Deposition Processes to Reduce Defects

By forming silicon oxide and silicon nitride material layers on the chamber surface, combined with flat substrate supports and bipolar electrostatic chucks, the problem of material falling during the deposition process is solved, improving the quality and adhesion of semiconductor devices, and reducing plasma Corrosion of body treatment.

CN114901859BActive Publication Date: 2024-10-18APPLIED MATERIALS INC
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202080091198.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-10-27
Publication Date
2024-10-18
Estimated Expiration
2040-10-27

AI Technical Summary

Technical Problem

During semiconductor processing, materials formed during the deposition process tend to adhere to chamber components and fall onto the substrate, causing device failure. Existing technologies are difficult to effectively solve this problem.

Method used

Silicon oxide material is first formed on the surface of the chamber, and then covered with silicon nitride material, capturing fluorine radicals and limiting their interaction with the aluminum surface, improving the adhesion of the deposited material, and through flat substrate supports and bipolar electrostatic chucks, etc. Measures to reduce falling particles.

Benefits of technology

Significantly reduces the number of dropped particles during the deposition process, improves material adhesion and substrate quality, and reduces chamber corrosion during plasma processing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114901859B_ABST
    Figure CN114901859B_ABST
Patent Text Reader

Abstract

An exemplary method of semiconductor processing may include forming a silicon oxide material on an exposed surface of a processing region of a semiconductor processing chamber. The method may include forming a silicon nitride material overlying the silicon oxide material. The method may include performing a deposition process on a semiconductor substrate disposed within a processing region of a semiconductor processing chamber. The method may include performing a chamber cleaning process.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims the benefit of priority to U.S. Patent Application No. 62 / 929,321, filed on November 1, 2019, the contents of which are incorporated herein by reference in their entirety for all purposes. Technical Field

[0003] The present technology relates to methods and components for semiconductor processing. More particularly, the present technology relates to substrate support assemblies and methods of performing deposition processes. Background Art

[0004] The fabrication of integrated circuits is made possible by creating layers of material with complex patterns on the surface of a substrate. Creating patterned material on a substrate requires controlled methods for forming and removing material. The deposition process may form material that adheres to many parts of the system. This material may fall off onto the wafer as defects after the deposition process, which, depending on the extent, may cause device failure.

[0005] Therefore, there is a need for improved systems and methods that can be used to produce high quality devices and structures. The present technology addresses these and other needs. Summary of the invention

[0006] An exemplary method of semiconductor processing may include forming a silicon oxide material on an exposed surface of a processing region of a semiconductor processing chamber. The method may include forming a silicon nitride material overlying the silicon oxide material. The method may include performing a deposition process on a semiconductor substrate disposed within a processing region of a semiconductor processing chamber. The method may include performing a chamber cleaning process.

[0007] In some embodiments, the deposition process may include a carbon-containing hard mask film. The silicon oxide material and the silicon nitride material may be formed on a substrate support within a processing region of a semiconductor processing chamber. The method may include positioning a semiconductor substrate on a substrate support before performing the deposition process. The semiconductor substrate may be located on the silicon nitride material formed on the substrate support. The chamber cleaning process may include plasma enhanced cleaning with a halogen-containing precursor. The semiconductor substrate may be disposed on a substrate support characterized by a substantially flat support surface. The substrate support may be a bipolar electrostatic chuck. The silicon oxide material may be formed to a first thickness, and the silicon nitride material may be formed to a second thickness greater than the first thickness.

[0008] Some embodiments of the present technology may encompass semiconductor processing methods. The method may include performing a chamber cleaning process in a processing region of a semiconductor processing chamber. The method may include forming a silicon oxide material on an exposed surface of a processing region of a semiconductor processing chamber. The method may include forming a silicon nitride material overlying the silicon oxide material. The method may include providing a semiconductor substrate to a substrate support located in a processing region of a semiconductor processing chamber. The method may include performing a deposition process on a semiconductor substrate.

[0009] In some embodiments, the deposition process may be a tungsten carbide hard mask film. A silicon oxide material and a silicon nitride material may be formed on a substrate support before providing the semiconductor substrate to the substrate support. The silicon oxide material may be formed to a first thickness, and the silicon nitride material may be formed to a second thickness greater than the first thickness. The first thickness may be less than or about 20 nm, and the second thickness may be greater than or about 50 nm. The substrate support may be characterized by a first surface on which the semiconductor substrate may be positioned. The first surface may be substantially flat across a diameter of the first surface. The substrate support may be a bipolar electrostatic chuck.

[0010] Some embodiments of the present technology may encompass semiconductor processing methods. The method may include forming a silicon oxide material to a first thickness on an inner surface of a processing region of a semiconductor processing chamber. The method may include forming a silicon nitride material overlying the silicon oxide material. The silicon nitride material may be formed to a second thickness greater than the first thickness. The method may include providing a semiconductor substrate to a substrate support located in a processing region of a semiconductor processing chamber. The method may include forming a tungsten-containing material on a semiconductor substrate.

[0011] In some embodiments, the method may include removing a semiconductor substrate from a semiconductor processing chamber. The method may include performing a chamber cleaning process in a processing region of the semiconductor processing chamber. The first thickness may be less than or about 20 nm, and the second thickness may be greater than or about 50 nm. The substrate support may be characterized by a first surface on which the semiconductor substrate is located. The first surface may be substantially flat, and there may be no edge ring and alignment tabs on the first surface of the substrate support. The substrate support may be a bipolar electrostatic chuck.

[0012] This technology can provide several benefits over conventional systems and techniques. For example, embodiments of the present technology can provide chamber treatments that reduce dropped particles during many deposition processes. Additionally, the present technology can reduce chamber corrosion during plasma processing. These and other embodiments, and many of their advantages and features, are described in more detail in conjunction with the following description and accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] The nature and advantages of the disclosed technology may be further understood by referring to the remaining portions of the specification and the accompanying drawings.

[0014] Figure 1 A schematic cross-sectional view of an exemplary plasma system according to some embodiments of the present technology is shown.

[0015] Figure 2 Operations in a method of semiconductor processing are illustrated in accordance with some embodiments of the present technology.

[0016] Figure 3 A schematic partial cross-sectional view of an exemplary substrate processing system according to some embodiments of the present technology is illustrated.

[0017] Several drawings are included as schematic diagrams. It should be understood that the drawings are for illustration purposes and should not be considered to be in actual size proportions unless specifically stated to be in actual size proportions. In addition, as schematic diagrams, the drawings are provided to aid understanding and may not include all aspects or information compared to actual presentation and may include content that is exaggerated for illustrative purposes.

[0018] In the drawings, similar components and / or features may have the same reference numeral. Furthermore, components of the same type may be distinguished by a letter following the reference numeral, which distinguishes similar components. If only the first reference numeral is used in the specification, the description applies to any of the similar components having the same first reference numeral, regardless of the letter. DETAILED DESCRIPTION

[0019] Plasma enhanced deposition processes may excite one or more component precursors to promote film formation on a substrate. However, the material formed may not be deposited only on the substrate. For example, material formed with an in-situ plasma may be deposited on many surfaces within the region, such as chamber walls, substrate supports, showerheads, or other components. Typically, additional cleaning operations may also be performed within the chamber, which may also be plasma-based, to remove deposited material from the surface. However, cleaning may occur after the substrate is subsequently removed from the chamber, and drop particle deposition often occurs while the substrate remains within the processing region of the chamber.

[0020] For example, in one exemplary deposition process for a hard mask material, a carbon-based material may be deposited that may also include a metal-containing material such as tungsten to produce a tungsten and carbon film. The tungsten and carbon film may also be deposited on many chamber components. The chamber components within the processing area may be aluminum in some chambers, and the adhesion of tungsten carbide may be limited. The deposited material may flake off the chamber components and fall onto the substrate. In addition, during the formation process, many particles may be trapped within the plasma. After the plasma is extinguished, the particles may fall onto the substrate.

[0021] For some processes, for example, a metal material such as tungsten may be included, for example, the metal precursor may be or include a metal halide such as a tungsten halide. During plasma deposition, a halogen component, such as fluorine, may dissociate from tungsten or metal and produce fluorine radicals. Fluorine may react with exposed aluminum surfaces of the chamber or chamber components and produce aluminum fluoride. Aluminum fluoride may desorb or sublimate from heated components and reform on cooler components within the processing area. The quality of the reformed material may be lower, with even lower adhesion levels to the deposited material, and may fall onto the substrate. Similarly, due to the deposition of material surrounding the chamber, a cleaning process may be performed after deposition. In one example, a plasma cleaning process may be performed, which may also use a halogen precursor. These precursors may also form aluminum fluoride and the challenges associated with the above. Therefore, some techniques may produce substrate films with thousands of intra-film defects.

[0022] The present technology overcomes these challenges by performing a chamber seasoning, in which silicon nitride material can be deposited on the surface of the chamber before forming a film on the substrate. For example, since silicon nitride may not be so easy to deposit on aluminum, a buffer layer of silicon oxide can be formed on aluminum first, and then silicon nitride can be formed on the oxide. Silicon nitride can capture fluorine radicals formed during processing and can limit the interaction between the generated fluorine radicals and any aluminum surface in the chamber. In addition, tungsten carbide or other materials produced during the deposition process can better adhere to silicon nitride, thereby reducing the amount of material falling onto the substrate. In some embodiments of the present technology, various aspects of the processing chamber, including substrate supports, can also be adjusted to further reduce falling particles. For example, in some embodiments, a substantially planar substrate support can be utilized, which can allow the generation of an expanded plasma space. This can extend the particles captured in the plasma to an area outside the substrate boundary, which can further reduce falling particles.

[0023] Although the remainder of the disclosure will routinely identify specific deposition processes utilizing the disclosed techniques, it will be readily appreciated that the systems and methods are equally applicable to other deposition, etching, and cleaning chambers, and processes that may occur therein. Therefore, the techniques should not be considered limited to use with only these specific deposition processes or chambers. Prior to describing additional variations and adjustments to the system in accordance with embodiments of the present technology, the present disclosure will discuss one possible chamber that may include a substrate support assembly in accordance with embodiments of the present technology.

[0024] Figure 1A schematic cross-sectional view of an exemplary processing chamber 100 according to an embodiment of the present technology is illustrated. The figure may show an overview of a system incorporating one or more aspects of the present technology, and / or a system that may be specifically configured to perform one or more operations according to an embodiment of the present technology. Additional details of the chamber 100 or the method performed may be further described below. According to some embodiments of the present technology, the chamber 100 may be used to form a film layer, although it should be understood that the method may be similarly performed in any chamber in which film formation may occur. The processing chamber 100 may include a chamber body 102, a substrate support 104 disposed within the chamber body 102, and a lid assembly 106 coupled to the chamber body 102 and enclosing the substrate support 104 in a processing volume 120. The substrate 103 may be provided to the processing volume 120 through an opening 126, which may be sealed by conventional means for processing using a slit valve or door. During processing, the substrate 103 may be located on a surface 105 of the substrate support. As indicated by arrow 145, the substrate support 104 may be rotated along an axis 147, which may be located at the location of the shaft 144 of the substrate support 104. Alternatively, the substrate support 104 may be lifted for rotation as needed during the deposition process.

[0025] A plasma profile modulator 111 may be disposed in the processing chamber 100 to control the plasma distribution on the substrate 103 disposed on the substrate support 104. The plasma profile modulator 111 may include a first electrode 108, which may be disposed adjacent to the chamber body 102 and may separate the chamber body 102 from other components of the lid assembly 106. The first electrode 108 may be part of the lid assembly 106, or may be a separate sidewall electrode. The first electrode 108 may be an annular or ring-shaped member, and may be an annular electrode. The first electrode 108 may be a continuous ring around the circumference of the processing chamber 100 surrounding the processing volume 120, or may be discontinuous at selected locations if desired. The first electrode 108 may also be a perforated electrode, such as a perforated ring or mesh electrode, or may be a flat plate electrode, such as a secondary gas distributor.

[0026] One or more isolators 110a, 110b may be a dielectric material, such as a ceramic or a metal oxide, such as aluminum oxide and / or aluminum nitride, may contact the first electrode 108 and electrically and thermally isolate the first electrode 108 from the gas distributor 112 and the chamber body 102. The gas distributor 112 may define an aperture 118 for dispensing process precursors into the processing volume 120. The gas distributor 112 may be coupled to a first power source 142, such as an RF generator, an RF power supply, a DC power supply, a pulsed DC power supply, a pulsed RF power supply, or any other power source that may be coupled to the processing chamber. In some embodiments, the first power source 142 may be an RF power supply.

[0027] The gas distributor 112 may be a conductive gas distributor or a non-conductive gas distributor. The gas distributor 112 may also be formed of conductive and non-conductive components. For example, the body of the gas distributor 112 may be conductive, while the panel of the gas distributor 112 may be non-conductive. The gas distributor 112 may be, for example, formed of Figure 1 The first power source 142 is shown to provide power, or in some embodiments, the gas distributor 112 may be grounded.

[0028] The first electrode 108 can be coupled to a first tuning circuit 128, which can control a ground path for the processing chamber 100. The first tuning circuit 128 can include a first electronic sensor 130 and a first electronic controller 134. The first electronic controller 134 can be or include a variable capacitor or other circuit element. The first tuning circuit 128 can be or include one or more inductors 132. The first tuning circuit 128 can be any circuit that achieves a variable or controllable impedance under the plasma conditions present in the processing volume 120 during processing. In some embodiments shown, the first tuning circuit 128 can include a first circuit branch and a second circuit branch coupled in parallel between ground and the first electronic sensor 130. The first circuit branch can include a first inductor 132A. The second circuit branch can include a second inductor 132B coupled in series with the first electronic controller 134. The second inductor 132B can be disposed between the first electronic controller 134 and a node connecting both the first circuit branch and the second circuit branch to the first electronic sensor 130. The first electronic sensor 130 may be a voltage or current sensor and may be coupled to a first electronic controller 134 , which may provide a degree of closed-loop control of the plasma conditions within the processing volume 120 .

[0029] The second electrode 122 may be coupled to the substrate support 104. The second electrode 122 may be embedded within the substrate support 104 or coupled to a surface of the substrate support 104. The second electrode 122 may be a plate, a perforated plate, a mesh, a wire mesh, or any other distributed arrangement of conductive elements. The second electrode 122 may be a tuning electrode and may be coupled to a second tuning circuit 136 through a conduit 146, such as a cable having a selected resistance (e.g., 50 ohms) disposed in the shaft 144 of the substrate support 104. The second tuning circuit 136 may have a second electronic sensor 138 and a second electronic controller 140, which may be a second variable capacitor. The second electronic sensor 138 may be a voltage or current sensor and may be coupled to the second electronic controller 140 to provide further control of the plasma conditions in the processing volume 120.

[0030] A third electrode 124, which may be a bias electrode and / or an electrostatic chuck electrode, may be coupled to the substrate support 104. The third electrode may be coupled to a second power source 150 through a filter 148, which may be an impedance matching circuit. The second power source 150 may be a DC power source, a pulsed DC power source, an RF bias power source, a pulsed RF power source or a bias power source, or a combination of these or other power sources. In some embodiments, the second power source 150 may be an RF bias power.

[0031] Figure 1 The lid assembly 106 and substrate support 104 of the process chamber 100 can be used with any process chamber for plasma or thermal processing. In operation, the process chamber 100 can provide real-time control of plasma conditions in the process volume 120. The substrate 103 can be placed on the substrate support 104, and the process gas can be flowed through the lid assembly 106 using the inlet 114 according to any desired flow plan. The gas can exit the process chamber 100 through the outlet 152. Electric power can be coupled to the gas distributor 112 to establish the plasma in the process volume 120. In some embodiments, the substrate can be subjected to an electrical bias using the third electrode 124.

[0032] When the plasma in the processing volume 120 is energized, a potential difference can be established between the plasma and the first electrode 108. A potential difference can also be established between the plasma and the second electrode 122. The electronic controllers 134, 140 can then be used to adjust the flow characteristics of the ground path represented by the two tuning circuits 128 and 136. Set points can be communicated to the first tuning circuit 128 and the second tuning circuit 136 to provide independent control of the deposition rate and plasma density uniformity from center to edge. In embodiments where both electronic controllers are variable capacitors, the electronic sensors can adjust the variable capacitors to independently maximize the deposition rate and minimize thickness non-uniformity.

[0033] Each of the tuning circuits 128, 136 may have a variable impedance that can be adjusted using the corresponding electronic controller 134, 140. In the case where the electronic controllers 134, 140 are variable capacitors, the capacitance range of each variable capacitor and the inductance of the first inductor 132A and the second inductor 132B may be selected to provide an impedance range. This range may depend on the frequency and voltage characteristics of the plasma, which may have a minimum value within the capacitance range of each variable capacitor. Therefore, when the capacitance of the first electronic controller 134 is at a minimum or maximum value, the impedance of the first tuning circuit 128 may be high, resulting in a plasma shape with minimal aerial or lateral coverage on the substrate support. When the capacitance of the first electronic controller 134 is close to a value that minimizes the impedance of the first tuning circuit 128, the aerial coverage of the plasma may grow to a maximum, effectively covering the entire working area of ​​the substrate support 104. When the capacitance of the first electronic controller 134 deviates from the minimum impedance setting, the plasma shape may shrink from the chamber wall and the aerial coverage of the substrate support may decrease. The second electronic controller 140 may have a similar effect, as the capacitance of the second electronic controller 140 may be varied, increasing and decreasing the air coverage of the plasma on the substrate support.

[0034] The electronic sensors 130, 138 can be used to tune the respective circuits 128, 136 in a closed loop. Depending on the type of sensor used, a set point for current or voltage can be installed in each sensor, and the sensors can be equipped with control software that determines the adjustment to each respective electronic controller 134, 140 to minimize the deviation from the set point. Thus, the plasma shape can be selected and dynamically controlled during processing. It should be understood that although the previous discussion is based on electronic controllers 134, 140 that can be variable capacitors, any electronic component with an adjustable characteristic can be used to provide an adjustable impedance for the tuning circuits 128 and 136.

[0035] Figure 2 200 according to some embodiments of the present technology. The method can be performed in various processing chambers including the processing system 100 described above. The method 200 may include a number of optional operations that may or may not be specifically related to some embodiments of the method according to the present technology. For example, many operations are described to provide a greater range of structural forms, but are not critical to the technology or can be performed by easily understood alternative methods. The method 200 may describe the use of Figure 3 It should be understood that the drawings show only partial schematic diagrams, and that the substrate support assembly may include any number of additional materials and features having the various features and aspects shown in the drawings.

[0036] Method 200 may include a processing method that can form a protective film on a surface within a substrate processing chamber before performing a deposition operation. The method may include optional operations before the method 200 begins, or the method may include additional operations. For example, method 200 may include operations performed in a different order than that shown. For example, in some embodiments, the method may be performed after a previous chamber clean. As previously described, the cleaning operation may utilize a plasma-enhanced halogen or other etchant precursor. The halogen material may interact with the aluminum chamber components as described above, which may cause aluminum fluoride to form and / or re-deposit around the processing area of ​​the chamber. In some embodiments, method 200 may include a plasma treatment, which may include a plasma-enhanced precursor that may be sent from a remote plasma unit or generated in situ in the processing area. The precursor may include, for example, a hydrogen-containing precursor, an oxygen-containing precursor, or any other precursor that may be used or promote the conversion of aluminum fluoride back to aluminum or aluminum oxide. In addition, the precursor may remove the aluminum fluoride material from the chamber.

[0037] Method 200 may then be used to generate a seasoned or treated film within the chamber. For example, an oxide material such as silicon oxide may be formed above a surface of the processing chamber at operation 205, such as a region within a processing region, such as the previously described processing volume 120. The region may be an internal plasma region, which may be at least partially defined by a plurality of chamber components. For example, chamber sidewalls, showerheads or panels, and pedestals may all be included in or at least partially define aspects of the processing region. A plasma may be formed within the processing region, and a precursor for depositing silicon oxide may be introduced. A silicon oxide film of a first thickness may be formed on the chamber surface, which may ensure a complete coating of the surface.

[0038] After forming the silicon oxide surface, method 200 may include forming a nitride material, such as silicon nitride, over the silicon oxide at operation 210. Silicon nitride may be formed to a second thickness on the silicon oxide. As previously described, the components within the processing chamber may be aluminum or include aluminum. Silicon nitride may not be easily deposited or adhered to the aluminum surface. However, silicon nitride may provide a film that resists etching under processing conditions where certain film deposition may occur. For example, in an exemplary method in which tungsten and carbon films are produced as previously described, the tungsten-containing precursor may include a tungsten halide precursor. The in-situ plasma may dissociate the precursor to form a halogen effluent that may react with unprotected aluminum. Silicon nitride may capture fluorine and may provide a better adhesion surface for tungsten and carbon films, which may reduce drop particles on the substrate. Silicon oxide may adhere better to aluminum, but may not provide sufficient adhesion for tungsten and carbon films, which may introduce additional drop particles into the substrate. Similarly, subsequent plasma cleaning may further expose the surface to fluorine, and silicon oxide may not be easily subjected to plasma treatment. Thus, the first surface layer of oxide and the second surface layer of nitride can readily adhere to chamber surfaces and can adequately withstand plasma effluents during processing to reduce or limit particles landing on the substrate.

[0039] Because the first layer and the second layer provide different benefits, the thickness of the first silicon oxide layer can be different from the thickness of the second silicon nitride layer. For example, in some embodiments, the role of silicon oxide can be to provide a complete coating on the chamber surface. Therefore, the first thickness can be defined as fully coating the chamber surface. Therefore, the first oxide layer can be characterized by a first thickness of less than or about 50nm, and can be characterized by a first thickness of less than or about 40nm, less than or about 30nm, less than or about 20nm, less than or about 10nm, less than or about 9nm, less than or about 8nm, less than or about 7nm, less than or about 6nm, less than or about 5nm, less than or about 4nm, or less. The first layer can be characterized by a thickness greater than or about 1nm or greater, which can ensure complete coverage of the inner surface. If a gap is formed in the cover layer, silicon nitride may not adhere easily, and aluminum exposure may occur.

[0040] In some embodiments, the role of silicon nitride can be to provide a resistant coating during plasma processing. Thus, in some embodiments, the second thickness can be greater than the first thickness, which can provide improved resistance, gettering, and protection from plasma effluents. For example, the second nitride layer can therefore be characterized by a second thickness greater than or about 50 nm, and can be characterized by a thickness greater than or about 60 nm, greater than or about 70 nm, greater than or about 80 nm, greater than or about 90 nm, greater than or about 100 nm, greater than or about 120 nm, greater than or about 140 nm, greater than or about 160 nm, greater than or about 180 nm, greater than or about 200 nm nm or more.

[0041] After coating or aging, the substrate may be placed in the processing area at optional operation 215. For example, during the method, the substrate support may be coated with oxides and nitrides, and the substrate may be placed on the first and second layers of the material on the substrate support. For example, the substrate may be located on a silicon nitride material formed above the substrate support. A deposition process, a removal process, or some other semiconductor process may be performed on the substrate in the processing area of ​​the chamber at operation 220. In an exemplary deposition process covered by the present technology, a carbon-containing hard mask, such as a tungsten and carbon film, may be deposited on the substrate. After processing, the substrate may be removed from the processing area at optional operation 225. Carbon materials or tungsten and carbon materials remaining in the process may have been collected on the surface of the silicon nitride. In other methods, alternative precursors may be placed on the surface protected by the silicon nitride. Therefore, in some embodiments, chamber cleaning may be performed at optional operation 230. Chamber cleaning may utilize a halogen-containing precursor, which may be plasma-enhanced in the processing area to facilitate the removal of residual materials. In some embodiments, the cleaning process may remove some or all aspects of residual tungsten and carbon materials, and may remove some or all of each layer of aged material.

[0042] The process may then be repeated for subsequent substrates. In some embodiments, the complete method may not be repeated. For example, in some processing operations, the silicon nitride material may not be completely removed over the entire processing area, so the silicon oxide material may remain intact. Therefore, in some embodiments, the method may include forming or reforming or repairing the silicon nitride film. In some embodiments, the method may be initiated with any of the operations mentioned. For example, in some embodiments, the method may start with an optional chamber clean that occurs in subsequent processing of the substrate. In some cases, the method may include performing a chamber clean and then forming an aged layer, or treating / repairing an adjustment layer. By making an aged layer as described above, tests have shown that in some processes, such as when a hard mask is formed using a tungsten-containing carbon film, the dropped particles can be removed from more than 15,000 to less than or less than 1,000. In addition, the dropped particles can be reduced to less than or about 800, less than or about 500, less than or about 400, less than or about 300, less than or about 250 or less.

[0043] Although in some embodiments of the present technology, adjustments can significantly reduce dropped particles, further reductions can be sought. For example, once deposition is complete and the plasma is extinguished, particles that may be trapped in the plasma envelope may still fall onto the substrate. Therefore, some embodiments of the present technology can modify various aspects of the processing chamber to further reduce dropped particles. Figure 3 A partial cross-sectional schematic diagram of an exemplary semiconductor processing chamber 300 is shown in accordance with some embodiments of the present technology. Figure 3 This may include the above Figure 1 One or more components discussed above may be described, and more details may be shown regarding the chamber. Chamber 300 may be used to perform semiconductor processing operations, including depositing stacks of dielectric materials, as previously described. Chamber 300 may show a partial view of a processing region of a semiconductor processing system, and may not include all components, such as the additional lid stack assembly previously described, which should be understood to be incorporated into some embodiments of chamber 300.

[0044] As mentioned above, Figure 3A portion of a processing chamber 300 may be shown. The chamber 300 may include a showerhead 305 and a substrate support assembly 310. The showerhead 305 and substrate support 310 may define, together with a chamber sidewall 315, a substrate processing region 320 in which a plasma may be generated. The substrate support assembly may include an electrostatic disc body 325, which may include one or more components embedded or disposed within the body. In some embodiments, the components incorporated in the top disc may not be exposed to the processing material and may be completely retained within the chuck body 325. The electrostatic chuck body 325 may define a substrate support surface 327 and may be characterized by a thickness, length, or diameter according to a particular geometry of the chuck body. In some embodiments, the chuck body may be elliptical and characterized by one or more radial dimensions from a central axis passing through the chuck body. It should be understood that the top chuck may be of any geometry and when radial dimensions are discussed, they may define any length from a central location of the chuck body.

[0045] The electrostatic chuck body 325 can be coupled to a rod 330, which can support the chuck body and can include channels for delivering and receiving electrical wires and / or fluid lines that can be coupled to internal components of the chuck body 325. The chuck body 325 can include associated channels or components to function as an electrostatic chuck, although in some embodiments, the components can function as or include components for a vacuum chuck or any other type of chuck system. The rod 330 can be coupled to the chuck body on a second surface of the chuck body opposite the substrate supporting surface. The electrostatic chuck body 325 can include one or more electrodes 335, which can be DC electrodes, embedded within the chuck body near the substrate supporting surface. The electrodes 335 can be discussed further below.

[0046] In operation, a substrate can be brought into at least partial contact with the substrate support surface of the electrostatic chuck body, which can create a contact gap that can substantially create a capacitive effect between the surface of the pedestal and the substrate. A voltage can be applied to the contact gap, which can create an electrostatic force for adsorption. The power supply 340 can provide charge that migrates from the electrode to the substrate support surface where it can accumulate and can create a charge layer with Coulomb attraction that has an opposite charge at the substrate and can electrostatically hold the substrate against the substrate support surface of the chuck body. Based on the finite resistance within the dielectric for a Johnsen-Rahbek type chuck, charge migration occurs when current flows through the dielectric material of the chuck body, which can be used in some embodiments of the present technology.

[0047] In some embodiments, the electrostatic chuck body 325 and / or the rod 330 may be an insulating or dielectric material. For example, oxides, nitrides, carbides, and other materials may be used to form the components. Exemplary materials may include ceramics, including aluminum oxide, aluminum nitride, silicon carbide, tungsten carbide, and any other metal or transition metal oxide, nitride, carbide, boride, or titanate, and combinations of these materials with other insulating or dielectric materials. Different grades of ceramic materials may be used to provide a composite material configured to operate within a specific temperature range, so in some embodiments, different ceramic grades of similar materials may be used for the top disk and the rod. As will be further explained below, dopants may be incorporated in some embodiments to adjust electrical properties. Exemplary dopant materials may include yttrium, magnesium, silicon, iron, calcium, chromium, sodium, nickel, copper, zinc, or any number of other elements known to be incorporated into ceramic or dielectric materials.

[0048] The electrostatic chuck body 325 may also include an embedded heater 350 housed within the chuck body. In embodiments, the heater 350 may include a resistive heater or a fluid heater. In some embodiments, the electrode 335 may function as a heater, but by decoupling these operations, more individual control may be provided and extended heater coverage may be provided while limiting the plasma formation region. The heater 350 may include a polymer heater bonded or coupled to the chuck body material, although the conductive element may be embedded within the electrostatic chuck body and configured to receive an electrical current such as an AC current to heat the top disk. The electrical current may be passed through the rod 330 through a similar channel as the DC power described above. The heater 350 may be coupled to a power source 365, which may provide electrical current to the resistive heating assembly to facilitate heating of the associated chuck body and / or substrate. In embodiments, the heater 350 may include a plurality of heaters, and each heater may be associated with a region of the chuck body, so an exemplary chuck body may include a similar number of heaters or more regions. In some embodiments, the suction mesh electrode 335 may be located between the heater 350 and the substrate supporting surface 327, and in some embodiments, a distance may be maintained between the electrode in the chuck body and the substrate supporting surface, as will be further described below.

[0049] The heater 350 may be capable of regulating the temperature on the electrostatic chuck body 325 and the substrate on the substrate support surface 327. The heater may have a range of operating temperatures to heat the chuck body and / or the substrate to greater than or about 100° C., and the heater may be configured to heat to greater than or about 125° C., greater than or about 150° C., greater than or about 175° C., greater than or about 200° C., greater than or about 250° C., greater than or about 300° C., greater than or about 350° C., greater than or about 400° C., greater than or about 450° C., greater than or about 500° C., greater than or about 550° C., greater than or about 600° C., greater than or about 650° C., greater than or about 700° C., greater than or about 750° C., greater than or about 800° C., greater than or about 850° C., greater than or equal to about 900° C., greater than or equal to about 950° C., greater than or equal to about 1000° C., or more. The heater can also be configured to operate within any range included between any two of these stated numbers, or within a smaller range included in any of these ranges.

[0050] The present technology can cover many substrate supports. In some embodiments, the substrate supports can be modified to further reduce falling particles. As described above, particles may be trapped in the formed plasma, and once the plasma is extinguished, the material may fall onto the substrate. Some substrate supports include materials that affect the formed plasma space and may constrain the plasma. For example, many substrate supports can form recessed pits on the surface of the substrate support, or edge rings can be incorporated into the substrate support. These components can both maintain the positioning of the substrate and control the space of the plasma to reduce deposition outside the radial dimension of the substrate. However, when the plasma is allowed to extend further and can extend closer to the sidewall 315, the particles can be pulled outward from the area covering the substrate and can be brought to the area radially outward from the substrate, or attracted to and / or captured in the nitride regulating film as described above.

[0051] Thus, in some embodiments, the substrate support may be characterized by a substantially flat support surface, such as surface 327, which may extend across the diameter of the substrate support and may allow for spatial expansion of plasma formed in the processing region. Thus, flat may mean that no pockets or limited pockets may be formed, and an edge ring may not be included on the substrate support. Additionally, in some embodiments, alignment tabs that may facilitate positioning and accommodation of the substrate may not be included on the substrate support.

[0052] However, by removing aspects of the substrate support that may contain the substrate, alignment challenges may arise. For example, without alignment tabs, edge rings, or recessed pockets, the substrate may move on the planar substrate support while a vacuum is being drawn within the processing chamber. In these cases, a monopolar chuck may not be able to hold the substrate. Therefore, in some embodiments, the substrate support 310 may include a bipolar chuck to ensure clamping of the substrate to limit or prevent movement along the planar support surface 327.

[0053] Any number of bipolar chuck electrode configurations may be included in the pedestal to ensure that the substrate remains chucked during processing. In one example shown, electrode 335a may be electrically coupled to power supply 340a. Additionally, electrode 335b may be electrically coupled to power supply 340b. Power supplies 340a and 340b may be configured to deliver voltages to the electrodes, and one power supply may deliver a positive voltage and one power supply may deliver a negative voltage. As described above, this may clamp the substrate in place to overcome the challenges of a monopolar chuck on a planar substrate. The gap between the two electrodes 335 may be limited to ensure uniform plasma density above the substrate.

[0054] As described above, when a seasoning material may be formed above the surface of the processing area, the substrate support may also be coated in this material. Because the substrate support may be used as an electrostatic chuck, the deposited material may affect or otherwise affect aspects of the chuck. In some embodiments, to ensure proper adsorption, the conditioning material should include and may be limited to dielectric materials to limit the possibility of short circuits or other effects. In some embodiments, the dielectric material of one or more seasoning layers may also be limited to materials that can reduce or limit leakage current through the substrate support. For example, some dielectric materials that can be effectively used as seasoning layers may include additional components such as carbon, boron, or other elements. However, these materials may add a certain amount of conductivity to the formed film. Although this is acceptable on other chamber components, on the substrate support, this may cause electrode leakage current. Therefore, in some embodiments, the seasoning material may be limited to dielectric materials, which may have reduced or limited conductivity to maintain sufficient adsorption. Therefore, in some embodiments, the seasoning material may limit or exclude conductive materials or elements.

[0055] The power supply 340 may be configured to provide energy or voltage to the conductive adsorption electrodes 335. This may be operated to form a plasma of a precursor within the processing region 320 of the semiconductor processing chamber 300, although other plasma operations may be similarly maintained. For example, each electrode 335 may be a chuck mesh used as an electrical ground for a capacitive plasma system including an RF source 307 electrically coupled to the showerhead 305. For example, the electrode 335 may serve as a ground path for the RF power from the RF source 307 while also serving as an electrical bias for the substrate to electrostatically adsorb the substrate to the substrate support surface. The power supply 340 may include a filter, a power supply, and a plurality of other electronic components configured to provide an adsorption voltage.

[0056] By including a substrate support characterized by a substantially flat surface, the fallen particles can be at least partially spread outside of the area covering the substrate. Therefore, in embodiments of the present technology, the fall of particles falling on the test substrate is further reduced to less than 200, and can be reduced to less than or about 100, less than or about 50, less than or about 45, less than or about 40, less than or about 35, less than or equal to about 30, less than or equal to about 25, less than or equal to about 20, less than or equal to about 15, less than or equal to about 10, or less. Therefore, by forming an aged layer in a processing chamber and / or utilizing a substantially flat substrate support, the fallen particles can be reduced by several orders of magnitude for processes covered by some embodiments of the present technology.

[0057] In the above description, for the purpose of explanation, various details are set forth to enhance the understanding of various embodiments of the present technology. However, it will be apparent to those skilled in the art that the implementation of a particular embodiment may not require some of these specific details (or require additional details).

[0058] After several embodiments have been disclosed, those skilled in the art will appreciate that various modifications, alternative structures and equivalents may be used without departing from the spirit of the disclosed embodiments. In addition, some well-known processes and elements are not described to avoid unnecessary obscurity of the present technology. Therefore, the above description should not be considered to limit the scope of the technology.

[0059] Where a range of values ​​is provided, it is understood that, unless the context clearly dictates otherwise, each intermediate value between the upper and lower limits of the range is also specifically disclosed, to the smallest fraction of the lower limit unit. Any narrower range between any stated value or unstated intervening value in the range and any other stated or intervening value in the range is included. The upper and lower limits of these smaller ranges may be independently included or excluded in this range, and each range in the smaller range that includes one, both, or neither of the upper and lower limits is also included in the present technology, and is subject to any specifically excluded limitations in the stated range. When the stated range includes one or both of the upper and lower limits, the range that excludes either or both of these upper and lower limits is also included.

[0060] As used in the specification and appended claims, the singular forms "a," "an," and "the" include plural referents unless the context clearly dictates otherwise. Thus, for example, reference to "a heater" includes a plurality of such heaters and reference to "the protrusion" includes reference to one or more protrusions and equivalents thereof known to those skilled in the art, and so forth.

[0061] In addition, the words “comprise(s)”, “comprising”, “contain(s)”, “containing”, “include(s)” and “including” used in this specification and the following claims are meant to specify the presence of stated features, integers, components, or operations, but they do not exclude the presence or addition of one or more other features, integers, components, operations, steps, or groups.

Claims

1. A semiconductor processing method comprising the following steps: forming a silicon oxide material on exposed surfaces of a processing region of a semiconductor processing chamber; forming a silicon nitride material covering the silicon oxide material; performing a deposition process on a semiconductor substrate disposed within the processing region of the semiconductor processing chamber, wherein the deposition process includes depositing a carbon-containing hard mask film, wherein the semiconductor substrate is disposed on a substrate support, the substrate support including a flat support surface, and wherein fewer than 200 particles fall onto the semiconductor substrate; and A chamber cleaning process is performed.

2. The semiconductor processing method of claim 1, wherein the silicon oxide material and the silicon nitride material are formed on the substrate support within the processing region of the semiconductor processing chamber.

3. The semiconductor processing method according to claim 2, further comprising the following steps: The semiconductor substrate is positioned on the substrate support before performing the deposition process, wherein the semiconductor substrate is positioned on the silicon nitride material formed on the substrate support.

4. The semiconductor processing method of claim 1, wherein the chamber cleaning process comprises plasma enhanced cleaning using a halogen-containing precursor.

5. The semiconductor processing method of claim 1, wherein the substrate support comprises a bipolar electrostatic chuck. 6 . The semiconductor processing method of claim 1 , wherein the silicon oxide material is formed to a first thickness, and wherein the silicon nitride material is formed to a second thickness greater than the first thickness.

7. A semiconductor processing method comprising the following steps: performing a chamber cleaning process in a processing region of a semiconductor processing chamber; forming a silicon oxide material on exposed surfaces of the processing region of the semiconductor processing chamber; forming a silicon nitride material covering the silicon oxide material; providing a semiconductor substrate to a substrate support located in the processing region of the semiconductor processing chamber, wherein the substrate support is characterized by a first surface, the semiconductor substrate is located on the first surface, and wherein the first surface is substantially flat across a diameter of the first surface; and A deposition process is performed on the semiconductor substrate, wherein the deposition process includes depositing a tungsten carbide hard mask film, and wherein fewer than 200 particles fall onto the semiconductor substrate. 8 . The semiconductor processing method of claim 7 , wherein the silicon oxide material and the silicon nitride material are formed on the substrate support before the semiconductor substrate is provided to the substrate support.

9. The semiconductor processing method of claim 7, wherein the silicon oxide material is formed to a first thickness of less than or about 20 nm, and wherein the silicon nitride material is formed to a second thickness of greater than or about 50 nm.

10. A semiconductor processing method comprising the following steps: forming a silicon oxide material to a first thickness on an inner surface of a processing region of a semiconductor processing chamber; forming a silicon nitride material covering the silicon oxide material, wherein the silicon nitride material is formed to a second thickness, and the second thickness is greater than the first thickness; providing a semiconductor substrate to a substrate support located in the processing region of the semiconductor processing chamber, wherein the substrate support is characterized by a first surface, the semiconductor substrate is located on the first surface, and wherein the first surface is substantially flat and is free of edge rings and alignment tabs on the first surface of the substrate support; and A tungsten-containing material is formed on the semiconductor substrate.

11. The semiconductor processing method according to claim 10, further comprising the following steps: removing the semiconductor substrate from the semiconductor processing chamber; and A chamber cleaning process is performed in the processing region of the semiconductor processing chamber.

Citation Information

Patent Citations

  • A-si seasoning effect to improve sin run-to-run uniformity

    US20120040536A1

  • Boron doped tungsten carbide for hardmask applications

    US20180218902A1