A design method for super solid solution heat-resistant magnesium rare earth alloy based on non-equilibrium solidification
By designing multi-element synergistic alloys in magnesium alloys, optimizing the solid solubility and second phase melting point, and using laser selective melting technology, the problem of poor performance of magnesium alloys at high temperatures has been solved, and high-temperature mechanical properties have been improved and improvements in additive manufacturing have been achieved. No cracks required.
Patent Information
- Application Number
- CN202210648731.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-06-09
- Publication Date
- 2024-10-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Magnesium alloys have fast atomic diffusion at high temperatures, the matrix is easy to slip, and the second phase is unstable, which limits its application as high-temperature structural components. It is also difficult to prepare magnesium alloy parts with good high-temperature mechanical properties using traditional manufacturing methods.
Adopting a super-solid solution heat-resistant rare earth magnesium alloy design method based on non-equilibrium solidification, by selecting appropriate multi-element synergistic alloy design elements, calculating the alloy thermal sensitivity index and critical temperature range, optimizing solid solubility, second phase melting point and grain boundaries Strengthen, construct Mg-X-M-N multi-component synergistic alloy system, and use laser selective melting technology to achieve high-temperature performance improvement.
The high-temperature mechanical properties of the magnesium alloy are improved, ensuring that it is crack-free during additive manufacturing, meets high density requirements, and is suitable for laser selective melting manufacturing processes.
Smart Images

Figure CN114918430B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of alloy design, and relates to a design method of a super solid solution heat-resistant rare earth magnesium alloy based on non-equilibrium solidification. Background Art
[0002] As one of the lightest metal structural materials, magnesium alloy has a density only equivalent to that of engineering plastics, but its strength and stiffness are much higher than those of engineering plastics, so it has attracted widespread attention from researchers. In the past few decades, magnesium alloys have been widely used in aerospace, weapons and equipment, transportation and other fields that pursue lightweight. However, the poor high-temperature mechanical properties of magnesium alloys have always been a key issue limiting their application as high-temperature structural components.
[0003] Due to their unique physical and chemical properties, rare earth elements have slow atomic diffusion in the magnesium matrix and can form high-melting-point precipitates and intermetallic compounds, which can improve the high-temperature service performance of magnesium alloys. Among them, the WE series of rare earth alloys, which are mainly formed by adding Y / Gd and combined with other beneficial elements, have significant advantages in high-temperature mechanical properties. However, conventional solidification methods such as powder metallurgy, stirring casting and spray deposition have certain limitations in the solid solution of rare earth elements in the matrix, and the formation of stable second phases is limited. Therefore, it is difficult to prepare magnesium alloy parts with good high-temperature mechanical properties.
[0004] Laser additive manufacturing technology, due to its instantaneous solidification speed, can significantly change the solute supersaturation, phase formation and element diffusion segregation behavior of the forming material compared to traditional forming manufacturing technology, thereby affecting its mechanical toughening mechanism and is expected to improve the high-temperature performance of the alloy. Among them, selective laser melting technology is a type of laser additive manufacturing, which uses CAD / CAE software for modeling and slices the complex model in the software. Each slice contains all the geometric information of the slice layer, and the file is saved in STL format and then imported into the printing device. The metal powder is melted layer by layer with a high-energy laser beam until a complete part is finally formed.
[0005] In summary, magnesium alloy is one of the lightest metal structural materials, and lightweight structural parts made of this material will bring huge weight reduction benefits. However, magnesium alloy has fast atomic diffusion, easy matrix slip, and unstable second phase at high temperature, which seriously limits its application as high-temperature structural parts. In addition, it is difficult to prepare magnesium alloy parts with good high-temperature mechanical properties using traditional manufacturing methods, while selective laser melting has great potential in improving the high-temperature mechanical properties of alloys due to its faster cooling rate. However, the mechanical behavior, grain and precipitation phase strengthening mechanism of magnesium alloys under non-equilibrium solidification conditions are different from those in the equilibrium state. When the magnesium alloy designed by the method in the prior art is applied to selective laser melting manufacturing, due to the lack of targeted performance enhancement, problems such as high-temperature mechanical properties cannot meet expectations and cracks are prone to occur. Summary of the invention
[0006] In view of this, the present invention provides a design method of a super solid solution heat-resistant rare earth magnesium alloy based on non-equilibrium solidification to solve the problem that the magnesium alloy designed in the prior art is not suitable for additive manufacturing and has poor high-temperature mechanical properties.
[0007] The method comprises:
[0008] Step 1: Select appropriate elements as multi-element synergistic alloy design elements with the design goal of achieving solid solution strengthening, second phase strengthening and grain boundary strengthening of magnesium alloy under high temperature conditions;
[0009] Step 2: Based on the characteristics of instantaneous non-equilibrium solidification in laser selective melting, the influence of the mass fraction of the selected synergistic alloy design elements on the thermal sensitivity index and critical temperature range of the alloy is calculated, and the optimal alloying composition range of each element is determined with the goal of minimizing the thermal sensitivity index and critical temperature range of the alloy.
[0010] Furthermore, the design goal of the solid solution strengthening under high temperature conditions is a higher solid solubility;
[0011] Furthermore, the design goal of the second phase strengthening is a higher high temperature resistant second phase melting point;
[0012] Furthermore, the design goal of the grain boundary strengthening is to have a larger second phase lattice constant and atomic bond slip resistance, as well as higher phase stability.
[0013] Furthermore, step 1 includes, in combination with the magnesium alloy phase diagram, selecting a plurality of candidate main rare earth elements X with the goal of having high solid solubility;
[0014] Combining the solubility curve of rare earth elements and the phase diagram of magnesium alloys, multiple candidate synergistic rare earth elements M are selected with the design goal of being beneficial to high temperature resistance but having limited solid solubility performance;
[0015] and, selecting a plurality of candidate modifying elements N with the goal of benefiting the precipitation of a high temperature resistant second phase;
[0016] Construct Mg-XM.-N multi-component synergistic alloying candidate system.
[0017] Preferably, the candidate main rare earth elements X include Gd and Y.
[0018] Preferably, the candidate synergistic rare earth elements M include Nd, Ce, and Sm.
[0019] Preferably, candidate modifying elements N include Zr, Zn, Ca.
[0020] Furthermore, step 1 also includes:
[0021] A typical WE series rare earth magnesium alloy model was established to simulate the time-temperature curve of the melting process of WE series rare earth magnesium alloy by laser selective melting rapid forming;
[0022] Based on the time-temperature curve of the melting process, the alloy solidification range, element solubility change curve and high-temperature resistant second phase melting point corresponding to each candidate X element after adding different contents of each candidate X element to Mg under Scheil-Gulliver non-equilibrium solidification conditions are calculated;
[0023] Select one of the candidate main rare earth elements X as the main rare earth element by satisfying the following criteria simultaneously or as much as possible: large solid solubility of the element, narrow alloy solidification range, and high melting point of the high temperature resistant second phase;
[0024] Similarly, different candidate synergistic rare earth elements M are added to the selected Mg-X alloy to perform the same calculation and selection, and the final element M is selected from the candidate synergistic rare earth elements M;
[0025] If more than one element meets two or three conditions at the same time during the selection of element M, the element is selected according to the weight of element solid solubility > high temperature resistant second phase melting point > alloy solidification range.
[0026] Furthermore, the standard WE series rare earth magnesium alloy is Mg-3.77Y-2.46Nd-1.23Gd-0.21Zn-0.4Zrwt(%) alloy.
[0027] Furthermore, in step 1, based on the selected Mg-XM alloy, VASP (Vienna Ab-initioSimulation Package) is used to calculate the effect of adding different candidate modifying elements N on the second phase lattice constant, phase structure stability and atomic bond slip resistance of the prepared alloy;
[0028] The final element N is selected from the candidate modifying elements N based on the criteria of simultaneously or as much as possible satisfying the second phase lattice constant, strong phase stability, and large atomic bond slip resistance;
[0029] If more than one element meets two or three conditions at the same time during the selection of N elements, the elements are selected according to the weight of atomic bond slip resistance > phase stability > second phase lattice constant.
[0030] Further, in step 2, first, the solid fraction f of the alloy formed by the main rare earth element X and Mg with different mass fractions during solidification is calculated. s As the temperature T changes, the Tf corresponding to each mass fraction is then plotted. s 1 / 2 curve;
[0031] Select the element mass fraction corresponding to the curve that meets the following conditions as the mass fraction of the main rare earth element X:
[0032] ① Arrive at T on the curve E = f at 568°C s 1 / 2 <0.99;
[0033] ②At temperature T E The absolute value of the slope at the thermal sensitivity index |dT / d(f s ) 1 / 2 |It is the minimum value relative to other curves;
[0034] ③Critical temperature range ΔT CTR It is the minimum value relative to other curves;
[0035] The critical temperature range ΔT CTR f is the curve s 1 / 2 = 0.31 and f s 1 / 2 =0.99 of the temperature difference corresponding to the point.
[0036] Secondly, according to the same idea, with 0.5wt% as the minimum value and 15wt% minus the mass fraction of the selected element Y as the maximum value, the thermal sensitivity index and critical temperature range of various Mg-XM alloys with different contents of the synergistic rare earth element M were sampled and calculated to determine the composition range of the element M, where the mass fraction of the main rare earth element X is the mass fraction selected above, and the rest of the alloy is Mg;
[0037] Finally, by analogy, with 0.5wt% as the minimum value and 15wt% as the maximum value, the thermal sensitivity index and critical temperature range of various Mg-XMN alloys with different N contents are sampled and calculated to determine the composition range of element N, wherein the mass fractions of the main rare earth element X and the synergistic rare earth element M are the mass fractions selected previously, and the rest of the alloy is Mg;
[0038] In the above selections, if two curves meet the thermal sensitivity index |dT / d(f s ) 1 / 2 |Minimum and critical temperature range ΔT CTR The minimum standard is to set the coefficient K = f s 1 / 2 (T=TE) / ΔT CTR , select the element mass fraction corresponding to the curve with the largest K value.
[0039] The beneficial effect of the present invention lies in that, in view of the problem that there is no clear and calculable specific parameter design target for improving high-temperature mechanical properties in the non-equilibrium supersolid solution synergistic alloying design of rare earth magnesium alloy under laser rapid solidification, and the high-temperature mechanical properties of the blindly designed alloy are poor, a new strengthening mechanism is proposed, namely, the solid solubility strengthening, second phase strengthening (melting point) and grain boundary strengthening (second phase lattice constant, phase structure stability (formation heat and binding energy), atomic bond slip resistance) of the magnesium alloy under high temperature conditions, so as to achieve the improvement of high-temperature mechanical properties. Firstly, rare earth elements and modifying elements are selected based on the magnesium alloy phase diagram, and the influence of the selected elements on the solidification parameters and thermophysical parameters of the alloy is calculated under non-equilibrium conditions, and the alloying design criteria of the magnesium alloy are established, so as to obtain the optimal alloying composition range, so that the designed alloy is suitable for the selective laser melting manufacturing process. The strengthening target selected by this method makes the designed alloy have excellent high-temperature performance. At the same time, the optimal alloying composition range is determined by minimizing the alloy thermal sensitivity index and critical temperature range, making the designed alloy more suitable for laser selective melting, a manufacturing process with the characteristics of instantaneous non-equilibrium solidification, and can meet the requirements of high density and crack-free in additive manufacturing. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1 This is a flow chart for preliminary screening of alloying elements in an embodiment of the present invention.
[0041] Figure 2 Part (a) is a schematic diagram of a typical WE series rare earth magnesium alloy model used for finite element temperature field simulation in an embodiment of the present invention, and part (b) is a time-temperature curve of the typical WE series rare earth magnesium alloy melting process simulated in an embodiment of the present invention.
[0042] Figure 3 Graphs showing the solidification characteristics of the alloy calculated in the embodiment of the present invention, wherein part (a) is a graph showing the solidification range of the alloy under Scheil non-equilibrium solidification conditions and the rare earth second phase content as a function of the mass fraction of the rare earth alloying element Y or Gd; and part (b) is a graph showing the change in the solid solubility of the alloying elements after changing the content of the Y or Gd element in pure Mg.
[0043] Figure 4 This is a comparison diagram of T-fs1 / 2 curves of alloys formed by adding different mass fractions of Y element to Mg in an embodiment of the present invention. DETAILED DESCRIPTION
[0044] The technical scheme of the present invention will be further described in detail below in conjunction with specific embodiments. It should be understood that the following embodiments are only exemplary descriptions and explanations of the present invention and should not be construed as limiting the scope of protection of the present invention. All technologies implemented based on the above content of the present invention are included in the scope that the present invention is intended to protect.
[0045] The design method in this embodiment includes step 1, selecting appropriate elements as multi-component synergistic alloy design elements with the design objectives of solid solution strengthening, second phase strengthening and grain boundary strengthening of magnesium alloy under high temperature conditions;
[0046] Step 2: Based on the characteristics of instantaneous non-equilibrium solidification of laser selective melting, the influence of the selected same alloy design elements on the alloy thermal sensitivity index and critical temperature range is calculated, and the optimal alloying composition range is determined with the goal of minimizing the alloy thermal sensitivity index and critical temperature range.
[0047] Specifically, in this embodiment, the alloying elements are first preliminarily selected. The process is basically as follows: Figure 1 As shown in the figure; according to the magnesium alloy phase diagram, with high solid solubility as the goal, the commonly used Mg-Gd / Y-based rare earth magnesium alloy is firstly designed, that is, Gd and Y are selected as the candidate main rare earth elements X, and then based on the rare earth element solubility curve and the magnesium alloy phase diagram, the commonly used high temperature beneficial but solid solubility limited candidate rare earth elements M, such as Nd, Ce, Sm, etc. are screened; secondly, based on the design principle of precipitating a high temperature resistant second phase, the beneficial candidate modifying elements N, such as Zr, Zn, Ca, etc. are screened to construct a Mg-XM.-N multi-component synergistic alloying system.
[0048] Next, in this embodiment, it is necessary to calculate the influence of alloy elements on the alloy solidification characteristics and thermophysical properties.
[0049] Firstly, the finite element temperature field simulation was used to simulate the time-temperature curve of the melting process of WE series rare earth magnesium alloy by laser selective melting rapid forming.
[0050] In this example, using Figure 2 The model shown in simulates the time-temperature curve of the solidification process of Mg-3.77Y-2.46Nd-1.23Gd-0.21Zn-0.4Zrwt(%) alloy. Since it is typical among magnesium alloys, this curve can be extended to this embodiment and used as a unified time-temperature curve of the solidification process for further calculations. Figure 1 Part a is a laser selective melting model of a single-layer multi-pass magnesium alloy. A laser heat source with Gaussian distribution is used as the incident heat source. The process parameters include laser scanning speed 1000mm / s, scanning spacing 70um, power 125W, and laser spot radius 0.04mm. Place a point probe at (250, 800, 35) of the model to obtain the temperature curve at that point, as shown in Figure 1. Figure 1 As shown in part b, in the additive manufacturing process, the entire process from melting to solidification of the material is within 0.3ms, which is a typical non-equilibrium solidification.
[0051] Under this melting process time-temperature curve, the temperature corresponding to each time point in the solidification process can be obtained. Considering the diffusion behavior of multi-component magnesium alloys, the time and temperature are matched one by one and imported into the Thermo-Calc software package, and then the Scheil-Gulliver non-equilibrium solidification calculation module in the software is combined to calculate the solidification characteristics of the alloy elements, including element solubility, alloy solidification range and high temperature resistant second phase types;
[0052] Figure 3 That is, the calculation results of adding different mass fractions of Gd or Y into pure magnesium. According to the high temperature strengthening principle of magnesium alloy, the elements that simultaneously or as much as possible meet the requirements of large element solid solubility, narrow alloy solidification range, and high melting point of high temperature resistant second phase are selected. Figure 2 From a and b, we can see that the Y element satisfies both the narrow solidification range of the alloy and the second phase Mg 24 The melting point of Y5 (848.44K) is higher than the melting point of the second phase Mg5Gd (805.02K), so the Y element is selected.
[0053] Similarly, different candidate M elements can be added to the Mg-Y alloy for calculation and finally determine the M element. If more than one element meets two or three conditions at the same time during the selection of the M element, the element is selected according to the weight of element solid solubility > high temperature resistant second phase melting point > alloy solidification range.
[0054] Then, the VASP (Vienna Ab-initio Simulation Package) first-principle software was used to establish a 3×3×2 Mg alloy (hcp) supercell model with 36 atoms, and the multi-component magnesium rare earth alloy model was established by the substitution method. The exchange correlation between electrons was treated by the Perdew-Burke-Ernzerhof functional and the generalized gradient approximation. The Brillouin zone K point was divided into 5×5×4 Monkhorst-Pack grids, and the plane wave cutoff energy was set to 520 eV. The total energy error of the system convergence was less than 1×10 -5 eV. The influence of alloying elements on the thermophysical properties is calculated, including the second phase lattice constant, phase structure stability (formation heat and binding energy), and atomic bond slip resistance. Similarly, according to the high temperature strengthening principle of magnesium alloys, elements that simultaneously or as many as possible meet the requirements of large second phase lattice constant, strong phase stability, and large atomic bond slip resistance are selected. If more than one element meets two or three conditions at the same time during the selection of N elements, the elements are selected according to the weight of atomic bond slip resistance>phase stability>second phase lattice constant.
[0055] Next, in this example, the composition content of the selected elements is changed, and the crack tendency of the rare earth magnesium alloy in laser selective melting is calculated by combining thermodynamic modeling and first-principles calculation to evaluate the formability of laser selective melting. In this example, the thermal sensitivity index (|dT / d(f s ) 1 / 2 |) and critical temperature range (ΔT CTR ) are used as indicators to evaluate the sensitivity of alloying design element composition to printing hot cracking.
[0056] First, for the selected main rare earth element Y, the Scheil-Gulliver non-equilibrium solidification module is executed using thermo-calc to calculate the solid fraction (f s ) changes with temperature (T), and then plots the Tf corresponding to each content s 1 / 2 Curve. When f s 1 / 2 When it is equal to 0.99, the alloy is fully solidified (no longer relevant after exceeding 0.99), so only the temperature reaching T is considered. E =568℃f s 1 / 2 <0.99 curve (T E Point at f s 1 / 2 =0.99 before the vertical line). The thermal sensitivity index (|dT / d(f s) 1 / 2 |) can be expressed as the temperature of the point on the curve is T E The absolute value of the slope at s ) 1 / 2 | will result in a smaller crystal growth rate and more liquid at the grain boundaries, thus reducing crack resistance. In summary, the curve reaches T E f at temperature s 1 / 2 <0.99 and at T E The element mass fraction corresponding to the curve whose absolute value of slope is the minimum relative to other curves is the mass fraction of the selected element Y; for example, Figure 4 The Tf of various alloys formed by sampling with a starting point of 1wt% and an end point of 5wt% in pure Mg with a step length of 0.5wt% during solidification s 1 / 2 According to the above selection criteria, the mass fraction of Y element should be selected as 5%. CTR Similarly, Tf s 1 / 2 Figure obtained, ΔT CTR is the curve f s 1 / 2 = 0.31 and f s 1 / 2 = 0.99 of the temperature difference. CTR The higher the value of , the longer the alloy spends in the crack-sensitive stage, and the higher the shrinkage strain is, the less favorable the crack resistance is. CTR The curve with the minimum value relative to other curves is the selected content. Figure 3 As shown in , according to this principle, the mass fraction of Y element in pure magnesium should be selected to be 5%.
[0057] At the same time, considering the economic cost, according to the principle that the mass fraction of the total amount of rare earth elements in the alloy does not exceed 15%, according to the same idea, with 0.5wt% as the minimum value, 15wt% minus the mass fraction of the selected element Y as the maximum value, and 0.5wt% as the step length, the thermal sensitivity index and critical temperature range of various Mg-XM alloys with different contents of the synergistic rare earth element M are sampled and calculated to determine the composition range of the element M, wherein the mass fraction of the main rare earth element X is the mass fraction selected above, and the rest of the alloy is Mg;
[0058] Finally, by analogy, with 0.5wt% as the minimum value and 15wt% as the maximum value, the thermal sensitivity index and critical temperature range of Mg-XMN alloys with different element N contents are sampled and calculated to determine the composition range of element N, where the mass fractions of the main rare earth element X and the synergistic rare earth element M are the mass fractions selected previously, and the rest of the alloy is Mg.
[0059] If two curves (different components) appear when selecting components, they satisfy |dT / d(f s ) 1 / 2 |Minimum and ΔT CTR When the minimum standard is used, the coefficient K is set to f s 1 / 2 (T=TE) / ΔT CTR , the curve with the largest K value is the selected component.
[0060] The method in this embodiment is based on the strengthening mechanism of solid solution strengthening, second phase strengthening (melting point) and grain boundary strengthening (second phase lattice constant, phase structure stability (formation heat and binding energy), atomic bond slip resistance) of magnesium alloy under high temperature conditions, and uses thermo-calc combined with the first principle calculation software VASP to select elements that are beneficial to magnesium alloy at high temperature. At the same time, in order to make the designed alloy meet the standard of high density and crack-free additive manufacturing, the thermal sensitivity index |dT / d(f s ) 1 / 2 | and critical temperature range ΔT CTR As an indicator to evaluate the sensitivity of alloying design element composition to printing hot cracks, the optimal composition range of the selected elements can be determined. Ensure that the designed alloy is suitable for non-equilibrium solidification conditions of additive manufacturing and has good high temperature performance.
Claims
1. A design method for a super solid solution heat-resistant rare earth magnesium alloy based on non-equilibrium solidification, characterized in that: include: Step 1: Select appropriate elements as multi-element synergistic alloy design elements with the design goal of achieving solid solution strengthening, second phase strengthening and grain boundary strengthening of magnesium alloy under high temperature conditions; The design goal of the second phase strengthening is a higher high temperature resistant second phase melting point; The design goal of the grain boundary strengthening is to have a larger second phase lattice constant and atomic bond slip resistance, as well as higher phase stability; Combined with the magnesium alloy phase diagram, multiple candidate main rare earth elements X are selected with the goal of having high solid solubility; Combining the solubility curve of rare earth elements and the phase diagram of magnesium alloys, multiple candidate synergistic rare earth elements M are selected with the design goal of being beneficial to high temperature resistance but having limited solid solubility performance; and, selecting a plurality of candidate modifying elements N with the goal of benefiting the precipitation of a high temperature resistant second phase; Construct Mg-XM.-N multi-component synergistic alloying candidate system; A typical WE series rare earth magnesium alloy model was established to simulate the time-temperature curve of the melting process of WE series rare earth magnesium alloy by laser selective melting rapid forming; Based on the time-temperature curve of the solidification process, the alloy solidification range, element solubility change curve and high-temperature resistant second phase melting point corresponding to each candidate X element after adding different contents of each candidate X element to Mg under Scheil-Gulliver non-equilibrium solidification conditions are calculated; Select one of the candidate main rare earth elements X as the main rare earth element by satisfying the following criteria simultaneously or as much as possible: large solid solubility of the element, narrow alloy solidification range, and high melting point of the high temperature resistant second phase; Similarly, different candidate synergistic rare earth elements M are added to the selected Mg-X alloy to perform the same calculation and selection, and the final element M is selected from the candidate synergistic rare earth elements M; If more than one element meets two or three conditions at the same time during the selection of element M, the element is selected according to the weight of element solid solubility > high temperature resistant second phase melting point > alloy solidification interval; Based on the selected Mg-XM alloy, VASP was used to calculate the effect of adding different candidate modifying elements N on the second phase lattice constant, phase structure stability and atomic bond slip resistance of the prepared alloy; The final element N is selected from the candidate modifying elements N based on the criteria of simultaneously or as much as possible satisfying the second phase lattice constant, strong phase stability, and large atomic bond slip resistance; If more than one element satisfies two or three conditions at the same time during the selection of N elements, the element is selected according to the weight of atomic bond slip resistance > phase stability > second phase lattice constant; Step 2: Based on the characteristics of instantaneous non-equilibrium solidification of laser selective melting, the influence of the mass fraction of the selected synergistic alloy design elements on the alloy thermal sensitivity index and critical temperature range is calculated, and the optimal alloying composition range of each element is determined with the goal of minimizing the alloy thermal sensitivity index and critical temperature range; First, calculate the solid fraction f of the alloy formed by the main rare earth element X and Mg with different mass fractions during solidification. s As the temperature T changes, the Tf corresponding to each mass fraction is then plotted. s 1 / 2 curve; Select the element mass fraction corresponding to the curve that meets the following conditions as the mass fraction of the main rare earth element X: ① Arrive at T on the curve E = f at 568°C s 1 / 2 <0.99; ②At temperature T E The absolute value of the slope at the thermal sensitivity index |dT / d(f s ) 1 / 2 |It is the minimum value relative to other curves; ③Critical temperature range ΔT CTR It is the minimum value relative to other curves; The critical temperature range ΔT CTR f is the curve s 1 / 2 = 0.31 and f s 1 / 2 =0.99 of the temperature corresponding to the point. Secondly, according to the same idea, with 0.5wt% as the minimum value and 15wt% minus the mass fraction of the selected element Y as the maximum value, the thermal sensitivity index and critical temperature range of various Mg-XM alloys with different contents of the synergistic rare earth element M were sampled and calculated to determine the composition range of the element M, where the mass fraction of the main rare earth element X is the mass fraction selected above, and the rest of the alloy is Mg; Finally, by analogy, with 0.5wt% as the minimum value and 15wt% as the maximum value, the thermal sensitivity index and critical temperature range of various Mg-XMN alloys with different N contents are sampled and calculated to determine the composition range of element N, wherein the mass fractions of the main rare earth element X and the synergistic rare earth element M are the mass fractions selected previously, and the rest of the alloy is Mg; In the above selections, if two curves meet the thermal sensitivity index |dT / d(f s ) 1 / 2 |Minimum and critical temperature range ΔT CTR The minimum standard is to set the coefficient K = f s 1 / 2 (T=TE) / ΔT CTR , select the element mass fraction corresponding to the curve with the largest K value.
2. The method according to claim 1, characterized in that Candidates for the main rare earth element X include Gd and Y.
3. The method according to claim 1, characterized in that Candidate synergistic rare earth elements M include Nd, Ce, and Sm.
4. The method according to claim 1, characterized in that: Candidate modifying elements N include Zr, Zn, and Ca.
5. The method according to claim 1, characterized in that The standard WE series rare earth magnesium alloy is Mg-3.77Y-2.46Nd-1.23Gd-0.21Zn-0.4Zr wt (%) alloy.
Citation Information
Patent Citations
High-strength heat-proof rare earth magnesium alloy and preparation method thereof
CN104278184A
Method for preparing high strength and ductility magnesium-rare earth alloy through selective laser melting additive manufacturing technology
CN110681869A