ≈1, electrochemical window ≥5.7V, can effectively inhibit the growth of lithium dendrites and has good flame retardant properties. The single-ion polymer gel electrolyte prepared by the present invention has high room temperature ionic conductivity, high lithium ion migration number, and wide electrochemical window, which is the result of the synergistic effect of multiple factors such as raw material type, raw material reaction ratio, free lithium ion content, migration rate, benzimidazole functional groups in the cross-linked structure, plasticizer, and preparation process. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 (a) and (b) are respectively the H NMR spectra of 2,2'-bis(propylene)-5,5'-bibenzimidazole and hexa(eugenol)cyclotriphosphazene in Example 1 of the present invention;

[0037] Figure 2 A graph showing the relationship between the voltage and the charge-discharge specific capacity at 25° C. and 0.2C for a battery assembled with a single-ion polymer gel electrolyte in Example 2 of the present invention;

[0038] Figure 3 This is a flame retardant performance test diagram of the single-ion polymer gel electrolyte in Example 2 of the present invention. DETAILED DESCRIPTION

[0039] Example 1 Synthesis of single ion polymer gel electrolyte 1

[0040] (1) Synthesis of 2,2'-bis(propylene)-5,5'-bibenzimidazole

[0041] 4.30 g of α-methylacrylic acid, 5.41 g of 3,3'-diaminobenzidine, 10 mL of polyphosphoric acid and 40 mL of phosphoric acid were added to a 100 mL three-necked flask, and the mixture was stirred mechanically at 185°C for 5 h under a N2 environment. After the reaction, the solution was poured into distilled water, and then sodium bicarbonate was added to neutralize the mixture to pH = 7. A precipitate appeared in the solution, which was then filtered, washed with water, recrystallized from an ethanol / water solution, and dried in vacuo to obtain 2,2'-bis(propylene)-5,5'-bibenzimidazole.

[0042] Among them, the synthetic route of 2,2'-bis(propylene)-5,5'-bibenzimidazole is:

[0043]

[0044] In addition, the chemical structure of 2,2'-bis(propylene)-5,5'-bibenzimidazole is as follows:

[0045]

[0046] The chemical structure above marks the active hydrogens of 2,2'-bis(propenyl)-5,5'-bibenzimidazole at different chemical shifts. 2.24 ppm is the proton hydrogen H of the methyl group on the propenyl group. a The chemical shifts of 5.48 ppm and 6.02 ppm are respectively due to the H b , H c The chemical shift of 12.6 ppm is due to the H g The chemical shift of 7.63ppm is due to the H e The chemical shift of 7.53ppm is due to the H d The chemical shift of 7.78 is due to the H f For details of chemical shift, see the instruction manual Figure 1(a) This proves that 2,2'-bis(propylene)-5,5'-bibenzimidazole was successfully prepared.

[0047] (2) Synthesis of hexa(eugenol)cyclotriphosphazene

[0048] Dissolve 42.5 g of eugenol in 200 mL of anhydrous acetonitrile, add 40 g of anhydrous potassium carbonate, and stir magnetically for 1 h. Under N2 environment, add 10 g of hexachlorocyclotriphosphazene dissolved in 50 mL of anhydrous acetonitrile dropwise to the above solution, react at 85 °C for 48 h, filter the solid, and collect the filtrate. Recrystallize with ethanol to obtain hexa-(eugenol)cyclotriphosphazene.

[0049] Among them, the synthetic route of hexa-(eugenol)cyclotriphosphazene is:

[0050]

[0051] In addition, the chemical structure of hexa(eugenol)cyclotriphosphazene is as follows:

[0052]

[0053] The chemical structure above labels the active hydrogens of hexa(eugenol)cyclotriphosphazene at different chemical shifts.

[0054] 5.04-5.08ppm, 3.28ppm, and 5.91ppm are H on the allyl group, respectively. f , H d , H e The chemical shift of 6.48ppm is due to the H c The chemical shift of 6.60ppm is due to the H b The chemical shift of 6.92ppm is due to the H a The chemical shift of 3.64 ppm is due to the H g For details of chemical shift, see the instruction manual Figure 1 (b) This proves that hexa(eugenol)cyclotriphosphazene was successfully prepared.

[0055] (3) Synthesis of lithium (trifluoromethanesulfonyl)-(vinylsulfonyl)imide

[0056] 18.0g trifluoromethanesulfonamide, 36.65g triethylamine and 150mL THF were added to a 500mL round-bottom flask. Then 20.67g of 2-chloroethanesulfonyl chloride was dissolved in 80mL of THF solution and added dropwise to the above solution, and magnetically stirred for 1h at 0℃. Then reacted at 25℃ for 20h. Filtered and the filtrate was concentrated under reduced pressure. The solid was dissolved in acetonitrile, 33.5g of potassium carbonate was added, magnetically stirred for 4h at 0℃, filtered, and dried to obtain the intermediate product (trifluoromethanesulfonyl)-(vinylsulfonyl)imide potassium. 11.6g of lithium perchlorate trihydrate and 20.0g of (trifluoromethanesulfonyl)-(vinylsulfonyl)imide potassium were dissolved in 50mL of acetonitrile, stirred at room temperature for 12h, filtered, and freeze-dried to obtain the product (trifluoromethanesulfonyl)-(vinylsulfonyl)imide lithium.

[0057] (4) Synthesis of single-ion polymer gel electrolyte 1

[0058] 0.0314g of 2,2'-bis(propylene)-5,5'-bibenzimidazole, 0.1113g of hexa(eugenol)cyclotriphosphazene, 0.1109g of (trifluoromethanesulfonyl)-(vinylsulfonyl)imide lithium, and 0.0051g of azobisisobutyronitrile were dissolved in 3mL of N-methylpyrrolidone to obtain a transparent casting solution. After nitrogen was introduced into the casting solution for 2h, it was cast on a clean glass plate and reacted at 80℃ for 12h to generate a cross-linked single-ion polymer electrolyte membrane in situ, which was then dried at 120℃ for 24h to completely remove the solvent and obtain a single-ion polymer solid electrolyte. The polymer solid electrolyte was soaked in ethylene carbonate / dimethyl carbonate (volume ratio of 1:1) to obtain a single-ion polymer gel electrolyte 1.

[0059] The single ion polymer gel electrolyte 1 obtained in Example 1 was subjected to relevant electrochemical performance tests, and relevant data of room temperature ionic conductivity, lithium ion migration number, and electrochemical window are listed in Table 1.

[0060] Example 2 Synthesis of single ion polymer gel electrolyte 2

[0061] 0.0628g of 2,2'-bis(propylene)-5,5'-bibenzimidazole, 0.1113g of hexa(eugenol)cyclotriphosphazene, 0.1386g of (trifluoromethanesulfonyl)-(vinylsulfonyl)imide lithium, and 0.0051g of azobisisobutyronitrile were dissolved in 3.7mL of N-methylpyrrolidone to obtain a transparent casting solution. After nitrogen was introduced into the casting solution for 2h, it was cast on a clean glass plate and reacted at 100℃ for 10h to generate a cross-linked single-ion polymer electrolyte membrane in situ, which was then dried at 140℃ for 30h to completely remove the solvent and obtain a single-ion polymer solid electrolyte. The polymer solid electrolyte was soaked in ethylene carbonate / dimethyl carbonate (volume ratio of 1:1) to obtain a single-ion polymer gel electrolyte 2.

[0062] The single ion polymer gel electrolyte 2 obtained in Example 2 was subjected to relevant electrochemical performance tests, and the relevant data of room temperature ionic conductivity, lithium ion migration number, and electrochemical window are listed in Table 1. The single ion polymer gel electrolyte obtained in Example 2 was assembled into a battery, and the discharge specific capacity reached 161 mA·h / g at 25°C and 0.2C. See the attached specification for details. Figure 2 .

[0063] Example 3 Synthesis of single ion polymer gel electrolyte 3

[0064] 0.0942g of 2,2'-bis(propylene)-5,5'-bibenzimidazole, 0.1113g of hexa(eugenol)cyclotriphosphazene, 0.1663g of (trifluoromethanesulfonyl)-(vinylsulfonyl)imide lithium, and 0.0051g of azobisisobutyronitrile were dissolved in 4.4mL of N-methylpyrrolidone to obtain a transparent casting solution. After nitrogen was introduced into the casting solution for 2h, it was cast on a clean glass plate and reacted at 100℃ for 12h to generate a cross-linked single-ion polymer electrolyte membrane in situ, which was then dried at 140℃ for 36h to completely remove the solvent and obtain a single-ion polymer solid electrolyte. The polymer solid electrolyte was soaked in ethylene carbonate / dimethyl carbonate (volume ratio of 1:1) to obtain a single-ion polymer gel electrolyte 3.

[0065] The single ion polymer gel electrolyte 3 obtained in Example 3 was subjected to relevant electrochemical performance tests, and the relevant data of room temperature ionic conductivity, lithium ion migration number, and electrochemical window are listed in Table 1.

[0066] Example 4 Synthesis of single ion polymer gel electrolyte 4

[0067] 0.0314g of 2,2'-bis(propylene)-5,5'-bibenzimidazole, 0.1113g of hexa(eugenol)cyclotriphosphazene, 0.1109g of 1-[3-(methacryloyloxy)propylsulfonyl]-1-(trifluoromethanesulfonyl)imide lithium, and 0.0051g of azobisisobutyronitrile were dissolved in 3mL of N-methylpyrrolidone to obtain a transparent casting solution. After nitrogen was introduced into the casting solution for 2h, it was cast on a clean glass plate and reacted at 80°C for 10h to generate a cross-linked single-ion polymer electrolyte membrane in situ, which was then dried at 120°C for 30h to completely remove the solvent and obtain a single-ion polymer solid electrolyte. The polymer solid electrolyte was soaked in ethylene carbonate / dimethyl carbonate (volume ratio of 1:1) to obtain a single-ion polymer gel electrolyte 4.

[0068] The single ion polymer gel electrolyte 4 obtained in Example 4 was subjected to relevant electrochemical performance tests, and the relevant data of room temperature ionic conductivity, lithium ion migration number, and electrochemical window are listed in Table 1.

[0069] Example 5 Synthesis of single ion polymer gel electrolyte 5

[0070] 0.0628g of 2,2'-bis(propylene)-5,5'-bibenzimidazole, 0.1113g of hexa(eugenol)cyclotriphosphazene, 0.1386g of 1-[3-(methacryloyloxy)propylsulfonyl]-1-(trifluoromethanesulfonyl)imide lithium, and 0.0051g of azobisisobutyronitrile were dissolved in 3.7mL of N-methylpyrrolidone to obtain a transparent casting solution. After nitrogen was introduced into the casting solution for 2h, it was cast on a clean glass plate and reacted at 100℃ for 12h to generate a cross-linked single-ion polymer electrolyte membrane in situ, which was then dried at 120℃ for 34h to completely remove the solvent and obtain a single-ion polymer solid electrolyte. The polymer solid electrolyte was soaked in ethylene carbonate / dimethyl carbonate (volume ratio of 1:1) to obtain a single-ion polymer gel electrolyte 5.

[0071] The single ion polymer gel electrolyte 5 obtained in Example 5 was subjected to relevant electrochemical performance tests, and the relevant data of room temperature ionic conductivity, lithium ion migration number, and electrochemical window are listed in Table 1.

[0072] Example 6 Synthesis of single ion polymer gel electrolyte 6

[0073] 0.0942g of 2,2'-bis(propylene)-5,5'-bibenzimidazole, 0.1113g of hexa(eugenol)cyclotriphosphazene, 0.1663g of 1-[3-(methacryloyloxy)propylsulfonyl]-1-(trifluoromethanesulfonyl)imide lithium, and 0.0051g of azobisisobutyronitrile were dissolved in 4.4mL of N-methylpyrrolidone to obtain a transparent casting solution. After nitrogen was introduced into the casting solution for 2h, it was cast on a clean glass plate and reacted at 100℃ for 12h to generate a cross-linked single-ion polymer electrolyte membrane in situ, which was then dried at 140℃ for 36h to completely remove the solvent and obtain a single-ion polymer solid electrolyte. The polymer solid electrolyte was soaked in ethylene carbonate / dimethyl carbonate (volume ratio of 1:1) to obtain a single-ion polymer gel electrolyte 6.

[0074] The single ion polymer gel electrolyte 6 obtained in Example 6 was subjected to relevant electrochemical performance tests, and the relevant data of room temperature ionic conductivity, lithium ion migration number, and electrochemical window are listed in Table 1.

[0075] Comparative Example 1 Flame-retardant single-ion conducting polymer electrolytes based on anion acceptors for high-safety lithium metal batteries, Kuirong Deng et al., J. Mater. Chem. A, 2021, 9, 7692. This article uses electrospun PVDF membrane as a support membrane, allyl boric acid pyranol ester, ethoxylated trimethylolpropane triacrylate, pentaerythritol tetrathioglycolate as monomers, 0.8M LiFSI+0.3M LiDFOB+0.02M LiPF6 in EC / FEC / PFPN (70:25:5vol) as a plasticizer, and UV curing to prepare a cross-linked single-ion polymer gel electrolyte. The room temperature ionic conductivity of the single-ion polymer gel electrolyte is 2.52×10 -3 S / cm, the lithium ion transfer number is 0.79, and the electrochemical window is 5.5V, all of which are lower than the single ion polymer gel electrolyte obtained in Example 1 of the present invention, which has the least ideal performance.

[0076] Comparative Example 2 Gel Polymer Electrolytes Based on Polymerizable Lithium Salt and Poly (ethylene glycol) for Lithium Battery Applications, Jong-Chan Lee et al., ACS Appl. Mater. Interfaces 2019, 11, 29718-29724. This article uses (trifluoromethanesulfonyl) - (vinylsulfonyl) imide lithium as a lithium source, poly (ethylene glycol) dimethacrylate (PEGDMA, Mn = 750) as a cross-linking agent and poly (ethylene glycol) methyl ether methacrylate (PEGMA, Mn = 500) as a lithium ion conductive carrier, PC as a plasticizer, AIBN as an initiator, to prepare a cross-linked single-ion polymer gel electrolyte, the room temperature ionic conductivity of the single-ion polymer gel electrolyte is 6.7 × 10 -4 S / cm, the lithium ion transfer number is 0.52, and the electrochemical window is 5.2V, all of which are lower than the single ion polymer gel electrolyte obtained in Example 1 of the present invention, which has the least ideal performance.

[0077] Table 1 Electrochemical performance test data of Examples 1-6

[0078] performance Room temperature ionic conductivity (S / cm) Lithium ion migration number Electrochemical Window (V) Example 1 <![CDATA[4.7×10 -3 ]]> 0.95 5.7 Example 2 <![CDATA[3.6×10 -2 ]]> 0.97 5.8 Example 3 <![CDATA[8.0×10 -3 ]]> 0.96 5.8 Example 4 <![CDATA[5.2×10 -3 ]]> 0.95 5.7 Example 5 <![CDATA[7.4×10 -2 ]]> 0.98 5.9 Example 6 <![CDATA[9.1×10 -3 ]]> 0.95 5.8 Comparative Example 1 <![CDATA[2.52×10 -3 ]]> 0.79 5.5 Comparative Example 2 <![CDATA[6.7×10 -4 ]]> 0.52 5.2

[0079] It can be seen from Table 1 that the room temperature ionic conductivity of the cross-linked single ion polymer gel electrolyte prepared in Examples 1-6 of the present invention is between 4.7×10 -3 -7.4×10 -2 S / cm, which can meet the commercialization of lithium battery gel electrolyte (≥10 -3 S / cm) requirement. It can be found from Examples 1-6 that with the increase in the content of lithium salt monomers containing double bonds, the ionic conductivity does not increase monotonically. It can be seen from Table 1 that the room temperature ionic conductivity, lithium ion transfer number and electrochemical window of Example 5 are all the highest, from which it can be concluded that the high ionic conductivity, high lithium ion migration number and wide electrochemical window of the cross-linked single-ion polymer gel electrolyte are the result of the synergistic effect of multiple factors such as the type of raw materials, the reaction ratio of the raw materials, the content of free lithium ions, the migration rate, the benzimidazole functional group in the cross-linked structure, the plasticizer and the preparation process. Compared with the comparative example, the ionic conductivity, lithium ion transfer number and electrochemical window of the single-ion polymer gel electrolyte of all Examples 1-6 of the present invention are significantly higher than those of the comparative example. In addition, the present invention can also effectively inhibit the growth of lithium dendrites. From Figure 3It can be seen that the prepared cross-linked single-ion polymer gel electrolyte has certain flame retardant properties. When encountering flames, it will hinder the spread of flames and will not curl, thus ensuring the size of the single-ion polymer gel electrolyte.

[0080] Example 7 Synthesis of single ion polymer gel electrolyte 7

[0081] (1) Synthesis of 2,2'-bis(chloromethyl)-5,5'-bibenzimidazole

[0082] 2.36 g of chloroacetic acid and 2.14 g of 3,3'-diaminobenzidine were added to a 250 mL three-necked flask, and then 80 mL of 3M hydrochloric acid solution was added to the three-necked flask. Under the protection of nitrogen, the reaction solution was mechanically stirred at 120° C. for 10 h, then the temperature was lowered to 90° C. and filtered. The filtrate was poured into water, and sodium hydroxide was added and stirred. The pH value of the solution was adjusted to 7. After suction filtration, washing, and freeze-drying, 2,2'-bis(chloromethyl)-5,5'-bibenzimidazole was obtained.

[0083] (2) Synthesis of single-ion polymer gel electrolyte 7

[0084] 0.0628g of 2,2'-bis(chloromethyl)-5,5'-bibenzimidazole, 0.2226g of hexa(eugenol)cyclotriphosphazene, 0.2218g of (4-styrenesulfonyl)-(trifluoromethanesulfonyl)imide lithium, and 0.0102g of azobisisobutyronitrile were dissolved in 6mL of N-methylpyrrolidone to obtain a transparent casting solution. After nitrogen was introduced into the casting solution for 2h, it was cast on a clean glass plate and reacted at 60°C for 12h to generate a single-ion polymer electrolyte membrane in situ, which was then dried at 140°C for 36h to completely remove the solvent and obtain a single-ion polymer solid electrolyte. The polymer solid electrolyte was soaked in ethylene carbonate / diethyl carbonate (volume ratio of 1:1) to obtain a single-ion polymer gel electrolyte 7.

[0085] Example 8 Synthesis of single ion polymer gel electrolyte 8

[0086] 0.0628g of 2,2'-bis(chloromethyl)-5,5'-bibenzimidazole, 0.2226g of hexa(eugenol)cyclotriphosphazene, 0.1386g of (4-styrenesulfonyl)-(trifluoromethanesulfonyl)imide lithium, and 0.0204g of azobisisobutyronitrile were dissolved in 4.7mL of N-methylpyrrolidone to obtain a transparent casting solution. After nitrogen was introduced into the casting solution for 2h, it was cast on a clean glass plate and reacted at 100℃ for 10h to generate a single-ion polymer electrolyte membrane in situ, which was then dried at 120℃ for 30h to completely remove the solvent and obtain a single-ion polymer solid electrolyte. The polymer solid electrolyte was soaked in ethylene carbonate / diethyl carbonate (volume ratio of 1:1) to obtain a single-ion polymer gel electrolyte 8.

[0087] Example 9 Synthesis of Single Ion Polymer Gel Electrolyte 9

[0088] 0.1884g of 2,2'-bis(chloromethyl)-5,5'-bibenzimidazole, 0.3339g of hexa(eugenol)cyclotriphosphazene, 0.2218g of (trifluoromethanesulfonyl)-(vinylsulfonyl)imide lithium, and 0.0102g of azobisisobutyronitrile were dissolved in 8.4mL of N-methylpyrrolidone to obtain a transparent casting solution. After nitrogen was introduced into the casting solution for 2h, it was cast on a clean glass plate and reacted at 100°C for 12h to generate a single-ion polymer electrolyte membrane in situ, which was then dried at 140°C for 36h to completely remove the solvent and obtain a single-ion polymer solid electrolyte. The polymer solid electrolyte was soaked in ethylene carbonate / propylene carbonate (volume ratio of 1:1) to obtain a single-ion polymer gel electrolyte 9.

Claims

1. A single-ion polymer electrolyte containing benzimidazole, characterized in that: Its preparation method comprises the following steps: (1) adding a cross-linking agent containing a benzimidazole functional group, a multifunctional cyclotriphosphazene derivative, a double-bond-containing lithium salt monomer, and an initiator to a solvent in sequence to obtain a uniform and transparent casting solution, wherein the initiator is a thermal initiator or a photoinitiator; (2) after passing an inert gas into the casting solution obtained in step (1), casting it on a clean substrate, reacting at 60-100° C. for 8-12 hours, drying at 100-140° C. for 24-36 hours, and then soaking it in a plasticizer to obtain a single-ion polymer electrolyte containing benzimidazole; the single-ion polymer electrolyte is a single-ion polymer gel electrolyte containing a benzimidazole cross-linked network structure; Step (1) is calculated by weight percentage: the weight percentage of the cross-linking agent containing benzimidazole functional groups is 10-30%; the weight percentage of the multifunctional cyclotriphosphazene derivative is 20-45%; the weight percentage of the lithium salt monomer containing double bonds is 40-60%; the weight percentage of the initiator to the total weight of the cross-linking agent, the cyclotriphosphazene derivative and the lithium salt monomer is 1-5%; The structure of the cross-linking agent containing benzimidazole functional groups described in step (1) is as follows: R1 is any of the following structures: The multifunctional cyclotriphosphazene derivative described in step (1) is any one of hexa-(eugenol)cyclotriphosphazene or hexa-(2-allylphenoxy)cyclotriphosphazene, and their structures are as follows: The double bond-containing lithium salt monomer described in step (1) is any one of (trifluoromethanesulfonyl)-(vinylsulfonyl)imide lithium, 1-[3-(methacryloyloxy)propylsulfonyl]-1-(trifluoromethanesulfonyl)imide lithium or (4-styrenesulfonyl)-(trifluoromethanesulfonyl)imide lithium, and their structures are as follows: R2 is any of the following structures: The inert gas in step (2) is any one of nitrogen or argon.

2. The single-ion polymer electrolyte containing benzimidazole according to claim 1, characterized in that: The cross-linking agent containing benzimidazole functional groups in step (1) is any one of 2,2'-bis(propylene)-5,5'-bibenzimidazole, 2,2'-bis(chloromethyl)-5,5'-bibenzimidazole, 2,2'-bis(vinyl)-5,5'-bibenzimidazole or 2,2'-bis(phenylvinyl)-5,5'-bibenzimidazole.

3. A single-ion polymer electrolyte containing benzimidazole according to claim 2, characterized in that: The 2,2'-bis(propylene)-5,5'-bibenzimidazole is prepared by the following method: α-methylacrylic acid and 3,3'-diaminobenzidine are dissolved in a mixed solution of polyphosphoric acid and phosphoric acid in a volume ratio of 1:4, wherein the mass ratio of the α-methylacrylic acid to the 3,3'-diaminobenzidine is 1:1-1:3; under the protection of an inert gas, the mixture is mechanically stirred at 160-185°C for 5-10 hours, poured into distilled water, and then sodium bicarbonate is added to adjust the pH value of the solution to 7-9 to obtain a precipitate; and then the precipitate is filtered, washed with water, recrystallized, and vacuum dried to obtain 2,2'-bis(propylene)-5,5'-bibenzimidazole.

4. The single-ion polymer electrolyte containing benzimidazole according to claim 2, characterized in that: The 2,2'-bis(chloromethyl)-5,5'-bibenzimidazole is prepared by the following method: chloroacetic acid and 3,3'-diaminobenzidine are mixed and dissolved in a 3M-6M hydrochloric acid solution, wherein the mass ratio of the chloroacetic acid to the 3,3'-diaminobenzidine is 1:1-3:1; under the protection of an inert gas, the reaction solution is mechanically stirred at 100-130°C for 8-10 hours, then the reaction solution is cooled to 60-90°C, filtered, the filtrate is poured into water, sodium hydroxide is added and stirred, the pH value of the solution is adjusted to 7-9, and then 2,2'-bis(chloromethyl)-5,5'-bibenzimidazole is obtained after suction filtration, washing and freeze drying.

5. A single-ion polymer electrolyte containing benzimidazole according to any one of claims 1 to 4, characterized in that: The photoinitiator in step (1) is any one of 2-hydroxy-2-methyl-1-phenylpropanone, 1-hydroxycyclohexyl phenyl ketone or benzoin dimethyl ether; the thermal initiator is any one of azobisisobutyronitrile, dibenzoyl peroxide or potassium persulfate.

6. The single-ion polymer electrolyte containing benzimidazole according to claim 5, characterized in that: The solvent in step (1) is any one of dimethyl sulfoxide, N,N-dimethylformamide, N,N-dimethylacetamide, acetone, tetrahydrofuran or N-methylpyrrolidone.

7. A single-ion polymer electrolyte containing benzimidazole according to claim 6, characterized in that: The multifunctional cyclotriphosphazene derivative described in step (1) is hexa-(eugenol) cyclotriphosphazene, which is prepared by the following method: dissolving eugenol and anhydrous potassium carbonate in anhydrous acetonitrile, stirring magnetically for 1-4 hours, and then adding an acetonitrile solution of hexachlorocyclotriphosphazene under N2 protection, wherein the mass ratio of eugenol, anhydrous potassium carbonate and hexachlorocyclotriphosphazene is 4:3:1-6:5:1, reacting at 85-120°C for 24-48 hours, filtering, and recrystallizing to obtain hexa-(eugenol) cyclotriphosphazene.

8. The single-ion polymer electrolyte containing benzimidazole according to claim 7, characterized in that: The substrate in step (2) is any one of a glass plate, a polytetrafluoroethylene plate, a steel plate or a silica gel plate; the plasticizer is any one of cyclopentane sulfone, ethylene carbonate, propylene carbonate, dimethyl carbonate, polyethylene glycol monomethyl ether, diethyl carbonate, a mixture of ethylene carbonate and propylene carbonate in a volume ratio of 1:1, a mixture of ethylene carbonate and dimethyl carbonate in a volume ratio of 1:1, or a mixture of ethylene carbonate and diethyl carbonate in a volume ratio of 1:

1.

9. Use of the benzimidazole-containing single-ion polymer electrolyte according to claim 8 in the field of lithium batteries.

10. The use of the single-ion polymer electrolyte containing benzimidazole in the field of lithium batteries according to claim 9, characterized in that: The single-ion polymer electrolyte containing benzimidazole can effectively inhibit the growth of lithium dendrites and has good flame retardancy and a room temperature ionic conductivity of 4.7×10 -3 -7.4×10 -2 S / cm, lithium ion migration number ≈1, electrochemical window ≥5.7V.