Oligomer receptor material, preparation method thereof and solar cell

By using oligomer acceptor materials with multi-arm structures in organic solar cells, the problem of poor stability in the existing technology is solved, organic solar cells with high efficiency and high stability are achieved, and their commercial application is promoted.

CN114891020BActive Publication Date: 2024-10-18THE NAT CENT FOR NANOSCI & TECH NCNST OF CHINA
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202210431759.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-04-22
Publication Date
2024-10-18
Estimated Expiration
2042-04-22

AI Technical Summary

Technical Problem

The poor stability of existing organic solar cells limits their commercial application, especially the insufficient efficiency and stability of single-junction organic solar cells based on polymer donor-non-fullerene acceptors.

Method used

An oligomer receptor material with a longer molecular skeleton is used, and a multi-arm structure is formed through a small molecule receptor and an intermediate linking group to form a stable active layer morphology and improve thermal stability and efficiency. The specific method includes reacting the dialdehyde terminal precursor with the acceptor unit to prepare an asymmetric precursor, and then performing a coupling reaction with the intermediate linking unit to prepare the oligomer acceptor material.

Benefits of technology

A high-efficiency organic solar cell device has been achieved, while the stability and purity of its photovoltaic device have been improved, meeting the requirements of industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114891020B_ABST
    Figure CN114891020B_ABST
Patent Text Reader

Abstract

The present invention provides an oligomer receptor material, a preparation method thereof and a solar cell. The compound of the present invention is based on a single small molecule receptor, and by selecting a suitable intermediate connecting group and an end group unit, the receptor monomer is connected into a two-arm, three-arm and four-arm oligomer receptor. The compound of the present invention has both a suitable energy level and good solubility, and can be used as a receptor material in an organic solar cell. Compared with a single receptor, an oligomer has a higher highest unoccupied orbital, making it possible for high-efficiency materials to obtain a high open circuit voltage; at the same time, compared with a polymer receptor based on a small molecule receptor, the oligomer material has a higher purity and no batch difference; secondly, the photovoltaic device based on the oligomer receptor exhibits excellent light stability, which is undoubtedly an important prerequisite for realizing industrial application. The invention of the oligomer receptor is of great value in the field of organic solar cells.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of organic material chemistry, and in particular relates to an oligomer receptor material, a preparation method thereof and a solar cell. Background Art

[0002] The increasingly serious problems of environmental pollution and fossil fuel depletion have turned people's attention to the development and utilization of green and pollution-free new energy. Solar energy is inexhaustible, and solar cells that directly convert solar energy into electrical energy are one of the effective uses of solar energy.

[0003] Compared with inorganic solar cells, organic solar cells have the advantages of being widely available, non-toxic, inexpensive, lightweight, and able to be prepared over a large area using a roll-to-roll process. They have long been one of the research hotspots in the industry.

[0004] In recent years, organic solar cells have developed rapidly, especially the rapid development of new non-fullerene acceptors, which has enabled the device efficiency of single-junction organic solar cells based on polymer donors and non-fullerene acceptors to exceed 19%, reaching an efficiency that can be used commercially. However, their stability is poor, far inferior to that of inorganic and organic-inorganic hybrid solar cells, which limits their commercial application.

[0005] The all-polymer solar cell has good thermal stability due to the stable interpenetrating network morphology of the active layer, but its efficiency is still lower than that of the non-fullerene small molecule acceptor solar cell. Based on this, the oligomer acceptor of the present invention has a long molecular skeleton, which can form a stable active layer morphology and maintain good thermal stability while achieving high efficiency, which is of great significance for the commercial application of organic solar cells. Summary of the invention

[0006] Therefore, the purpose of the present invention is to overcome the defects in the prior art and provide an oligomer receptor material, a preparation method thereof and a solar cell. The oligomer receptor material of the present invention has a long molecular skeleton and can form a stable active layer morphology while achieving high efficiency and maintaining good thermal stability.

[0007] Before describing the present invention, the terms used in this article are defined as follows:

[0008] The term "Y series" refers to non-fullerene organic acceptor photovoltaic materials with electron-deficient unit benzothiadiazole and its derivative quinoxaline as the core.

[0009] The term "IDT" refers to non-fullerene organic acceptor photovoltaic materials with indacendithiophene and its derivatives as the core.

[0010] The term "Pd2(dba)3" refers to: tris(dibenzylideneacetone)palladium.

[0011] The term "ITO" means: Indium Tin Oxide Anode.

[0012] The term "2PACz" refers to: [2-(9H-carbazol-9-yl)ethyl]phosphonic acid, which is used as the hole transport layer of the oligomer receptor material device of the present invention.

[0013] The term "Y6" refers to: non-fullerene acceptor: 2,2'-(2Z,2'Z)-((12,13-di(2-ethylhexyl)-3,9-heneicosyl-12,13-dihydro-[1,2,5]thiadiazolo[3,4-e]thieno[2",3':4',5']thieno[2',3':4,5]pyrrolo[3,2-g]thieno[3,2':4,5]thieno[3,2-b]indole-2,10-diyl)bis(formylmethylene)bis(5,6-difluoro-3-oxo-2,3-dihydro-1H-indene-2,1-diylidene)dicarbonitrile.

[0014] The term "PM6" refers to: polymer donor: poly[2,6-(4,8-bis(5-(2-ethylhexyl-3-fluoro)thiophene-2-yl)benzo[1,2-b:4,5-bithiophene)-alt-(5,5-(1',3'-di-2-thienyl-5',7'-bis(2-ethylhexyl)benzo[1',2'-c:4',5'-c]bithiophene-4,8-dione)].

[0015] The term "PNDIT-F3N" refers to: poly [[2,7-bis(2-ethylhexyl)-1,2,3,6,7,8-hexahydro-1,3,6,8-tetraoxobenzo[lmn][3,8]phenanthroline-4,9-diyl]-2,5-thiophenedioyl [9,9-bis[3-(dimethylamino)propyl]-9H-fluorene-2,7-diyl]-2,5-thiophenedioyl], as the electron transport layer of the oligomer receptor material device of the present invention.

[0016] The term "Pd(OAc)2" means: palladium acetate.

[0017] The term "P(o-tolyl)3" refers to: tri(o-methylphenyl)phosphine.

[0018] The term "ADA type small molecule receptor" refers to a small molecule receptor with a receptor-donor-acceptor structure.

[0019] The term "IDIC" refers to: non-fullerene acceptor compound: 2,2'-(2Z,2'Z)-((4,4,9,9-tetrahexyl-4,9-dihydroindole[1,2-b:5,6-b']dithiophene-2,7-diyl)bis(formylmethylene)bis(3-oxo-2,3-dihydro-1H-indene-2,1-diylidene))diaminonitrile.

[0020] The term "ITIC" refers to: non-fullerene acceptor compound: 3,9-bis(2-methylene-(3-(1,1-dicyanomethylene)-indanone)-5,5,11,11-tetrakis(4-hexylphenyl)-dithieno[2,3-d:2',3'-d']-s-indolone[1,2-b:5,6-b']dithiophene.

[0021] The term "BO-4Cl" refers to: non-fullerene acceptor compound: 2,2'-(2Z,2'Z)-(12,13-bis(2-butyloctyl)-3,9-heneicosyl-12,13-dihydro-[1,2,5]thiadiazolo[3,4-e]thieno[2",3':4',5']thieno[2',3':4,5]pyrrolo[3,2-g]thieno[3,2':4,5]thieno[3,2-b]indole-2,10-diacyl)bis(formylidene)bis(5,6-dichloro-3-oxo-2,3-dihydro-1H-inden-2,1-diylidene)bis(5,6-dichloro-3-oxo-2,3-dihydro-1H-inden-2,1-diylidene)dicarbonitrile.

[0022] The term "CH1007" refers to: non-fullerene acceptor compound: 2,2'-(2Z,2'Z)-(12,13-bis(2-butyloctyl)-3,9-heneicosyl-12,13-dihydroselenobenzo[2",3':4',5']thieno[2',3':4,5]pyrrolo[3,2-g]selenopheno[2',3':4,5]thieno[3,2-b][1,2,5]thiadiazolo[3,4-e]indole-2,10-diyl)bis(methanemethylene))bis(5,6-difluoro-3-oxo-2,3-dihydro-1H-inden-2,1-diylidene)diamine.

[0023] The term "L8-BO" refers to: non-fullerene acceptor compound: 2,2'-(2Z,2'Z)-((3,9-bis(2-butyloctyl)-12,13-bis(2-ethylhexyl)-12,13-dihydro-[1,2,5]thiadiazolo[3,4-e]thieno[2",3":4',5']thieno[2',3':3,2-g]thieno[2',3':4,5]thieno[3,2-b]indole-2,10-diyl)bis(5,6-difluoro-3-oxo-2,3-dihydro-1H-inden-2,1-diylidene)bis(5,6-difluoro-3-oxo-2,3-dihydro-1H-inden-2,1-diylidene)xylenetriane.

[0024] To achieve the above-mentioned object, the first aspect of the present invention provides an oligomer receptor material, which comprises a small molecule receptor and an intermediate connecting group and has a multi-arm structure; wherein:

[0025] The molecular weight of the small molecule receptor is 1000-3000, and its skeleton structure is preferably an ADA type small molecule receptor skeleton structure, more preferably a non-fullerene ADA type small molecule receptor compound, further preferably a skeleton structure of Y6 and IDT, and further preferably a skeleton structure of IDIC, ITIC, Y6, BO-4Cl, CH1007, and L8-BO; and / or

[0026] The intermediate connecting group is selected from one or more of the following: thiophene, selenophene, furan, thiophene, thiophene, benzodithiophene, benzene ring group, pyrrole, dithiophene imide, vinyl, fluorene, trimerized indene, s-triazine, triphenylamine, porphyrin, trithiophene triazine, trithiophene acene, tetraphenylethylene, spirofluorene, and pyrene.

[0027] According to the oligomer receptor material of the first aspect of the present invention, the structural formula of the small molecule receptor is selected from one or more of the following:

[0028]

[0029] Preferably

[0030] More preferably

[0031]

[0032] in,

[0033] X is selected from one or more of the following: F, Cl, H; and / or

[0034] R is a straight chain alkyl or a branched chain alkyl;

[0035] Preferably, R is a linear or branched alkyl group having 1 to 30 carbon atoms.

[0036] According to the oligomer receptor material of the first aspect of the present invention, the structural formula of the intermediate connecting group is selected from one or more of the following:

[0037]

[0038] Preferably

[0039]

[0040] More preferably

[0041]

[0042] in,

[0043] X1 is selected from one or more of the following: F, Cl, H;

[0044] X2 is selected from one or more of the following: C, O, S;

[0045] X3 is selected from one or more of the following: O, S, Se;

[0046] R is a straight chain alkyl or a branched chain alkyl;

[0047] n is a natural number; and / or

[0048] The dotted line indicates the connection location;

[0049] Preferably, R is a straight-chain alkyl group or a branched-chain alkyl group having 1 to 30 carbon atoms; and / or n is a natural number within 10.

[0050] The oligomeric receptor material according to the first aspect of the present invention, wherein:

[0051] The multi-arm structure is selected from one or more of the following: a two-arm structure, a three-arm structure, and a four-arm structure; preferably, the two-arm structure is:

[0052]

[0053] Preferably, the three-arm structure is:

[0054]

[0055] Preferably, the four-arm structure is:

[0056] in,

[0057] X is selected from one or more of the following: F, Cl, H; and / or

[0058] Y is selected from one or more of the following: H, F, Cl.

[0059] The second aspect of the present invention provides a method for preparing the oligomeric receptor material described in the first aspect, the method comprising the following steps:

[0060] (1) reacting a dialdehyde terminal group precursor with an acceptor unit to prepare an asymmetric precursor compound;

[0061] (2) reacting the asymmetric precursor compound prepared in step (1) with an intermediate connecting unit to prepare the oligomer receptor material;

[0062] Preferably, in the steps (1) and (2), after the reaction is completed, the steps further include: cooling to room temperature, extracting and purifying;

[0063] More preferably, the eluent used in the purification is a mixed solution of dichloromethane and petroleum ether.

[0064] According to the method of the second aspect of the present invention, the step (1) further comprises: adding the dialdehyde terminal group precursor, two acceptor units and a catalyst to an organic solvent under the protection of an inert gas to carry out a condensation reaction to obtain an asymmetric precursor compound; wherein,

[0065] The inert gas is nitrogen or argon;

[0066] The catalyst is selected from one or more of the following: pyridine, triethylamine, 1,8-diazabicyclo[5.4.0]undec-7-ene, most preferably pyridine; and / or

[0067] The organic solvent is chloroform;

[0068] Preferably, the molar ratio of the dialdehyde terminal group precursor to the two acceptor units is 0.1-5:0.6-6:0.6-6, more preferably 0.5-3:0.6-4:0.6-4, further preferably 0.8-1.5:0.9-1.8:0.9-1.8, and most preferably 1:1.2:1.2;

[0069] Preferably, the molar amount of the catalyst is 10 to 60 times that of the dialdehyde terminal group precursor, more preferably 20 to 50 times, and further preferably 20 to 40 times;

[0070] Preferably, the condensation reaction temperature is 25 to 70° C., more preferably 40 to 70° C., and further preferably 60 to 70° C.; and / or

[0071] Preferably, the condensation reaction time is 12 to 48 hours, more preferably 12 to 24 hours.

[0072] According to the method of the second aspect of the present invention, in said step (1):

[0073] The dialdehyde terminal group precursor is selected from one or more of the following:

[0074]

[0075] Preferably More preferably wherein R is a straight chain alkyl or a branched chain alkyl, preferably a straight chain alkyl or a branched chain alkyl having 1 to 30 carbon atoms; and / or

[0076] The receptor unit is selected from one or more of the following:

[0077] Preferably More preferably Wherein, X is selected from one or more of the following: F, Cl, H; and / or Y is selected from one or more of the following: H, F, Cl.

[0078] According to the method of the second aspect of the present invention, the step (2) further comprises: adding the asymmetric precursor compound, the intermediate connecting unit, the catalyst and the catalyst ligand prepared in the step (1) into a solvent to undergo a coupling reaction to prepare the oligomer receptor material; wherein,

[0079] The intermediate connecting unit is an intermediate connecting group substituted by trimethyl(butyl)tin or borate;

[0080] The catalyst is selected from one or more of the following: diphenylphosphinocene palladium dichloride, tetrakistriphenylphosphine palladium, dichlorobistriphenylphosphine palladium, tris(dibenzylideneacetone)palladium, palladium acetate, preferably tris(dibenzylideneacetone)palladium or palladium acetate; and / or

[0081] The catalyst ligand is selected from one or more of the following: triphenylphosphine, tri(o-methylphenyl)phosphine, 2-(di-tert-butylphosphine)biphenyl, 2-di-tert-butylphosphine-2-(N,N-dimethylamino)biphenyl, 2-(dicyclohexylphosphine)biphenyl, preferably tri(o-methylphenyl)phosphine or 2-(dicyclohexylphosphine)biphenyl;

[0082] The solvent is selected from one or more of the following: toluene, chlorobenzene, o-dichlorobenzene, most preferably toluene;

[0083] Preferably, the molar ratio of the asymmetric precursor compound to the intermediate connecting unit is 1:1.5-8, more preferably 1:2-7, and further preferably 1:2.5-6;

[0084] Preferably, the molar amount of the catalyst is 1% to 20% of the intermediate connecting unit, more preferably 5% to 15%, and further preferably 5% to 10%;

[0085] Preferably, the molar amount of the catalyst ligand is 4 to 20 times that of the catalyst, preferably 5 to 15 times, and more preferably 5 to 10 times;

[0086] Preferably, the coupling reaction temperature is 95 to 125° C., more preferably 100 to 120° C., and further preferably 105 to 115° C.; and / or

[0087] Preferably, the coupling reaction time is 12 to 72 hours, more preferably 24 to 48 hours.

[0088] According to the method of the second aspect of the present invention, in the step (2), the intermediate connecting unit is selected from one or more of the following:

[0089]

[0090]

[0091] Preferably

[0092]

[0093]

[0094] More preferably

[0095]

[0096]

[0097] in,

[0098] X1 is selected from one or more of the following: F, Cl, H;

[0099] X2 is selected from one or more of the following: C, O, S;

[0100] X3 is selected from one or more of the following: S, O, Se;

[0101] R is a straight chain alkyl or a branched chain alkyl, preferably a straight chain alkyl or a branched chain alkyl of 1 to 30 carbon atoms;

[0102] M is a coordination metal, preferably selected from one or more of the following: magnesium, zinc, cobalt; and / or

[0103] E is trimethyl(butyl)tin or a borate coupling group.

[0104] The third aspect of the present invention provides an organic solar cell, which comprises the oligomer acceptor material described in the first aspect or the oligomer acceptor material prepared according to the method described in the second aspect.

[0105] According to a specific embodiment of the present invention, the organic photoelectric conversion material of the present invention is based on a small molecule receptor and an intermediate connecting group as a basic unit to form a multi-arm structure, and its structural formula is as follows:

[0106] Two-arm structure

[0107]

[0108] Three-arm structure

[0109]

[0110] Four-arm structure

[0111]

[0112] Wherein, X represents any one or more of H, F, and Cl; Y represents any one of H and F; the patent structure and the following description are all based on the Y6 series of small molecule receptors as an example, but the repeating unit small molecule receptors are not limited to the Y6 series receptors. Modifications made to IDT and other single small molecule receptor monomers should all belong to the spirit and principles of this patent invention and should be within the scope of protection of this patent invention.

[0113] The intermediate connecting group is any one of the following structures but is not limited to the structures shown:

[0114]

[0115]

[0116]

[0117] Among them, X1 represents F, Cl, H; X2 represents C, O, S; X3 represents O, S, Se; R represents a straight chain alkyl or a branched chain alkyl, preferably a straight chain alkyl or a branched chain alkyl with 1-30 carbon atoms; n represents a natural number within 10; and the dotted line represents the connection position.

[0118] The method for preparing an organic solar cell oligomer receptor material comprises: subjecting a dialdehyde compound to a Novegrin condensation reaction with two receptor units to prepare an asymmetric precursor compound; and then subjecting the asymmetric compound to a coupling reaction with a connecting group to prepare the oligomer receptor compound.

[0119] Preferably, the preparation method comprises the following steps:

[0120] (1) Under the protection of an inert gas, a dialdehyde terminal group precursor, two acceptor units, and a catalyst are added to an organic solvent and heated to react to obtain an asymmetric precursor compound;

[0121] (2) Adding the above-mentioned asymmetric precursor, trimethyl(butyl)tin or borate-substituted intermediate linking group, catalyst and catalyst ligand into a solvent for reaction to obtain the target compound.

[0122] The inert gas in step (1) is nitrogen or argon; preferably, the dialdehyde terminal group precursor structure is any one of the following structures but is not limited to the structure shown:

[0123]

[0124]

[0125] Wherein, R represents a straight chain alkyl group or a branched chain alkyl group, preferably a straight chain or branched chain alkyl group with 1 to 30 carbon atoms.

[0126] In step (1), the structure of the intermediate linking group substituted with trimethyl(butyl)tin or borate is any one of the following:

[0127]

[0128]

[0129] Wherein, X1 represents F, Cl, H;

[0130] X2 represents C, O, S;

[0131] X3 represents S, O, Se;

[0132] R represents a straight chain alkyl or a branched chain alkyl, preferably a straight chain alkyl or a branched chain alkyl with 1 to 30 carbon atoms; M represents a coordination metal, preferably selected from one or more of the following: magnesium Mg, zinc Zn, cobalt Co; E represents trimethyl(butyl)tin or a borate coupling group.

[0133] Preferably, the catalyst is pyridine, and the solvent is chloroform;

[0134] Preferably, the molar ratio of the dialdehyde terminal group precursor to the two acceptor units is 1:1.2:1.2;

[0135] Preferably, the molar amount of the catalyst is 20-40 times that of the dialdehyde terminal group precursor;

[0136] Preferably, the amount of chloroform solvent used in step (1) is 10-100 mL / mmo1 relative to the dialdehyde terminal group precursor.

[0137] Preferably, the temperature of the heating reaction is 25-70°C, and the reaction time is 12-48h, preferably 12-24h;

[0138] Preferably, after the reaction in step (1) is completed, the crude product is purified by column purification;

[0139] Preferably, the column purification uses a mixed solvent of dichloromethane and petroleum ether as an eluent.

[0140] The molar ratio of the asymmetric precursor to the linking group in step (2) is 1:2.5-6;

[0141] The catalyst is selected from one or more of the following: diphenylphosphinocene palladium dichloride, tetrakistriphenylphosphine palladium, dichlorobistriphenylphosphine palladium, Pd2(dba)3, palladium acetate Pd(OAc)2, preferably Pd2(dba)3, Pd(OAc)2

[0142] The catalyst ligand is selected from one or more of the following: triphenylphosphine, tri(o-methylphenyl)phosphine, 2-(di-tert-butylphosphine)biphenyl, 2-di-tert-butylphosphine-2-(N,N-dimethylamino)biphenyl, 2-(dicyclohexylphosphine)biphenyl, preferably tri(o-methylphenyl)phosphine or 2-(dicyclohexylphosphine)biphenyl;

[0143] The solvent is selected from one or more of the following: toluene, chlorobenzene, o-dichlorobenzene, preferably toluene; preferably, the molar amount of the catalyst is 5%-10% of the linking group;

[0144] Preferably, the molar amount of the catalyst ligand is 4 to 20 times that of the catalyst, preferably 5 to 10 times;

[0145] Preferably, the amount of toluene solvent used in step (2) is 10-100 mL / mmo1 relative to the linking group.

[0146] Preferably, the temperature of the heating reaction is 110°C, and the reaction time is 12-72h, preferably 24-48h;

[0147] Preferably, after the reaction in step (2) is completed, the reaction solution is concentrated to obtain a crude product and then purified by column;

[0148] Preferably, the column purification uses a mixed solvent of chloroform and petroleum ether as an eluent.

[0149] According to another specific embodiment of the present invention, the preparation method of the above oligomer receptor has the following reaction formula

[0150]

[0151] Preferably, the above preparation method comprises the following steps:

[0152] (1) Under the protection of an inert gas, a dialdehyde terminal group precursor, two acceptor units, and a catalyst are added to an organic solvent and heated to react to obtain an asymmetric precursor compound;

[0153] (2) Adding the above-mentioned asymmetric precursor, intermediate connecting unit and catalyst into a solvent for reaction to obtain the target compound.

[0154] The oligomeric receptor material of the present invention may have, but is not limited to, the following beneficial effects:

[0155] 1. The compounds of the present invention are based on a single small molecule receptor, and the receptor monomers are connected into two-arm, three-arm and four-arm oligomer receptors by selecting appropriate intermediate linking groups and terminal units. The compounds of the present invention have both suitable energy levels and good solubility, and can be used as receptor materials in organic solar cells.

[0156] 2. Compared with single receptors, oligomers have a higher highest unoccupied orbital, making it possible for high-efficiency materials to obtain high open-circuit voltages; at the same time, compared with polymer receptors based on small molecule receptors, oligomer materials have higher purity and no batch differences; secondly, photovoltaic devices based on oligomer receptors show excellent light stability, which is undoubtedly an important prerequisite for industrial application. The invention of oligomer receptors is of great value in the field of organic solar cells. BRIEF DESCRIPTION OF THE DRAWINGS

[0157] The embodiments of the present invention are described in detail below with reference to the accompanying drawings, wherein:

[0158] Figure 1 The mass spectrum of the two-arm receptor 1 in Example 1 of the present invention is shown.

[0159] Figure 2 The nuclear magnetic resonance spectrum of the two-arm receptor 1 in Example 1 of the present invention is shown.

[0160] Figure 3 The UV-visible absorption spectrum of the two-arm receptor 1 in Example 1 of the present invention is shown.

[0161] Figure 4 A schematic diagram of the structure of an organic solar cell device prepared in Example 6 of the present invention is shown.

[0162] Figure 5 The UV-visible absorption spectrum of the three-arm acceptor in Example 4 of the present invention is shown.

[0163] Figure 6 The cyclic voltammetry curve of the three-arm acceptor in Example 4 of the present invention is shown.

[0164] Figure 7 The light stability curves of three receptor materials in Comparative Example 1 of the present invention are shown.

[0165] Figure 8The nuclear magnetic resonance spectrum of the two-arm receptor 2 in Example 2 of the present invention is shown. DETAILED DESCRIPTION

[0166] The present invention is further described below by means of specific examples. However, it should be understood that these examples are only used for more detailed and specific description and should not be understood as limiting the present invention in any form.

[0167] This section generally describes the materials and test methods used in the experiments of the present invention. Although many materials and operating methods used to achieve the purpose of the present invention are well known in the art, the present invention is still described as detailed as possible. It is clear to those skilled in the art that in the context, if not specifically stated, the materials and operating methods used in the present invention are well known in the art.

[0168] The reagents and instruments used in the following examples are as follows:

[0169] Reagents:

[0170] Dichloromethane, petroleum ether, chloroform, and toluene were purchased from Sinopharm Chemical Reagent Co., Ltd.;

[0171] Catalyst Pd2(dba)3 and ligand P(o-tolyl)3 were purchased from Shanghai Bid Pharmaceutical Technology Co., Ltd.;

[0172] Catalyst pyridine was purchased from Beijing Bailingwei Technology Co., Ltd.;

[0173] The dialdehyde precursor M1, terminal groups M2, M3, and trimethyltin chloride-substituted thiophene M4 were all purchased from Jiaxing Hepu Optoelectronics Technology Co., Ltd.;

[0174] Trimethyltin chloride-substituted trithienoacene M5 was purchased from Suzhou Nakai Technology Co., Ltd.

[0175] instrument:

[0176] Solar simulator, model SS-F5-3A, purchased from Enlighten Technology Co., Ltd.

[0177] Spectrometer, model Shimadzu UV-3600, purchased from Shanghai Na-Ning Industrial Co., Ltd.;

[0178] The electrochemical workstation, model CHI660E, was purchased from Shanghai Chenhua Instrument Co., Ltd.

[0179] The organic solar cell two-arm acceptor material and device provided by the present invention will be further described below in conjunction with the accompanying drawings.

[0180] The small molecule receptors described in the drawings of this application and the scheme descriptions of the following specific embodiments are all based on Y series compounds as an example, but technicians in the relevant field should understand that the repeating unit small molecule receptors are not limited to Y series receptors, and modifications made to IDT and other single small molecule receptor monomers should all belong to the spirit and principles of this patent invention and should be within the scope of protection of this patent invention.

[0181] Example 1

[0182] This example is used to illustrate the preparation method of the optoelectronic material of the oligomer two-arm receptor 1 of the present invention.

[0183] The structural formula of the two-arm receptor 1 is shown in Formula I:

[0184]

[0185] The synthesis route of the method for preparing the optoelectronic material of the oligomer two-arm receptor 1 is as follows:

[0186]

[0187] Specific synthesis steps:

[0188] In the first step, the reactant dialdehyde compound M1 (500 mg), end group M2 (110.3 mg), end group M3 (130.9 mg) and catalyst pyridine (0.9 ml) were added to a 100 ml three-necked flask containing 40 mL of chloroform, nitrogen was pumped three times, the reaction temperature was heated to 65 ° C, and stirred overnight. After cooling to room temperature, it was extracted with dichloromethane three times. The crude product was further purified by silica gel column chromatography (developing solvent is dichloromethane: petroleum ether, volume ratio is 1:3) to obtain the precursor asymmetric compound (220 mg, 32%).

[0189] In the second step, under nitrogen protection, the precursor asymmetric compound (56 mg) and the intermediate connecting unit M4 (4.7 mg) were dissolved in dry toluene, and the catalyst Pd2(dba)3 (0.63 mg) and the ligand P(o-tolyl)3 (2.1 mg) were added and the nitrogen was replaced 3 times. The mixture was heated to 110°C and reacted for 48 hours. The reaction solution was cooled and extracted with chloroform. The crude product was developed with chloroform: petroleum ether (volume ratio of 3:1) and silica gel column chromatography was performed to obtain the photoelectric material of the oligomer two-arm receptor 1 (34 mg, 78.2%).

[0190] Figure 1 The mass spectrum of the two-arm receptor 1 in Example 1 of the present invention is shown. Figure 2 The nuclear magnetic resonance spectrum of the two-arm receptor 1 in Example 1 of the present invention is shown. Figure 3 The UV-visible absorption spectrum of the two-arm receptor 1 in Example 1 of the present invention is shown.

[0191] Example 2

[0192] This example is used to illustrate the preparation method of the optoelectronic material of the oligomeric two-arm receptor 2 of the present invention.

[0193] The structural formula of the two-arm receptor 2 is shown in Formula II:

[0194]

[0195] The synthesis route of the method for preparing the optoelectronic material of the oligomer two-arm receptor 2 is as follows:

[0196]

[0197] Specific synthesis steps:

[0198] The synthesis steps of the first asymmetric precursor are the same as those of the two-arm receptor 1 asymmetric precursor in Example 1;

[0199] In the second step, under nitrogen protection, the precursor asymmetric compound (58.8 mg), the intermediate linking group trimethyltin substituted thiophene alkoxy (6 mg) were dissolved in dry toluene, and the catalyst Pd2(dba)3 (0.63 mg) and the ligand P(o-tolyl)3 (2.08 mg) were added and the nitrogen was replaced 3 times. The mixture was heated to 110°C and reacted for 48 hours. The reaction solution was cooled and extracted with chloroform. The crude product was subjected to silica gel column chromatography using chloroform: petroleum ether (volume ratio of 2:1 to 3:1) as the developing solvent to obtain the photoelectric material of the oligomer two-arm receptor 1 (26.2 mg, 66%).

[0200] Figure 8 The nuclear magnetic resonance spectrum of the two-arm receptor 2 in Example 2 of the present invention is shown.

[0201] Example 3

[0202] This example is used to illustrate the preparation method of the optoelectronic material of the oligomer two-arm receptor 3 of the present invention.

[0203] The structural formula of the two-arm receptor 3 is shown in Formula III:

[0204]

[0205] The synthesis route of the method for preparing the optoelectronic material of the oligomer two-arm receptor 3 is as follows:

[0206]

[0207] Specific synthesis steps:

[0208] In the first step, the reactant dialdehyde compound (700 mg), end group 1 (176.5 mg), end group 2 (195.3 mg) and catalyst pyridine (1.2 ml) were added to a 100 ml three-necked flask containing 50 mL of chloroform, nitrogen was pumped three times, the reaction temperature was heated to 65 ° C, and stirred overnight. After cooling to room temperature, it was extracted with dichloromethane three times. The crude product was further purified by silica gel column chromatography (developing solvent is dichloromethane: petroleum ether, volume ratio is 1:2) to obtain the precursor asymmetric compound (433 mg, 43.75%).

[0209] In the second step, under nitrogen protection, the precursor asymmetric compound (152 mg), the intermediate connecting unit trimethyltin substituted thiophene (11.8 mg) were dissolved in dry toluene, and the catalyst Pd2(dba)3 (1.6 mg) and the ligand P(o-tolyl)3 (5.2 mg) were added and replaced with nitrogen three times, and the mixture was heated to 110°C and reacted for 48 hours. The reaction solution was cooled and extracted with chloroform. The crude product was developed with chloroform: petroleum ether (volume ratio of 3:1) and silica gel column chromatography to obtain the photoelectric material of the oligomer two-arm receptor 3 (68.2 mg, 69.6%).

[0210] Example 4

[0211] This example is used to illustrate the preparation method of the optoelectronic material of the oligomer three-arm receptor of the present invention.

[0212] The structural formula of the three-arm receptor is shown in Formula IV:

[0213]

[0214] The synthetic route of the method for preparing the optoelectronic material of the above oligomer three-arm receptor is as follows:

[0215]

[0216] Specific synthesis steps:

[0217] The synthesis steps of the first asymmetric precursor are the same as those of the two-arm receptor 1 asymmetric precursor in Example 1;

[0218] In the second step, under nitrogen protection, the precursor asymmetric compound (60 mg) and the intermediate connecting unit M5 (6.4 mg) were dissolved in dry toluene, and the catalyst Pd2(dba)3 (0.8 mg) and the ligand P(o-tolyl)3 (2.6 mg) were added, and the nitrogen was replaced 3 times. The mixture was heated to 110°C and reacted for 48 hours. The reaction solution was cooled and extracted with chloroform. The crude product was subjected to silica gel column chromatography using chloroform: petroleum ether: methanol (volume ratio of 3:1:0.01) as the developing solvent to obtain the photoelectric material of the oligomer three-arm receptor (26 mg, 57.8%).

[0219] Figure 5 The UV-visible absorption spectrum of the three-arm acceptor in Example 4 of the present invention is shown. Figure 6 The cyclic voltammetry curve of the three-arm acceptor in Example 4 of the present invention is shown.

[0220] Example 5

[0221] This example is used to illustrate the preparation method of the optoelectronic material of the oligomeric four-arm receptor of the present invention.

[0222] The structural formula of the four-arm receptor is shown in Formula V:

[0223]

[0224] The synthetic route of the method for preparing the optoelectronic material of the oligomer four-arm receptor is as follows:

[0225]

[0226] Specific synthesis steps:

[0227] The first step of synthesizing the asymmetric precursor is the same as the asymmetric precursor of the two-arm receptor 1 in Example 1;

[0228] In the second step, under nitrogen protection, the precursor asymmetric compound (50 mg) and the intermediate linking group boronic acid ester substituted pyrene (6 mg) were dissolved in toluene, and 2M potassium carbonate aqueous solution was added at the same time. After replacing nitrogen three times, the catalyst Pd2(dba)3 (0.4 mg) and the ligand P(o-tolyl)3 (1.8 mg) were added. After blowing nitrogen into the reaction system for 20 minutes, the mixture was heated to 110°C and reacted for 48 hours. The reaction solution was cooled and extracted with chloroform. The crude product was subjected to silica gel column chromatography using chloroform: petroleum ether (volume ratio of 4:1) as the developing solvent to obtain the photoelectric material of the oligomer four-arm receptor (18.5 mg, 46.6%).

[0229] Example 6

[0230] This example is used to illustrate the preparation method and performance test of an organic solar cell device prepared using the oligomer acceptor material of the present invention.

[0231] The materials obtained in Examples 1 and 3 were used as electron acceptor materials to prepare forward organic solar cell devices. The specific preparation process is as follows:

[0232] The transparent conductive glass with ITO was ultrasonically cleaned with deionized water, ethanol, and isopropanol for 30 minutes respectively, and finally stored in an isopropanol solution.

[0233] The ITO glass was blown dry with a nitrogen gun and placed in a UV ozone box to treat the substrate surface for 10 minutes to increase the hydrophilicity of the substrate surface and improve the work function of the ITO electrode.

[0234] 2PACz was spin-coated on ITO and dried at 150 °C for 15 min as a hole transport layer.

[0235] A solution of active layer material (PM6: dimer 1 = 1: 1.2, solution concentration = 14 mg / ml) was spin-coated in a glove box, followed by annealing on a 100° C. hot stage for 10 min.

[0236] F3N solution was spin-coated as the cathode interfacial layer in a glove box.

[0237] In the vacuum evaporation chamber, a 160 nanometer Ag layer was evaporated as the cathode.

[0238] Figure 4 A schematic diagram of the structure of an organic solar cell device prepared in Example 6 of the present invention is shown.

[0239] A 500W xenon lamp and an AM1.5 filter were used as a white light source to simulate sunlight, and the light intensity at the device measurement point was adjusted to 100mW / cm 2 The prepared device was tested for current-voltage curve using Keithley, and the relevant performance parameters were shown in Table 1. This shows that the organic solar cell device prepared with the oligomer acceptor material of the present invention can maintain a high short-circuit current and fill factor while obtaining a high open-circuit voltage. The device efficiency exceeds 18%, which is one of the highest efficiencies of binary organic solar cells currently.

[0240] Table 1 Performance parameters of organic solar cell devices

[0241]

[0242]

[0243] Comparative Example 1

[0244] This comparative example is used to compare the device performance and stability differences between the oligomer two-arm receptor material of the present invention and the monomer receptor and the polymer receptor based on the small molecule receptor.

[0245] In this comparative example, the precursor of the multi-arm receptor, the monomer receptor, and the published polymer receptor PYF-T based on the small molecule receptor were selected as the comparative materials of the two-arm receptor 1; the polymer donor PM6 and the above three receptors were respectively optimized according to the organic solar cell device preparation method in Example 6. The structures of the three receptor materials are shown below:

[0246] 1. Monomeric receptors:

[0247]

[0248] 2. Two-arm receptor 1:

[0249]

[0250] 3. Polymer receptor PYF-T:

[0251]

[0252] Among them, the device based on the two-arm receptor 1 achieved much better device efficiency than those based on small molecule receptors and polymer receptors; secondly, in the stability study, the three devices were compared under light conditions (100mW cm -2 ) under T80 lifetime, the device based on PM6:two-arm acceptor 1 shows higher stability. Figure 7 The light stability curves of three acceptor materials in comparative example 1 of the present invention are shown. The above shows that the two-arm acceptor based on small molecule acceptors can not only improve the device efficiency, but also achieve good light stability, which is of great value for realizing the industrial application of organic solar cells.

[0253] Table 2 Device parameters of organic solar cells based on donor PM6 and three acceptors

[0254]

[0255] Although the present invention has been described to a certain extent, it is obvious that appropriate changes in various conditions can be made without departing from the spirit and scope of the present invention. It is understood that the present invention is not limited to the embodiments described, but belongs to the scope of the claims, which includes equivalent replacements of each factor described.

Claims

1. An oligomer receptor material, characterized in that The oligomer receptor material is a two-arm structure; wherein, The two-arm structure is: Wherein, X is selected from one or more of the following: F, Cl, H, and Y is selected from one or more of the following: H, F, Cl; And wherein the structural formula of the linking group is selected from one or more of the following: Wherein, X1 is selected from one or more of the following: F, Cl, H; X2 is selected from one or more of the following: O, S; X3 is selected from one or more of the following: O, S, Se; the dotted line is the connection position; and R is a straight-chain or branched alkyl group of 1 to 30 carbon atoms.

2. An oligomer receptor material, characterized in that The oligomer receptor material is a three-arm structure; wherein, The three-arm structure is: Wherein, X is selected from one or more of the following: F, Cl, H, and Y is selected from one or more of the following: H, F, Cl; And wherein the structural formula of the linking group is selected from one or more of the following: Wherein, X3 is selected from one or more of the following: O, S, Se; the dotted line is the connection position; and R is a straight-chain or branched-chain alkyl group with 1 to 30 carbon atoms.

3. A method for preparing the oligomeric receptor material according to claim 1 or 2, characterized in that: The method comprises the following steps: (1) reacting a dialdehyde terminal group precursor with two acceptor units to prepare an asymmetric precursor compound, wherein the dialdehyde terminal group precursor is: The receptor unit is Wherein X is selected from one or more of the following: F, Cl, H; Y is selected from one or more of the following: H, F, Cl; (2) reacting the asymmetric precursor compound prepared in step (1) with an intermediate connecting unit to prepare the oligomer receptor material; Wherein, the intermediate connection unit is selected from one or more of the following: in, X1 is selected from one or more of the following: F, Cl, H; X2 is selected from one or more of the following: O, S; X3 is selected from one or more of the following: S, O, Se; E is trimethyl(butyl)tin or borate coupling group; R is a straight chain alkyl or branched chain alkyl of 1 to 30 carbon atoms.

4. The method according to claim 3, characterized in that In the steps (1) and (2), after the reaction is completed, the method further comprises: cooling to room temperature, extracting and purifying.

5. The method according to claim 4, characterized in that The eluent used in the purification is a mixed solution of dichloromethane and petroleum ether.

6. The method according to claim 3, characterized in that The step (1) further comprises: under the protection of an inert gas, adding the dialdehyde terminal group precursor, two acceptor units and a catalyst into an organic solvent to carry out a condensation reaction to obtain an asymmetric precursor compound; wherein, The inert gas is nitrogen or argon; The catalyst is selected from one or more of the following: pyridine, triethylamine, 1,8-diazabicyclo[5.4.0]undec-7-ene; and / or The organic solvent is chloroform.

7. The method according to claim 6, characterized in that In the step (1), the catalyst is pyridine.

8. The method according to claim 6, characterized in that The molar ratio of the dialdehyde terminal group precursor to the two acceptor units is 0.1-5:0.6-6:0.6-6; The molar amount of the catalyst is 10 to 60 times that of the dialdehyde terminal group precursor; The condensation reaction temperature is 25-70°C; and / or The condensation reaction time is 12 to 48 hours.

9. The method according to claim 8, characterized in that The molar ratio of the dialdehyde terminal group precursor to the two acceptor units is 0.5-3:0.6-4:0.6-4; The molar amount of the catalyst is 20 to 50 times that of the dialdehyde terminal group precursor; The condensation reaction temperature is 40-70°C; and / or The condensation reaction time is 12 to 24 hours.

10. The method according to claim 9, characterized in that The molar ratio of the dialdehyde terminal group precursor to the two acceptor units is 0.8-1.5:0.9-1.8:0.9-1.8; The molar amount of the catalyst is 20 to 40 times that of the dialdehyde terminal group precursor; and / or The temperature of the condensation reaction is 60-70°C.

11. The method according to claim 10, characterized in that The molar ratio of the dialdehyde terminal group precursor to the two acceptor units is 1:1.2:1.

2.

12. The method according to claim 3, characterized in that The step (2) further comprises: adding the asymmetric precursor compound, the intermediate connecting unit, the catalyst and the catalyst ligand prepared in the step (1) into a solvent to cause a coupling reaction to prepare the oligomer receptor material; wherein, The catalyst is selected from one or more of the following: diphenylphosphinocene palladium dichloride, tetrakis(triphenylphosphine palladium), bis(triphenylphosphine)palladium dichloride, tris(dibenzylideneacetone)palladium, palladium acetate; The catalyst ligand is selected from one or more of the following: triphenylphosphine, tri(o-methylphenyl)phosphine, 2-(di-tert-butylphosphine)biphenyl, 2-di-tert-butylphosphine-2-(N,N-dimethylamino)biphenyl, 2-(dicyclohexylphosphine)biphenyl; and / or The solvent is selected from one or more of the following: toluene, chlorobenzene, and o-dichlorobenzene.

13. The method according to claim 12, characterized in that In the step (2), The catalyst is tris(dibenzylideneacetone)palladium or palladium acetate; The catalyst ligand is tri(o-methylphenyl)phosphine or 2-(dicyclohexylphosphine)biphenyl; and / or The solvent is toluene.

14. The method according to claim 12, characterized in that In the step (2): The molar ratio of the asymmetric precursor compound to the intermediate connecting unit is 1:1.5-8; The molar amount of the catalyst is 1% to 20% of the intermediate connecting unit; The molar amount of the catalyst ligand is 4 to 20 times that of the catalyst; The coupling reaction temperature is 95-125°C; and / or The coupling reaction time is 12 to 72 hours.

15. The method according to claim 14, characterized in that In the step (2): The molar ratio of the asymmetric precursor compound to the intermediate connecting unit is 1:2-7; The molar amount of the catalyst is 5% to 15% of the intermediate connecting unit; The molar amount of the catalyst ligand is 5 to 15 times that of the catalyst; The coupling reaction temperature is 100-120°C; and / or The coupling reaction time is 24 to 48 hours.

16. The method according to claim 15, characterized in that In the step (2): The molar ratio of the asymmetric precursor compound to the intermediate connecting unit is 1:2.5-6; The molar amount of the catalyst is 5% to 10% of the intermediate connecting unit; The molar amount of the catalyst ligand is 5 to 10 times that of the catalyst; and / or The temperature of the coupling reaction is 105-115°C.

17. An organic solar cell, characterized in that: The organic solar cell comprises the oligomer acceptor material according to claim 1 or 2.

Citation Information

Patent Citations

  • Preparation method and application of photovoltaic compound modified by thiophthene (benzoselenophene selenonaphthene)

    CN107759621A

  • Fluorinated fused ring benzothiadiazole polymer acceptor material and preparation method thereof

    CN113174032A

  • Polymer containing dithienyl[3, 2-f: 2', 3'-h]quinoxaline, and preparation method and application thereof

    CN113831511A

  • Organic small molecule photovoltaic material based on benzopyrazine donor core and preparation method and application thereof

    CN114181229A

  • Pi-bridge fluorine-substituted selenized polymer acceptor material and preparation and application thereof

    CN114262426A