Sulfonium salt, photoacid generator, curable composition and resist composition
Through the combination of new sulfonium salts and cationic polymerizable compounds, the problem of poor reactivity of large light absorption in photoresist compositions is solved, high photosensitivity and stability are achieved, the problem of using sensitizers is avoided, and the improvement Improve the efficiency and stability of photocuring.
Patent Information
- Application Number
- CN202180007534.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-01-04
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2041-01-04
AI Technical Summary
When the existing photoacid generator has large light absorption, the reactivity of the photoresist composition is poor, and a sensitizer needs to be used to improve the photosensitivity. However, the compatibility between the sensitizer and the resin is low, resulting in the use of Restricted.
A new type of sulfonium salt was developed, which has high photosensitivity without significantly increasing light absorption, and is used in conjunction with cationic polymerizable compounds such as epoxy compounds to form a stable curable composition that can be used without the need for a sensitizer. achieve good photocuring.
It achieves high light sensitivity and good reactivity, avoids coloration and deterioration problems caused by sensitizer residue, and has excellent storage stability and cost-effectiveness.
Smart Images

Figure CN114901638B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates first to a sulfonium salt, second to a photoacid generator, and more specifically to a photoacid generator containing a specific sulfonium salt suitable for curing a cationic polymerizable compound by the action of active energy rays such as light, electron beams or X-rays. The present invention relates third to a curable composition containing the photoacid generator and a cured product obtained by curing the curable composition. The present invention relates fourth to a chemically amplified positive photoresist composition containing the photoacid generator and a method for preparing a resist pattern using the chemically amplified positive photoresist composition. The present invention relates fifth to a chemically amplified negative photoresist composition containing the photoacid generator and a cured product obtained by curing the chemically amplified negative photoresist composition. Background Art
[0002] Photoacid generator is a general term for compounds that generate acids by decomposing them when irradiated with active energy rays such as light, electron beams or X-rays. The acids generated by irradiation with active energy rays are used as active species in various reactions such as polymerization, crosslinking and deprotection reactions.
[0003] Specifically, examples include polymerization of cationic polymerizable compounds in fields such as coatings, adhesives, and stereolithography, production of electronic components, and photolithography in semiconductor element formation (crosslinking reaction in the presence of a phenolic resin and a crosslinking agent, and acid-catalyzed deprotection reaction of a polymer formed by introducing a protecting group into an alkali-soluble resin).
[0004] In recent years, the manufacture of electronic components and the formation of semiconductor elements have been actively carried out using photolithography technology using photoresists, and i-rays (light with a wavelength of 365nm) are widely used as active energy rays in the manufacture of various precision components such as semiconductor packaging, especially in the manufacture of various precision components such as semiconductor packaging, because medium-pressure and high-pressure mercury lamps that are inexpensive and have good luminous intensity can be used as irradiation light sources.
[0005] In addition, in the fields of coating, bonding, stereolithography, etc. other than photolithography, medium-pressure and high-pressure mercury lamps are most often used, and recently LED lamps are used due to their advantages such as energy saving and long life. In addition to the existing LED lamps with a light emission wavelength in the i-ray region (360nm to 390nm), LED lamps with a longer wavelength such as the h-ray region (400nm to 420nm) with higher light transmittance and the visible light region are used, and the photosensitivity wavelengths required for the photoacid generator are various.
[0006] Among the existing photoacid generators, triarylsulfonium salts (Patent Document 1), phenacylsulfonium salts with a naphthalene skeleton (Patent Document 2), and dialkylbenzylsulfonium salts (Patent Document 3) have extremely low photosensitivity, and in order to improve the sensitivity, a sensitizer needs to be used in combination. However, most sensitizers have low compatibility with resins and photoacid generators, and there are cases where their use is restricted. The triarylsulfonium salts described in Patent Documents 4 to 7 increase the light absorption of i-rays, h-rays or visible rays by expanding the π conjugated system, thereby improving photosensitivity without using a sensitizer in combination. However, in the case of large light absorption, when a curable composition or a photoresist composition is prepared, the irradiated light is strongly absorbed only on the surface of the composition, and the light does not penetrate deep into the composition, resulting in poor reactivity. Therefore, ideally, a photoacid generator with high photosensitivity without increasing light absorption is preferred.
[0007] Prior art literature
[0008] Patent Literature
[0009] Patent Document 1: Japanese Patent Application Laid-Open No. 50-151997
[0010] Patent Document 2: Japanese Patent Application Laid-Open No. 9-118663
[0011] Patent Document 3: Japanese Patent Application Laid-Open No. 2-178303
[0012] Patent Document 4: Japanese Patent Application Laid-Open No. 10-287643
[0013] Patent Document 5: Japanese Patent Application No. 2009-533377
[0014] Patent Document 6: Japanese Patent Application Publication No. 2010-215616
[0015] Patent Document 7: Japanese Patent Application Publication No. 2018-24598 Summary of the invention
[0016] Under the above background, a first object of the present invention is to provide a novel sulfonium salt having high photosensitivity without significantly increasing light absorption.
[0017] A second object of the present invention is to provide a novel photoacid generator comprising a sulfonium salt having high photosensitivity and excellent storage stability in a complex with a cationically polymerizable compound such as an epoxy compound.
[0018] A third object of the present invention is to provide an energy-ray-curable composition and a cured product using the above-mentioned photoacid generator.
[0019] A fourth object of the present invention is to provide a chemically amplified positive photoresist composition using the above-mentioned photoacid generator and a method for producing the same.
[0020] A fifth object of the present invention is to provide a chemically amplified negative photoresist composition using the above-mentioned photoacid generator and a cured product thereof.
[0021] The present inventors synthesized a sulfonium salt represented by the following general formula (1), and found that it is suitable for the above-mentioned purposes.
[0022] That is, the present invention provides a sulfonium salt represented by the following general formula (1).
[0023]
[0024] [In formula (1), R1 and R2 are mutually independently an aryl group having 6 to 14 carbon atoms, and a part of the hydrogen atoms of these aryl groups may be substituted by a substituent (t). The substituent (t) is an alkyl group having 1 to 8 carbon atoms or an aryl group having 6 to 10 carbon atoms, and these substituents (t) may be bonded to R1 and R2 directly by a single bond or via any of the groups represented by -SO-, -SO2- or -CO-. A1 and A2 are mutually independently a hydrogen atom, a branched alkyl group having 3 to 7 carbon atoms, a branched alkoxy group having 3 to 7 carbon atoms, a tertiary silyl group having 3 to 9 carbon atoms, or a tertiary siloxy group having 3 to 9 carbon atoms, wherein A1 and A2 are not simultaneously a hydrogen atom. T1 and T2 are mutually independently an alkyl group having 1 to 7 carbon atoms, an alkoxy group having 1 to 7 carbon atoms, a silyl group having 3 to 9 carbon atoms, or a siloxy group having 3 to 9 carbon atoms. m1 and m2 represent the number of T1 and T2, respectively. m1 is an integer of 0 to 3, and m2 is an integer of 0 to 4. L represents a group represented by -O-, -S-, -SO-, -SO2- or -CO-, S represents a sulfur atom, O represents an oxygen atom, C represents a carbon atom, and X represents - represents a monovalent polyatomic anion]
[0025] Furthermore, the present invention provides a photoacid generator characterized by containing the above-mentioned sulfonium salt.
[0026] The present invention also provides an energy-ray-curable composition comprising the above-mentioned photoacid generator and a cationically polymerizable compound.
[0027] Furthermore, the present invention provides a cured product characterized by being obtained by curing the above-mentioned energy ray-curable composition.
[0028] Furthermore, the present invention is a chemically amplified positive photoresist composition, characterized in that it contains the above-mentioned photoacid generator and a component (B), wherein the above-mentioned component (B) is a resin whose solubility in alkali increases due to the action of an acid.
[0029] Furthermore, the present invention is a method for preparing a resist pattern, characterized in that it includes: a stacking step, in which photoresist layers with a film thickness of 5 to 150 μm composed of the above-mentioned chemically amplified positive photoresist composition are stacked to obtain a photoresist stack; an exposure step, in which light or radiation is selectively irradiated to a portion of the photoresist stack; and a development step, in which the photoresist stack is developed after the exposure step to obtain a resist pattern.
[0030] Furthermore, the present invention is a chemically amplified negative photoresist composition, characterized in that it contains the above-mentioned photoacid generator, component (F) and crosslinking agent component (G), and the above-mentioned component (F) is an alkali-soluble resin having a phenolic hydroxyl group.
[0031] Furthermore, the present invention provides a cured product characterized by being obtained by curing any one of the above-mentioned chemically amplified negative photoresist compositions.
[0032] The sulfonium salt of the present invention has excellent photosensitivity to active energy rays such as visible light, ultraviolet light, electron beams, and X-rays, has high compatibility with solvents and cationically polymerizable compounds such as epoxy compounds, and has excellent storage stability in complexes with cationically polymerizable compounds such as epoxy compounds. In addition, since the sulfonium salt of the present invention has high photosensitivity and does not increase the light absorption of ultraviolet light, it has excellent permeability and reactivity when prepared into a curable composition or a photoresist composition.
[0033] When the photoacid generator of the present invention is used for curing a cationically polymerizable compound, it has excellent curability by ultraviolet light, particularly i-rays and h-rays, and can cure the cationically polymerizable compound without using a sensitizer.
[0034] The energy-ray curable composition of the present invention contains the above-mentioned photoacid generator, so it can be cured by ultraviolet light. In addition, the energy-ray curable composition of the present invention has high storage stability and does not require the use of a sensitizer, so it is excellent in cost and workability. Furthermore, since the energy-ray curable composition of the present invention has high transmittance of ultraviolet light, the curability of thick films is also excellent.
[0035] The cured product of the present invention can be obtained without using a sensitizer, and therefore, there is no problem of coloration or deterioration due to residual sensitizer.
[0036] The chemically amplified positive photoresist composition and the chemically amplified negative photoresist composition of the present invention contain the above-mentioned photoacid generator, so that a resist having high sensitivity to i-rays and h-rays can be obtained (a pattern can be formed at a low exposure compared to existing resists). In addition, the chemically amplified positive photoresist composition and the chemically amplified negative photoresist composition of the present invention have high storage stability and good resist pattern shape. Furthermore, since the chemically amplified positive photoresist composition and the chemically amplified negative photoresist composition of the present invention have high transmittance to ultraviolet light, the photoreactivity (sensitivity) of the thick film is also excellent. DETAILED DESCRIPTION
[0037] Hereinafter, embodiments of the present invention will be described in detail.
[0038] The sulfonium salt contained in the photoacid generator of the present invention is represented by the following formula (1).
[0039]
[0040] [In formula (1), R1 and R2 are mutually independently an aryl group having 6 to 14 carbon atoms, and a part of the hydrogen atoms of these aryl groups may be substituted by a substituent (t). The substituent (t) is an alkyl group having 1 to 8 carbon atoms or an aryl group having 6 to 10 carbon atoms, and these substituents (t) may be bonded to R1 and R2 directly by a single bond or via any of the groups represented by -SO-, -SO2- or -CO-. A1 and A2 are mutually independently a hydrogen atom, a branched alkyl group having 3 to 7 carbon atoms, a branched alkoxy group having 3 to 7 carbon atoms, a tertiary silyl group having 3 to 9 carbon atoms, or a tertiary siloxy group having 3 to 9 carbon atoms, wherein A1 and A2 are not simultaneously a hydrogen atom. T1 and T2 are mutually independently an alkyl group having 1 to 7 carbon atoms, an alkoxy group having 1 to 7 carbon atoms, a silyl group having 3 to 9 carbon atoms, or a siloxy group having 3 to 9 carbon atoms. m1 and m2 represent the number of T1 and T2, respectively. m1 is an integer of 0 to 3, and m2 is an integer of 0 to 4. L is a group represented by -O-, -S-, -SO-, -SO2- or -CO-, S represents a sulfur atom, O represents an oxygen atom, C represents a carbon atom, and X - represents a monovalent polyatomic anion]
[0041] In R1 and R2, examples of the aryl group include aryl groups having 6 to 14 carbon atoms (phenyl, tolyl, dimethylphenyl, biphenyl, naphthyl, fluorenyl, fluorenone, anthracenyl, anthraquinone, etc.).
[0042] R1 and R2 may be the same or different, or may be partially different, but are preferably the same.
[0043] A portion of the hydrogen atoms of the aryl group of R1 and R2 may be substituted by a substituent (t), and the substituent (t) is an alkyl group having 1 to 8 carbon atoms or an aryl group having 6 to 10 carbon atoms. These substituents (t) may be bonded to R1 and R2 directly through a single bond or via any of the groups represented by -SO-, -SO2- or -CO-.
[0044] In the substituent (t), examples of the alkyl group having 1 to 8 carbon atoms include straight-chain alkyl groups (methyl, ethyl, n-propyl, n-butyl, n-pentyl and n-octyl, etc.), branched-chain alkyl groups (isopropyl, isobutyl, sec-butyl, tert-butyl, isopentyl, neopentyl, tert-pentyl, isohexyl and isooctyl, etc.) and cycloalkyl groups (cyclopropyl, cyclobutyl, cyclopentyl and cyclohexyl, etc.).
[0045] In the substituent (t), examples of the aryl group having 6 to 10 carbon atoms include phenyl, tolyl, dimethylphenyl and naphthyl.
[0046] In A1 and A2, examples of the branched alkyl group having 3 to 7 carbon atoms include isopropyl, isobutyl, sec-butyl, tert-butyl, isopentyl, neopentyl, tert-pentyl and isohexyl.
[0047] In A1 and A2, examples of the branched alkoxy group having 3 to 7 carbon atoms include isopropoxy, isobutoxy, sec-butoxy and tert-butoxy.
[0048] In A1 and A2, examples of the tertiary silyl group having 3 to 9 carbon atoms include trimethylsilyl, triethylsilyl, tert-butyldimethylsilyl and triisopropylsilyl.
[0049] In A1 and A2, examples of the tertiary silyloxy group having 3 to 9 carbon atoms include trimethylsilyloxy, triethylsilyloxy, tert-butyldimethylsilyloxy and triisopropylsilyloxy.
[0050] A1 and A2 may be the same or different, but they are not both hydrogen atoms. Preferably, at least one of A1 and A2 is a group selected from tert-butyl, tert-butoxy and trimethylsiloxy, and tert-butyl is more preferably from the viewpoint of obtaining industrial raw materials.
[0051] In T1 and T2, examples of the alkyl group having 1 to 7 carbon atoms include straight-chain alkyl groups (methyl, ethyl, propyl, butyl, pentyl and benzyl, etc.), branched-chain alkyl groups (isopropyl, isobutyl, sec-butyl, tert-butyl, isopentyl, neopentyl, tert-pentyl and isohexyl, etc.) and cycloalkyl groups (cyclopropyl, cyclobutyl, cyclopentyl and cyclohexyl, etc.).
[0052] In T1 and T2, examples of the alkoxy group having 1 to 7 carbon atoms include linear or branched alkoxy groups (methoxy, ethoxy, propoxy, isopropoxy, butoxy, isobutoxy, sec-butoxy, tert-butoxy, hexyloxy, etc.).
[0053] In T1 and T2, examples of the silyl group having 3 to 9 carbon atoms include trimethylsilyl, triethylsilyl, tert-butyldimethylsilyl and triisopropylsilyl.
[0054] In T1 and T2, examples of the silyloxy group having 3 to 9 carbon atoms include a trimethylsilyloxy group, a triethylsilyloxy group, a tert-butyldimethylsilyloxy group, and a triisopropylsilyloxy group.
[0055] T1 and T2 may be the same as, or different from, each other, or may be partially different.
[0056] m1 represents the number of T1, and is an integer of 0-3, preferably 0-2, and more preferably 0 or 1. m2 represents the number of T2, and is an integer of 0-4, and preferably 0-2.
[0057] L is a group represented by -O-, -S-, -SO-, -SO2- or -CO-, and is preferably -S-, -SO- or -SO2-.
[0058] S represents a sulfur atom, O represents an oxygen atom, and C represents a carbon atom.
[0059] X - There is no limitation as long as it is a monovalent polyatomic anion, and it is an anion corresponding to the acid (HX) generated by irradiating the sulfonium salt of the present invention with active energy rays (visible light, ultraviolet light, electron beam, X-ray, etc.), preferably MY a - 、(Rf) b PF 6-b - , R 3 c BY 4-c - , R 3 c GaY 4-c - , R 4 SO3 - , (R 4 SO2)3C - or (R 4 SO2)2N - Represents anion.
[0060] M represents a phosphorus atom, a boron atom or an antimony atom. Y represents a halogen atom (preferably a fluorine atom).
[0061] Rf represents an alkyl group (preferably an alkyl group having 1 to 8 carbon atoms) in which 80 mol% or more of hydrogen atoms are substituted with fluorine atoms. Examples of the alkyl group that is substituted with fluorine to become Rf include straight-chain alkyl groups (methyl, ethyl, propyl, butyl, pentyl, and octyl groups, etc.), branched-chain alkyl groups (isopropyl, isobutyl, sec-butyl, and tert-butyl groups, etc.), and cycloalkyl groups (cyclopropyl, cyclobutyl, cyclopentyl, and cyclohexyl groups, etc.). In Rf, the ratio of hydrogen atoms of these alkyl groups to be substituted with fluorine atoms is preferably 80 mol% or more, more preferably 90% or more, and particularly preferably 100%, based on the number of moles of hydrogen atoms in the original alkyl group. If the substitution ratio based on fluorine atoms is within these preferred ranges, the photosensitivity of the sulfonium salt becomes further improved. Particularly preferred Rf includes CF3-, CF3CF2-, (CF3)2CF-, CF3CF2CF2-, CF3CF2CF2CF2-, (CF3)2CFCF2-, CF3CF2(CF3)CF-, and (CF3)3C-. The b Rfs are independent of each other and may be the same or different.
[0062] P represents a phosphorus atom, and F represents a fluorine atom.
[0063] R 3 It represents a phenyl group in which a part of hydrogen atoms is replaced by at least one element or electron-withdrawing group. Examples of such an element include halogen atoms, such as fluorine atoms, chlorine atoms, and bromine atoms. Examples of electron-withdrawing groups include trifluoromethyl, nitro, and cyano groups. Among these, a phenyl group in which one hydrogen atom is replaced by a fluorine atom or a trifluoromethyl group is preferred. 3 They are independent of each other and therefore can be the same or different.
[0064] B represents a boron atom, and Ga represents a gallium atom.
[0065] R 4 It represents an alkyl group having 1 to 20 carbon atoms, a perfluoroalkyl group having 1 to 20 carbon atoms, or an aryl group having 6 to 20 carbon atoms. The alkyl group and the perfluoroalkyl group may be linear, branched, or cyclic. The aryl group may be unsubstituted or may have a substituent.
[0066] S represents a sulfur atom, O represents an oxygen atom, C represents a carbon atom, and N represents a nitrogen atom. a represents an integer of 4 to 6. b is preferably an integer of 1 to 5, more preferably 2 to 4, and particularly preferably 2 or 3. c is preferably an integer of 1 to 4, more preferably 4.
[0067] As MY a - The anion represented by SbF6 - PF6 - and BF4 -Indicates anions, etc.
[0068] As (Rf) b PF 6-b - The anion represented by (CF3CF2)2PF4 - 、(CF3CF2)3PF3 - 、((CF3)2CF)2PF4 - 、((CF3)2CF)3PF3 - 、(CF3CF2CF2)2PF4 - 、(CF3CF2CF2)3PF3 - 、((CF3)2CFCF2)2PF4 - 、((CF3)2CFCF2)3PF3 - 、(CF3CF2CF2CF2)2PF4 - and (CF3CF2CF2CF2)3PF3 - Among these, (CF3CF2)3PF3 is preferred. - 、(CF3CF2CF2)3PF3 - 、((CF3)2CF)3PF3 - 、((CF3)2CF)2PF4 - 、((CF3)2CFCF2)3PF3 - and ((CF3)2CFCF2)2PF4 - The anion represented by is particularly preferably (CF3CF2)3PF3 - 、(CF3CF2CF2CF2)3PF3 - .
[0069] As R 3 c BY 4-c - The anion represented by (C6F5)4B - 、((CF3)2C6H3)4B - 、(CF3C6H4)4B - 、(C6F5)2BF2 - 、C6F5BF3 - and (C6H3F2)4B - Among these, (C6F5)4B is preferred. - 、(C6H5)(C6F5)3B - and ((CF3)2C6H3)4B - Represents anion.
[0070] As R 3 c GaY 4-c - The anion represented by (C6F5)4Ga - 、((CF3)2C6H3)4Ga - 、(CF3C6H4)4Ga - 、(C6F5)2GaF2 - 、C6F5GaF3 - and (C6H3F2)4Ga - Among these, (C6F5)4Ga - and ((CF3)2C6H3)4Ga - Represents anion.
[0071] As R 4 SO3 - The anion represented by , includes trifluoromethanesulfonate anion, pentafluoroethanesulfonate anion, heptafluoropropanesulfonate anion, nonafluorobutanesulfonate anion, pentafluorophenylsulfonate anion, p-toluenesulfonate anion, benzenesulfonate anion, camphorsulfonate anion, methanesulfonate anion, ethanesulfonate anion, propanesulfonate anion and butanesulfonate anion, etc. Among these, trifluoromethanesulfonate anion, nonafluorobutanesulfonate anion, methanesulfonate anion, camphorsulfonate anion, benzenesulfonate anion and p-toluenesulfonate anion are preferred.
[0072] As (R 4 SO2)3C - The anion represented by (CF3SO2)3C - 、(C2F5SO2)3C - 、(C3F7SO2)3C - and (C4F9SO2)3C - Indicates anions, etc.
[0073] As (R 4 SO2)2N - The anion represented by (CF3SO2)2N - 、(C2F5SO2)2N - 、(C3F7SO2)2N - and (C4F9SO2)2N - Indicates anions, etc.
[0074] As a monovalent polyatomic anion (X - ), except MY a - 、(Rf) b PF6-b - , R 3 c BY 4-c - , R 3 c GaY 4-c - , R 4 SO3 - , (R 4 SO2)3C - or (R 4 SO2)2N - In addition to the anions shown, perhalate ions (ClO4 - BrO4 - etc.), halide sulfonate ions (FSO3 - 、ClSO3 - etc.), sulfate ions (CH3SO4 - CF3SO4 - 、HSO4 - etc.), carbonate ions (HCO3 - 、CH3CO3 - etc.), aluminate ions (AlCl4 - 、AlF4 - etc.), hexafluorobismuthate ion (BiF6 - ), carboxylate ion (CH3COO - CF3COO - 、C6H5COO - 、CH3C6H4COO - 、C6F5COO - CF3C6H4COO - etc.), aryl borate ions (B(C6H5)4 - 、CH3CH2CH2CH2B(C6H5)3 - etc.), thiocyanate ion (SCN - ) and nitrate ions (NO3 - )wait.
[0075] The sulfonium salt can be produced by the production method described below.
[0076] <Manufacturing method>
[0077] The following reaction formula can be cited as a method (for example, the method described in Experimental Chemistry Lectures, Vol. 24, 4th edition, published by Maruzen Co., Ltd. in 1992, p. 376, Japanese Patent Application Publication No. 7-329399, Japanese Patent Application Publication No. 8-165290, Japanese Patent Application Publication No. 10-212286 or Japanese Patent Application Publication No. 10-7680, etc.).
[0078]
[0079] In the above reaction formula, R1, R2, A1, A2, T1, T2, L, S, O, X - , m1 and m2 are the same as those defined in the general formula (1). H represents a hydrogen atom.
[0080] HX' represents a conjugate acid of a monovalent polyatomic anion. HX' is preferably methanesulfonic acid, perfluoroalkylsulfonic acid, and sulfuric acid from the viewpoints of easy availability, acid stability, and reaction yield.
[0081] The dehydrating agent includes, for example, phosphoric anhydride, acetic anhydride, concentrated sulfuric acid, or perfluoroalkylsulfonic anhydride.
[0082] Monovalent polyatomic anions (X' - ) can be converted into other anions (X - ).
[0083] MX represents an alkali metal (lithium, sodium, potassium, etc.) cation and other anions of the present invention {e.g., MY a - 、(Rf) b PF 6-b - , R 3 c BY 4-c - , R 3 c GaY 4-c - , R 4 SO3 - , (R 4 SO2)3C - or (R 4 SO2)2N - etc.}.
[0084] In the above reaction formula, the reaction in the first stage can be carried out without solvent, or in an organic solvent (acetonitrile, tetrahydrofuran, dihydrogen ether, etc.) as required. The reaction is carried out in an aqueous solution of 1,2-dichloromethane, 1,2-dichloro ...
[0085] The reaction of the second stage can be carried out following the reaction of the first stage, or the reaction intermediate (G2) can be separated (purified as needed) and then carried out. The reaction intermediate (G2) and the aqueous solution of the salt (MX) of the anion used in the present invention are mixed and stirred with the alkali metal cation, and double decomposition reaction is carried out, and the precipitated solid is separated by filtering or the separated oily substance is extracted with an organic solvent and the organic solvent is removed, so as to obtain the sulfonium salt of the present invention in the form of a solid or a viscous liquid. The obtained solid or viscous liquid can be cleaned with a suitable organic solvent as needed, or purified by recrystallization or column chromatography.
[0086] The chemical structure of the sulfonium salt of the present invention can be determined by general analytical methods (e.g., 1 H- 11 B- 13 C-、 19 F-, 31 P-NMR spectrum, infrared absorption spectrum and / or elemental analysis, etc.) for identification.
[0087] The photoacid generator of the present invention is characterized by containing the sulfonium salt represented by the general formula (1), but may contain other conventionally known photoacid generators in addition thereto.
[0088] When other photoacid generators are contained, the content (mol %) of other photoacid generators is preferably 0.1 to 100, more preferably 0.5 to 50, based on the total molar number of the sulfonium salt represented by the general formula (1) of the present invention.
[0089] As other photoacid generators, there are Salt (sulfonium, iodine Selenium, ammonium and etc.) and the salts of transition metal complex ions and anions and other conventionally known photoacid generators.
[0090] When the photoacid generator of the present invention is used, it may be dissolved in advance in a solvent that does not inhibit polymerization, crosslinking, deprotection reaction, etc., in order to facilitate dissolution in a cationically polymerizable compound or a chemically amplified resist composition.
[0091] Examples of the solvent include carbonates such as propylene carbonate, ethylene carbonate, 1,2-butylene carbonate, dimethyl carbonate and diethyl carbonate; ketones such as acetone, methyl ethyl ketone, cyclohexanone, methyl isoamyl ketone and 2-heptanone; polyols such as monomethyl ether, monoethyl ether, monopropyl ether, monobutyl ether or monophenyl ether of ethylene glycol, ethylene glycol monoacetate, diethylene glycol, diethylene glycol monoacetate, propylene glycol, propylene glycol monoacetate, dipropylene glycol and dipropylene glycol monoacetate and their derivatives; dipropylene glycol monoacetate; Cyclic ethers such as alkanes; esters such as ethyl formate, methyl lactate, ethyl lactate, methyl acetate, ethyl acetate, butyl acetate, methyl pyruvate, methyl acetoacetate, ethyl acetoacetate, ethyl pyruvate, ethyl ethoxyacetate, methyl methoxypropionate, ethyl ethoxypropionate, methyl 2-hydroxypropionate, ethyl 2-hydroxypropionate, ethyl 2-hydroxy-2-methylpropionate, methyl 2-hydroxy-3-methylbutyrate, 3-methoxybutyl acetate, 3-methyl-3-methoxybutyl acetate, β-propiolactone, β-butyrolactone, γ-butyrolactone, δ-valerolactone and ε-caprolactone; aromatic hydrocarbons such as toluene and xylene, etc.
[0092] When a solvent is used, the solvent is preferably used in an amount of 15 to 1000 parts by weight, more preferably 30 to 500 parts by weight, based on 100 parts by weight of the photoacid generator containing the sulfonium salt of the present invention. The solvent may be used alone or in combination of two or more.
[0093] The energy-ray-curable composition of the present invention contains the above-mentioned photoacid generator and a cationically polymerizable compound.
[0094] Examples of the cationically polymerizable compounds that are components of the energy-ray-curable composition include cyclic ethers (epoxides, oxetanes, etc.), ethylenically unsaturated compounds (vinyl ethers, styrenes, etc.), bicyclic orthoesters, spirocyclic orthocarbonates, and spirocyclic orthoesters {Japanese Patent Application Publication No. 11-060996, Japanese Patent Application Publication No. 09-302269, Japanese Patent Application Publication No. 2003-026993, etc.}.
[0095] As the epoxide, known epoxides and the like can be used, including aromatic epoxides, alicyclic epoxides, and aliphatic epoxides.
[0096] Examples of the aromatic epoxide include glycidyl ethers of monohydric or polyhydric phenols (phenol, bisphenol A, phenol novolac, and compounds obtained by adding alkylene oxides thereof) having at least one aromatic ring.
[0097] Examples of the alicyclic epoxide include compounds obtained by epoxidizing a compound having at least one cyclohexene ring or cyclopentene ring with an oxidizing agent (such as 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexanecarboxylate).
[0098] Examples of the aliphatic epoxides include polyglycidyl ethers of aliphatic polyols or alkylene oxide adducts thereof (1,4-butanediol diglycidyl ether, 1,6-hexanediol diglycidyl ether, etc.), polyglycidyl esters of aliphatic polybasic acids (tetrahydrophthalic acid diglycidyl ether, etc.), and epoxides of long-chain unsaturated compounds (epoxidized soybean oil, epoxidized polybutadiene, etc.).
[0099] As the oxetane, known oxetanes can be used, for example, 3-ethyl-3-hydroxymethyloxetane, 2-ethylhexyl (3-ethyl-3-oxetanyl methyl) ether, 2-hydroxyethyl (3-ethyl-3-oxetanyl methyl) ether, 2-hydroxypropyl (3-ethyl-3-oxetanyl methyl) ether, 1,4-bis [(3-ethyl-3-oxetanyl methoxy) methyl] benzene, oxetanyl silsesquioxane, and phenol novolac oxetane can be mentioned.
[0100] As the ethylenically unsaturated compound, known cationically polymerizable monomers and the like can be used, including aliphatic monovinyl ethers, aromatic monovinyl ethers, polyfunctional vinyl ethers, styrenes, and cationically polymerizable nitrogen-containing monomers.
[0101] Examples of the aliphatic monovinyl ether include methyl vinyl ether, ethyl vinyl ether, butyl vinyl ether and cyclohexyl vinyl ether.
[0102] Examples of the aromatic monovinyl ether include 2-phenoxyethyl vinyl ether, phenyl vinyl ether, and p-methoxyphenyl vinyl ether.
[0103] Examples of the polyfunctional vinyl ether include butanediol-1,4-divinyl ether and triethylene glycol divinyl ether.
[0104] Examples of the styrenes include styrene, α-methylstyrene, p-methoxystyrene, and p-tert-butoxystyrene.
[0105] Examples of the cationically polymerizable nitrogen-containing monomer include N-vinylcarbazole and N-vinylpyrrolidone.
[0106] Examples of the bicyclic orthoesters include 1-phenyl-4-ethyl-2,6,7-trioxabicyclo[2.2.2]octane and 1-ethyl-4-hydroxymethyl-2,6,7-trioxabicyclo-[2.2.2]octane.
[0107] Examples of the spiro orthocarbonate include 1,5,7,11-tetraoxaspiro[5.5]undecane and 3,9-dibenzyl-1,5,7,11-tetraoxaspiro[5.5]undecane.
[0108] Examples of the spiroorthoester include 1,4,6-trioxaspiro[4.4]nonane, 2-methyl-1,4,6-trioxaspiro[4.4]nonane, and 1,4,6-trioxaspiro[4.5]decane.
[0109] Furthermore, polyorganosiloxane having at least one cationically polymerizable group in one molecule (described in JP-A-2001-348482, Journal of Polym. Sci., Part A, Polym. Chem., Vol. 28, 497 (1990), etc.) can be used.
[0110] These polyorganosiloxanes may be linear, branched, or cyclic, or may be a mixture thereof.
[0111] Among these cationically polymerizable compounds, epoxides, oxetanes and vinyl ethers are preferred, epoxides and oxetanes are more preferred, and alicyclic epoxides and oxetanes are particularly preferred. In addition, these cationically polymerizable compounds may be used alone or in combination of two or more.
[0112] The content of the photoacid generator containing the sulfonium salt of the present invention in the energy-ray curable composition is preferably 0.05 to 20 parts by weight, and more preferably 0.1 to 10 parts by weight, relative to 100 parts by weight of the cationic polymerizable compound. If it is within this range, the polymerization of the cationic polymerizable compound becomes more sufficient, and the physical properties of the cured product become further good. It should be noted that the content is determined by considering various important factors such as the properties of the cationic polymerizable compound, the type and irradiation amount of the energy ray, the temperature, the curing time, the humidity, the thickness of the coating film, and is not limited to the above range.
[0113] The energy-ray-curable composition of the present invention may contain known additives (sensitizers, pigments, fillers, antistatic agents, flame retardants, defoamers, flow regulators, light stabilizers, antioxidants, adhesion-imparting agents, ion scavengers, anti-coloring agents, solvents, non-reactive resins, and free radical polymerizable compounds, etc.) as needed.
[0114] As the sensitizer, known sensitizers (such as those disclosed in Japanese Unexamined Patent Application Publication No. 11-279212 and Japanese Unexamined Patent Application Publication No. 09-183960) can be used, and examples thereof include anthracenes {anthracene, 9,10-dibutoxyanthracene, 9,10-dimethoxyanthracene, 9,10-diethoxyanthracene, 2-ethyl-9,10-dimethoxyanthracene, 9,10-dipropoxyanthracene, etc.}; pyrene; 1,2-benzanthracene; perylene; tetracene; coronene; thioxanthones {thioxanthone, 2-methylthioxanthone, 2-ethylthioxanthone, 2-chlorothioxanthone, 2-isopropylthioxanthone, and 2,4-diethylthioxanthone, etc.}; phenothiazines {phenothiazine, N-methylphenothiazine, N-ethylphenothiazine, N-phenylphenothiazine, etc.}; Tonone; Naphthalene {1-naphthol, 2-naphthol, 1-methoxynaphthalene, 2-methoxynaphthalene, 1,4-dihydroxynaphthalene and 4-methoxy-1-naphthol, etc.}; Ketone {dimethoxyacetophenone, diethoxyacetophenone, 2-hydroxy-2-methyl-1-phenylpropane-1-one, 4'-isopropyl-2-hydroxy-2-methylpropiophenone and 4-benzoyl-4'-methyldiphenyl sulfide, etc.}; Carbazole {N-phenylcarbazole, N-ethylcarbazole, poly-N-vinylcarbazole and N-glycidylcarbazole, etc.}; {1,4-dimethoxy and 1,4-di-α-methylbenzyloxy etc.}; phenanthrene {9-hydroxyphenanthrene, 9-methoxyphenanthrene, 9-hydroxy-10-methoxyphenanthrene and 9-hydroxy-10-ethoxyphenanthrene, etc.}, etc.
[0115] When a sensitizer is contained, the content of the sensitizer is preferably 1 to 300 parts by weight, more preferably 5 to 200 parts by weight, based on 100 parts of the photo-acid generator of the present invention.
[0116] As the pigment, known pigments can be used, and examples thereof include inorganic pigments (such as titanium oxide, iron oxide, and carbon black) and organic pigments (such as azo pigments, cyanine pigments, phthalocyanine pigments, and quinacridone pigments).
[0117] When a pigment is contained, the content of the pigment is preferably 0.5 to 400,000 parts by weight, more preferably 10 to 150,000 parts by weight, based on 100 parts of the photoacid generator of the present invention.
[0118] As the filler, a known filler can be used, and examples thereof include fused silica, crystalline silica, calcium carbonate, alumina, aluminum hydroxide, zirconium oxide, magnesium carbonate, mica, talc, calcium silicate, and lithium aluminum silicate.
[0119] When a filler is contained, the content of the filler is preferably 50 to 600,000 parts by weight, more preferably 300 to 200,000 parts by weight, based on 100 parts of the photo-acid generator of the present invention.
[0120] As the antistatic agent, a known antistatic agent or the like can be used, and examples thereof include nonionic antistatic agents, anionic antistatic agents, cationic antistatic agents, amphoteric antistatic agents, and polymer antistatic agents.
[0121] When an antistatic agent is contained, the content of the antistatic agent is preferably 0.1 to 20,000 parts by weight, more preferably 0.6 to 5,000 parts by weight, based on 100 parts of the photo-acid generator of the present invention.
[0122] As flame retardants, known flame retardants can be used, and examples include inorganic flame retardants {antimony trioxide, antimony pentoxide, tin oxide, tin hydroxide, molybdenum oxide, zinc borate, barium metaborate, red phosphorus, aluminum hydroxide, magnesium hydroxide and calcium aluminate, etc.}; bromine flame retardants {tetrabromophthalic anhydride, hexabromobenzene and decabromodiphenyl ether, etc.}; and phosphate flame retardants {tris(tribromophenyl)phosphate, etc.}, etc.
[0123] When a flame retardant is contained, the content of the flame retardant is preferably 0.5 to 40,000 parts by weight, more preferably 5 to 10,000 parts by weight, based on 100 parts of the photo-acid generator of the present invention.
[0124] As the defoaming agent, a known defoaming agent may be used, and examples thereof include alcohol defoaming agents, metal soap defoaming agents, phosphate ester defoaming agents, fatty acid ester defoaming agents, polyether defoaming agents, silicone defoaming agents, and mineral oil defoaming agents.
[0125] As the flowability adjusting agent, a known flowability adjusting agent can be used, and examples thereof include hydrogenated castor oil, polyethylene oxide, organic bentonite, colloidal silica, amide wax, metal soap, and acrylic acid ester polymer.
[0126] As the light stabilizer, known light stabilizers can be used, and examples thereof include ultraviolet absorbing stabilizers {benzotriazole, benzophenone, salicylic acid ester, cyanoacrylate and their derivatives, etc.}; radical scavenging stabilizers {hindered amines, etc.}; and extinction stabilizers {nickel complexes, etc.}.
[0127] As the antioxidant, a known antioxidant can be used, and examples thereof include phenolic antioxidants (monophenolic antioxidants, bisphenolic antioxidants, polymeric phenolic antioxidants, etc.), sulfur-based antioxidants, and phosphorus-based antioxidants.
[0128] As the adhesion-imparting agent, a known adhesion-imparting agent or the like can be used, and examples thereof include a coupling agent, a silane coupling agent, and a titanium coupling agent.
[0129] As the ion scavenger, a known ion scavenger or the like can be used, and examples thereof include organic aluminum (alkoxyaluminum, phenoxyaluminum, and the like).
[0130] As the anti-coloring agent, a known anti-coloring agent can be used. Generally speaking, antioxidants are effective, and examples thereof include phenolic antioxidants (monophenolic, bisphenolic, and polymeric phenolic), sulfur-based antioxidants, and phosphorus-based antioxidants. However, these are almost ineffective in preventing coloring during heat resistance tests at high temperatures.
[0131] When a defoamer, a flow regulator, a light stabilizer, an antioxidant, an adhesion-imparting agent, an ion scavenger or an anti-coloring agent is contained, the content of each is preferably 0.1 to 20,000 parts by weight, more preferably 0.5 to 5,000 parts by weight, based on 100 parts of the photoacid generator of the present invention.
[0132] The solvent is not limited as long as it can be used to dissolve the cationically polymerizable compound and adjust the viscosity of the energy-ray curable composition, and any solvent listed as the solvent for the photoacid generator can be used.
[0133] When a solvent is contained, the content of the solvent is preferably 50 to 2,000,000 parts by weight, more preferably 200 to 500,000 parts by weight, based on 100 parts of the photo-acid generator of the present invention.
[0134] Examples of non-reactive resins include polyester, polyvinyl acetate, polyvinyl chloride, polybutadiene, polycarbonate, polystyrene, polyvinyl ether, polyvinyl butyral, polybutene, hydrogenated styrene butadiene block copolymer, (meth)acrylate copolymers, and polyurethanes. The number average molecular weight of these resins is preferably 1,000 to 500,000, and more preferably 5,000 to 100,000 (the number average molecular weight is a value measured by a general method such as GPC).
[0135] When a non-reactive resin is contained, the content of the non-reactive resin is preferably 5 to 400,000 parts by weight, more preferably 50 to 150,000 parts by weight, based on 100 parts of the photo-acid generator of the present invention.
[0136] When a non-reactive resin is contained, it is preferably dissolved in a solvent in advance in order to make the non-reactive resin easily dissolve in the cationically polymerizable compound and the like.
[0137] As free radical polymerizable compounds, known free radical polymerizable compounds such as those disclosed in {Photosensitive Polymer Symposium, "Photosensitive Polymer Handbook" (1989, Industrial Research Council), Comprehensive Technology Center, "UV·EB Curing Technology" (1982, Comprehensive Technology Center), RadTech Research Institute, "UV·EB Curing Materials" (1992, CMC), etc.} can be used, including monofunctional monomers, bifunctional monomers, polyfunctional monomers, epoxy (meth) acrylates, polyester (meth) acrylates, and urethane (meth) acrylates.
[0138] When a radical polymerizable compound is contained, the content of the radical polymerizable compound is preferably 5 to 400,000 parts by weight, more preferably 50 to 150,000 parts by weight, based on 100 parts of the photoacid generator of the present invention.
[0139] When a radical polymerizable compound is contained, it is preferred to use a radical polymerization initiator which initiates polymerization by heat or light in order to increase the molecular weight of the compound by radical polymerization.
[0140] As the free radical polymerization initiator, known free radical polymerization initiators can be used, including thermal free radical polymerization initiators (organic peroxides, azo compounds, etc.) and photoradical polymerization initiators (acetophenone-based initiators, benzophenone-based initiators, Michler's ketone-based initiators, benzoin-based initiators, thioxanthone-based initiators, acylphosphine-based initiators, etc.).
[0141] When a radical polymerization initiator is contained, the content of the radical polymerization initiator is preferably 0.01 to 20 parts by weight, more preferably 0.1 to 10 parts by weight, based on 100 parts of the radical polymerizable compound.
[0142] The energy-ray-curable composition of the present invention can be prepared by uniformly mixing and dissolving the cationically polymerizable compound, the photoacid generator and the additives as required at room temperature (about 20 to 30° C.) or under heating (about 40 to 90° C.) as required, or further kneading using a three-roll mill or the like.
[0143] The energy-ray-curable composition of the present invention can be cured by irradiating energy rays to obtain a cured product.
[0144] As energy rays, any energy rays may be used as long as they have energy to cause decomposition of the photoacid generator of the present invention, and energy rays in the ultraviolet to visible light region (wavelength: about 100 to about 800 nm) obtained by low-pressure, medium-pressure, high-pressure or ultra-high-pressure mercury lamps, metal halide lamps, LED lamps, xenon lamps, carbon arc lamps, fluorescent lamps, semiconductor solid lasers, argon lasers, He-Cd lasers, KrF excimer lasers, ArF excimer lasers or F2 lasers are preferred. It should be noted that energy rays may also be high-energy radiation such as electron beams or X-rays.
[0145] The irradiation time of energy rays is affected by the intensity of the energy rays and the permeability of the energy rays to the energy-ray-curable composition, but it is sufficient to perform it at room temperature (about 20 to 30°C) for about 0.1 seconds to 10 seconds. However, in the case where the permeability of the energy rays is low, the film thickness of the energy-ray-curable composition is thick, etc., it is sometimes preferred to apply a time longer than that. Most energy-ray-curable compositions are cured by cationic polymerization 0.1 seconds to several minutes after energy-ray irradiation, but as needed, after irradiation with energy rays, they can be heated at room temperature (about 20 to 30°C) to 200°C for several seconds to several hours for post-curing (after-cure).
[0146] Specific uses of the energy-ray-curable composition of the present invention include coatings, coating agents, various coating materials (hard coatings, anti-fouling coating materials, anti-fogging coating materials, touch-resistant coating materials, optical fibers, etc.), back treatment agents for adhesive tapes, release coating materials for release sheets for adhesive labels (release paper, release plastic films, release metal foils, etc.), printed boards, dental materials (dental compounds, dental composite materials), inks, inkjet inks, positive resists (circuit boards, CSPs, MEMS elements, etc., for connecting terminals and wiring pattern formation in the manufacture of electronic components), resist films, liquid resists, negative resists (surface protective films for semiconductor elements, etc., interlayer insulating films, planarization films, etc., permanent film materials), resists for MEMS, positive photosensitive materials, negative photosensitive materials, various adhesives (temporary fixing agents for various electronic components, adhesives for HDDs, pickup lenses (pick up The products include adhesives for optical lenses, adhesives for functional films for FPD (deflection plates, anti-reflection films, etc.), resins for holography, FPD materials (color filters, black matrices, partition materials, photo spacers, flanges, orientation films for liquid crystals, sealants for FPD, etc.), optical components, molding materials (building materials, optical components, lenses), casting molding materials, putty, glass fiber impregnation agents, filling materials, sealing materials, packaging materials, optical semiconductor (LED) packaging materials, optical waveguide materials, nanoimprint materials, materials for stereolithography and micro-stereolithography, etc.
[0147] The photoacid generator of the present invention generates a strong acid by light irradiation, and therefore can also be used as a photoacid generator for chemically amplified resist materials as known in the art (Japanese Patent Application Laid-Open Nos. 2003-267968, 2003-261529, and 2002-193925).
[0148] Chemically amplified resist materials include (1) a two-component chemically amplified positive resist having as essential components a resin soluble in an alkaline developer under the action of an acid and a photoacid generator, (2) a three-component chemically amplified positive resist having as essential components a resin soluble in an alkaline developer, a dissolution inhibitor soluble in an alkaline developer under the action of an acid, and a photoacid generator, and (3) a chemically amplified negative resist having as essential components a resin soluble in an alkaline developer, a crosslinking agent which crosslinks the resin by heating in the presence of an acid and makes it insoluble in an alkaline developer, and a photoacid generator.
[0149] The chemically amplified positive photoresist composition of the present invention is characterized in that it contains a component (A) and a resin component (B), wherein the component (A) contains a compound that generates an acid when irradiated with light or radiation, namely, the photoacid generator of the present invention, and the resin component (B) increases its solubility in alkali due to the action of the acid.
[0150] In the chemically amplified positive photoresist composition of the present invention, component (A) may be used in combination with other known photoacid generators. In addition to salt compounds, sulfone compounds, sulfonate compounds, sulfonimide compounds, disulfonyldiazomethane compounds, disulfonylmethane compounds, oximesulfonate compounds, hydrazinesulfonate compounds, triazine compounds, and nitrobenzyl compounds, organic halides, disulfones, and the like can be mentioned.
[0151] As other conventionally known photoacid generators, preferably One or more of a compound, a sulfonimide compound, a diazomethane compound and an oxime sulfonate compound.
[0152] When such other conventionally known photoacid generators are used in combination, the proportion thereof may be arbitrary, but is usually 10 to 900 parts by weight, preferably 25 to 400 parts by weight, per 100 parts by weight of the total weight of the sulfonium salt represented by the general formula (1).
[0153] The content of the component (A) in the solid content of the chemically amplified positive photoresist composition is preferably 0.05 to 5% by weight.
[0154] <Resin component (B) whose solubility in alkali is increased by the action of an acid>
[0155] The above-mentioned "resin (B) whose solubility in alkali is increased by the action of acid" (referred to as "component (B)" in this specification) used in the chemically amplified positive photoresist composition of the present invention is at least one resin selected from phenolic varnish resin (B1), polyhydroxystyrene resin (B2) and acrylic resin (B3), or a mixed resin or copolymer thereof.
[0156] [Novolac resin (B1)]
[0157] As the novolac resin (B1), a resin represented by the following general formula (b1) can be used.
[0158]
[0159] In the above general formula (b1), R 1b represents an acid dissociative dissolution inhibitory group, R 2b , R3b Each independently represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms, and n represents the number of repeating units of the structure in parentheses.
[0160] Furthermore, as the above R 1b The acid dissociative dissolution inhibitory group represented by is preferably a linear alkyl group having 1 to 6 carbon atoms, a branched alkyl group having 3 to 6 carbon atoms, a cyclic alkyl group having 3 to 6 carbon atoms, a tetrahydropyranyl group, a tetrahydrofuranyl group or a trialkylsilyl group.
[0161] Here, as the above R 1b Specific examples of the acid dissociative solubility inhibitory group represented by include methoxyethyl, ethoxyethyl, n-propoxyethyl, isopropoxyethyl, n-butoxyethyl, isobutoxyethyl, tert-butoxyethyl, cyclohexyloxyethyl, methoxypropyl, ethoxypropyl, 1-methoxy-1-methyl-ethyl, 1-ethoxy-1-methylethyl, tert-butoxycarbonyl, tert-butoxycarbonylmethyl, trimethylsilyl and tri-tert-butyldimethylsilyl.
[0162] [Polyhydroxystyrene resin (B2)]
[0163] As the polyhydroxystyrene resin (B2), a resin represented by the following general formula (b4) can be used.
[0164]
[0165] In the above general formula (b4), R 8b represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms, R 9b represents an acid dissociative solubility inhibitory group, and n represents the number of repeating units of the structure in parentheses.
[0166] The above-mentioned alkyl group having 1 to 6 carbon atoms is a straight-chain alkyl group having 1 to 6 carbon atoms, a branched alkyl group having 3 to 6 carbon atoms, or a cyclic alkyl group having 3 to 6 carbon atoms, and examples thereof include methyl, ethyl, propyl, isopropyl, n-butyl, isobutyl, tert-butyl, pentyl, isopentyl, neopentyl, etc., and examples of the cyclic alkyl group include cyclopentyl, cyclohexyl, etc.
[0167] As the above R 9b The acid dissociative dissolution inhibiting group represented by 1b The acid-dissociable solubility-inhibiting groups are the same as those exemplified in .
[0168] Furthermore, in the polyhydroxystyrene resin (B2), other polymerizable compounds may be contained as constituent units for the purpose of appropriately controlling physical and chemical properties. As such polymerizable compounds, known free radical polymerizable compounds and anionic polymerizable compounds may be cited. For example, monocarboxylic acids such as acrylic acid; dicarboxylic acids such as maleic acid, fumaric acid, and itaconic acid; methacrylic acid derivatives having a carboxyl group and an ester bond such as 2-methacryloyloxyethyl succinic acid; (meth)acrylic acid alkyl esters such as methyl (meth)acrylate; (meth)acrylic acid hydroxyalkyl esters such as (meth)ethyl ester; dicarboxylic acid diesters such as diethyl maleate; aromatic compounds containing vinyl groups such as styrene and vinyltoluene; aliphatic compounds containing vinyl groups such as vinyl acetate; conjugated dienes such as butadiene and isoprene; polymerizable compounds containing nitrile groups such as acrylonitrile; polymerizable compounds containing chlorine such as vinyl chloride; polymerizable compounds containing amide bonds such as acrylamide, etc.
[0169] [Acrylic resin (B3)]
[0170] As the acrylic resin (B3), resins represented by the following general formulas (b5) to (b10) can be used.
[0171]
[0172] In the above general formulae (b5) to (b7), R 10b ~R 17b each independently represents a hydrogen atom, a linear alkyl group having 1 to 6 carbon atoms, a branched alkyl group having 3 to 6 carbon atoms, a fluorine atom, or a linear fluorinated alkyl group having 1 to 6 carbon atoms or a branched fluorinated alkyl group having 3 to 6 carbon atoms, and X b Together with the carbon atom to which it is bonded, it forms a hydrocarbon ring having 5 to 20 carbon atoms, b represents an aliphatic cyclic group or an alkyl group which may have a substituent, n represents the number of repeating units of the structure in the brackets, p is an integer of 0 to 4, and q is 0 or 1.
[0173] In the general formula (b8), the general formula (b9) and the general formula (b10), R 18b , R 20b and R 21b are independently a hydrogen atom or a methyl group. In the general formula (b8), each R 19b independently represent a hydrogen atom, a hydroxyl group, a cyano group or a COOR group 23b Base (where R 23b represents a hydrogen atom, a linear alkyl group having 1 to 4 carbon atoms, a branched alkyl group having 3 to 4 carbon atoms, or a cycloalkyl group having 3 to 20 carbon atoms), in the general formula (b10), each R 22beach independently represents a monovalent alicyclic hydrocarbon group having 4 to 20 carbon atoms or a derivative thereof, or a linear alkyl group having 1 to 4 carbon atoms or a branched alkyl group having 3 to 4 carbon atoms, and R 22b At least one of R is the alicyclic hydrocarbon group or its derivative, or any two R 22b are bonded to each other and together with the common carbon atom to which they are bonded form a divalent alicyclic hydrocarbon group having 4 to 20 carbon atoms or a derivative thereof, and the remaining R 22b It represents a linear alkyl group having 1 to 4 carbon atoms, a branched alkyl group having 3 to 4 carbon atoms, or a monovalent alicyclic hydrocarbon group having 4 to 20 carbon atoms, or a derivative thereof.
[0174] Among the above-mentioned components (B), it is preferred to use acrylic resin (B3).
[0175] The polystyrene-equivalent weight average molecular weight of the component (B) is preferably 10000 to 600000, more preferably 50000 to 600000, and even more preferably 230000 to 550000. With such a weight average molecular weight, the resin properties of the resist are excellent.
[0176] Furthermore, component (B) is preferably a resin having a dispersion degree of 1.05 or more. Here, "dispersion degree" is a value obtained by dividing the weight average molecular weight by the number average molecular weight. With such a dispersion degree, the plating resistance and resin properties of the resist are excellent.
[0177] The content of the component (B) in the solid content of the chemically amplified positive photoresist composition is preferably 5 to 60% by weight.
[0178] <Alkali-soluble resin (C)>
[0179] In the chemically amplified positive photoresist composition of the present invention, in order to improve the resin properties of the resist, it is preferred to further contain an alkali-soluble resin (referred to as "component (C)" in this specification). As component (C), at least one selected from novolac resin, polyhydroxystyrene resin, acrylic resin and polyvinyl resin is preferred.
[0180] The content of the component (C) is preferably 5 to 95 parts by weight, more preferably 10 to 90 parts by weight, relative to 100 parts by weight of the component (B). By being 5 parts by weight or more, the resin properties of the resist can be improved, and by being 95 parts by weight or less, there is a tendency to prevent the film from being reduced during development.
[0181] <Acid diffusion control agent (D)>
[0182] In the chemically amplified positive photoresist composition of the present invention, in order to improve the resist pattern shape, post-exposure delay stability, etc., it is preferred to further contain an acid diffusion controller (D) (referred to as "component (D)" in this specification). As component (D), a nitrogen-containing compound is preferred, and an organic carboxylic acid or a phosphorus oxyacid or a derivative thereof may be further contained as needed.
[0183] The chemically amplified positive photoresist composition of the present invention may further contain an adhesion aid in order to improve adhesion to a substrate. The adhesion aid used is preferably a functional silane coupling agent.
[0184] The chemically amplified positive photoresist composition of the present invention may further contain a surfactant in order to improve coating properties, defoaming properties, leveling properties, and the like.
[0185] The chemically amplified positive photoresist composition of the present invention may further contain an acid, an acid anhydride or a high boiling point solvent in order to finely adjust the solubility in an alkaline developer.
[0186] In addition, the chemically amplified positive photoresist composition of the present invention basically does not require a sensitizer, but may contain a sensitizer as a compound to supplement sensitivity as needed. As such a sensitizer, a conventionally known sensitizer may be used, and specifically, the above-mentioned sensitizers may be mentioned.
[0187] The amount of these sensitizers used is 5 to 500 parts by weight, preferably 10 to 300 parts by weight, based on 100 parts by weight of the total weight of the sulfonium salt represented by the general formula (1).
[0188] In addition, the chemically amplified positive photoresist composition of the present invention may contain an appropriate amount of an organic solvent in order to adjust the viscosity. Specific examples of the organic solvent include the above-mentioned organic solvents.
[0189] The amount of these organic solvents used is preferably in a range where the solid content concentration is 30% by weight or more so that the thickness of the photoresist layer obtained by using the chemically amplified positive photoresist composition of the present invention (for example, by spin coating) is 5 μm or more.
[0190] The chemically amplified positive photoresist composition of the present invention can be prepared by, for example, mixing and stirring the above-mentioned components by a conventional method, and can also be dispersed and mixed using a dispersing machine such as a dissolver, a homogenizer, or a three-roll mill as required. In addition, after mixing, it can also be filtered using a mesh, a membrane filter, or the like.
[0191] The chemically amplified positive photoresist composition of the present invention is suitable for forming a photoresist layer having a film thickness of usually 5 to 150 μm, more preferably 10 to 120 μm, and even more preferably 10 to 100 μm on a support. The photoresist laminate has a photoresist layer composed of the chemically amplified positive photoresist composition of the present invention laminated on a support.
[0192] The support is not particularly limited, and any known support may be used, such as a substrate for electronic components, or a substrate on which a predetermined wiring pattern is formed on the substrate for electronic components. As the substrate, for example, a substrate made of metal such as silicon, silicon nitride, titanium, tantalum, palladium, titanium tungsten, copper, chromium, iron, aluminum, or a glass substrate may be cited. In particular, the chemically amplified positive photoresist composition of the present invention can form a resist pattern well even on a copper substrate. As the material of the wiring pattern, for example, copper, solder, chromium, aluminum, nickel, gold, or the like may be used.
[0193] The above-mentioned photoresist laminate can be manufactured, for example, in the following manner. That is, a solution of the chemically amplified positive photoresist composition prepared in the above manner is applied to a support, and the solvent is removed by heating to form a desired coating. As a method for coating on a support, spin coating, slit coating, roller coating, screen printing, applicator method and the like can be used. The pre-baking conditions of the coating of the composition of the present invention vary depending on the type of each component in the composition, the proportion, the coating film thickness, etc., as long as it is usually carried out at 70 to 150°C, preferably at 80 to 140°C for about 2 to 60 minutes.
[0194] The film thickness of the photoresist layer may generally be in the range of 5 to 150 μm, preferably 10 to 120 μm, and more preferably 10 to 100 μm.
[0195] When forming a resist pattern using the photoresist laminate obtained as described above, the obtained photoresist layer portion may be selectively irradiated (exposed) with light or radiation, such as ultraviolet rays or visible light having a wavelength of 300 to 500 nm, through a mask of a predetermined pattern.
[0196] Here, "light" is any light that activates the photoacid generator to generate acid, including ultraviolet rays, visible rays, and far ultraviolet rays. In addition, "radiation" refers to X-rays, electron beams, ion beams, etc. As the source of light or radiation, low-pressure mercury lamps, high-pressure mercury lamps, ultra-high-pressure mercury lamps, metal halide lamps, argon lasers, LED lamps, etc. can be used. In addition, the radiation exposure varies depending on the type of each component in the composition, the amount of the component, the film thickness of the coating, etc. For example, when using an ultra-high-pressure mercury lamp, the radiation exposure is 50 to 10,000 mJ / cm2 .
[0197] Then, after exposure, the acid diffusion is promoted by heating using a known method, so that the alkali solubility of the photoresist layer in the exposed part changes. Then, for example, a predetermined alkaline aqueous solution is used as a developer to dissolve and remove unnecessary parts to obtain a predetermined resist pattern.
[0198] The development time varies depending on the type and proportion of each component of the composition and the dry film thickness of the composition, and is generally 1 to 30 minutes. In addition, the development method may be any of a liquid pool method, an immersion method, a puddle method, a spray development method, etc. After development, washing with running water for 30 to 90 seconds is performed, and drying is performed using an air gun, an oven, etc.
[0199] In the non-resist part (the part removed with alkaline developer) of the resist pattern obtained in the above manner, a conductor such as metal is embedded by, for example, plating, so that connection terminals such as metal columns and bumps can be formed. It should be noted that the plating treatment method is not particularly limited, and various existing known methods can be used. As the plating solution, solder plating, copper plating, gold plating, and nickel plating solutions can be particularly preferably used. The remaining resist patterns are finally removed using a stripping solution according to a conventional method.
[0200] The chemically amplified positive photoresist composition of the present invention can also be used as a dry film. The dry film has protective films formed on both sides of the layer composed of the chemically amplified positive photoresist composition of the present invention. The film thickness of the layer composed of the chemically amplified positive photoresist composition is usually in the range of 10 to 150 μm, preferably 20 to 120 μm, and more preferably 20 to 80 μm. In addition, the protective film is not particularly limited, and a resin film used in the dry film can be used. As an example, one of them can be a polyethylene terephthalate film, and the other can be one selected from a polyethylene terephthalate film, a polypropylene film, and a polyethylene film.
[0201] The chemically amplified positive dry film as described above can be manufactured, for example, in the following manner. That is, a solution of the chemically amplified positive photoresist composition prepared in the above manner is applied to a protective film, and the solvent is removed by heating to form a desired coating film. The drying conditions vary depending on the type of each component in the composition, the proportion, the coating film thickness, etc., and can usually be carried out at 60 to 100° C. for about 5 to 20 minutes.
[0202] When forming a resist pattern using the chemically amplified dry film obtained in the above manner, one protective film of the chemically amplified positive dry film is peeled off, and the exposed surface is laminated on the support body with the exposed surface facing the support body side to obtain a photoresist layer. Then, after pre-baking to dry the resist, the other protective film can be peeled off.
[0203] On the photoresist layer obtained on the support in the above manner, a resist pattern can be formed by the same method as that described above with respect to the photoresist layer formed by coating directly on the support.
[0204] The chemically amplified negative photoresist composition of the present invention is characterized in that it contains a component (E), an alkali-soluble resin (F) and a crosslinking agent (G), wherein the above-mentioned component (E) is a compound that generates an acid when irradiated with light or radiation, namely, the photoacid generator of the present invention, and the above-mentioned alkali-soluble resin (F) has a phenolic hydroxyl group.
[0205] Alkali-soluble resin having phenolic hydroxyl groups (F)
[0206] As the "alkali-soluble resin having a phenolic hydroxyl group" (hereinafter referred to as "phenolic resin (F)") of the present invention, for example, novolac resin, polyhydroxystyrene, copolymers of polyhydroxystyrene, copolymers of hydroxystyrene and styrene, hydroxystyrene, copolymers of styrene and (meth) acrylic acid derivatives, phenol-benzenedimethanol condensation resins, cresol-benzenedimethanol condensation resins, phenol-dicyclopentadiene condensation resins, etc. can be used. Among these, novolac resin, polyhydroxystyrene, copolymers of polyhydroxystyrene, copolymers of hydroxystyrene and styrene, hydroxystyrene, copolymers of styrene and (meth) acrylic acid derivatives, and phenol-benzenedimethanol condensation resins are preferred. It should be noted that these phenolic resins (F) may be used alone or in combination of two or more.
[0207] Furthermore, the phenol resin (F) may contain a phenolic low molecular weight compound as a part of its components.
[0208] Examples of the phenolic low molecular weight compound include 4,4′-dihydroxydiphenylmethane and 4,4′-dihydroxydiphenyl ether.
[0209] Crosslinking agent (G)
[0210] The "crosslinking agent" (hereinafter, also referred to as "crosslinking agent (G)") of the present invention is not particularly limited as long as it functions as a crosslinking component (curing component) that reacts with the above-mentioned phenolic resin (F). Examples of the above-mentioned crosslinking agent (G) include compounds having at least two or more alkyl-etherified amino groups in the molecule, compounds having at least two or more alkyl-etherified benzene groups as a skeleton in the molecule, compounds containing ethylene oxide rings, compounds containing ethylene sulfide rings, compounds containing oxetane groups, compounds containing isocyanate groups (including blocked compounds), and the like.
[0211] Among these crosslinking agents (G), compounds having at least two or more alkyl-etherified amino groups and compounds containing ethylene oxide rings are preferred. Furthermore, it is more preferred to use a compound having at least two or more alkyl-etherified amino groups and a compound containing ethylene oxide rings in combination.
[0212] The amount of the crosslinking agent (G) of the present invention is preferably 1 to 100 parts by weight, more preferably 5 to 50 parts by weight, relative to 100 parts by weight of the phenolic resin (F). When the amount of the crosslinking agent (G) is 1 to 100 parts by weight, the curing reaction proceeds sufficiently, and the obtained cured product has a good pattern shape with high resolution, and is excellent in heat resistance and electrical insulation, which is preferred.
[0213] In addition, when a compound having an alkyl-etherified amino group and a compound containing an ethylene oxide ring are used together, when the total of the compound having an alkyl-etherified amino group and the compound containing an ethylene oxide ring is set to 100 weight %, the content ratio of the compound containing an ethylene oxide ring is preferably 50 weight % or less, more preferably 5 to 40 weight %, and particularly preferably 5 to 30 weight %.
[0214] In this case, the obtained cured film is excellent in chemical resistance without impairing high resolution, which is preferable.
[0215] Cross-linked microparticles (H)
[0216] The chemically amplified negative photoresist composition of the present invention may further contain crosslinked fine particles (hereinafter also referred to as "crosslinked fine particles (H)") in order to improve the durability and thermal shock resistance of the obtained cured product.
[0217] The average particle size of the crosslinked fine particles (H) is usually 30 to 500 nm, preferably 40 to 200 nm, and more preferably 50 to 120 nm.
[0218] The method for controlling the particle size of the crosslinked fine particles (H) is not particularly limited. For example, when the crosslinked fine particles are synthesized by emulsion polymerization, the number of micelles in the emulsion polymerization can be controlled by controlling the amount of the emulsifier used to control the particle size.
[0219] The average particle size of the crosslinked fine particles (H) is a value measured by diluting a dispersion of the crosslinked fine particles according to a conventional method using a light scattering flow distribution measuring apparatus or the like.
[0220] The amount of the crosslinked fine particles (H) is preferably 0.5 to 50 parts by weight, more preferably 1 to 30 parts by weight, relative to 100 parts by weight of the phenolic resin (F). When the amount of the crosslinked fine particles (H) is 0.5 to 50 parts by weight, the compatibility or dispersibility with other components is excellent, and the thermal shock resistance and heat resistance of the obtained cured film can be improved.
[0221] Sealing agent
[0222] Furthermore, the chemically amplified negative photoresist composition of the present invention may contain an adhesion aid in order to improve adhesion to a substrate.
[0223] Examples of the adhesion aid include functional silane coupling agents having a reactive substituent such as a carboxyl group, a methacrylic group, an isocyanate group, and an epoxy group.
[0224] The amount of the adhesion aid is preferably 0.2 to 10 parts by weight, more preferably 0.5 to 8 parts by weight, based on 100 parts by weight of the phenolic resin (F). When the amount of the adhesion aid is 0.2 to 10 parts by weight, the storage stability is excellent and good adhesion can be obtained, which is preferred.
[0225] Solvents
[0226] The chemically amplified negative photoresist composition of the present invention may contain a solvent in order to improve the handling properties of the resin composition or to adjust the viscosity and storage stability.
[0227] The solvent is not particularly limited, and specific examples include the solvents listed above.
[0228] The chemically amplified negative photoresist composition of the present invention may contain a sensitizer as needed. As such a sensitizer, a conventionally known sensitizer may be used, and specific examples thereof include the above-mentioned sensitizers.
[0229] The amount of these sensitizers used is 5 to 500 parts by weight, preferably 10 to 300 parts by weight, based on 100 parts by weight of the total weight of the sulfonium salt represented by the general formula (1).
[0230] In addition, the chemically amplified negative photoresist composition of the present invention may contain other additives as needed within the range that does not impair the characteristics of the present invention. Examples of such other additives include inorganic fillers, quenchers, leveling agents, surfactants, and the like.
[0231] The preparation method of the chemically amplified negative photoresist composition of the present invention is not particularly limited and can be prepared by a known method. Alternatively, the composition can be prepared by placing each component in a sample bottle, completely plugging the bottle, and stirring the bottle on a wave rotor.
[0232] The cured product of the present invention is characterized in that it is obtained by curing the chemically amplified negative photoresist composition.
[0233] The chemically amplified negative photoresist composition of the present invention has a high residual film rate and excellent resolution, and its cured product has excellent electrical insulation and thermal shock resistance. Therefore, its cured product can be used as surface protection film, planarization film, interlayer insulation film material, etc. for electronic components such as semiconductor elements and semiconductor packages.
[0234] When forming the cured product of the present invention, the chemically amplified negative photoresist composition of the present invention is first applied to a support (resin coated copper foil, copper-clad laminate, or silicon wafer with a metal sputtering film, alumina substrate, etc.), and dried to volatilize the solvent and the like to form a coating film. Then, exposure is performed through the desired mask pattern, and a heat treatment is performed (hereinafter, this heat treatment is referred to as "PEB") to promote the reaction of the phenolic resin (F) and the crosslinking agent (G). Next, development is performed using an alkaline developer to dissolve and remove the unexposed part, thereby obtaining the desired pattern. Furthermore, a heat treatment is performed to exhibit insulating film characteristics, thereby obtaining a cured film.
[0235] As a method for applying the resin composition to a support, for example, a coating method such as dipping, spraying, rod coating, roller coating or spin coating can be used. In addition, the thickness of the coating film can be appropriately controlled by adjusting the coating means, the solid content concentration of the composition solution, and the viscosity.
[0236] Examples of radiation used in exposure include ultraviolet rays, electron beams, laser beams, etc., from low-pressure mercury lamps, high-pressure mercury lamps, metal halide lamps, g-ray steppers, h-ray steppers, i-ray steppers, gh-ray steppers, ghi-ray steppers, etc. In addition, the exposure amount can be appropriately selected according to the light source used, the thickness of the resin film, etc. For example, when ultraviolet rays from a high-pressure mercury lamp are irradiated, when the thickness of the resin film is 1 to 50 μm, the exposure amount is 100 to 50,000 J / m 2 about.
[0237] After exposure, the above-mentioned PEB treatment is performed to promote the curing reaction of the phenolic resin (F) and the crosslinking agent (G) based on the generated acid. The PEB conditions vary depending on the amount of the resin composition, the thickness of the film used, etc., and are usually performed at 70 to 150°C, preferably at 80 to 120°C for about 1 to 60 minutes. Then, development is performed using an alkaline developer to dissolve and remove the unexposed parts, thereby forming the desired pattern. As the development method at this time, spray development, spray development, immersion development, immersion development, etc. can be cited. As the development conditions, it is usually performed at 20 to 40°C for about 1 to 10 minutes.
[0238] Furthermore, in order to fully exhibit the characteristics as an insulating film after development, it can be fully cured by performing a heat treatment. Such curing conditions are not particularly limited, and the composition can be cured by heating at a temperature of 50 to 250°C for about 30 minutes to 10 hours depending on the purpose of the cured product. In addition, in order to fully perform the curing or prevent the deformation of the obtained pattern shape, it can also be heated in two stages. For example, it can be heated at a temperature of 50 to 120°C for about 5 minutes to 2 hours in the first stage, and then heated at a temperature of 80 to 250°C for about 10 minutes to 10 hours to cure it. If it is such a curing condition, a general oven or infrared furnace can be used as a heating device.
[0239] Example
[0240] Hereinafter, the present invention will be specifically described with reference to Examples and Comparative Examples, but the present invention is not limited thereto. It should be noted that the part in each example represents a part by weight.
[0241] (Production Example 1) Synthesis of 4-[(2-tert-butylphenyl)thio]biphenyl
[0242] Mix 3.0 parts of 4-bromo-biphenyl, 1.9 parts of 2-tert-butylthiophenol, 1.2 parts of potassium hydroxide (purity 85%) and 7.0 parts of N-methylpyrrolidone, and stir at 120°C for 1 hour to make it uniformly dissolved. Then react at 180°C for 5 hours. After cooling the reaction solution to room temperature (about 25°C), add 7.0 parts of dichloromethane to dissolve it, and wash it with 6.5 parts of ion exchange water until the pH becomes neutral. Move the dichloromethane layer to a rotary evaporator and distill off the solvent, then add 20 parts of isopropanol and heat to 70°C to make it uniformly dissolved. Then, crystals are precipitated by cooling to room temperature. The crystals are separated by filtration to obtain 4-[(2-tert-butylphenyl)thio]biphenyl with a yield of 80%. The product is obtained by 1 Identification was performed by H-NMR.
[0243] (Production Example 2) Synthesis of 4-[(2-tert-butylphenyl)thio]benzophenone
[0244] In Preparation Example 1, except that "3.0 parts of 4-bromo-biphenyl" was changed to "3.0 parts of 4-bromobenzophenone", the same procedure as in Preparation Example 1 was carried out to obtain 4-[(2-tert-butylphenyl)thio]benzophenone with a yield of 84%. 1 Identification was performed by H-NMR.
[0245] (Production Example 3) Synthesis of 4-[(2-tert-butoxyphenyl)thio]benzophenone
[0246] In Preparation Example 2, except that "1.9 parts of 2-tert-butylthiophenol" was changed to "2.2 parts of 2-tert-butyloxythiophenol", the same procedure as in Preparation Example 2 was carried out to obtain 4-[(2-tert-butoxyphenyl)thio]benzophenone with a yield of 65%. 1 Identification was performed by H-NMR.
[0247] (Production Example 4) Synthesis of 4-[(2-trimethylsilyloxyphenyl)thio]benzophenone
[0248] In Preparation Example 2, except that "1.9 parts of 2-tert-butylthiophenol" was changed to "2.7 parts of 2-trimethylsiloxythiophenol", and "1.2 parts of potassium hydroxide (purity 85%)" was changed to "1.5 parts of potassium hydroxide (purity 85%)", the same procedure as in Preparation Example 2 was carried out to obtain 4-[(2-trimethylsiloxyphenyl)thio]benzophenone with a yield of 70%. The product was obtained by 1 Identification was performed by H-NMR.
[0249] (Production Example 5) Synthesis of 4-[(5-tert-butyl-2-methylphenyl)thio]benzophenone
[0250] In Preparation Example 2, except that "1.9 parts of 2-tert-butylthiophenol" was changed to "2.7 parts of 5-tert-butyl-2-methylthiophenol", the same procedure as in Preparation Example 2 was carried out to obtain 4-[(5-tert-butyl-2-methylphenyl)thio]benzophenone with a yield of 87%. The product was obtained by 1 Identification was performed by H-NMR.
[0251] (Production Example 6) Synthesis of 2-[(5-tert-butyl-2-methylphenyl)thio]anthraquinone
[0252] In Production Example 5, except that "3.0 parts of 4-bromobenzophenone" was changed to "3.1 parts of 2-chloroanthraquinone", the same procedure as in Production Example 5 was carried out to obtain 2-[(5-tert-butyl-2-methylphenyl)thio]anthraquinone with a yield of 68%. 1 Identification was performed by H-NMR.
[0253] (Production Example 7) Synthesis of 4-[(5-tert-butyl-2-methylphenyl)thio]phenyl phenyl sulfone
[0254] In Preparation Example 5, except that "3.0 parts of 4-bromobenzophenone" was changed to "3.0 parts of 4-bromophenyl phenyl sulfone", the same procedure as in Preparation Example 5 was carried out to obtain 4-[(5-tert-butyl-2-methylphenyl)thio]phenyl phenyl sulfone with a yield of 70%. 1 Identification was performed by H-NMR.
[0255] (Example 1) Synthesis of Compound P1-TF
[0256]
[0257] 3.0 parts of 4-[(2-tert-butylphenyl)thio]biphenyl synthesized in Preparation Example 1, 10 parts of acetonitrile, 0.04 parts of sulfuric acid and 0.40 parts of 35% aqueous hydrogen peroxide solution were uniformly mixed and reacted at 65°C for 3 hours. The reaction solution was transferred to a rotary evaporator and the solvent was distilled off to obtain a mixture of 48% of 4-[(2-tert-butylphenyl)sulfinyl]biphenyl and 52% of 4-[(2-tert-butylphenyl)thio]biphenyl. The content was calculated from the peak area ratio based on HPLC analysis of the mixture.
[0258] The mixture was dissolved in 15 parts of dichloromethane, and 1.6 parts of trifluoromethanesulfonic anhydride was added dropwise. Stirred at room temperature for 1 hour, and the reaction solution was washed with 15 parts of water. The washing operation was repeated until the pH became neutral. Then, 15 parts of hexane was added to the organic layer twice and stirred, and then the upper layer was removed after standing for 30 minutes to remove the unreacted raw materials. By transferring the lower layer to a rotary evaporator and distilling off the solvent, compound P1-TF was obtained with a yield of 55%. The product was obtained by 1 H-NMR, 19 The products were identified by F-NMR and LC-MS.
[0259] (Example 2) Synthesis of Compound P1-SB
[0260]
[0261] 1.0 part of P1-TF synthesized in Example 1 was dissolved in 5.8 parts of dichloromethane, 0.40 parts of potassium hexafluoroantimonate and 5.1 parts of ion exchange water were added thereto, and stirred at room temperature for 1 hour. The organic layer was washed 5 times with 5 parts of ion exchange water, transferred to a rotary evaporator and the solvent was distilled off, thereby obtaining P1-SB with a yield of 95%. The product was obtained by 1 H-NMR, 19 F-NMR was used for identification.
[0262] (Example 3) Synthesis of Compound P1-FP
[0263]
[0264] In Example 2, except that "0.40 parts of potassium hexafluoroantimonate" was changed to "0.65 parts of potassium tris(pentafluoroethyl)trifluorophosphate", the same procedure as in Example 2 was carried out to obtain compound P1-FP at a yield of 94%.
[0265] (Example 4) Synthesis of Compound P1-B
[0266]
[0267] In Example 2, except that "0.40 parts of potassium hexafluoroantimonate" was changed to "0.90 parts of sodium tetrakis(pentafluorophenyl)borate", the same procedure as in Example 2 was carried out to obtain compound P1-B with a yield of 95%.
[0268] (Example 5) Synthesis of Compound P1-GA
[0269]
[0270] In Example 2, except that “0.40 parts of potassium hexafluoroantimonate” was changed to “0.95 parts of sodium tetrakis(pentafluorophenyl)gallate”, the same procedure as in Example 2 was carried out to obtain compound P1-GA at a yield of 95%.
[0271] (Example 6) Synthesis of Compound P2-FP
[0272]
[0273] 3.0 parts of 4-[(2-tert-butylphenyl)thio]benzophenone synthesized in Preparation Example 2, 10 parts of acetonitrile, 0.04 parts of sulfuric acid and 0.40 parts of a 35% aqueous hydrogen peroxide solution were uniformly mixed and reacted at 65°C for 3 hours. The reaction solution was transferred to a rotary evaporator and the solvent was distilled off to obtain a mixture containing 48% of 4-[(2-tert-butylphenyl)sulfinyl]benzophenone and 52% of 4-[(2-tert-butylphenyl)thio]benzophenone. The content was calculated from the peak area ratio based on HPLC analysis of the mixture.
[0274] The mixture was dissolved in 15 parts of dichloromethane, and 1.6 parts of trifluoromethanesulfonic anhydride was added dropwise. Stir at room temperature for 1 hour, and wash the reaction solution with 15 parts of water. Repeat the washing operation until the pH becomes neutral. Next, add 2.0 parts of potassium tris(pentafluoroethyl)trifluorophosphate and 15 parts of water, and stir at room temperature for 1 hour. Repeat the operation of washing the organic layer with 15 parts of water three times. Then, add 15 parts of hexane to the organic layer twice and stir, then let it stand for 30 minutes and remove the upper layer to remove the unreacted raw materials. By transferring the lower layer to a rotary evaporator and distilling off the solvent, compound P2-FP was obtained with a yield of 65%. The product is obtained by 1 H-NMR, 19 The products were identified by F-NMR and LC-MS.
[0275] (Example 7) Synthesis of Compound P3-FP
[0276]
[0277] 2.9 parts of 4-[(2-tert-butoxyphenyl)thio]benzophenone synthesized in Preparation Example 3, 10 parts of acetonitrile, 0.04 parts of sulfuric acid and 0.39 parts of a 35% aqueous hydrogen peroxide solution were uniformly mixed and reacted at 65°C for 3 hours. The reaction solution was transferred to a rotary evaporator and the solvent was distilled off to obtain a mixture containing 47% of 4-[(2-tert-butoxyphenyl)sulfinyl]benzophenone and 53% of 4-[(2-tert-butoxyphenyl)thio]benzophenone. The content was calculated from the peak area ratio based on HPLC analysis of the mixture.
[0278] The mixture was dissolved in 15 parts of dichloromethane, and 1.6 parts of trifluoromethanesulfonic anhydride was added dropwise. Stir at room temperature for 1 hour, and wash the reaction solution with 15 parts of water. Repeat the washing operation until the pH becomes neutral. Next, add 2.0 parts of potassium tris(pentafluoroethyl)trifluorophosphate and 15 parts of water, and stir at room temperature for 1 hour. Repeat the operation of washing the organic layer with 15 parts of water 3 times. Then, add 15 parts of hexane to the organic layer twice and stir, then let it stand for 30 minutes and remove the upper layer to remove the unreacted raw materials. The lower layer was transferred to a rotary evaporator and the solvent was distilled off. The residue was separated and purified by column chromatography (eluent: ethyl acetate / hexane = 3 / 1: volume ratio), thereby obtaining compound P3-FP with a yield of 35%. The product is obtained by 1 H-NMR, 19 The products were identified by F-NMR and LC-MS.
[0279] (Example 8) Synthesis of Compound P4-FP
[0280]
[0281] 2.9 parts of 4-[(2-trimethylsiloxyphenyl)thio]benzophenone synthesized in Preparation Example 4, 10 parts of acetonitrile, 0.04 parts of sulfuric acid and 0.38 parts of a 35% aqueous hydrogen peroxide solution were uniformly mixed and reacted at 65°C for 3 hours. The reaction solution was transferred to a rotary evaporator and the solvent was distilled off to obtain a mixture containing 47% of 4-[(2-trimethylsiloxyphenyl)sulfinyl]benzophenone and 53% of 4-[(2-trimethylsiloxyphenyl)thio]benzophenone. The content was calculated from the peak area ratio based on HPLC analysis of the mixture.
[0282] The mixture was dissolved in 15 parts of dichloromethane, and 1.6 parts of trifluoromethanesulfonic anhydride was added dropwise. Stir at room temperature for 1 hour, and wash the reaction solution with 15 parts of water. Repeat the washing operation until the pH becomes neutral. Next, add 2.0 parts of potassium tris(pentafluoroethyl)trifluorophosphate and 15 parts of water, and stir at room temperature for 1 hour. Repeat the operation of washing the organic layer with 15 parts of water three times. Then, add 15 parts of hexane to the organic layer twice and stir, then let it stand for 30 minutes and remove the upper layer to remove the unreacted raw materials. The lower layer was transferred to a rotary evaporator and the solvent was distilled off. The residue was separated and purified by column chromatography (eluent: ethyl acetate / hexane = 2.5 / 1: volume ratio) to obtain compound P4-FP with a yield of 13%. The product was obtained by 1 H-NMR, 19 The products were identified by F-NMR and LC-MS.
[0283] (Example 9) Synthesis of Compound P5-FP
[0284]
[0285] 3.0 parts of 4-[(5-tert-butyl-2-methylphenyl)thio]benzophenone synthesized in Preparation Example 5, 10 parts of acetonitrile, 0.04 parts of sulfuric acid and 0.35 parts of a 35% aqueous hydrogen peroxide solution were uniformly mixed and reacted at 65°C for 3 hours. The reaction solution was transferred to a rotary evaporator and the solvent was distilled off to obtain a mixture containing 48% of 4-[(5-tert-butyl-2-methylphenyl)sulfinyl]benzophenone and 52% of 4-[(5-tert-butyl-2-methylphenyl)thio]benzophenone. The content was calculated from the peak area ratio based on HPLC analysis of the mixture.
[0286] The mixture was dissolved in 15 parts of dichloromethane, and 1.6 parts of trifluoromethanesulfonic anhydride was added dropwise. Stir at room temperature for 1 hour, and wash the reaction solution with 15 parts of water. Repeat the washing operation until the pH becomes neutral. Next, add 2.0 parts of potassium tris(pentafluoroethyl)trifluorophosphate and 15 parts of water, and stir at room temperature for 1 hour. Repeat the operation of washing the organic layer with 15 parts of water three times. Then, add 15 parts of hexane to the organic layer twice and stir, then let it stand for 30 minutes and remove the upper layer to remove the unreacted raw materials. By transferring the lower layer to a rotary evaporator and distilling off the solvent, compound P5-FP was obtained with a yield of 47%. The product is obtained by 1 H-NMR, 19 The products were identified by F-NMR and LC-MS.
[0287] (Example 10) Synthesis of Compound P6-FP
[0288]
[0289] 1.0 part of the sulfonium salt P5-FP obtained in Example 9, 4.2 parts of acetonitrile, 0.01 parts of sulfuric acid, and 0.10 parts of 35% hydrogen peroxide solution were uniformly mixed and reacted at 40°C for 3 hours. The reaction solution was cooled to room temperature, added with 10 parts of ion exchange water, and extracted with 5 parts of dichloromethane. The water layer was removed, and 10 parts of ion exchange water were added again to wash the organic layer. The washing operation was carried out until the pH became neutral, and then the organic layer was transferred to a rotary evaporator and the solvent was distilled off. The residue was separated and purified by column chromatography (eluent: ethyl acetate / hexane = 3 / 1: volume ratio), thereby obtaining compound P6-FP with a yield of 80%. The product was obtained by 1 H-NMR, 19 F-NMR and LC-MS were used for identification.
[0290] (Example 11) Synthesis of Compound P7-FP
[0291]
[0292] 1.0 part of the sulfonium salt P5-FP obtained in Example 9, 4.2 parts of acetonitrile, 0.01 parts of sulfuric acid, and 0.25 parts of 35% hydrogen peroxide solution were uniformly mixed and reacted at 80°C for 5 hours. The reaction solution was cooled to room temperature, added with 10 parts of ion exchange water, and extracted with 5 parts of dichloromethane. The water layer was removed, and 10 parts of ion exchange water were added again to wash the organic layer. The washing operation was carried out until the pH became neutral, and then the organic layer was transferred to a rotary evaporator and the solvent was distilled off. The residue was separated and purified by column chromatography (eluent: ethyl acetate / hexane = 2 / 1: volume ratio) to obtain compound P7-FP with a yield of 37%. The product was obtained by 1 H-NMR, 19 F-NMR and LC-MS were used for identification.
[0293] (Example 12) Synthesis of Compound P8-FP
[0294]
[0295] 3.0 parts of 2-[(5-tert-butyl-2-methylphenyl)thio]anthraquinone synthesized in Preparation Example 5, 20 parts of acetonitrile, 0.04 parts of sulfuric acid and 0.35 parts of 35% aqueous hydrogen peroxide solution were uniformly mixed and reacted at 65°C for 3 hours. The reaction solution was transferred to a rotary evaporator and the solvent was distilled off to obtain a mixture containing 47% of 2-[(5-tert-butyl-2-methylphenyl)sulfinyl]anthraquinone and 53% of 2-[(5-tert-butyl-2-methylphenyl)thio]anthraquinone. The content was calculated from the peak area ratio based on HPLC analysis of the mixture.
[0296] The mixture was dissolved in 15 parts of dichloromethane, and 1.6 parts of trifluoromethanesulfonic anhydride was added dropwise. Stirred at room temperature for 1 hour, and the reaction solution was washed with 15 parts of water. The washing operation was repeated until the pH became neutral. Next, 2.0 parts of tris(pentafluoroethyl) potassium trifluorophosphate and 15 parts of water were added, and stirred at room temperature for 1 hour. The operation of washing the organic layer with 15 parts of water was repeated 3 times. Then, 15 parts of toluene was added to the organic layer twice and stirred, and then the upper layer was removed after standing for 30 minutes to remove the unreacted raw materials.
[0297] The lower layer was transferred to a rotary evaporator to distill off the solvent, and 20 parts of acetonitrile, 0.04 parts of sulfuric acid, and 0.8 parts of 35% hydrogen peroxide were uniformly mixed and reacted at 80°C for 7 hours. The reaction solution was cooled to room temperature, 20 parts of ion exchange water were added, and extracted with 20 parts of dichloromethane. The water layer was removed, and 20 parts of ion exchange water were added again to wash the organic layer. This washing operation was carried out until the pH became neutral, and then the organic layer was transferred to a rotary evaporator and the solvent was distilled off. The residue was separated and purified by column chromatography (eluent: ethyl acetate / hexane = 4 / 1: volume ratio) to obtain compound P8-FP with a yield of 32%. The product was obtained by 1 H-NMR, 19 F-NMR and LC-MS were used for identification.
[0298] (Example 13) Synthesis of Compound P9-FP
[0299]
[0300] 3.0 parts of 4-[(5-tert-butyl-2-methylphenyl)thio]phenyl phenyl sulfone synthesized in Preparation Example 7, 10 parts of acetonitrile, 0.04 parts of sulfuric acid and 0.35 parts of 35% aqueous hydrogen peroxide solution were uniformly mixed and reacted at 65°C for 7 hours. The reaction solution was transferred to a rotary evaporator and the solvent was distilled off to obtain a mixture containing 48% of 4-[(5-tert-butyl-2-methylphenyl)sulfinyl]phenyl phenyl sulfone and 52% of 4-[(5-tert-butyl-2-methylphenyl)thio]phenyl phenyl sulfone. The content was calculated from the peak area ratio based on HPLC analysis of the mixture.
[0301] The mixture was dissolved in 15 parts of dichloromethane, and 1.6 parts of trifluoromethanesulfonic anhydride was added dropwise. Stir at room temperature for 2 hours, and the reaction solution was washed with 15 parts of water. Repeat the washing operation until the pH becomes neutral. Next, 2.0 parts of potassium tris(pentafluoroethyl)trifluorophosphate and 15 parts of water were added, and stirred at room temperature for 1 hour. The operation of washing the organic layer with 15 parts of water was repeated 4 times. Then, 15 parts of toluene were added to the organic layer 4 times and stirred, and then the upper layer was removed after standing for 30 minutes to remove the unreacted raw materials. By transferring the lower layer to a rotary evaporator and distilling off the solvent, compound P9-FP was obtained with a yield of 59%. The product is obtained by 1 H-NMR, 19 The products were identified by F-NMR and LC-MS.
[0302] (Comparative Example 1) Synthesis of Compound H1-TF
[0303]
[0304] 2.0 parts of 4-(phenylthio)biphenyl, 8.0 parts of acetonitrile, 0.03 parts of sulfuric acid and 0.32 parts of 35% aqueous hydrogen peroxide solution were uniformly mixed and reacted at 65°C for 3 hours. The reaction solution was transferred to a rotary evaporator and the solvent was distilled off, then dissolved in 15 parts of dichloromethane and 1.0 parts of trifluoromethanesulfonic anhydride was added dropwise. Stir at room temperature for 1 hour and wash the reaction solution with 15 parts of water. Repeat the washing operation until the pH becomes neutral. Then, 15 parts of hexane were added to the organic layer twice and stirred, and the upper layer was removed after standing for 30 minutes to remove the unreacted raw materials. Compound H1-TF was obtained by transferring the lower layer to a rotary evaporator and distilling off the solvent.
[0305] (Comparative Example 2) Synthesis of Compound H1-FP
[0306]
[0307] 2.0 parts of 4-(phenylthio)biphenyl, 8.0 parts of acetonitrile, 0.03 parts of sulfuric acid and 0.32 parts of 30% aqueous hydrogen peroxide solution were uniformly mixed and reacted at 65°C for 2 hours. After the reaction solution was transferred to a rotary evaporator and the solvent was distilled off, 6.5 parts of acetonitrile, 1.2 parts of acetic anhydride, 2.0 parts of tris(pentafluoroethyl) potassium trifluorophosphate and 0.7 parts of sulfuric acid were uniformly mixed and reacted at 60°C for 2 hours. The reaction solution was cooled to room temperature, put into 30 parts of water, extracted with 15 parts of dichloromethane, and washed with water until the pH of the aqueous layer became neutral. Then, 15 parts of hexane were added to the organic layer twice and stirred, and the upper layer was removed after standing for 30 minutes to remove the unreacted raw materials. Compound H1-FP was obtained by transferring the lower layer to a rotary evaporator and distilling off the solvent.
[0308] (Comparative Example 3) Synthesis of Compound H2-FP
[0309]
[0310] In Comparative Example 2, a compound H2-FP was obtained in the same manner as in Comparative Example 2, except that "2.0 parts of 4-(phenylthio)biphenyl" was changed to "2.0 parts of 4-(phenylthio)benzophenone".
[0311] (Comparative Example 4) Synthesis of Compound H3-FP
[0312]
[0313] 1.0 part of the compound H2-FP obtained in Comparative Example 3, 4.2 parts of acetonitrile, 0.01 parts of sulfuric acid, and 0.11 parts of 35% hydrogen peroxide water were uniformly mixed and reacted at 40°C for 3 hours. The reaction solution was cooled to room temperature, added with 10 parts of ion exchange water, and extracted with 5 parts of dichloromethane. The water layer was removed, and 10 parts of ion exchange water were added again to wash the organic layer. The washing operation was performed until the pH became neutral, and then the organic layer was transferred to a rotary evaporator and the solvent was distilled off. The residue was separated and purified by column chromatography (eluent: ethyl acetate / hexane = 3 / 1: volume ratio) to obtain compound H3-FP.
[0314] (Comparative Example 5) Synthesis of Compound H4-FP
[0315]
[0316] 1.0 parts of the compound H2-FP obtained in Comparative Example 3, 4.2 parts of acetonitrile, 0.01 parts of sulfuric acid, and 0.27 parts of 35% hydrogen peroxide water were uniformly mixed and reacted at 80°C for 5 hours. The reaction solution was cooled to room temperature, 10 parts of ion exchange water were added, and extracted with 5 parts of dichloromethane. The water layer was removed, and 10 parts of ion exchange water were added again to wash the organic layer. The washing operation was performed until the pH became neutral, and then the organic layer was transferred to a rotary evaporator and the solvent was distilled off. The residue was separated and purified by column chromatography (eluent: ethyl acetate / hexane = 2 / 1: volume ratio) to obtain compound H4-FP.
[0317] (Comparative Example 6) Synthesis of Compound H5-FP
[0318]
[0319] 2.9 parts of 2-(phenylthio)anthraquinone, 20 parts of acetonitrile, 0.04 parts of sulfuric acid and 0.35 parts of 35% aqueous hydrogen peroxide solution were uniformly mixed and reacted at 65°C for 3 hours. The reaction solution was transferred to a rotary evaporator and the solvent was distilled off to obtain a mixture containing 47% of 2-(phenylsulfinyl)anthraquinone and 53% of 2-(phenylthio)anthraquinone. The content was calculated from the peak area ratio based on HPLC analysis of the mixture.
[0320] The mixture was dissolved in 15 parts of dichloromethane, and 1.6 parts of trifluoromethanesulfonic anhydride was added dropwise. Stirred at room temperature for 1 hour, and the reaction solution was washed with 15 parts of water. The washing operation was repeated until the pH became neutral. Next, 2.0 parts of tris(pentafluoroethyl) potassium trifluorophosphate and 15 parts of water were added, and stirred at room temperature for 1 hour. The operation of washing the organic layer with 15 parts of water was repeated 3 times. Then, 15 parts of toluene was added to the organic layer twice and stirred, and then the upper layer was removed after standing for 30 minutes to remove the unreacted raw materials.
[0321] The lower layer was transferred to a rotary evaporator and the solvent was distilled off. 20 parts of acetonitrile, 0.04 parts of sulfuric acid, and 0.8 parts of 35% hydrogen peroxide were uniformly mixed and reacted at 80°C for 7 hours. The reaction solution was cooled to room temperature, 20 parts of ion exchange water were added, and extracted with 20 parts of dichloromethane. The water layer was removed, and 20 parts of ion exchange water were added again to wash the organic layer. The washing operation was performed until the pH became neutral, and then the organic layer was transferred to a rotary evaporator and the solvent was distilled off to obtain compound H5-FP.
[0322] (Comparative Example 7) Synthesis of Compound H6-FP
[0323]
[0324] 2.0 parts of 4-[(phenylthio)phenyl]phenyl sulfone, 8.0 parts of acetonitrile, 0.03 parts of sulfuric acid and 0.32 parts of 30% aqueous hydrogen peroxide solution were uniformly mixed and reacted at 65°C for 7 hours. After the reaction solution was transferred to a rotary evaporator and the solvent was distilled off, 6.5 parts of acetonitrile, 1.2 parts of acetic anhydride, 2.0 parts of tris(pentafluoroethyl) potassium trifluorophosphate and 0.7 parts of sulfuric acid were uniformly mixed and reacted at 60°C for 6 hours. The reaction solution was cooled to room temperature, poured into 30 parts of water, extracted with 15 parts of dichloromethane, and washed with water until the pH of the aqueous layer became neutral. Then, 15 parts of toluene were added to the organic layer 4 times and stirred, and the upper layer was removed after standing for 30 minutes to remove the unreacted raw materials. Compound H6-FP was obtained by transferring the lower layer to a rotary evaporator and distilling off the solvent.
[0325] [Evaluation of light absorption characteristics of sulfonium salts]
[0326] The photoacid generator (sulfonium salt) of the present invention and the photoacid generator (sulfonium salt) of the comparative example were dissolved and diluted to 0.25 mmol / L in acetonitrile (Examples A1 to A13, Comparative Examples HA1 to HA7). The solution was measured for absorbance in the range of 200 nm to 500 nm with a cell length of 1 cm using an ultraviolet-visible spectrophotometer (manufactured by Shimadzu Corporation, UV-2550). The molar absorption coefficient (ε) of i-ray (365 nm) was calculated by the following formula: 365 ), and the results are shown in Table 1.
[0327] ε 365 (L·mol -1 cm -1 )=A 365 / (0.00025mol / L×1cm)[where A 365 Indicates absorbance at 365nm.]
[0328] [Table 1]
[0329]
[0330] [Preparation and evaluation of energy-ray curable composition]
[0331] <Preparation of curable composition>
[0332] The photoacid generator (sulfonium salt) of the present invention and the photoacid generator (sulfonium salt) of the comparative example were dissolved in solvent-1 (propylene carbonate) in the amounts shown in Table 2, and then uniformly mixed with an epoxide (described below) as a cationically polymerizable compound in the amounts (parts by weight) shown in Table 2 to prepare energy-ray-curable compositions (Examples C1 to C15, Comparative Examples HC1 to HC9).
[0333] <Epoxy resin>
[0334] EP-1: 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexanecarboxylate
[0335] EP-2: 2,2-bis(4-glycidyloxyphenyl)propane
[0336] EP-3: 3-ethyl-3-{[(3-ethyloxetane-3-yl)methoxy]methyl}oxetane
[0337] [Table 2]
[0338]
[0339] It should be noted that the sulfonium salt obtained in Example 1 and Comparative Example 1 is a trifluoromethanesulfonate, and the strength of the acid generated is weaker than that of the hexafluoroantimonate, tris(pentafluoroethyl)trifluorophosphate, tetrakis(pentafluorophenyl)borate, and tetrakis(pentafluorophenyl)gallium salt obtained in Examples 2 to 13 and Comparative Examples 2 to 7, and the activity for cationic polymerization is low, so in order to be able to evaluate under the same conditions, the amount of the sulfonium salt was increased. At the same time, the amount of solvent-1 was also increased.
[0340] In addition, as can be seen from the results in Table 1, the molar absorption coefficients of the sulfonium salts obtained in Example 12 and Comparative Example 6 were large, so the amount of the sulfonium salt was reduced to allow evaluation under the same conditions. At the same time, the amount of the solvent-1 was also reduced.
[0341] <Photosensitivity (photocuring) evaluation>
[0342] The energy-ray-curable composition obtained above was applied to a polyethylene terephthalate (PET) film using an applicator (40 μm). The PET film was irradiated with ultraviolet light of a wavelength limited by a filter using an ultraviolet irradiation device. It should be noted that the filter used was L-34 (manufactured by Kenko Optical Co., Ltd., a filter that cuts off light below 340 nm). After irradiation, the hardness of the coating film after 40 minutes was measured using a pencil hardness (JIS K5600-5-4: 1999), and the evaluation was performed using the following criteria (the thickness of the coating film after curing was about 40 μm). The results are shown in Table 3. The higher the pencil hardness, the better the photocurability of the energy-ray-curable composition, that is, the polymerization initiation ability of the sulfonium salt to the cationic polymerizable compound (the photosensitivity of the sulfonium salt) is excellent.
[0343] (Evaluation Criteria)
[0344] ◎: Pencil hardness H or above
[0345] ○: Pencil hardness is HB~B
[0346] △: Pencil hardness is 2B to 4B
[0347] ×: Liquid ~ viscous, pencil hardness cannot be measured
[0348] (Ultraviolet light irradiation conditions)
[0349] Ultraviolet irradiation device: Conveyor-type UV irradiation device (manufactured by Eye Graphics Co., Ltd.)
[0350] Lamp: 1.5kW high pressure mercury lamp
[0351] Filter: L-34 (manufactured by Kenko Optical Co., Ltd.)
[0352] Illuminance (measured with a 365nm head illuminometer): 100mW / cm 2
[0353] Cumulative light intensity (measured with a 365nm probe illuminometer):
[0354] Condition 1: 100mJ / cm 2
[0355] Condition-2: 200mJ / cm 2
[0356] Condition-3: 300mJ / cm 2
[0357] [Table 3]
[0358]
[0359] In the results of Tables 1 and 3, according to the comparison of Examples C1 to C5 of the photoacid generator (sulfonium salt) with Comparative Examples HC1 to HC2, Examples C6 to C11 with Comparative Examples HC3 to HC5, Example C12 with Comparative Example HC6, Example C13 with Comparative Example HC7, Example C14 with Comparative Example HC8, and Example C15 with Comparative Example HC9, although the photoacid generator of the present invention does not have a significantly increased light absorption compared to the comparative photoacid generator, the curing performance (photosensitivity) of the cationic polymerizable compound is excellent due to the substituent A1 or A2 in the general formula (1).
[0360] [Evaluation of chemically amplified positive photoresist compositions]
[0361] <Preparation of evaluation samples>
[0362] As shown in Table 4, 1 part by weight of component (A) as a photoacid generator, 40 parts by weight of a resin represented by the following chemical formula (resin-1) as a resin component (B), and 60 parts by weight of a novolac resin obtained by addition condensation of m-cresol and p-cresol in the presence of formaldehyde and an acid catalyst as a resin component (C) were uniformly dissolved in solvent-2 (propylene glycol monomethyl ether acetate), and filtered using a membrane filter having a pore size of 1 μm to prepare a chemically amplified positive photoresist composition having a solid content concentration of 40% by weight (Examples P1 to P13).
[0363] In addition, the comparative examples were also carried out in the same manner using the blending amounts shown in Table 4 to prepare chemically amplified positive photoresist compositions (Comparative Examples HP1 to HP7).
[0364] [Table 4]
[0365]
[0366]
[0367] <Sensitivity evaluation>
[0368] After the positive resist composition prepared in the above-mentioned Examples P1 to P13 and Comparative Examples HP1 to HP7 was spin-coated on a silicon wafer substrate, it was dried to obtain a photoresist layer having a film thickness of about 20 μm. The resist layer was pre-baked at 130°C for 6 minutes using a hot plate. After pre-baking, pattern exposure (i-ray) was performed using TME-150RSC (manufactured by TOPCON), and post-exposure heating (PEB) was performed at 75°C for 5 minutes using a hot plate. Then, a 5-minute development treatment was performed by an immersion method using a 2.38 wt% tetramethylammonium hydroxide aqueous solution, and running water cleaning was performed, and nitrogen was blown to obtain a 10 μm line and space (L&S) pattern. Furthermore, the minimum exposure amount below which no residue of the pattern was confirmed was measured, that is, the minimum required exposure amount (corresponding to the sensitivity) required to form a resist pattern. The smaller the required exposure amount, the better the photoreactivity of the positive resist composition, that is, the better the photosensitivity of the sulfonium salt.
[0369] <Storage stability evaluation>
[0370] Furthermore, using the chemically amplified positive resist composition prepared above, photosensitivity was evaluated immediately after preparation and after storage at 40° C. for one month as described above, and storage stability was determined based on the following criteria.
[0371] ○: The change in sensitivity after storage at 40°C for one month is less than 5% of the sensitivity immediately after preparation.
[0372] ×: The sensitivity change after storage at 40°C for one month is 5% or more of the sensitivity immediately after preparation
[0373] <Pattern shape evaluation>
[0374] The lower side dimension La and the upper side dimension Lb of the cross-section of the 10 μm L&S pattern formed on the silicon wafer substrate by the above operation were measured using a scanning electron microscope, and the pattern shape was determined based on the following criteria.
[0375] ◎:0.90≤Lb / La≤1
[0376] ○:0.85≤Lb / La<0.90
[0377] ×: Lb / La<0.85
[0378] [Table 5]
[0379]
[0380] In the results of Table 1 and Table 5, according to the comparison of Examples P1 to P5 of the photoacid generator (sulfonium salt) with Comparative Examples HP1 to HP2, Examples P6 to P9 with Comparative Example HP3, Example P10 with Comparative Example HP4, Example P11 with Comparative Example HP5, Example P12 with Comparative Example HP6, and Example P13 with Comparative Example HP7, although the photoacid generator of the present invention does not have a significant increase in light absorption compared to the comparative photoacid generator, it has excellent photosensitivity when made into a chemically amplified positive resist by having the substituent A1 or A2 in the general formula (1).
[0381] [Evaluation of chemically amplified negative photoresist composition]
[0382] <Preparation of evaluation samples>
[0383] As shown in Table 6, 1 part by weight of the component (E) as a photoacid generator, 100 parts by weight of a copolymer (Mw=10000) composed of p-hydroxystyrene / styrene=80 / 20 (molar ratio) as a phenolic resin component (F), and hexamethoxymethylmelamine (manufactured by Sanwa Chemical Co., Ltd., trade name “Nikalac”) as a crosslinking agent, component (G) were mixed. MW-390”), 20 parts by weight of a copolymer (average particle size = 65 nm, Tg = -38°C) composed of butadiene / acrylonitrile / hydroxybutyl methacrylate / methacrylic acid / divinylbenzene = 64 / 20 / 8 / 6 / 2 (wt%) as crosslinked microparticles, i.e. component (H), and 5 parts by weight of γ-glycidoxypropyltrimethoxysilane (manufactured by Chisso, trade name "S510") as a bonding aid, i.e. component (I), were uniformly dissolved in 145 parts by weight of solvent-3 (ethyl lactate) to prepare a chemically amplified negative photoresist composition of the present invention (Examples N1 to N13).
[0384] In addition, the comparative examples were also carried out in the same manner using the blending amounts shown in Table 6 to prepare chemically amplified negative photoresist compositions (Comparative Examples HN1 to HN7).
[0385] [Table 6]
[0386]
[0387] <Sensitivity evaluation>
[0388] After each composition was spin-coated on a silicon wafer substrate, it was dried by heating at 110°C for 3 minutes using a hot plate to obtain a resin coating having a film thickness of about 20 μm. Then, a TME-150RSC (manufactured by TOPCON) was used for pattern exposure (i-ray), and a post-exposure heating (PEB) was performed at 110°C for 3 minutes using a hot plate. Then, a development treatment was performed for 2 minutes by an immersion method using a 2.38 wt % tetramethylammonium hydroxide aqueous solution, and running water cleaning was performed, and nitrogen was blown to obtain a 10 μm line and space pattern. Furthermore, the minimum required exposure (corresponding to the sensitivity) required to form a pattern with a residual film ratio of more than 95%, which represents the residual film ratio before and after development, was determined. The smaller the required exposure, the better the photoreactivity of the negative resist composition, that is, the better the photosensitivity of the sulfonium salt.
[0389] <Storage stability evaluation>
[0390] Furthermore, using the chemically amplified negative resist composition prepared above, photosensitivity was evaluated immediately after preparation and after storage at 40° C. for one month as described above, and storage stability was determined based on the following criteria.
[0391] ○: The change in sensitivity after storage at 40°C for one month is less than 5% of the sensitivity immediately after preparation.
[0392] ×: The sensitivity change after storage at 40°C for one month is 5% or more of the sensitivity immediately after preparation
[0393] <Pattern shape evaluation>
[0394] The lower side dimension La and the upper side dimension Lb of the cross-section of the 20 μm L&S pattern formed on the silicon wafer substrate by the above operation were measured using a scanning electron microscope, and the pattern shape was determined based on the following criteria.
[0395] ◎:0.90≤La / Lb≤1
[0396] ○: 0.85≤La / Lb<0.90
[0397] ×: La / Lb<0.85
[0398] [Table 7]
[0399]
[0400] In the results of Table 1 and Table 7, the comparison of Examples N1 to N5 of the photoacid generator (sulfonium salt) with Comparative Examples HN1 to HN2, Examples N6 to N9 with Comparative Example HN3, Example N10 with Comparative Example HN4, Example N11 with Comparative Example HN5, Example N12 with Comparative Example HN6, and Example N13 with Comparative Example HN7 shows that the photoacid generator of the present invention has excellent photosensitivity when made into a chemically amplified negative resist by having the substituent A1 or A2 in the general formula (1), although the light absorption is not significantly increased compared with the comparative photoacid generator.
[0401] Availability of production
[0402] The sulfonium salt of the present invention can be suitably used as a coating material, a coating agent, various coating materials (hard coatings, anti-fouling coating materials, anti-fogging coating materials, touch-resistant coating materials, optical fibers, etc.), a back treatment agent for adhesive tapes, a release coating material for release sheets for adhesive labels (release paper, release plastic film, release metal foil, etc.), a printed board, a dental material (dental compound, dental composite material), an ink, an inkjet ink, a positive resist (circuit boards, CSP, MEMS elements, etc., for connecting terminals and wiring pattern formation in the production of electronic components), a resist film, a liquid resist, a negative resist (surface protection films of semiconductor elements, etc., interlayer insulating films, planarization films, etc., permanent film materials), a resist for MEMS, a positive photosensitive material, a negative photosensitive material, various adhesives (temporary fixing agents for various electronic components, adhesives for HDDs, pickup lenses (pick up The invention also can be used as a photoacid generator in adhesives for optical lenses, adhesives for functional films for FPD (deflection plates, anti-reflection films, etc.), resins for holography, FPD materials (color filters, black matrices, partition materials, photo spacers, flanges, orientation films for liquid crystals, sealants for FPD, etc.), optical components, molding materials (building materials, optical components, lenses), casting molding materials, putty, glass fiber impregnation agents, filling materials, sealing materials, packaging materials, optical semiconductor (LED) packaging materials, optical waveguide materials, nanoimprint materials, stereolithography and microstereolithography materials, etc.
Claims
1. A sulfonium salt represented by the following general formula (1): In formula (1), R1 and R2 are independently an aryl group having 6 to 14 carbon atoms, a part of the hydrogen atoms of these aryl groups may be substituted by a substituent (t), the substituent (t) is an aryl group having 6 to 10 carbon atoms, these substituents (t) may be bonded to R1 and R2 directly through a single bond or via any of the groups represented by -SO-, -SO2- or -CO-, A1 and A2 are independently a group selected from a hydrogen atom, a tert-butyl group, a tert-butoxy group, and a trimethylsilyloxy group, wherein, A1 and A2 are not hydrogen atoms at the same time, T1 and T2 independently represent an alkyl group having 1 to 7 carbon atoms, an alkoxy group having 1 to 7 carbon atoms, a silyl group having 3 to 9 carbon atoms, or a silyloxy group having 3 to 9 carbon atoms, m1 and m2 represent the number of T1 and T2, respectively, m1 is an integer from 0 to 3, m2 is an integer from 0 to 4, L is a group represented by -O-, -S-, -SO- or -SO2-, S represents a sulfur atom, O represents an oxygen atom, C represents a carbon atom, and X - For MY a - 、(Rf) b PF 6-b - , R 3 c BY 4-c - , R 3 c GaY 4-c - , R 4 SO3 - , (R 4 SO2)3C - or (R 4 SO2)2N - wherein M represents a phosphorus atom, a boron atom, an arsenic atom or an antimony atom, Y represents a halogen atom, Rf represents an alkyl group in which 80 mol % or more of hydrogen atoms are substituted by fluorine atoms, P represents a phosphorus atom, F represents a fluorine atom, and R 3 represents a phenyl group in which at least one hydrogen atom is substituted by a halogen atom, a trifluoromethyl group, a nitro group or a cyano group, B represents a boron atom, Ga represents a gallium atom, and R 4 represents an alkyl group having 1 to 20 carbon atoms, a perfluoroalkyl group having 1 to 20 carbon atoms, or an aryl group having 6 to 20 carbon atoms, S represents a sulfur atom, O represents an oxygen atom, C represents a carbon atom, N represents a nitrogen atom, a represents an integer of 4 to 6, b represents an integer of 1 to 5, and c represents an integer of 1 to 4.
2. The sulfonium salt according to claim 1, wherein L is a group represented by -S-, -SO- or -SO2-, and R1 and R2 are the same group.
3. The sulfonium salt according to claim 1 or 2, wherein X - SbF6 - PF6 - 、BF4 - 、(CF3CF2)3PF3 - 、(CF3CF2CF2CF2)3PF3 - 、(C6F5)4B - 、(C6H5)(C6F5)3B - 、((CF3)2C6H3)4B - 、(C6F5)4Ga - 、((CF3)2C6H3)4Ga - , trifluoromethanesulfonate anion, nonafluorobutanesulfonate anion, methanesulfonate anion or benzenesulfonate anion.
4. A photoacid generator, characterized in that: Contains the sulfonium salt according to any one of claims 1 to 3. 5 . An energy-ray-curable composition comprising the photoacid generator according to claim 4 and a cationically polymerizable compound.
6. A solidified body, characterized in that: The composition is obtained by curing the energy-ray-curable composition according to claim 5.
7. A chemically amplified positive photoresist composition comprising a component (A) and a component (B), wherein the component (A) contains the photoacid generator according to claim 4, and the component (B) is a resin whose solubility in alkali increases due to the action of an acid.
8. The chemically amplified positive photoresist composition according to claim 7, wherein The component (B), which is a resin whose solubility in alkali increases due to the action of an acid, contains at least one resin selected from a novolac resin (B1), a polyhydroxystyrene resin (B2), and an acrylic resin (B3). 9 . The chemically amplified positive photoresist composition according to claim 7 , further comprising an alkali-soluble resin (C) and an acid diffusion controller (D).
10. A method for producing a resist pattern, characterized in that: include: The lamination step comprises laminating a film having a thickness of 5 to 150 nm composed of the chemically amplified positive photoresist composition according to any one of claims 7 to 9. μ m photoresist layer is stacked on a support to obtain a photoresist stack; an exposure step of selectively irradiating light or radiation to a portion of the photoresist stack; and a development step of developing the photoresist stack after the exposure step to obtain a resist pattern.
11. A chemically amplified negative photoresist composition comprising a component (E), a component (F) and a crosslinking agent component (G), wherein the component (E) comprises the photoacid generator according to claim 4, and the component (F) is an alkali-soluble resin having a phenolic hydroxyl group. 12 . The chemically amplified negative photoresist composition according to claim 11 , further comprising a crosslinked fine particle component (H).
13. A solidified body, characterized in that: The photoresist is obtained by curing the chemically amplified negative photoresist composition according to claim 11 or 12.
Citation Information
Patent Citations
JP1975151997A
Photopolymerization catalyst and curable composition containing the same
JP1990178303A
Device for forming image
JP1995329399A
Photopolymerization initiator, energy ray curing composition containing the same and its cured product
JP1996165290A
New sulfonium salt compound, polymerization initiator, curable composition containing the same compound and curing
JP1997118663A