Metal-organic frameworks for the removal of iodine oxyanions
By using zirconium-based metal organic framework MOFs such as NU-1000 and MOF-808, the problems of low efficiency and high cost of oxygen anion removal in the prior art are solved, and efficient and low-cost oxygen anion removal is achieved, suitable for water and liquids Application in streams.
Patent Information
- Application Number
- CN202080076601.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-09-04
- Filing Date
- 2020-09-03
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2040-09-03
AI Technical Summary
The prior art is difficult to efficiently and specifically remove oxygen anions, such as selenium, antimony, lead and iodates from water and liquid streams, especially in the presence of competing species, and the existing methods are costly and efficient Low, it is difficult to achieve low concentration removal effect.
Using zirconium-based metal organic frameworks (MOFs) such as NU-1000 and MOF-808, the concentration of oxygen anion in the liquid is reduced by contacting the structures of these MOFs and in the presence of competitive species. Maintain high binding energy and irreversibility.
Achieve efficient removal of oxygen anions, reduce the concentration of oxygen anions in the liquid, and maintain low levels of removal efficiency even when the concentration of competing species is high, and reduce the cost reduction measures such as the use of lower purity zirconium materials and regeneration procedures. commercial costs.
Smart Images

Figure CN114929385B_ABST
Abstract
Description
Technical Field
[0001] The present invention and its embodiments relate to the removal of a given chemical species from a liquid. In particular, the present invention and its embodiments relate to the use of a metal organic framework having specific properties suitable for the removal of oxygen anions such as iodine oxyanions from a liquid stream. Background Art
[0002] Nuclear utilities are challenged to remove several impurities that significantly contribute to or drive doses, generation of radioactive waste, environmental wastewater issues, and material degradation issues. Similarly, fossil-based power generation facilities are challenged with regulatory discharge requirements for wastewater from flue gas desulfurization and scrubbers, fireside wash and boiler wash operations, and groundwater remediation requirements due to coal pile runoff and ash pond leachate. Current technologies (e.g., ion exchange) lack the ability to remove these impurities to the desired extent due to factors associated with capture and competing mechanisms with other impurities.
[0003] Recently developed isolation media provide organometallic ligands embellished on the resin backbone (in positions that would otherwise carry cation exchange groups) that significantly improve the media for the removal of cationic analytes such as cobalt. Unfortunately, such ligands cannot accommodate larger geometrical oxyanion species such as selenium present in subject water streams. For example, ion exchange and adsorption techniques are commonly used to capture chemical impurities in water streams. However, these techniques have several significant disadvantages. These techniques are non-specific (i.e., many different species will be captured to some extent), are subject to competition (i.e., species with higher concentrations will dominate), and are reversible (i.e., the captured species will be released when water conditions change).
[0004] Removing selenium from water streams is of great concern. Selenium is a naturally occurring element that is essential to human health at low concentrations. However, of all the essential elements, selenium has the most limited range between dietary deficiency (<40 μg / day) and toxicity (>400 μg / day). Selenium enters waterways through a variety of different sources, such as agricultural runoff, mining, industrial processes, and flue gas desulfurization processes. Due to the narrow range between deficiency and toxicity, it is very important to monitor and control the amount of bioavailable selenium in drinking water. The U.S. Environmental Protection Agency recognizes the hazards of selenium and has established a maximum acceptable level of selenium in drinking water of 50 ppb. However, in recent proposals, regulatory plans to reduce selenium emission requirements to 14 ppb, and then to 10 ppb, making it impossible for many flue gas desulfurization wastewater purification facilities currently operated to achieve such purities without methods other than typical ion exchange or adsorption engineering unit operations.
[0005] Selenium can exist in both organic and inorganic forms, but as selenite (SeO3 2- ) and selenate (SeO 4 2- ) and therefore bioavailability make these anions a major focus of remediation technologies. Many technologies have been explored to remove selenite and selenate from water, including the use of vertical flow wetlands and bioreactors, but high startup costs and size requirements limit the application of these technologies. Alternative methods that have been studied involve the use of adsorption media to absorb and remove unwanted inorganic selenium. Iron oxides (hematite, goethite and ferrihydrite) have been widely studied as potential adsorbents for selenite and selenate in aqueous solutions. The surface area of these iron-based materials is very small, which means that a lot of material is wasted due to the lack of available adsorption sites. Iron oxides also tend to be effective for selenite removal due to the formation of inner-sphere complexes between the selenite anion and the iron oxide surface, while selenate removal is not sufficient because only weak outer-sphere interactions occur.
[0006] In addition, in certain situations in nuclear power plants, it may also be desirable to remove other oxyanions from water or water streams, such as waste streams or contaminated liquids, such as liquids with radioactive oxyanions. Such other oxyanions include oxyanions of antimony, lead, and iodates from water associated with nuclear fuel plants, which may also be a problem in some situations.
[0007] Therefore, a new technology is needed to effectively and efficiently remove specific impurities, such as oxyanions, including selenium, antimony, lead, iodate and other oxyanions from water and other liquid streams, such as other industrial water-based streams or a certain amount of liquid stored for treatment. Such technology is needed to remove these impurities in the presence of other competing species or species that may compete for removal, thereby effectively reducing the removal efficiency of the species used for removal. Such technology is also needed to remove these impurities in a manner specifically for capturing the impurity and minimizing any reversibility or releasing from the capture, thereby making it have a higher binding energy. Specifically, different types of structural media are needed to specifically address the removal of low-level specific species, such as aqueous oxyanions of selenium, wherein sufficiently high binding energy is required to maintain near-irreversible uptake when the analyte concentration is reduced and the competitor concentration is simultaneously increased. Summary of the invention
[0008] The present invention provides the use of metal organic frameworks (MOFs) in removing specific chemical species or compounds, particularly oxygen anions, from liquids or liquid streams. In some embodiments, the removed oxygen anions include, for example, selenium, selenite (SeO 3 2- ) and selenate (SeO 4 2-) oxygen anions; antimony oxygen anions, including oxygen anions in the redox state of Sb[III] (antimonite) or Sb[V] (antimonate); lead oxygen anions, including oxygen anions in the redox state of Pb[II] or Pb[IV], such as Pb(OH) 6 2- 、Pb(OH) 6 4- , PbO 3 2- and PbO 2 2- Oxygen anions; and iodine, such as IO 3 - (iodate) oxygen anion.
[0009] In one embodiment, the present invention provides a metal organic framework for removing oxygen anions, such as the oxygen anions described above, from a liquid stream such as an industrial process liquid stream, including, for example, a wastewater stream or a given amount of liquid stored for processing. Specifically, the present invention provides a method for reducing the concentration of oxygen anions in a liquid stream or liquid, the method comprising: contacting a liquid stream or liquid comprising oxygen anions with a Zr 6 (μ 3 -O) 4 (μ 3 OH) 4 (OH) 4 (H 2 O) 4 (TBAPy) 2 The invention relates to a method for contacting a structure of a MOF of the invention, wherein TBAPy is 1,3,6,8-tetrakis(p-benzoic acid)pyrene (referred to as NU-1000); and complexing at least a portion of the oxygen anions to the metal organic framework by binding to the zirconium-derived node features of the MOF structure, or by binding to specialized ligands tethered to the nodes of the MOF and providing ligands that are selective for oxygen anion uptake, or both, thereby reducing the concentration of oxygen anions in a liquid stream or liquid. The ability of NU-1000 to reduce the concentration of oxygen anions in water provides a more environmentally acceptable water stream. In other embodiments, before activation, the molecular formula is Zr 6 O 5 (OH) 3 (BTC) 2 (HCOO) 5 (H 2 O) 2 MOF-808, in which BTC is 1,3,5-benzenetricarboxylate, can be used in a similar manner and has a molecular formula of Zr after activation. 6 (μ 3 -O) 4 (μ 3 -OH)4 (BTC) 2 (OH) 6 (H 2 O) 6 MOF-808, where BTC = 1,3,5-benzenetricarboxylate, can be used in a similar manner.
[0010] The present invention is also characterized by the additional ability to reduce the concentration of oxygen anions in an aqueous liquid stream or liquid to ultra-low levels when the stream also includes competing species, such as oxygen anions of sulfur or boron, and sodium ions present in the local fluid near the nodal uptake point for charge balancing purposes, wherein the competing species are those that compete for nodal adsorption sites on the MOF such that the effluent concentration of these oxygen anions can be maintained at a lower level even when the concentration of such competing species initially exceeds the effluent concentration of oxygen anions for removal, in some embodiments by a substantial factor. The present invention further achieves the desired effluent oxygen anion concentration even when the temperature is increased from room temperature to the process temperatures of condensed cooling water more often encountered in typical power plants. The present invention also encompasses potential embodiments in which one skilled in the art should be able to apply known methodologies to reduce the commercial cost of using NU-1000 or MOF-808 for water treatment applications by applying regeneration procedures known in the art on MOF-based media, such as NU-1000 or MOF-808, that have been previously exposed to oxygen anions, or by applying metallization chemistries known in the art to replace lower cost metal components in the MOF, such as hafnium (Hf) replacing zirconium (Zr), or both.
[0011] Since the manufacturing cost of MOF may be relatively high, in some cases, its cost of use may be too high. Therefore, the present invention also describes a method for connecting certain MOFs to substrates to form a product containing MOF, which can be used in a variety of ways according to the specific MOF connected to the substrate. Therefore, it should be understood that a specific MOF with a specific characteristic such as affinity for a specific species to be removed from a given fluid can be selected to be connected to the substrate. The substrate can be any substrate that can be connected to a given MOF, and the form and shape of the substrate can be selected based on its final use. For example, the configuration or shape of the substrate can be selected to allow the use of the selected MOF in a given environment, such as a given industrial process or a given device, and the appropriate exposure of the MOF is provided in the environment, such as exposing the MOF to a given fluid in a given process or a device.
[0012] It should be understood that the MOF can be any of the MOFs described herein. For example, in one embodiment, the MOF can be a MOF capable of removing certain chemical species from a given fluid. For example, the MOF can be a MOF capable of or configured to remove certain liquid phase species from a given liquid or liquid stream. In some embodiments, the MOF is a Zr-based MOF such as NU-1000 or MOF-808 for removing certain anions from a liquid or liquid stream, such as oxygen anions, including oxygen anions of iodine such as iodates. In some embodiments, the liquid or liquid stream can be an industrial liquid or liquid stream, such as a liquid stream or liquid associated with a nuclear power plant, comprising a waste liquid stream or a contaminated liquid containing certain liquid phase species to be removed, including, for example, oxygen anions, including oxygen anions of iodine such as iodates.
[0013] In one embodiment, the substrate can be any inert substrate to which the MOF can be attached. For example, the substrate can be inert polypropylene polymer resin beads, macroscopic fabrics such as mesh materials or mesh filters, molecular fabrics, or any other three-dimensional shaped substrates.
[0014] In one embodiment, MOF, including any MOF described herein, such as Zr-based MOF, such as NU-1000 or MOF-808 can be connected to an inert substrate, such as polypropylene polymer resin beads, macroscopic fabrics, such as mesh materials or mesh filters or molecular fabrics. In one embodiment for connecting MOF, the substrate is first subjected to a metal oxide, such as an atomic layer of aluminum oxide, titanium oxide or zinc oxide to be deposited on the substrate surface. Separately, MOF can be connected to CTAB in solution, which is then combined with a substrate having a metal oxide. This results in the connection of MOF to the substrate and the production of a commercial product consisting of a substrate having a connected MOF. In another embodiment for connecting MOF to a substrate, MOF can be connected to β-CD in a solution and then combined with the substrate. This results in the connection of MOF to the substrate through β-CD and the production of a commercial product consisting of a substrate having a connected MOF.
[0015] It should be understood that the substrate containing the MOF, which can be a commercial product, can be used in a variety of ways, depending on the MOF selected for attachment to a given substrate. As described above, in some embodiments, the MOF can be a MOF capable of removing certain chemical species from a given fluid. For example, the MOF can be a Zr-based MOF, such as NU-1000 or MOF-808, which is configured to remove certain anions, such as certain oxygen anions and certain cations, from a liquid or liquid stream. Specifically, NU-1000 is based on zirconium (Zr) and has a molecular formula of Zr 6 (μ 3 -O) 4 (μ 3OH) 4 (OH) 4 (H 2 O) 4 (TBAPy) 2 , where TBAPy is 1,3,6,8-tetra(p-benzoic acid)pyrene. The molecular formula of MOF-808 is Zr 6 O 5 (OH) 3 (BTC) 2 (HCOO) 5 (H 2 O) 2 , where BTC is 1,3,5-benzenetricarboxylate (before activation) and the molecular formula is Zr 6 (μ 3 -O) 4 (μ 3 -OH) 4 (BTC) 2 (OH) 6 (H 2 O) 6 , where BTC = 1,3,5-benzenetricarboxylate (after activation with hydrochloric acid), although other linkers that can be linked via carboxylates can be used. NU-1000 or MOF-808 can be used on substrates to remove selenium, including selenite (SeO 3 2- ) and selenate (SeO 4 2- ) oxygen anions; antimony oxygen anions, including oxygen anions in the redox state of Sb[III] (antimonite) or Sb[V] (antimonate); lead oxygen anions, including oxygen anions in the redox state of Pb[II] or Pb[IV], such as Pb(OH)6 2- 、Pb(OH)6 4- 、PbO3 2- and PbO 2 2- Oxygen anions; and iodine, such as IO 3 - Thus, such MOFs may provide the ability to remove anionic species from a given liquid or liquid stream, such as power plant coolant or waste streams, including nuclear power plant liquid streams or contaminated liquids stored for treatment. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 A metal organic framework (MOF) according to an embodiment of the present invention is shown;
[0017] Figure 2 A specific MOF, namely NU-1000, is presented;
[0018] Figure 3 Shown Figure 2 The structural characteristics of MOF, namely NU-1000;
[0019] Figure 4A Shown highlighting the hexagonal aperture and Zr 6 The structure of the node is the structure of NU-1000;
[0020] Figure 4B The octahedral aperture and Zr 6 The structure of the node is the structure of UiO-66;
[0021] Figure 5 is a bar graph showing the number of selenate molecules or selenite molecules adsorbed at each node in a series of Zr-based MOFs;
[0022] Figure 6 It is to display NU-1000, UiO66-NH 2 and UiO66-(NH 2 ) 2 A graph showing the kinetics of selenate uptake and selenite uptake in ;
[0023] Figure 7 A flow chart outlining the screening process for selenate adsorption and selenite adsorption in Zr-based MOFs is presented;
[0024] Fig. 8A DRIFTS spectra of synthesized NU-1000 (lower trace) and after adsorption of two selenite molecules (middle trace) and a selenate molecule (upper trace) are shown;
[0025] Figure 8B Showing from 4000-2000cm -1 Amplified DRIFTS spectrum;
[0026] Figure 8C The potential binding mode of selenate (or selenite) to the NU-1000 node is shown;
[0027] Fig.9A The calculated difference pair distribution functions (PDF) of selenite-loaded and selenate-loaded NU-1000 are shown;
[0028] Fig. 9B The experimental difference PDFs of NU-1000 loaded with selenite and selenate are shown, with only the differences with η 2 μ 2 Combine peaks at matching distances;
[0029] Fig.10 The selenate uptake and selenite uptake in NU-1000 (2 mg) at low concentrations and at an initial concentration of 1000 ppb Se versus time are shown;
[0030] Fig.11 The selenate uptake and selenite uptake in NU-1000 (2 mg) at low concentrations and 40°C with a starting concentration of 1000 ppb Se are shown with respect to time;
[0031] Fig.12 Selenate uptake and selenite uptake in NU-1000 (2 mg) versus time at low concentrations and pH 6 and a starting concentration of 1000 ppb Se are shown;
[0032] Fig.13A -E shows the amount (q) adsorbed by each node of NU-1000 at different concentrations of selenate and selenite versus time, where the amount adsorbed is expressed as the weight of all oxygen anions (in mg), normalized to the weight of bare NU-1000 MOF (in g);
[0033] Fig.14A -C shows the Langmuir plots (linear, type I) of selenite adsorption and selenate adsorption on NU-1000, where the adsorbed amount is the weight of all oxygen anions;
[0034] Fig.15A Powder X-ray diffraction patterns of synthesized NU-1000 compared to NU-1000 after adsorption of selenite or selenate are shown;
[0035] Fig. 15B Nitrogen adsorption isotherms of synthesized NU-1000 compared to NU-1000 after adsorption of selenite or selenate are shown;
[0036] Fig.16A -C shows the changes in selenate uptake and selenite uptake over time using 2 mg of NU-1000 and 10 mL of an aqueous solution containing 100 ppb Se and (a) 100 ppb sulfur S and (b) 500 ppb S and (c) 1000 ppb S as sulfate;
[0037] Fig.17A -B shows Sb(OH) 6 - Ingestion over time, expressed as ingestion per node;
[0038] Fig.18 Langmuir fits of the Sb[V] adsorption isotherms from Figure 17 are shown;
[0039] Fig.19 NU-1000 and Sb(OH) 3 - A powder x-ray diffraction pattern of NU-1000; and
[0040] Fig. 20 NU-1000 and Sb(OH) 6 - Nitrogen isotherm of NU-1000. DETAILED DESCRIPTION
[0041] The present invention is described more fully below with reference to the accompanying drawings. Although the present invention will be described in conjunction with specific embodiments, it should be understood that the present invention can be applied to a variety of applications, and the description herein is intended to cover alternatives, modifications and equivalents within the spirit and scope of the present invention and claims. Therefore, the following description is exemplary, because several embodiments are described (for example, by using the terms "preferably", "for example" or "in one embodiment"), but this description should not be regarded as limiting or elaborating the only embodiment of the present invention, because the present invention encompasses other embodiments not specifically listed in this specification. Further, the terms "invention", "present invention", "embodiment" and similar terms used throughout the specification are widely used, and are not intended to mean that the present invention requires or is limited to any specific aspect described or that such description is the only way to prepare or use the present invention.
[0042] In general, the present invention relates to the use of metal organic frameworks (MOFs) in removing specific compounds, particularly oxygen anions, from liquids or liquid streams. In some embodiments, the MOF is a Zr-based MOF, such as NU-1000 or MOF-808, and the oxygen anions removed include, for example, selenium, including selenite (SeO 3 2- ) and selenate (SeO 4 2- ) oxygen anions; antimony oxygen anions, including oxygen anions in the redox state of Sb[III] (antimonite) or Sb[V] (antimonate); lead oxygen anions, including oxygen anions in the redox state of Pb[II] or Pb[IV], such as Pb(OH) 6 2- 、Pb(OH) 6 4- , PbO 3 2- and PbO 2 2- Oxygen anions; and iodine, such as IO 3 -(iodate). It will be appreciated that the preferred mechanism for oxygen anion adsorption is nodal uptake through the zirconium oxide / zirconium hydroxide nodal features of the MOF. In some embodiments, MOF-808 is used to remove iodate. It will be appreciated that references to liquid streams also include a given amount of liquid stored, for example, in a tank that may not flow as a stream. In this case, the stored liquid may be treated in the same manner as described for the given liquid stream, and in some embodiments, may be made into a flowing liquid stream for treatment.
[0043] In one embodiment, the present invention provides a use of a metal organic framework for removing oxygen anions, such as the oxygen anions described above, from a liquid stream, such as an industrial process liquid stream, including, for example, a wastewater stream. Specifically, the present invention provides a method for reducing the concentration of oxygen anions in a liquid stream, the method comprising: mixing a liquid stream comprising oxygen anions with a liquid stream comprising a molecular formula of Zr 6 (μ 3 O)4(μ 3 OH) 4 (OH) 4 (H 2 O) 4 (TBAPy) 2 The invention relates to a method for contacting a structure of a MOF of the present invention, wherein TBAPy is 1,3,6,8-tetrakis(p-benzoic acid)pyrene (referred to as NU-1000); and complexing at least a portion of the oxygen anions to the metal organic framework by binding to the zirconium-derived node features of the MOF structure, or by binding to a specialized ligand tethered to the node of the MOF and providing a ligand selective for oxygen anion uptake, or both, thereby reducing the concentration of oxygen anions in the liquid stream. The ability of NU-1000 to reduce the concentration of oxygen anions in water provides a more environmentally acceptable water stream. In other embodiments, before activation, the molecular formula is Zr 6 O 5 (OH) 3 (BTC) 2 (HCOO) 5 (H 2 O) 2 MOF-808, in which BTC is 1,3,5-benzenetricarboxylate, can be used in a similar manner and has a molecular formula of Zr after activation. 6 (μ 3 -O) 4 (μ 3 -OH) 4 (BTC) 2 (OH) 6 (H 2 O) 6MOF-808, where BTC = 1,3,5-benzenetricarboxylate, can be used in a similar manner.
[0044] Figure 1 A MOF according to one embodiment of the present invention is presented. MOFs are structurally diverse porous materials constructed from metal nodes bridged by organic linkers. MOFs consist of multifunctional organic linkers and metal-based nodes that are interconnected by moderately strong coordination bonds. MOFs containing zirconium metal nodes have attracted much attention for the adsorption or complexation of analyte molecules in aqueous solutions due to their inherent stability over a wide pH range in water. This stability stems from the strong Zr(IV)-0 bonds, which also make these frameworks mechanically and thermally stable at temperatures >500°C. MOFs in aqueous solution are suitable candidates for pre-coated filter / desalter applications or stand-alone packed column separation applications, which may also be consistent with the use of containers that already exist in a given plant, such as nuclear power plants (e.g., containers that are already used for ion exchange) or flue gas desulfurization wastewater treatment facilities at fossil fuel power plants.
[0045] While MOFs in their native structure can be used for such liquid flow applications, the amount of pressure required to permeate a packed bed of such small particles (typical sizes are in the range of 75 to 1200 nanometers, with 5 micron crystallites formed by the MOF particles) may exceed the available fluid-driving equipment, meaning that the MOF particles may need to be transferred to some other larger particulate carrier (closer to the order of resin particles, typically in the form of powders or beads with diameters of 50 to 850 microns) so that the fluid can more easily permeate the aggregates of the carrier particles. One of ordinary skill in the art should be able to construct a variety of methodologies for contacting the MOF particles to some suitable carrier particles so that the hydraulic permeability of the aggregates of such carrier particles is high enough to provide the required fluid volume throughput in a columnar flow through a bed of such carrier particles, or in a flow through a filter that provides a porous surface on which such carrier particles are coated. Therefore, the adsorption properties of the MOF will still be manifested because the MOF itself will be exposed to the analyte in the water stream as it flows around the carrier particles to which the MOF medium is attached.
[0046] Figure 2 A specific MOF, NU-1000, is shown. NU-1000 is a Zr-based MOF and has the molecular formula Zr 6 (μ 3 -O) 4 (μ 3 OH) 4 (OH) 4 (H 2 O) 4 (TBAPy) 2, where TBAPy is 1,3,6,8-tetra(p-benzoyl)pyrene which can be used as the MOF in the present invention. The parent skeleton node of this MOF consists of one consisting of four μ 3 -OH ligand and four μ 3 -O ligand-terminated octahedral Zr 6 Eight of the twelve octahedral edges are connected to the TBAPy unit, while the remaining Zr coordination sites (after activation) consist of four terminal -OH and four terminal -OH 2 Ligand occupancy. The 3D structure can be described as 2D kagome sheets connected by TBAPy ligands. Two of the four terminal -OH groups point into the mesoporous channels, while the remaining terminal hydroxyl group resides in the smaller pores between the kagome sheets.
[0047] Figure 3 Shown Figure 2 The structural features of the MOF, NU-1000. Additional features of this MOF and its synthesis techniques are described in Mondloch, JE, W Bury, D Fairen-Jimenez, S Kwon, EJ DeMarco, MH Weston, AA Sarjeant, ST Nguyen, PC Stair, RQ Smurr, OK Farha and JT Hupp, "Vapor-Phase Metalation by Atomic Layer Deposition in a Metal-Organic Framework", J. Am. Chem. Soc. (2013) 135, 10294-10297, which is incorporated herein by reference in its entirety. For example, the synthesis of the organic linker of NU-1000 involves the following two steps: Suzuki coupling between 1,3,6,8-tetrabromopyrene and 4-(ethoxycarbonyl)phenyl)boronic acid, followed by hydrolysis of the resulting tetraester compound to give the tetracarboxylic acid linker, i.e., 1,3,6,8-tetra(p-benzoic acid)-pyrene. To synthesize NU-1000, zirconium oxychloride octahydrate was first formed by reacting zirconium oxychloride octahydrate with an excess of benzoic acid modifier in N,N-dimethylformamide at 80°C for 1 hour. 6 After the reaction mixture was cooled to room temperature, 0.2 equivalents of 1,3,6,8-tetrakis(p-benzoic acid)-pyrene linker were added and the mixture was heated at 100°C for 24 hours to give benzoic acid-terminated NU-1000. In order to remove the benzoic acid ligand and reveal the terminal -OH and -OH 2, MOF was activated with 8M HCl for 24 h. It should also be understood that the lower purity starting material ZrOCl 2 8H 2 O and HfOCl 2 H 2 O can reduce the manufacturing cost of NU-1000. For example, 99.99% pure ZrOCl 2 8H 2 O and HfOCl 2 xH 2 The cost of O is about 400% higher than that of the 98% pure precursor. Moreover, the structural features of this MOF are defined in Planas, N.; Mondloch, JE; Tussupbayev, S.; Borycz, J.; Gagliardi, L.; Hupp, JT; Farha, OK; Cramer, CJ. 6 Defining the Proton Topology of the Zr 6 -Based Metal-Organic Framework NU-1000). It is described in Journal of Physical Chemistry Letters (J. Phys. Chem. Lett.) 2014, 5, 3716-3723, which is incorporated herein by reference in its entirety.
[0048] Surprisingly, it was found that bare NU-1000 complexes with selenium oxyanions, including selenite (SeO 3 2- ) and selenate (SeO 4 2- ). The results to date indicate that the selenium oxyanions are bound with significant strength so that these anions can be removed in a simple continuously stirred tank environment in reasonable and relatively fast times to levels down to 20 ppb, and even to lower concentrations, such as 10 ppb and below, 6 ppb and below, and 2 ppb and below in other examples. The bonding of selenate and selenite is shown as being directly attached to the zirconium nodes of the MOF without concern for ligand interactions with the MOF cavity. It should be appreciated that the ability of NU-1000 to complex with selenite and selenate has been achieved without modifying the structure of NU-1000, for example, by functionalizing NU-1000 by solvent-assisted linker exchange (SALE) rather than by solvent-assisted ligand incorporation (SALI) using metallization by atomic layer deposition (ALD).
[0049] Specifically, a series of zirconium-based MOFs were tested for their ability to adsorb and remove selenate and selenite anions from aqueous solutions. The MOFs were tested for their adsorption capacity and uptake time at different concentrations. Figure 7 is a flow chart outlining the screening process for selenate adsorption and selenite adsorption in Zr-based MOFs. ) In this test, NU-1000 was shown to have the highest adsorption capacity among all Zr-based MOFs and the fastest uptake rates for both selenate and selenite.
[0050] Adsorbents at different ratios: The adsorbates were tested to understand how the ratio affects uptake. 2, 4, 6, and 8 mg of NU-1000 samples were exposed to a 1000 ppb Se (as SeO 4 2- or SeO 3 2- ) in 10 mL of solution. At all adsorbent:adsorbate ratios tested, 98.3% or more of SeO in solution 3 2- was adsorbed, resulting in an average adsorption of 10-17 ppb in solution. Similarly, at all adsorbent:adsorbate ratios tested, 97.7% or more of SeO in solution 4 2- was adsorbed so that the average adsorption amount in the solution was 20-23 ppb. In general, these experiments show that changing the adsorbent: at these concentration levels, the adsorbate ratio of 4x has no significant effect on the total Se adsorbed from the solution. It should be noted that throughout the Se uptake process of testing NU-1000, such as studies conducted at pH 6, and similar batch studies conducted using a Se starting concentration of 100 ppb instead of 1000 ppb, when 2 mg of NU-1000 was exposed to 1000 ppb and 100 ppb Se, respectively, residual Se concentrations below 10 ppb (down to 6 ppb and 2 ppb) were observed. In such embodiments, the present invention can be used to reduce the total selenium concentration (i.e., the total concentration of all selenium species) to less than 10 ppb or to an amount set for a suitable drinking water standard. Therefore, in some embodiments, the present invention can reduce the total Se concentration in a given liquid or liquid stream by more than 90%, more than 94%, and more than 98%.
[0051] Figure 4A Shown highlighting the hexagonal aperture and Zr 6 The structure of the node is the structure of the NU-1000. Figure 4B The octahedral aperture and Zr 6 The structure of the node is the structure of UiO-66. Figure 4A )、UiO-66( Figure 4B) and UiO-67 families were screened for their selenate and selenite uptake capabilities. For the initial screening, two samples of each MOF were exposed to aqueous solutions of selenate (100 ppm Se) or selenite (100 ppmSe), respectively. After 72 h of exposure, UiO-66 had adsorbed 54% and 34% of the selenite and selenate present in the respective solutions, indicating that anion exchange occurred both on and within the MOF. This suggests that, despite the strong bridging properties of the OH groups in the nodes of UiO-66, the Zr-bound hydroxides in the MOF are useful for the adsorption of selenoxy anions. In addition, the presence of Lewis / Bronsted basic amine groups on the terephthalate linkers appears to enhance anion exchange, with UiO-66-(NH 2 ) 2 and UiO-66-NH 2 Some of the MOFs studied have Zr 6 The highest selenate and selenite adsorption of the node ( Figure 5 Without being bound by theory, this may be the result of hydrogen bonding interactions between the amine groups and the selenate and selenite anions, similar to the hydrogen bonding motifs in the amine-containing macrocyclic skeleton that have a high affinity for sulfate and selenate anions.
[0052] Figure 5 is a bar graph showing the number of selenate or selenite molecules adsorbed per node in a series of Zr-based MOFs. Figure 5 The results showed that of the seven MOFs examined, NU-1000 had the highest uptake of selenate and selenite, both by weight and on a per-node basis. It also most thoroughly uptakes selenate from a 100 ppm Se test solution, i.e., 88% (SeO 4 2- ) and 90% (SeO 3 2- ) to remove these ions. These results highlight the value and importance of MOFs with unstructured ligand instability in achieving anion uptake.
[0053] Again, without being bound by theory, an alternative uptake mode can be imagined to be adsorption of sodium selenate / selenite salts via, for example, oxygen-selenium-anion / node-water (hydroxyl) hydrogen bonds. ICP-OES (Inductively Coupled Plasma-Optical Emission Spectroscopy) measurements revealed no sodium adsorption in the MOF, indicating that the adsorbate could not be a salt and implying that each adsorbed oxygen selenium dianion must be charge balanced by the loss of two anionic ligands (probably hydroxides) from the MOF. ICP-OES measurements additionally established that there was no loss of zirconium to the solution.
[0054] Figure 6 It is to display NU-1000, UiO66-NH 2 and UiO66-(NH 2 ) 2 The kinetics of selenate uptake and selenite uptake in UiO-66-NH 2 、UiO-66-(NH 2 ) 2 and NU-1000 for selenate and selenite, and SeOx 2- Kinetics of uptake. Figure 6 As shown in 2 ) 2 High-volume uptake from a 100 ppm solution requires about 70 hours or more with UiO-66-NH 2 It takes about 27 hours for NU-1000 and less than 3 hours for NU-1000. Compared with UiO-66 and its derivatives, NU-1000 has a faster uptake, which may be related to the pores and pore size. The diameters of the triangular pores and hexagonal pores of NU-1000 are 12A and 30A, respectively, with the same pore size ( Figure 4A ), while the diameters of tetrahedral and octahedral pores included in UiO-66 are 8A and 11A respectively, and the diameter of the pore is 7A. ( Figure 4B Octahedral pores are shown. ) It is expected that UiO-66-NH 2 and UiO-66-(NH 2 ) 2 The pores of NU-1000 would be even smaller. The radii of the selenate and selenite anions are 2.4 Å and 2.6 Å, respectively. Therefore, based solely on pore size versus analyte size, it is expected that diffusion of selenate and selenite through the pores of NU-1000 would be faster than diffusion within the UiO-66 derivative.
[0055] NU-1000 and UiO-66-NH 2 The notable feature of both is their ability to absorb selenate and selenite with essentially the same efficacy - both kinetically and in terms of uptake capacity. The ability to adsorb both forms of inorganic selenium is an important characteristic of selenium remediation. The combination of high adsorption capacity and rapid uptake time using NU-1000 suggests that pore size and Zr 6 The presence of substitutable ligands (water and hydroxyl groups) at the nodes may be important for obtaining high uptake capacity and fast uptake kinetics.
[0056] Examination of the periodic table shows that the oxyanions of the following elements can also be expected to be taken up by such MOFs as NU-1000 or MOF-808 in a manner similar to selenium, namely, oxyanions of aluminum (i.e., water-soluble aluminum oxides / hydroxides), silicon (i.e., silicates and hydrogen silicates), phosphorus (as phosphates and hydrogen phosphates), sulfur (i.e., sulfates), chlorine (as chlorates and perchlorates), pyrite (i.e., water-soluble oxides / hydroxides of pyrite), arsenic (as arsenates), tin (i.e., stannates), antimony (as antimonates and antimonites), iodine (as iodates, periodates, and iodites), and lead (i.e., water-soluble oxides / hydroxides of lead).
[0057] To gain insight into the adsorption mechanism of selenate and selenite on NU-1000, the adsorption of each Zr 6 Maximum adsorption capacity of nodes. When exposed to aqueous solutions containing varying concentrations of selenate and selenite anions ranging from 2-7 anions per node, the maximum adsorption capacity of NU-1000 was found to be two anions per node (Table S1). Additionally, under these conditions, NU-1000 had similar affinities for selenate and selenite, suggesting that these two analytes may bind in a similar manner. At initial concentrations corresponding to more than six nodes per node (>90 ppm Se for solution volume and amount of adsorbent examined), NU-1000 was shown to take up more than two anions per node, while also adsorbing sodium cations. This adsorption of sodium suggests that NU-1000 may no longer be inherently charge balanced when adsorption exceeds two anions per node. In the absence of Na + In the case of co-incorporation, for each doubly charged selenate or selenite anion adsorbed, the MOF must give up two negative charges to maintain charge balance. One way NU-1000 can accommodate two selenate or selenite anions (-4 charge) per node is to replace the Zr 6 All four terminal hydroxyl groups (OH - ); as detailed below, water molecules may also be replaced ( Figure 4A ).
[0058] Table S1: Selenate adsorption and selenate adsorption per node in NU-1000 when exposed to different concentrations of aqueous sodium selenate and sodium selenite. * Na + Also adsorbed.
[0059]
[0060]
[0061] Diffuse reflectance infrared Fourier transform spectroscopy (DRIFTS) was used to gain insight into the locations of two analyte molecules at each node of the NU-1000. Fig. 8A DRIFTS spectra of as-synthesized NU-1000 (lower trace) and after adsorption of two selenite molecules (middle trace) and a selenate molecule (upper trace) are shown. Figure 8B Showing from 4000-2000cm -1 Zoomed in DRIFTS spectrum. Figure 8C The potential binding mode of selenate (or selenite) to the NU-1000 node is shown. Before analyte adsorption, the IR spectrum of NU-1000 contains 3670 cm -1 The peak at Fig. 8A / B, lowest trace), the sharp peak corresponds to the stretching of the -OH group at the end of the node (Figure 4a). The spectrum also contains a peak at 2745 cm -1 The small peak ( Fig. 8A / B, lower trace), the small peak corresponds to Zr 6 The OH extension of the hydrogen bond between water and the hydroxyl ligand in the node ( Figure 4A ). After adsorption of approximately two selenate or selenite molecules per node, 3670 cm -1 The OH stretching at 2745 cm -1 The OH stretching based on hydrogen bonding completely disappears at Fig. 8A / B, middle and upper traces, respectively). Based on this information, it is reasonable to suggest that each SeO 4 2- Anion or SeO 3 2- Anion replacement Zr 6 Therefore, when each node binds two analyte molecules, all four terminal hydroxyl groups are displaced, and analyte binding can be carried out at n 2 μ 2 or μ 2 occurs in the manner ( Figure 8C ).
[0062] Pair distribution function (PDF) analysis of the total X-ray scattering data was used to assess the structural changes accompanying the binding of selenate and selenite anions. Fig.9A Shown are the calculated difference pair distribution functions (PDFs) of selenite-loaded and selenate-loaded NU-1000. Fig. 9B The experimental difference PDFs of NU-1000 loaded with selenite and selenate are shown, with only the differences with η 2 μ 2 The simulated PDF indicates the peaks at the distances that match.2 μ 2 and μ 2 The combined Se-Zr distances are 3.41A and 2.72A respectively. Fig.9A The experimental PDF results for evaluating the interatomic distances unique to the separate adsorbent / adsorbate combinations from the differential data show features at about 3.4 A (3.36 A for selenite and 3.37 A for selenate) instead of 2.7 A, clearly indicating that these anions are present only in the presence of η 2 μ 2 Mode combination ( Fig. 9B , where the curve for selenite starts higher on the left). Both difference PDFs show a peak at about 1.7 A that is assignable to the Se-O distance within the anion, and a feature at 2.0-2.3 A consistent with a slight contraction of the average Zr-O distance.
[0063] Fig.10 The relationship between selenate uptake and selenite uptake in NU-1000 (2 mg) at low concentrations and an initial concentration of 1000 ppb Se is shown with respect to time. In order to test whether the current EPA standard for selenium in water can be met by using NU-1000 as an adsorbent, the uptake of selenate and selenite at low concentrations was also studied. When exposed to 5 mL of an aqueous solution of sodium selenite or sodium selenate at 1000 ppb, 2 mg of NU-1000 adsorbed 98% of the selenite or selenate in the solution in less than 5 minutes. After 3 hours, the amount adsorbed remained unchanged, which means that the adsorbed anions were not subsequently leached from the adsorbent after 5 minutes. Since the selenium concentration of the residual solution was only about 20 ppb, the test sample treated with NU-1000 met the EPA standard for drinking water <50 ppb selenium. It is expected that those skilled in the art of engineering fluid purification equipment and the like will be able to optimize these results to contact the NU-1000MOF with a continuously flowing stream of aqueous solutions of selenate and selenite and produce, after an appropriate contact time, a wastewater stream having a concentration of these ions on the order of about 10 parts per billion of selenium.
[0064] Still at 40℃( Fig.11 ) and pH 6( Fig.12 ) to simulate the conditions of recirculating cooling water in the flue gas desulfurization process of a power plant, where selenate remediation and selenite remediation are an issue. Fig.11 Selenate uptake and selenite uptake in NU-1000 (2 mg) versus time at low concentrations and 40°C and a starting concentration of 1000 ppb Se are shown. Fig.12Selenate uptake and selenite uptake in NU-1000 (2 mg) versus time at low concentrations and pH 6 and a starting concentration of 1000 ppb Se are shown. Successful testing indicates that NU-1000 is a promising candidate for the removal of selenite or selenate under power plant operating conditions.
[0065] Fig.13A -E shows the amount (q) adsorbed by each node of NU-1000 at different concentrations of selenate and selenite versus time, where the adsorbed is expressed as the weight of all oxygenated anions (in mg), normalized to the weight of bare NU-1000 MOF (in g). Fig.14A -C shows the Langmuir plots (linear, type I) of selenite and selenate adsorption on NU-1000, where the adsorbed amount is the weight of all oxygen anions. The amount of selenite and selenate adsorbed per gram of NU-1000 was probed by exposing the MOF to different concentrations of selenite or selenate and monitoring the adsorption amount (q) in mg (analyte) / g (adsorbent) over time ( Fig.13A -E). The adsorption isotherm data were fitted using the Langmuir model and a high correlation coefficient was obtained ( Fig.14A -C). Using the Langmuir equation, the maximum adsorption capacity (Q) of NU-1000 for selenite is 95 mg / g, and the maximum adsorption capacity for selenate is 85 mg / g. These data are roughly equivalent to millimolar levels of analyte per gram of uptake medium. At each node corresponding to the amount (i.e., concentration and volume) of 1.00 to 3.00 selenite anions or selenate anions, NU-1000 was found to reach its maximum adsorption within 1 minute of exposure (Figure 13). The adsorption capacity of NU-1000 makes it one of the highest capacity selenate and selenite adsorption materials described to date; the size of these analyte oxygen anions is much larger than typical sulfate anions or chloride anions, and it is more difficult to achieve overall uptake capacity in many typical commercially available adsorption or ion exchange media. Specifically, the uptake time of <1 minute distinguishes NU-1000 from other materials, such as aluminum oxide derivatives and iron oxide derivatives, as well as ion exchange and polymer resins, each of which requires 30 minutes or more to reach maximum adsorption capacity under equivalent conditions. This feature, together with the low equilibrium final Se concentration observed for NU-1000, is likely a manifestation of the significantly improved binding capacity of MOFs for larger oxygen anions compared to other available adsorption media.
[0066] FIG. 14 shows the adsorption capacity as a function of time at different concentrations (q), where q = (C i -C f )x V / m and C i= initial concentration of selenate or selenite, C f = final concentration at a given time, V = volume of selenate solution or selenite solution used and m = mass of NU-1000. For the Langmuir plots shown, a Type I linear equation was used (Figure 14), where C e = equilibrium concentration of selenate or selenite in solution, q e = equilibrium adsorption capacity, Q = maximum adsorption capacity of NU-1000, and K L = Langmuir adsorption constant. q e and C e q and C taken from Figure 13 and the above analysis, respectively f The average value of .
[0067] Table S2: C for selenate adsorption and selenite adsorption on NU-1000 in Figure 14 e and q e The value of .
[0068]
[0069] Fig.15A Shown are powder X-ray diffraction patterns of synthesized NU-1000 compared to NU-1000 after adsorption of selenite or selenate. Fig. 15B Nitrogen adsorption isotherms of synthesized NU-1000 compared to NU-1000 after adsorption of selenite or selenate are shown. Characterization of NU-1000 before and after adsorption of selenite and selenite showed that the framework remained intact. The powder X-ray diffraction pattern did not change before and after adsorption. The Brunauer-Emmett-Teller (BET) volume surface area of NU-1000 before adsorption was 1035 ± 5 m 2 / cm 3 (Weight surface area: 2130±5m 2 / g), while the volume surface area after adsorption of selenate and selenite decreased slightly to 682±10m 2 / cm 3 and 705±10m 2 / cm 3 (Weight surface area: 1240±10 and 1300±10m 2 / g)( Fig. 15B ). Similarly, a modest reduction has been reported after installing Al(III) on the nodes of NU-1000 by atomic layer deposition.
[0070] Fig.16A-C shows the changes in selenate uptake and selenite uptake over time using 2 mg of NU-1000 and 10 mL of an aqueous solution containing 100 ppb Se and (a) 100 ppb sulfur S and (b) 500 ppb S and (c) 1000 ppb S as sulfate. Specifically, Fig.16A -C demonstrates the performance of NU-1000MOF using nodal uptake of selenate and selenite in the presence of competing sulfate anions.
[0071] Batch adsorption studies of selenate uptake and selenite uptake were performed in the presence of sulfate during initial exposure to the bare MOF, as well as in the presence of sulfate during exposure to the MOF to which selenium oxyanions had been adsorbed as a “knockout study”. Competitive adsorption was studied by exposing 2 mg of NU-1000 to 10 mL of aqueous solutions containing 100 ppbSe as SeO 4 2- or SeO 3 2- And 100ppb S, 500ppb S or 1000ppb S as SO 4 2- In all cases, >95% of the Se in solution was adsorbed ( Fig.16A -C), and SO 4 2- The presence of SeO at these concentrations (ten times higher in ppb) 4 2- Uptake or SeO 3 2- In addition, it was found that SeO 3 2- or SeO 4 2- The residual Se concentrations of the samples were between 2-7 and 4-9 ppb Se, respectively.
[0072] By first exposing 2 mg of NU-1000 to 10 mL of 24 ppm Se as SeO 4 2- and SeO 3 2- This corresponds to an exposure level of 3.3Se / node, which was used to ensure that NU-1000 was covered with SeO 4 2- and SeO 3 2- Then NU-1000-2SeO 4 2- and NU-1000-2SeO 32- Exposure to 25 ppm SO 4 2- (equivalent to 3S / node) in aqueous solution and detect SeO as a function of time 4 2- and SeO 3 2- In the presence of SO 4 2- case, from NU-1000-2SeO 3 2- SeO leached from 3 2- Minimum (3%), while in the presence of SO 4 2- case, from NU-1000-2SeO 4 2- SeO leached from 4 2- more significantly (20%); but still low compared to many other types of adsorption media, and it is difficult to even obtain adsorption of the two species of selenium oxyanions in the absence of sulfate, let alone in the case of a knockout challenge.
[0073] The general method used for the above analysis is described below. 2 、UiO-66-(NH 2 ) 2 、UiO-66-(OH) 2 UiO-66 and UiO-67 were prepared according to the procedures described in Katz, MJ; Brown, ZJ; Colon, YJ; Siu, PW; Scheldt, KA; Snurr, RQ; Hupp, JT; Farha, OK. Afacile synthesis of UiO-66, UiO-67 and their derivatives. Chem. Commun. 2013, 49, 9449-9451, which is incorporated herein by reference in its entirety. NU-1000 was prepared according to Planas, N.; Mondloch, JE; Tussupbayev, S.; Borycz, J.; Gagliardi, L.; Hupp, JT; Farha, OK; Cramer, CJ. 6Proton topology of the metal organic framework NU-1000. Prepared by the procedure described in Journal of Physical Chemistry Letters 2014, 5, 3716-3723, which is incorporated herein by reference in its entirety. Powder X-ray diffraction measurements were obtained using a Bruker MX IμS microsource with Cu-Kα radiation and an Apex II CCD detector. Measurements were performed in the range of 2° < 2θ < 37°. N 2 Adsorption and desorption isotherm measurements were performed on a Micromeritics Tristar II at 77 K. The samples were activated by heating at 120 °C for 12 h under high vacuum on a Micromeritics Smart VacPrep. All gases used were ultra-high purity grade 5 gases obtained from Airgas Specialty Gases. DRIFTS were recorded on a Nicolet 6700FTIR spectrometer equipped with an MCT detector cooled to 77 K. The spectra were collected in KBr mixtures under argon purge (samples were prepared in air). Pure KBr was measured as background and subtracted from the sample spectra. ICP-OES data were collected on a Varian Vista MPX ICP spectrometer. ICP-MS data were collected on a ThermoFisher XSeries II instrument equipped with collision cell technology (CCT) to reduce interference from double peaks for accurate detection of Se. ICP standards were purchased from Fluka Analytical. The purchased Na and Se ICP standards were dissolved in 2% nitric acid, The Zr standard was 1000 mg / L in 4 wt % HCl and the Zr standard was 10 000 μg / mL in 4 wt % HCl. The standards (0.25-10 ppm) measured by ICP-OES were 2 SO 4 The standards (4-1000 ppb) for ICP-MS measurements were prepared by serial dilution in 3% HNO 3 The scattering data for PDF analysis were collected at beamline 11-ID-B at the Advanced Photon Source (APS) at Argonne National Laboratory (ANL). High-energy X-rays (58.66 keV, ) was used in combination with a Perkin Elmer amorphous silicon-based area detector. The samples were loaded into Kapton capillaries for PDF measurements under ambient conditions. PDF measurements were collected on NU-1000 samples containing selenate or selenite by exposing 60 frames / 2 seconds each time. The 2-D scattering images were integrated using the software Fit2D to obtain 1-D scattering intensity data. The structure function S(Q) was obtained in the software PDFgetX3. The direct Fourier transform of the simplified structure function F(Q)=Q[S(Q)-1] leads to the simplified pair distribution function G(r), where Q max =23A -1 The contribution of the original MOF was measured under exactly the same conditions and subtracted to obtain the differential PDF (dPDF). The dPDF data shows the new contribution from the Se atomic correlation. The Se coordination pattern (η) of the MOF Zr-cluster was constructed in CrystalMaker. 2 μ 2 or μ 2 ) model. Using PDFGui 32 The PDFs of both models are simulated and compared with the experimental results.
[0074] Initial selenite / selenate uptake studies were performed by exposing 10 mg of MOF to 5 mL of a 100 ppm aqueous selenium solution as either sodium selenite or sodium selenate in a 15 mL polypropylene centrifuge tube. Control solutions of 100 ppm sodium selenite and sodium selenate were also prepared. The solutions were centrifuged for 1 min to allow the MOF to settle to the bottom of the tube. After 72 h, 0.5 mL of the supernatant was removed and lysed in 3% H 2 SO 4 The samples were diluted to 10 mL in 4% ethanol for ICP-OES measurement. ICP-OES was used to determine the concentrations of Se, Zr, and Na in each solution. The control solution was compared with the solution containing MOF to determine the amount of selenate or selenite adsorbed by MOF.
[0075] In a 15 mL polypropylene centrifuge tube, 10 mg of UiO-66-(NH 2 ) 2 、UiO-66-NH 2 Kinetic studies were performed by exposing NU-1000 to 5 mL of 100 ppm aqueous selenium solution as sodium selenite or sodium selenate. The solution was centrifuged for 1 min to allow the MOF to settle to the bottom of the tube. 0.5 mL aliquots of the supernatant were removed at 3, 27, and 72 hours and spun at 3% H 2 SO4 The samples were diluted to 10 mL in 4% ethanol for analysis by ICP-OES. ICP-OES was used to determine the concentrations of Se, Zr, and Na in each solution. The control solution was compared with the solution containing MOF to determine the amount of selenate or selenite adsorbed by the MOF each time.
[0076] The maximum uptake of each node of NU-1000 was determined by exposing 2 mg of NU-1000 to 5 ml of sodium selenite or sodium selenate aqueous solution in a 15 ml polypropylene centrifuge tube, where the selenium concentration was 30 ppm, 45 ppm, 60 ppm, 75 ppm, 90 ppm, and 105 ppm. These concentrations correspond to the maximum uptake of each MOF node (i.e., Zr 6 The solution was centrifuged for 1 minute to allow the MOF to settle to the bottom of the tube. An aliquot of the supernatant was removed and spun in 3% H 2 SO 4 The samples were diluted to 10 mL in 1% PBS for analysis by ICP-OES. ICP-OES was used to determine the concentrations of Se, Zr, and Na in each solution. The control solution was compared to the solution containing MOF to determine the amount of selenate or selenite anions adsorbed per node of NU-1000.
[0077] Low concentration kinetic studies were performed by exposing six 2 mg samples of NU-1000 to 5 mL of a 1 ppm aqueous solution of selenium as sodium selenite or sodium selenate in 15 mL polypropylene centrifuge tubes. The solutions were centrifuged for 1 min to allow the MOF to settle to the bottom of the tube. 2895 μL aliquots of the supernatant were removed from each solution at different times (5 min, 10 min, 15 min, 30 min, 60 min, and 180 min) and heated in 3% HNO 3 The samples were diluted to 3 mL in HCl for analysis by ICP-MS. ICP-MS was used to determine the concentrations of Se, Zr, and Na in each solution. The control solution was compared to the solution containing MOF to determine the amount of selenate or selenite adsorbed by the MOF each time. The studies were conducted in the same manner at 40°C and pH 6. For testing at 40°C, the selenate solution and the selenite solution were heated in a beaker filled with Lab ARMOR BEADS and tested at pH 6, thereby preparing the selenate solution and the selenite solution in pH 6 HCl.
[0078] The amount of selenate or selenite adsorbed per gram of NU-1000 was determined by exposing 5 mg of NU-1000 to 10 mL of an aqueous solution of sodium selenite or selenate in a 15 mL polypropylene centrifuge tube, wherein the solution had a concentration of about 18 ppm, 27 ppm, 36 ppm, 45 ppm, and 55 ppm. These concentrations correspond to 100% selenite or 55% selenite per gram of NU-1000. 6 The exposure levels of 1.00 analyte, 1.50 analyte, 2.00 analyte, 2.50 analyte, and 3.00 analyte molecules were determined. The solution was centrifuged for 30 seconds to allow the MOF to settle to the bottom of the tube. An aliquot of the supernatant was removed and the supernatant was stirred at 3% H2O at 1 min, 2 min, 3 min, 4 min, 5 min, 10 min, 15 min, 30 min, 60 min, 90 min, 120 min, and 180 min. 2 SO 4 The MOF-containing solutions were diluted to 10 mL for analysis by ICP-OES. ICP-OES was used to determine the concentrations of Se, Zr, and Na in each solution. The control solutions were compared to those containing MOF for determining the amount of selenate or selenite adsorbed by NU-1000 (q) in mg / g, where q = (Ci-Cf) x V / m, Ci = initial concentration, Cf = final concentration, V = volume of solution exposed to NU-1000, and m = mass of NU-1000 in g.
[0079] As described above, Zr-based MOFs including, for example, NU-1000 and MOF-808 can remove other oxygen anions, such as oxygen anions of aluminum (i.e., water-soluble aluminum oxides / hydroxides), silicon (i.e., silicates and hydrogen silicates), phosphorus (e.g., phosphates and hydrogen phosphates), sulfur (i.e., sulfates), chlorine (e.g., chlorates and perchlorates), pyrochloride (i.e., water-soluble oxides / hydroxides of pyrochloride), arsenic (e.g., arsenates), tin (i.e., stannates), antimony (e.g., antimonates and antimonites), iodine (e.g., iodates, periodates, and iodites), and lead (i.e., water-soluble oxides / hydroxides of lead).
[0080] In some embodiments, Zr-based MOFs including NU-1000 are used to adsorb antimony oxyanions, including Sb[III] (antimonite) or Sb[V] (antimonate) oxyanions in the redox state. Antimony is used as a neutron source (paired with beryllium) in pressurized water reactors, and, therefore, is a component of wastewater produced by nuclear power plants. Antimony is also released from the fuel oxide layer into the primary coolant water during nuclear power plant shutdowns, resulting in severe radiation doses to personnel and the surrounding environment. Common forms of antimony present in aqueous solution under oxidizing conditions include Sb(OH) 6 - HSbO 2、Sb(OH) 3 and Sb(OH) 4+ Therefore, Zr-based MOFs including NU-1000 can be used to remove antimony oxyanions, including those listed above, from these sources.
[0081] NU-1000 was exposed to Sb(OH) corresponding to 2-7 Sb / node 6 - The concentration of Sb(OH) adsorbed by NU-1000 was shown in Table S3. 6 - Use b(OH) 6 - Antimony adsorption per node of NU-1000 after 24 and 48 hours as an antimony source.
[0082] Table S3: Use of b(OH) 6 - Antimony adsorption per node of NU-1000 after 24 and 48 hours as an antimony source.
[0083]
[0084] Fig.17A -B shows Sb(OH) 6 - Uptake over time, expressed as uptake per node. 6 Node Sb(OH) 6 - The concentration of Sb(OH) was tested to determine 6 - Uptake over time. Aliquots were taken from each solution at 1 minute, 5 minutes, 10 minutes, 15 minutes, 30 minutes, 60 minutes, 90 minutes, 120 minutes, 180 minutes, 240 minutes, 300 minutes, 360 minutes, 420 minutes, 1440 minutes, 1800 minutes and 2880 minutes. These show the uptake of Sb(OH) 6 - The adsorption kinetics in NU-1000 were fast, with more than 60% of the total capacity reached in less than 1 min. Fig.18 Shows from Fig.17A Langmuir fitting of the Sb adsorption isotherm of α-B. Fig.18 Shows Sb(OH) in NU-1000 6 _The maximum adsorption capacity is 260 mg / g (or only 142 mg / g Sb).
[0085] Fig.19 NU-1000 and Sb(OH) 6 - Powder X-ray diffraction pattern of NU-1000. This shows that NU-1000 has a high adsorption capacity when Sb(OH) is adsorbed. 6 - Stability after PXRD, nitrogen adsorption-desorption isotherms and ICP-OES measurements were used to determine the overall crystallinity, porosity and Zr leaching, respectively. The PXRD pattern showed that the overall crystallinity of NU-1000 after adsorption remained unchanged. Fig. 20 NU-1000 and Sb(OH) 6 - Nitrogen isotherm of NU-1000. This shows that the surface area of the material is reduced to approximately the value expected from the addition of mass to the framework. Finally, no Zr leaching from the framework was observed by ICP-OES.
[0086] Similar to the adsorption of selenium oxyanions, the adsorption of lead oxyanions using Zr-based MOFs including NU-1000 and MOF-808 is contemplated. As previously identified above, lead that forms oxyanions in caustic solutions is believed to be associated with intergranular corrosion / stress corrosion cracking of nuclear power plant steam generator tubes. Therefore, it would be beneficial to remove these oxyanions from the relevant liquid streams, which contain Ph[II] or Pb[IV] redox states, such as Pb(OH) 6 2- 、Pb(OH) 6 4- , PbO 3 2- and PbO 2 2- It is also understood that, similar to the adsorption of selenium oxyanions, adsorption of iodine oxyanions using Zr-based MOFs comprising NU-1000 and MOF-808 is contemplated.
[0087] It should be understood that in some embodiments, the MOFs of the present invention provide adsorption of oxygen anions even in the presence of other species that may compete for adsorption sites on the MOF. Specifically, in some liquid streams, such as in a liquid stream in a flue gas desulfurization system, oxygen anions of boron and sulfur in the liquid phase may compete for adsorption sites on the MOF. However, even in the presence of these species, it has been found that the MOFs of the present invention still provide adsorption of oxygen anions. Those skilled in the art will understand that when determining the concentration of the MOF to be used in the liquid stream of interest, the concentrations of various species should be considered, including the oxygen anions to be adsorbed and any competing species.
[0088] Tables S4, S5, and S6 show the results of testing using NU-1000 in samples of the FGD liquid stream before and after the addition of NU-1000. (Regarding Table S4, it should be recognized that the Stage 1 FGD wastewater may contain more selenate / selenite in particulate form than soluble oxyanions, which may account for the relatively small amount of adsorption after exposure to the MOF.)
[0089] Table S4: FGD wastewater (10 mL) before and after treatment with NU-1000 (10 mg)
[0090]
[0091] Table S5: FGD wastewater (10 mL) before and after treatment with NU-1000 (10 mg)
[0092] Sample name selenium sulfur boron sodium Phase 3 - FGD (before) 19.6ppb 865.3ppm 19.5ppm 147.0ppm Using NU-1000 (after) 2.3ppb 788.0ppm 18.4ppm 146.8ppm
[0093] Table S6: Se uptake from FGD wastewater using different amounts of NU-1000
[0094]
[0095]
[0096] Regarding Tables S4 and S5, 10 mg of NU-1000 was added to 10 mL of wastewater, which is equivalent to 15B / Zr 6 Node, 26S / Zr 6 Node and only 0.007Se / Zr 6The exposure level of the node, which is a very challenging competitive condition. Table S4 shows the B, Se and S levels in the wastewater after treatment with NU-1000, and the MOF absorbed only 100ppb B, 43ppb Se and 160ppb S. Given that the exposure levels of B and S are 2100x and 3700x of Se, respectively, NU-1000 is still able to adsorb Se. Therefore, in some embodiments, in the presence of ions present in a range of 100-10,000x the concentration of selenium oxyanions, adsorption of selenium oxyanions still occurs.
[0097] Referring to Table S6, different amounts of NU-1000 (50 mg, 25 mg, 10 mg, 5 mg) were tested for SeOx removal from stage 3 FGD water 2- , and data points were obtained at shorter times (5 minutes, 10 minutes, 30 minutes). This shows the minimum amount and shortest time of MOF that may achieve the desired results. It is obvious from Table S6 that the effluent concentration of residual oxygen anions in the power plant water samples decreases with increasing amounts of MOF and exposure time. MOF exposure time and MOF loading improvements appear to be equivalent in their ability to improve oxygen anion uptake.
[0098] The Zr-based MOFs of the present invention can be within a range of crystalline sizes and still provide the adsorption of oxygen anions described above. In some embodiments, the crystalline size of NU-1000 can be within a range of about 75-5000nm. In some embodiments, the crystalline size of NU-1000 can be within a range of about 75-1200nm or about 300-5000nm. In some embodiments, NU-1000 can be within a range of 75-1200nm. In some embodiments, the MOFs of the present invention can have relatively large pores, such as up to about 30A or larger, which facilitates diffusion of analytes and improves uptake kinetics. It should be understood that larger pore MOFs will allow oxygen anions to diffuse into available nodes for easier uptake compared to smaller geometries.
[0099] In use and according to one embodiment of the present invention, the MOF of the present invention can be used to selectively remove specific species from a liquid stream. In general, it should be understood that the amount of MOF required will depend on several factors. For example, for a specific analyte to be removed (e.g., iodine containing iodate oxyanions), the Langmuir adsorption capacity (number of moles of ions per unit weight of MOF) can be obtained to determine the amount of MOF required to contact the liquid stream or influent stream, for example, in a desalter bed, in combination with the influent stream concentration of the stream or analyte to be treated. Other factors include the adequacy of contact between the liquid stream and the MOF on the substrate, which will depend on the geometry or design of the corresponding equipment used for contact between the liquid stream and the MOF, as well as the loss of MOF during any loading or unloading of the substrate, such as loading or unloading beads in a desalter or other equipment being used. In the case of a desalter, it should be understood that the desalter beads can be a mixture of beads or a mixed bed of beads containing beads for both cation removal (e.g., by ion exchange) and anion removal (by MOF). In this case, the amount of contact between the liquid stream and the MOF beads will also need to be specifically considered when determining the amount of MOF beads to be used.
[0100] A specific MOF can be connected to any structure for promoting contact between a liquid stream having a specific species to be removed and the MOF. For example, the MOF can be connected to a pre-coated filter / desalter or a stand-alone packed column, including such devices that have been used in a given facility or power plant (e.g., existing containers for ion exchange). For example, the MOF can be pre-coated on a filter braid of an existing filter desalter or similar filter system. Thereafter, the structure can be appropriately installed to allow contact between the liquid stream and the MOF on the structure. For example, using a desalter or similar filter coated with MOF, the liquid or water to be treated will flow through the filter braid, such as from the outside of a cylindrical filter through the filter fibers and into the inner cavity to allow contact between the MOF and the water. Once in contact with the liquid stream, the specific species to be removed is adsorbed onto the MOF, thereby reducing the concentration of the species in the liquid stream.
[0101] Because there are established chemistries in the literature for varying the metal component of a MOF, one sufficiently skilled in the art should be able to produce MOFs related to NU-1000 that contain less expensive metal components, such as using a zirconium metal precursor that is only 90% pure and contains hafnium. In fact, in the present invention, one embodiment was tested in which a NU-1000 MOF analog contained a 9:1 ratio of Zr:Hf within the node component. In experiments similar to those specified above for NU-1000 itself, it was found that the 90% Zr / 10% Hf MOF did exhibit similarly excellent node uptake of selenium-derived oxyanions (i.e., 90% to as high as 95% uptake observed with pure Zr NU-1000 MOF), meaning that it should be possible to reduce commercial costs by using less pure zirconium starting materials to prepare NU-1000.
[0102] Similarly, since there are established chemistries in the literature for modifying the linker moiety of MOFs, such as SALE (Solvent-Assisted Linker Exchange) and SALI (Solvent-Assisted Ligand Incorporation: see, e.g., P. Deria, W. Bury, JT Hupp and OK Farha, "Versatile Functionalization of the NU-1000 Platform by Solvent-Assisted Ligand Incorporation", Chemical Communications 2014, 50, 1965-1068; and P. Deria, JE Mondloch, O. Karagiardi, W. Bury, JT Hupp and OK Farha, "Beyond Post-Synthesis Modification: Evolution of Metal-Organic Frameworks via Building Block Replacement" Replacement," Chem. Soc. Rev., 2014, 43, 5896-5912), those skilled in the art should be able to devise appropriate algorithms to apply such chemistries to introduce appropriate ligand functionality that further attracts oxygen anions (such as selenate and selenite) into the NU-1000 or MOF-808 cavities to enhance the overall binding capacity of the material for these analyte species and thus improve the engineering of water treatment functions using these media. In the specific case of selenate or selenite, one linker chemistry expected by experts in the field of theoretical bond calculations is a functionalized urea chemistry, such as a pyridyl-urea that remains pendant on a carbon or ether oxygen linear chain of sufficient length (e.g., six to twelve elemental carbon or oxygen atoms in length) to allow the urea-derived ligand to contact the selenoxy anions that penetrate the MOF cavity with appropriate terminal groups to connect the ligand to the MOF cavity and pore-forming components.
[0103] Finally, as is well known, an expert in the art should generally be able to derive a procedure for regenerating anion removal media by acid treatment, such as, but not limited to, hydrochloric acid washing, sulfuric acid washing, or nitric acid washing, in order to recover previously used removal media for reuse with the overall goal of reducing operating costs. Thus, an expert in the art should be able to subject the MOF to similar acid washing techniques to regenerate NU-1000 or MOF-808 for continued reuse after saturation with oxyanion impurities, thereby reducing the overall cost of water treatment operations employing MOFs to an economically viable level.
[0104] As noted, the present invention also describes methods for connecting a MOF to a substrate to form a product containing a MOF, which can be used in a variety of ways depending on the specific MOF connected to the substrate. It should be understood that the substrate can be any substrate that can be connected to a given MOF and is suitable for use in an environment or process where certain chemical species or compounds are removed from a liquid or liquid stream. In some embodiments, the substrate can be an inert substrate to avoid any chemical interaction with the treated liquid or liquid stream. In some embodiments, the physical shape of the substrate allows it to be deployed and used in a given process or in a specific type of processing equipment for removing certain chemical species from a given liquid stream. In some embodiments, the substrate can be a bead or multiple beads. In some embodiments, the beads can be inert polypropylene polymer resin beads. In some embodiments, the substrate can be a macroscopic fabric, such as a mesh material or a mesh filter. In some embodiments, the substrate can be a molecular fabric prepared from organic chains, essentially consisting of a two-dimensional copolymer backbone or an organic woven material.
[0105] It should be understood that the following description of methods for connecting a given MOF to a substrate and the description of methods for using a substrate with the connected MOF refer to MOFs in general. However, it should be understood that in all embodiments described herein, the above-mentioned specific MOFs can be used. Therefore, it should be understood that while some of the above-mentioned specific MOFs are capable of removing or being configured to remove specific liquid phase anionic species, other MOFs capable of removing other liquid phase species from a liquid or liquid stream can be similarly used and connected to a given substrate. In addition, although the following methods are described with reference to specific substrates, it should be understood that other substrates, including substrates with different chemical compositions or with different geometries, can be used in any combination with any suitable MOF.
[0106] In general, the method used to connect a given MOF particle to a substrate can depend on the specific substrate used. Thus, the following describes a method for connecting a given MOF comprising any suitable MOF and including NU-1000 and MOF-808 to beads comprising a plurality of beads, a macroscopic fabric such as a mesh fabric or mesh filter, and a molecular fabric made of organic chains, which consists essentially of a two-dimensional copolymer backbone or an organic woven material.
[0107] In some embodiments, a given MOF can be attached to a substrate as a bead or multiple beads. In some embodiments, the beads can be inert polypropylene polymer resin beads. In some embodiments, the beads are used to remove anions, including selenium oxyanions, including selenite (SeO 3 2- ) and selenate (SeO 4 2-) oxygen anions; antimony oxygen anions, including oxygen anions in the redox state of Sb[III] (antimonite) or Sb[V] (antimonate); lead oxygen anions, including oxygen anions in the redox state of Pb[II] or Pb[IV], such as Pb(OH) 6 2- 、Pb(OH) 6 4- , PbO 3 2- and PbO 2 2- Oxygen anions; and iodine, such as IO 3 - (iodate) oxygen anion.
[0108] In general, the method for attaching MOF is performed using a buffer modifier that adheres the MOF to the bead surface. In some embodiments, the buffer modifier can be a buffer modifier commonly used for capillary electrophoresis, such as a permeation flow modifier, including hexadecyl-trimethylammonium bromide (CTAB) and β-cyclodextrin (β-CD). Both CTAB and β-CD are compounds that bind well to MOF particles at room temperature and cause the MOF to be chemically adsorbed onto the bead surface.
[0109] In one embodiment, CTAB can be used to connect MOF to the surface of beads. In this case, atomic layer deposition (ALD) is used to seed the beads with metal oxides, which provide surface hydroxyls that can form chemical bonds with MOF particles by CTAB. In certain embodiments, metal oxides are chemically adsorbed to the surface of beads in water, thereby making hydroxyls available for connection to CTAB by, for example, the cationic head group of CTAB. These metal oxides include, but are not limited to, aluminum oxide, titanium oxide, zinc oxide, and combinations thereof. Once exposed to water, in the reverse application of the capillary electrophoresis permeation flow of CTAB, deposited metal oxides similar to silicon dioxide / surface hydroxides will appear. Therefore, MOF is then connected to CTAB by hydrogen bonds, electrostatic interactions, and van der Waals forces. Not limited by theory, it is believed that the non-polar surface of MOF, such as the trimethyl "arm" of the organic linker of MOF, is connected to CTAB.
[0110] In one embodiment using CTAB, the beads can first be subjected to ALD to chemically adsorb the metal oxide to the surface of the beads. Separately, CTAB and MOF can be combined at room temperature to connect MOF to CTAB and form a solution of CTAB connected to MOF. The beads connected to the metal oxide can then be contacted with a solution or combined with CTAB having the connected MOF, thereby causing CTAB to be connected to the bead surface through the metal oxide, and again, this can be performed in an aqueous solution at room temperature and in an alkaline aqueous solution in some embodiments. Alternatively, the beads after ALD is performed to connect the metal oxide can be mixed in an aqueous solution containing MOF, and in some embodiments, it is mixed in an alkaline aqueous solution containing MOF. Subsequently, CTAB can be added to the solution to connect both MOF and the metal oxide, thereby causing MOF to be connected to the bead surface. Thereafter, the beads can be washed and dried. Therefore, at this point, MOF adsorption beads, such as multiple MOF adsorption polypropylene beads, have been produced, and can constitute a commercial product that can be used as further described below.
[0111] In another embodiment, β-CD can be used to connect MOF to the surface of the beads. In this case, the substrate does not need to be subjected to ALD. Instead, the non-polar regions of β-CD will be connected to the corresponding non-polar parts of the polypropylene beads through hydrogen bonds, electrostatic interactions, and van der Waals forces. The MOF can then be connected to β-CD by the interaction between one or more polar parts on the MOF surface and the negative charges on the β-CD. In some embodiments, MOF can be connected to the beads in an aqueous solution containing β-CD. In some embodiments, a less polar solvent such as an alcohol can be used. Thereafter, the beads can be washed and dried. Therefore, at this point, MOF adsorption beads, such as a plurality of MOF adsorption polypropylene beads, have been produced, and can constitute a commercial product that can be used as further described below.
[0112] It should be understood that in some embodiments, both β-CD and CTAB may be used in combination. In this case, the substrate or beads would be subjected to ALD, after which a solution containing both the MOF and CTAB and β-CD would be added.
[0113] It should also be understood that in some embodiments, the surface of the beads for functionalization of CTAB and β-CD can be silica. In some cases, a silane hydroxide chemistry can be used to functionalize the polymer beads to accept the silicon adduct, followed by a hydroxide to provide the chemistry required to attach CTAB or β-CD.
[0114] It will be appreciated that in some embodiments, the ion exchange resin beads are polystyrene divinylbenzene crosslinked (2-12%) copolymer beads that are functionalized in the pores by attaching the exchange ligand chemistry to pendant benzyl rings from the polymer backbone. In such cases, in order to achieve adequate water washing of the anion beads from the mixed bed in the case of replacement of the MOF coated substrate beads, the density of the latter beads needs to match that of the anion exchange resin beads. Further, there are several choices for polypropylene depending on the local stereochemistry of the propylene adduct during the free radical polymerization process.
[0115] Thus, in some embodiments, a process for preparing an appropriate plurality of beads for use, for example, in a power plant desalter deep bed would include: determining the MOF specific gravimetric capacity for the analyte / oxyanion of interest; calculating the amount of MOF that would need to be associated with each bead, thereby allowing an assessment of the number concentration of MOF-coated beads in water that would have to be flushed into an existing desalter deep bed pre-existing in the process stream; testing the density balance of existing anion exchange beads within the power plant desalter deep bed and examining the potential for exchange between these beads and the MOF-coated beads through typical power plant flushing methods; and adjusting the MOF-coated bead number concentration to account for the loss of beads in the preceding steps.
[0116] In another embodiment, the present invention includes a method for connecting a MOF to a macroscopic fabric for subsequent use. In some embodiments, the macroscopic fabric can be any fabric, including a material based on artificial fibers that can be connected to a given MOF. In some embodiments, the macroscopic fabric is a mesh material or a mesh filter, including a mesh material or a filter based on inert polypropylene. Therefore, it should be understood that the fabric can have any size, such as any area or surface area, as desired or determined by the final use of the fabric. The MOF particles can be connected to the fibers of the fabric in the same manner as described above for connecting to beads. Therefore, it should be understood that buffer modifiers, such as β-CD and CTAB, can be used in combination with the ALD treatment of the fabric as described above to connect the MOF to the fabric. After the MOF is connected to the macroscopic fabric, a macroscopic fabric adsorbed with MOF has been produced and can constitute a commercial product that can be used as further described below. It should be understood that the term "macro" is used to distinguish whether this fabric is a fabric visible to the naked eye or a fabric that can be physically manipulated by hand, rather than a molecular fabric as described below.
[0117] In another embodiment, the present invention includes a method for connecting a MOF to a molecular fabric for subsequent use. In some embodiments, the molecular fabric is made of organic chains, essentially forming a two-dimensional copolymer backbone or an organic woven material, to which a given MOF can be connected. The MOF particles can be connected to the chains of the fabric in the same manner as described above for connecting to beads. Therefore, it should be understood that buffer modifiers such as β-CD and CTAB can be used in combination with the ALD treatment of the fabric as described above to connect the MOF to the fabric. After the MOF is connected to the molecular fabric, a MOF-adsorbed molecular fabric has been produced and can constitute a commercial product that can be used as further described below. It should be understood that the molecular fabric is a fabric formed at the molecular level, and therefore its size is much smaller than, for example, the above-mentioned macroscopic fabric.
[0118] Once connected, the substrate with the connected MOF can be used to remove certain chemical species from a liquid or liquid stream, such as an industrial liquid stream (e.g., a power plant coolant stream, such as a nuclear power plant stream) or a waste stream. Typically, the substrate with the connected MOF will be positioned to allow contact between a liquid containing one or more liquid species to be removed from the liquid and the MOF. After contact, the liquid species to be removed will be connected to the MOF and thus removed from the liquid. In this regard, the manner in which the substrate with the MOF connected is used depends on the specific MOF connected and the liquid phase species that can be removed, as well as the physical configuration of the inert substrate (e.g., beads or fabric) used.
[0119] In the case of beads, certain chemical species can be removed from a liquid in the same manner as conventional resin beads, for example, by placing the beads in a resin bed in a given container through which the liquid to be treated will pass. It should be understood that existing equipment designed to manage resin beads can be adjusted to manage the use of beads coated with MOF particles if necessary. In one embodiment, a cylindrical container containing a bead bed coated with MOF particles can be used. In this case, the bead bed will be stationary within the container, and the liquid feed stream will pass through the container, thereby passing through the bead bed and providing contact between the liquid containing the liquid species to be removed and the MOF particles. After contact, the liquid species to be removed will connect to the MOF and thereby remove it from the liquid passing through the container.
[0120] It should be understood that in some embodiments where the container contains resin beads for removing certain liquid phase species, such resin beads can be replaced with beads coated with a given MOF according to the present invention. In one embodiment, when it is necessary to replace the resin beads, it can be easily replaced with beads coated with a given MOF according to the present invention in the same device. Alternatively, the resin beads can be replaced with inert polypropylene beads, and the connection of the selected MOF can be carried out in situ. In this case, the beads can be pre-treated with ALD to connect a given metal oxide, and then placed in the container, or such treatment can also be carried out in situ with ALD to connect the metal oxide. In the latter case, the beads will be placed in the container, and then treated with ALD to connect the metal oxide. Thereafter, a solution containing CTAB and the selected MOF can be added to the container to connect CTAB and MOF to the beads, or a solution of CTAB can be added to the container, followed by a solution of the selected MOF. The result will be to replace the original resin beads with beads coated with the selected MOF without changing or altering any existing equipment for the original resin beads.
[0121] Alternatively, the beads would be placed in a container, and thereafter, a solution containing β-CD and the selected MOF could be added to the container to attach the β-CD and MOF to the beads, or a solution of β-CD could be added to the container followed by a solution of the selected MOF. The result would be replacement of the original resin beads with beads coated with the selected MOF without modifying or changing any existing equipment used for the original resin beads.
[0122] In the case of a macroscopic fabric coated with a selected MOF, such a fabric can be positioned or placed so that a liquid stream will pass through the fabric, thereby providing contact between the liquid containing the liquid species to be removed and the MOF particles attached to the fibers of the fabric. After contact, the liquid species to be removed will be attached to the MOF and thereby removed from the liquid passing through the fabric. It should be understood that the fabric can be placed in a container or pipe or any kind of equipment so that the liquid will pass through the fabric.
[0123] In one embodiment, a desalter through which a liquid stream passes can be used. In this case, the macrofabric can be a mesh filter that can be wound into a spiral, thereby creating an inner cavity in the center. The liquid can enter the desalter and surround the outside of the wound mesh filter. The liquid will then pass through the wound mesh filter and enter the inner cavity or center of the desalter and flow out through the center of the desalter. It should be understood that in some embodiments, the existing mesh filter can be coated with the selected MOF. In this case, the MOF can be connected in situ to the existing mesh filter in the same manner as described above for in situ coating of beads in an existing container.
[0124] It should also be understood that MOF coated fabrics can be used in many different situations. In one embodiment, MOF coated fabrics can be used on top of a resin bed to facilitate removal of liquid species, provide removal of other liquid species relative to those removed by the resin bed, or otherwise remove the same or similar species. In addition, it should be understood that in embodiments where a bead bed is in-situ coated with a selected MOF, the macroscopic fabric used on top of the bed can also be in-situ coated with a selected MOF and be applied simultaneously with the coating of the bead bed. Therefore, it should also be understood that the MOFs used for beads and fabrics can be the same or different, noting that if different, either the beads or fabric may need to be coated before both are placed in a given container.
[0125] In the case of a molecular fabric coated with a selected MOF, such fabric can be positioned or placed so that a liquid stream will pass through the fabric, thereby providing contact between a liquid containing the liquid species to be removed and the MOF particles connected to the fibers of the fabric. After contact, the liquid species to be removed will be connected to the MOF, and thus it will be removed from the liquid passing through the fabric. It should be understood that the fabric can be placed in a container or a pipeline or any kind of equipment so that the liquid will pass through the fabric. It should also be understood that the molecular fabric can be generated in situ and thereafter connected to the selected MOF particles. In some embodiments, the molecular fabric can be constructed so that it is positioned at the outlet of a container, such as a container containing resin beads in a bed or desalter.
[0126] Regardless of the substrate used, however, it will be appreciated that for a given liquid stream and the concentrations of the various liquid phase components to be removed, the capacity of the selected MOF to remove those liquid phase components is generally much greater, such that saturation of the MOF is not limiting. Thus, using a substrate coated with MOF particles will still provide the surface area necessary to obtain the desired removal of a given liquid phase species, as compared to using, for example, a bed filled with MOF particles.
[0127] Various embodiments of the present invention have been described above. However, it should be understood that alternative embodiments are possible and the present invention is not limited to the specific embodiments described above. For example, in some embodiments, the adsorption of aqueous selenate and aqueous selenite can be obtained by a series of highly porous water-stable Zr-based MOFs. Among the seven MOFs examined, NU-1000 was found to show the highest gravimetric adsorption capacity and the fastest uptake rate. The results show that large MOF pores and a large number of node-based adsorption sites, i.e., replaceable unstable Zr (IV) coordination sites, are important for the rapid and effective adsorption and removal of selenate and selenite. Both anions show the importance of bridging (η 2 μ 2) in a manner that binds to the node, with one di-anion bridging the two zirconium metal centers. In contrast to many selenium restorative materials and related technologies that are only reasonably effective for selenite, NU-1000 exhibits a strong affinity for both selenate and selenite. In some embodiments, antimony oxyanions, including oxyanions in the redox state of Sb[III] (antimonite) or Sb[V] (antimonate); lead oxyanions, including oxyanions in the redox state of Pb[II] or Pb[IV], such as Pb(OH) 6 2- 、Pb(OH) 6 4- , PbO 3 2- and PbO 2 2- Oxygen anions; and iodine, such as IO 3 - Adsorption of oxyanions of (iodate) can be achieved through a series of highly porous, water-stabilized Zr-based MOFs. Further, adsorption of these species can be achieved even in the presence of competing species.
Claims
1. A method for reducing the oxyanion concentration of iodine in a liquid stream from a nuclear power plant, the method comprising: contacting a liquid stream from a nuclear power plant comprising oxyanions of iodine with a zirconium-based metal organic framework, wherein the zirconium-based metal organic framework comprises MOF-808; and The iodine oxyanions are complexed with the MOF-808, thereby reducing the concentration of the iodine oxyanions in the liquid stream.
2. The method of claim 1, wherein the contacting is performed using a desalter. The method of claim 1 , wherein the zirconium-based metal-organic framework is disposed on a substrate. The method of claim 3 , wherein the substrate comprises a plurality of polypropylene beads.
5. The method of claim 3, wherein the substrate comprises a macrotextile.
6. The method of claim 3, wherein the substrate comprises a molecular fabric comprising organic chains.
7. The method of claim 1, wherein the zirconium-based metal organic framework comprises MOF-808 before activation.
8. The method of claim 1, wherein the zirconium-based metal organic framework comprises activated MOF-808.
9. The method of claim 1, wherein the oxyanion comprises iodate.
10. The method of claim 1, wherein the complexing comprises η2μ2 binding.
11. A method for reducing the iodine oxyanion concentration of a power plant coolant stream, the method comprising: contacting a power plant coolant stream comprising oxyanions of iodine with a zirconium-based metal-organic framework, wherein the zirconium-based metal-organic framework comprises MOF-808; and The iodine oxyanions are complexed with the MOF-808, thereby reducing the concentration of the iodine oxyanions in the coolant stream.
12. The method of claim 11, wherein the contacting is performed using a desalter.
13. The method of claim 11, wherein the zirconium-based metal-organic framework is disposed on a substrate.
14. The method of claim 13, wherein the substrate comprises a plurality of polypropylene beads.
15. The method of claim 13, wherein the substrate comprises a macrotextile.
16. The method of claim 13, wherein the substrate comprises a molecular fabric comprising organic chains.
17. The method of claim 11, wherein the zirconium-based metal organic framework comprises MOF-808 before activation.
18. The method of claim 11, wherein the zirconium-based metal organic framework comprises activated MOF-808.
19. The method of claim 11, wherein the oxyanion comprises iodate.
20. The method of claim 11, wherein the complexing comprises η2μ2 binding.
Citation Information
Patent Citations
Application of metal-organic framework functional material
CN105214612A
Preparation method of modified zirconium-based metal-organic framework material MOF-808
CN113368824A
Methods of applying a sorbent coating on a substrate, a support, and / or a substrate coated with a support
US20130095996A1
Metal-Organic Frameworks for Adsorption of Liquid Phase Compounds
US20160318773A1
Metal-Organic Frameworks for Adsorption of Liquid Phase Compounds
US20180134581A1