Inorganic coating layer cross-linked separator
By using silane grafted modified polyolefin and crosslinked inorganic porous layer in the LIB separator, a stable crosslinking structure is formed, and the problem of insufficient cycle characteristics and safety in the prior art is solved, and a more efficient battery is achieved Performance and security.
Patent Information
- Application Number
- CN202180008639.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-04-13
- Filing Date
- 2021-01-08
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2041-01-08
AI Technical Summary
The existing LIB separators still have room for improvement in improving circulation characteristics and safety, and the crosslinked structure formed by light irradiation is uneven, resulting in deformation of LIB during heating.
A microporous film is made of a polyolefin resin containing silane grafted modified polyolefin, and a crosslinked inorganic porous layer is arranged on its surface, so that the peeling ratio of the inorganic porous layer is controlled to be 0 to 35% to form a stable crosslinked structure. .
The cycle characteristics and safety of the power storage device are improved, and the LIB deformation problem caused by the uneven crosslinked structure is avoided.
Smart Images

Figure CN114930630B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a separator for a power storage device, and more specifically, to a separator for a power storage device including an inorganic coating layer (inorganic porous layer) forming a crosslinked structure. Background Art
[0002] Microporous membranes are widely used as separation membranes or selective permeation separation membranes for various substances and insulating materials, and examples of their use include microfiltration membranes, separators for fuel cells and capacitors, or substrates for functional membranes for filling functional materials into pores to exert new functions, separators for power storage devices, etc. Among them, microporous membranes made of polyolefin resins are suitable for use as separators or constituent materials for lithium ion secondary batteries (LIBs) widely used in notebook personal computers, mobile phones, digital cameras, etc.
[0003] Here, in order to improve heat resistance, etc., a separator having a cross-linked coating layer (e.g., an inorganic porous layer containing inorganic particles and a resin binder) on the surface of a microporous membrane has been proposed (see Patent Documents 1 to 5). In addition, in order to ensure the safety of the battery, a technology has been proposed in which a cross-linked structure is formed in a microporous membrane by ring-opening norbornene by irradiation with ultraviolet rays, electron beams, etc. (see Patent Document 6).
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent No. 6187464
[0007] Patent Document 2: International Publication No. 2013 / 080938
[0008] Patent Document 3: Japanese Patent Application Publication No. 2015-211006
[0009] Patent Document 4: Japanese Patent Application Publication No. 2008-287888
[0010] Patent Document 5: Japanese Patent Application Publication No. 2014-179321
[0011] Patent Document 6: Japanese Patent Application Publication No. 2011-071128 Summary of the invention
[0012] Problem that the invention aims to solve
[0013] In recent years, the high density and high energy density of LIB are being promoted. Therefore, further improvements in the cycle characteristics and safety (for example, safety evaluated by battery destruction tests) of LIB are expected, and further improvements are also expected for LIB separators. However, the separators described in Patent Documents 1 to 5 still have room for improvement in seeking to improve the above-mentioned performance of LIB. In addition, when a cross-linked structure is formed in a microporous membrane by light irradiation as described in Patent Document 6, there is a situation where the light irradiation becomes uneven and the cross-linked structure becomes inhomogeneous. It can be considered that this is because the periphery of the crystalline part of the resin constituting the microporous membrane is easily cross-linked by light. If a microporous membrane with an inhomogeneous cross-linked structure is used as a separator for LIB, there is a situation where the LIB is deformed when heated. This problem exists not only in separators for LIB, but also in separators for power storage devices represented by LIB.
[0014] In view of the above problems, the object of the present invention is to provide a separator for a storage device that can further improve the performance of the storage device (for example, cycle characteristics and safety evaluated by device destruction or heating test). In addition, the object of the present invention is to provide a secondary battery and a storage device including the separator for the storage device.
[0015] Solutions for solving problems
[0016] The present inventors have repeatedly conducted in-depth research and found that the above-mentioned problems can be solved by making the separator for the power storage device contain a polyolefin resin microporous membrane containing a silane-grafted modified polyolefin and a cross-linked inorganic porous layer disposed on at least one surface thereof, and / or, disposing an inorganic porous layer on the polyolefin resin microporous membrane and controlling the peeling ratio of the inorganic porous layer from the polyolefin resin microporous membrane in the solvent immersion test within a specified range, thereby completing the present invention. That is, the present invention is as follows. (1)
[0018] A separator for an electric storage device, comprising a polyolefin resin microporous film and an inorganic porous layer disposed on at least one surface of the polyolefin resin microporous film.
[0019] The inorganic porous layer has at least one selected from the group consisting of (i) covalent bonds between inorganic particles, (ii) covalent bonds between resin binders, and (iii) covalent bonds between inorganic particles and resin binders.
[0020] The polyolefin resin microporous film includes a silane-grafted modified polyolefin, and when the power storage device separator comes into contact with an electrolyte solution, a silane cross-linking reaction of the silane-grafted modified polyolefin starts. (2)
[0022] The separator for a power storage device according to item 1, wherein the electrolyte solution is non-aqueous and contains a fluorine (F)-containing lithium salt. (3)
[0024] The separator for a power storage device according to item 1 or 2, wherein the polyolefin resin microporous film contains a polyolefin other than the silane graft-modified polyolefin. (4)
[0026] The separator for a power storage device according to any one of items 1 to 3, wherein the inorganic porous layer includes a crosslinked structure. (5)
[0028] A separator for an electric storage device, comprising a polyolefin resin microporous film and an inorganic porous layer disposed on at least one surface of the polyolefin resin microporous film.
[0029] In the solvent immersion test, the area of the inorganic porous layer peeled off from the polyolefin resin microporous membrane is 0 to 35% based on the area of the inorganic porous layer before the test. (6)
[0031] The separator for a power storage device according to item 5, wherein the inorganic porous layer has at least one selected from the group consisting of (i) covalent bonds between inorganic particles, (ii) covalent bonds between resin binders, and (iii) covalent bonds between inorganic particles and resin binders. (7)
[0033] The separator for a power storage device according to item 6, wherein the inorganic porous layer includes a cross-linked structure formed by at least one selected from the group consisting of the covalent bonds (i) to (iii). (8)
[0035] The separator for a power storage device according to any one of Items 5 to 7, wherein the polyolefin resin microporous film comprises a silane-graft-modified polyolefin. (9)
[0037] The separator for an electric storage device according to item 8, wherein a silane cross-linking reaction of the silane-graft-modified polyolefin starts when the separator for an electric storage device comes into contact with an electrolyte solution. (10)
[0039] The separator for a power storage device according to item 9, wherein the electrolyte is non-aqueous and contains a fluorine (F)-containing lithium salt. (11)
[0041] The separator for a power storage device according to any one of Items 8 to 10, wherein the polyolefin resin microporous film contains a polyolefin other than the silane graft-modified polyolefin. (12)
[0043] The separator for a power storage device according to any one of items 5 to 11, wherein the surface roughness of a region of the polyolefin resin microporous film facing the inorganic porous layer is 0.2 to 3.0 μm. (13)
[0045] The separator for a power storage device according to item 4 or 7, wherein in the inorganic porous layer, the crosslinked structure is formed by at least one selected from the group consisting of a nucleophilic substitution reaction, a nucleophilic addition reaction, an electrophilic addition reaction, and a silane coupling reaction. (14)
[0047] The separator for a power storage device according to any one of items 1 to 4, 6, 7, and 13, wherein the resin binder is in the form of an emulsion, a suspension, or a colloid. (15)
[0049] The separator for a power storage device according to any one of items 1 to 4, 6, 7, 13, and 14, wherein the resin binder has a nucleophilic substitution reactive functional group or a nucleophilic addition reactive functional group. (16)
[0051] The separator for a power storage device according to any one of items 1 to 4, 6, 7, and 13 to 15, wherein the nucleophilic substitution reactive functional group or the nucleophilic addition reactive functional group of the resin binder is at least one selected from the group consisting of a carboxyl group, a hydroxyl group, and an amino group. (17)
[0053] The separator for a power storage device according to any one of items 1 to 16, wherein the inorganic porous layer contains inorganic particles, and polar functional groups exist on surfaces of the inorganic particles. (18)
[0055] The separator for a power storage device according to any one of items 1 to 17, wherein the inorganic porous layer contains inorganic particles, and a silicon-containing functional group exists on the surface of the inorganic particles. (19)
[0057] The separator for a power storage device according to item 18, wherein the silicon-containing functional group is at least one selected from the group consisting of an alkoxysilyl group, a halogen-substituted silyl group, and a silazane group. (20)
[0059] The separator for a power storage device according to any one of items 1 to 19, wherein the inorganic porous layer contains a cross-linking agent. (twenty one)
[0061] The separator for a power storage device according to item 20, wherein the cross-linking agent has a nucleophilic substitution reactive functional group and / or an electrophilic addition reactive functional group. (twenty two)
[0063] The separator for a power storage device according to item 20 or 21, wherein the crosslinking agent has a nucleophilic substitution reactive functional group and an electrophilic addition reactive functional group. (twenty three)
[0065] The separator for a power storage device according to item 21 or 22, wherein the nucleophilic substitution reactive functional group of the crosslinking agent is an oxazoline group and / or an epoxy group. (twenty four)
[0067] The separator for a power storage device according to item 21 or 22, wherein the electrophilic addition-reactive functional group of the cross-linking agent is at least one selected from the group consisting of an isocyanate group, a thioisocyanate group, a carbodiimide group, an allene group, an oxime group, and a carbonyl group. (25)
[0069] A separator for a storage device according to any one of items 20 to 24, wherein the inorganic porous layer contains inorganic particles and a resin binder, polar functional groups exist on the surface of the inorganic particles, the cross-linking agent exists between the polar functional groups and the resin binder, and a cross-linking structure is formed by covalent bonds between the polar functional groups, the cross-linking agent and the resin binder. (26)
[0071] The separator for a power storage device according to any one of Items 20 to 25, wherein the cross-linking agent is in the form of an emulsion, a suspension, or a colloid. (27)
[0073] An electric storage device comprising an electrode, an electrolyte, and the separator for an electric storage device according to any one of items 1 to 26. (28)
[0075] A secondary battery comprising an electrode, an electrolyte, and the separator for an electrical storage device according to any one of items 1 to 26.
[0076] Effects of the Invention
[0077] According to the present invention, a separator for an electric storage device can be provided that can further improve the performance of the electric storage device (for example, cycle characteristics and safety evaluated by device destruction or heating test). In addition, according to the present invention, a secondary battery and an electric storage device having the separator can be provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0078] Figure 1 This is a diagram showing an example of a histogram used when deriving the ratio (%) of the peeling area according to one embodiment of the present invention.
[0079] Figure 2 This is a diagram showing another example of a histogram used when deriving the ratio (%) of the peeling area according to one embodiment of the present invention.
[0080] Figure 3 This is a diagram showing an example of a monochrome image according to one embodiment of the present invention.
[0081] Figure 4 This is a diagram showing an example of a binarized image according to one embodiment of the present invention. DETAILED DESCRIPTION
[0082] The following describes an embodiment of the present invention (referred to as "this embodiment"), but the present invention is not limited to this embodiment. The present invention can be modified in various ways without departing from the main purpose thereof. In this specification, unless otherwise stated, "to" means that the numerical values at both ends are included as the upper limit and the lower limit. In addition, in this specification, the upper limit and the lower limit of the numerical range can be arbitrarily combined. In addition, the term "separator for a storage device" is sometimes referred to as "separator" hereinafter.
[0083] <Separators for power storage devices>
[0084] The separator for an electricity storage device can be used in an electricity storage device, and can be disposed between the positive and negative electrodes of the electricity storage device, for example.
[0085] <Implementation method 1>
[0086] The separator for a power storage device of the first embodiment comprises a polyolefin resin microporous membrane containing a silane-grafted modified polyolefin and an inorganic porous layer disposed on at least one surface thereof, and may further comprise a layer other than the polyolefin resin microporous membrane and the inorganic porous layer as desired. The inorganic porous layer may be disposed on both sides of the polyolefin resin microporous membrane, or the inorganic porous layer may be disposed on one side of the polyolefin resin microporous membrane and a layer other than the polyolefin resin microporous membrane and the inorganic porous layer may be disposed on the other side of the polyolefin resin microporous membrane.
[0087] The inorganic porous layer of the separator of embodiment 1 has at least one selected from the group consisting of (i) covalent bonds between inorganic particles, (ii) covalent bonds between resin binders, and (iii) covalent bonds between inorganic particles and resin binders, and when the separator of embodiment 1 comes into contact with an electrolyte, a silane cross-linking reaction of the silane grafted modified polyolefin contained in the polyolefin resin microporous membrane begins.
[0088] The inorganic porous layer of embodiment 1 is arranged on at least one surface of the polyolefin resin microporous membrane. Therefore, the method of arranging the inorganic porous layer only on one surface of the polyolefin resin microporous membrane and the method of arranging the inorganic porous layer on both sides of the polyolefin resin microporous membrane are both included in the scope of embodiment 1. When the inorganic porous layer is arranged on both sides of the polyolefin resin microporous membrane, the inorganic porous layers of the same composition may be arranged, or the inorganic porous layers of different compositions may be arranged.
[0089] The inorganic porous layer of Embodiment 1 may contain inorganic particles and / or a resin binder.
[0090] The inorganic porous layer of Embodiment 1 may form a crosslinked structure by any of the covalent bonds (i) to (iii) or include a crosslinked structure.
[0091] The above-mentioned record does not mean that a cross-linked structure must be formed between the inorganic particles. For example, if a cross-linked structure is formed between the inorganic particles and the resin binder, then a cross-linked structure may not be formed between the inorganic particles. Similarly, the above-mentioned record does not mean that a cross-linked structure must be formed between the resin binder. For example, if a cross-linked structure is formed between the inorganic particles and the resin binder, then a cross-linked structure may not be formed between the resin binder.
[0092] That is, at least one of the above cross-linked structures may be formed in the inorganic porous layer. Among them, it is preferred that all of the covalent bonds (i) to (iii) form a cross-linked structure in order to facilitate the effect of the present invention.
[0093] It should be noted that the covalent bonds between inorganic particles, the covalent bonds between resin binders, and the covalent bonds between inorganic particles and the resin binder referred to in Embodiment 1 include covalent bonds interposed with a crosslinking agent as necessary.
[0094] The polyolefin resin microporous membrane of embodiment 1 contains silane grafted modified polyolefin as a polyolefin resin, and may contain polyolefins other than silane grafted modified polyolefin, additional components, etc. as desired. When the separator of embodiment 1 is in contact with the electrolyte, the silane grafted modified polyolefin can be cross-linked, so the timing of the silane cross-linking reaction can be controlled, thereby, for example, it is possible to achieve a cross-linking reaction in the manufacturing process of the separator instead of in the manufacturing process of the storage device or when the separator is arranged in the storage device, so that the separator can be prevented from being produced poorly and the safety of the storage device (for example, safety evaluated by device destruction or heating test) and improved cycle characteristics and high output can be achieved. From the viewpoint of the silane cross-linking reaction, the electrolyte in contact with the silane grafted modified polyolefin is preferably non-aqueous and / or preferably contains a fluorine (F)-containing lithium salt.
[0095] <Implementation method 2>
[0096] The separator for a power storage device of the second embodiment comprises a polyolefin resin microporous membrane and an inorganic porous layer disposed on at least one surface thereof, and may further comprise a layer other than the polyolefin resin microporous membrane and the inorganic porous layer as desired. The inorganic porous layer may be disposed on both sides of the polyolefin resin microporous membrane, or the inorganic porous layer may be disposed on one side of the polyolefin resin microporous membrane and a layer other than the polyolefin resin microporous membrane and the inorganic porous layer may be disposed on the other side of the polyolefin resin microporous membrane.
[0097] In the solvent immersion test of the separator of embodiment 2, the area of the inorganic porous layer peeled off from the polyolefin microporous membrane is 0 to 35% based on the area of the inorganic porous layer before the test. By setting the area to less than 35%, it is possible to suppress the inorganic porous layer peeled off from the polyolefin microporous membrane in the electrolyte from having an adverse effect on the charge and discharge reaction or reliability of the power storage device, and as a result, it is possible to provide a separator that can further improve the performance of the power storage device (for example, cycle characteristics and safety evaluated by a destruction test or a heating test of a device such as a battery). The area can be measured based on the method described in the embodiment.
[0098] The significance of the solvent immersion test described in the examples is as follows.
[0099] The electrolyte commonly used in the battery is a mixture of cycloalkyl carbonates such as propylene carbonate and linear alkyl carbonates such as ethyl methyl carbonate. In addition, each battery manufacturer adjusts their functional groups or formulations according to the battery design each time. The SP value (solubility parameter: Solubility Parameter) of the electrolyte will change with the adjustment, so it is not possible to evaluate the stripping caused by the infiltration of the electrolyte into the inorganic porous layer, the swelling of the inorganic porous layer and the structural destruction of the inorganic porous layer. Therefore, the solvent immersion test recorded in the embodiment can be carried out to appropriately evaluate the above area. For example, acetone is a solvent with a molecular weight lower than that of various electrolytes and a non-protonic polar functional group. Therefore, it is known from experiments that by using a relatively low molecular weight solvent (acetone, etc.) in the solvent immersion test, the solvent is immersed in the inorganic porous layer, so that the inorganic porous layer is easily swollen, which can cause the stripping caused by the structural destruction of the inorganic porous layer. Therefore, if a good evaluation result is obtained in the immersion test in the solvent described in the Examples, it can be judged that the electrolyte is also stable in other various electrolyte solutions.
[0100] One of the factors for controlling the area of the inorganic porous layer peeling off from the polyolefin microporous membrane is to control the crosslinking structure in the inorganic porous layer. Specifically, the area can be controlled by controlling the items related to the inorganic porous layer described in Tables 3 to 6 of Examples.
[0101] If a cross-linked structure is not formed in the inorganic porous layer, the resin binder in the inorganic porous layer swells due to the electrolyte, and the swollen resin binder is likely to fall off from the inorganic porous layer and enter the electrolyte. On the other hand, if a cross-linked structure is excessively formed in the inorganic porous layer, the flexibility of the inorganic porous layer is easily reduced, and as a result, the resin binder is likely to fall off from the inorganic porous layer and enter the electrolyte. That is, by appropriately forming a cross-linked structure in the inorganic porous layer, the swelling of the resin binder caused by the electrolyte can be suppressed and the appropriate flexibility of the inorganic porous layer can be ensured. Thus, the resin binder can be prevented from falling into the electrolyte, and it can be expected that the area of the inorganic porous layer peeled off from the polyolefin microporous membrane can be controlled to 0 to 35%. From the perspective of the shape stability of the separator during long-term use in a storage device such as a battery, the area of the inorganic porous layer peeled off from the polyolefin resin microporous membrane is preferably 0 to 30%, more preferably 0 to 15%, and further preferably 0 to 8%.
[0102] The inorganic porous layer of Embodiment 2 is arranged on at least one surface of the polyolefin microporous membrane. Therefore, both the method of arranging the inorganic porous layer only on one surface of the polyolefin microporous membrane and the method of arranging the inorganic porous layer on both sides of the polyolefin microporous membrane are included in the scope of Embodiment 2. When the inorganic porous layer is arranged on both sides of the polyolefin microporous membrane, the inorganic porous layers of the same composition may be arranged, or the inorganic porous layers of different compositions may be arranged.
[0103] From the viewpoint of controlling the performance of the power storage device, the cross-linked structure in the inorganic porous layer, and the like, the inorganic porous layer of the second embodiment preferably contains inorganic particles and / or a resin binder.
[0104] From the perspective of controlling the performance of the power storage device, the cross-linked structure in the inorganic porous layer, etc., the inorganic porous layer of embodiment 2 preferably has at least one selected from the group consisting of (i) covalent bonds between inorganic particles, (ii) covalent bonds between resin binders, and (iii) covalent bonds between inorganic particles and resin binders, and more preferably forms a cross-linked structure or includes a cross-linked structure through any of the covalent bonds (i) to (iii).
[0105] The above-mentioned record is not necessarily formed between inorganic particles crosslinked structure meaning. For example, if formed between inorganic particles and resin binder crosslinked structure, then the inorganic particles may not form crosslinked structure. Similarly, the above-mentioned record is not necessarily formed between resin binder crosslinked structure meaning. For example, if formed between inorganic particles and resin binder crosslinked structure, then the resin binder may not form crosslinked structure.
[0106] That is, at least one of the above cross-linked structures may be formed in the inorganic porous layer. Among them, it is preferred that all of the covalent bonds (i) to (iii) form a cross-linked structure in order to facilitate the effect of the present invention.
[0107] It should be noted that the covalent bonds between inorganic particles, the covalent bonds between resin binders, and the covalent bonds between inorganic particles and the resin binder referred to in Embodiment 2 include covalent bonds interposed with a crosslinking agent as necessary.
[0108] From the viewpoint of further improving the performance of the power storage device, the polyolefin resin microporous membrane of Embodiment 2 preferably contains a silane-grafted modified polyolefin as the polyolefin resin, and more preferably contains a polyolefin other than the silane-grafted modified polyolefin in addition to the silane-grafted modified polyolefin. The polyolefin resin microporous membrane may contain additional components other than the polyolefin resin as desired.
[0109] When the separator of the preferred embodiment 2 contacts the electrolyte, the silane crosslinking reaction of the silane grafted modified polyolefin contained in the polyolefin resin microporous membrane begins. When the separator of the embodiment 2 contacts the electrolyte, the crosslinking of the silane grafted modified polyolefin can be carried out, so the timing of the silane crosslinking reaction can be controlled, thereby, for example, it is possible to achieve a crosslinking reaction in the manufacturing process of the separator instead of in the manufacturing process of the storage device or when it is arranged in the storage device, so that the separator can be prevented from being produced poorly and the safety of the storage device (for example, safety evaluated by device destruction or heating test) and improved cycle characteristics and high output can be achieved. From the viewpoint of the silane crosslinking reaction, the electrolyte in contact with the silane grafted modified polyolefin is more preferably a non-aqueous system, and / or more preferably contains a fluorine (F) lithium salt.
[0110] In Embodiment 2, by controlling the surface roughness of the area of the polyolefin microporous membrane opposite to the inorganic porous layer within a specified range, it is easier to prevent the resin binder from falling off the inorganic porous layer. In Embodiment 2, it is precisely because the cross-linked structure is appropriately formed in the inorganic porous layer to ensure the desired adhesion between the inorganic porous layer and the polyolefin microporous membrane that the inorganic porous layer becomes susceptible to the influence of the control of the surface roughness of the polyolefin microporous membrane. In addition, by controlling the surface roughness of the polyolefin microporous membrane, it is easier to suppress the swelling of the resin binder caused by the electrolyte, and as a result, it can be expected that the area where the inorganic porous layer can be peeled off from the polyolefin microporous membrane can be controlled to 0 to 35%.
[0111] On the other hand, when the inorganic porous layer has no crosslinked structure or has excessively formed crosslinked structure, the inorganic porous layer is hardly affected by the control of the surface roughness of the polyolefin microporous membrane, and the concept of controlling the surface roughness of the polyolefin microporous membrane cannot be obtained.
[0112] Therefore, the surface roughness of the region of the polyolefin microporous membrane facing the inorganic porous layer is preferably 0.2 to 3.0 μm from the viewpoint of easily exhibiting the effects of the present invention.
[0113] Specifically, the surface roughness is preferably 0.20 μm or more, more preferably 0.21 μm or more, and further preferably 0.220 μm or more. On the other hand, the surface roughness is preferably 3.00 μm or less, more preferably 2.80 μm or less, and further preferably 0.80 μm or less. The surface roughness can be measured according to the method described in the examples, and can be controlled by changing various structures or various manufacturing conditions of the polyolefin microporous membrane.
[0114] The following describes the common components of the first and second embodiments and the preferred components of the two embodiments.
[0115] <Polyolefin resin microporous membrane>
[0116] The polyolefin resin microporous membrane (hereinafter sometimes referred to as "polyolefin microporous membrane") itself may be used as a separator in the past. The polyolefin microporous membrane is not limited to a single layer, and may include multiple layers. Therefore, for example, a laminated body formed by laminating multiple layers of different polyolefin microporous membranes containing polyolefin resins is also included in the polyolefin microporous membrane of embodiment 1 or 2.
[0117] The content of the polyolefin resin in the polyolefin resin microporous membrane is preferably 75 mass % or more, more preferably 85 mass % or more, further preferably 90 mass % or more, further preferably 95 mass % or more, particularly preferably 98 mass % or more, relative to the total mass of the polyolefin resin microporous membrane, and may be 100 mass %.
[0118] (Polyolefin resin)
[0119] As polyolefin resin, there is no particular limitation, and examples thereof include homopolymers of ethylene or propylene or copolymers formed by at least two monomers selected from the group consisting of ethylene, propylene, 1-butene, 4-methyl-1-pentene, 1-hexene, 1-octene and norbornene. Among them, from the viewpoint of not clogging holes and being able to perform heat setting (sometimes denoted as "HS") at higher temperatures, high-density polyethylene (homopolymer) or low-density polyethylene is preferred, and high-density polyethylene (homopolymer) is more preferred. In polyolefin resin, in addition to polyethylene, polyolefin resins other than polyethylene may be included, or polyolefin resins other than polyethylene may be included to replace polyethylene. As polyolefin resins other than polyethylene, polypropylene, polybutene, etc. may be listed. It should be noted that polyolefins may be used alone or in combination of two or more.
[0120] From the viewpoint of resistance to redox degradation and dense and uniform porous structure, the polyolefin resin microporous membrane preferably contains both silane grafted modified polyolefin and ultra-high molecular weight polyethylene (UHMWPE). It is known that the weight average molecular weight of ultra-high molecular weight polyethylene (UHMWPE) is generally above 1,000,000. More preferably, the mass ratio of silane grafted modified polyolefin to ultra-high molecular weight polyethylene in the separator (mass of silane grafted modified polyolefin / mass of ultra-high molecular weight polyethylene) is 0.05 / 0.95 to 0.40 / 0.60.
[0121] In addition, the polyolefin resin microporous film preferably includes a polyolefin having a weight average molecular weight less than 1200000. By using a polyolefin having a weight average molecular weight less than 1200000, there is a tendency to relax the polymer shrinkage in the early stage in the heating test of the storage device, and to be particularly easy to maintain safety in the heating safety test. From the same point of view, the weight average molecular weight of the polyolefin is more preferably less than 1000000, more preferably more than 100000 and less than 1000000, and particularly preferably more than 150000 and less than 800000. It should be noted that the use of a polyolefin having a weight average molecular weight less than 1000000 is compared with the use of a polyolefin having a weight average molecular weight of more than 1000000, and there is a tendency that the elastic modulus in the thickness direction of the obtained microporous film becomes smaller, so a relatively easy transfer core concave and convex microporous film can be obtained. The polyolefin having a weight average molecular weight within the above range may be contained in a ratio of preferably 40% by mass or more, more preferably 80% by mass or more, based on the total mass of the polyolefin resin included in the polyolefin microporous membrane.
[0122] (Silane grafted modified polyolefin)
[0123] The silane grafted modified polyolefin is composed of a structure in which the main chain is a polyolefin and an alkoxysilyl group is grafted onto the main chain. It should be noted that the alkoxide replaced with the alkoxysilyl group is not particularly limited, and examples thereof include methoxide, ethoxide, butoxide, etc. In addition, the main chain and the graft are connected by a covalent bond, and structures such as alkyl, ether, glycol or ester can be listed. If the manufacturing process of the separator of embodiment 1 or 2 is considered, at the stage before the cross-linking treatment step described later, the unit containing silanol in the silane grafted modified polyolefin is less than 10 mol% in terms of the modification amount relative to the total ethylene units of the main chain, preferably less than 5 mol%, and more preferably less than 2 mol%.
[0124] For the preferred silane grafted modified polyolefin, the density is 0.90 to 0.96 g / cm 3 And the melt flow rate (MFR) at 190° C. is 0.2 to 5 g / min.
[0125] The silane-grafted modified polyolefin can be obtained, for example, by grafting an alkoxysilyl group to the main chain of the silane-grafted non-modified polyolefin in the polyolefin resin described above. It should be noted that in this specification, the solid content change rate (hereinafter referred to as "gel fraction") of the microporous membrane made of polyolefin resin that does not include the silane-grafted modified polyolefin before and after heating at 160° C. in a decalin solution is 10% or less. It should be noted that when measuring the gel fraction, the solid content refers only to the resin and does not include other materials such as inorganic substances.
[0126] The polyolefin resin microporous membrane not containing silane grafted modified polyolefin can be produced by using, for example, any one selected from the group consisting of polyethylene (PE) (X, viscosity average molecular weight 100,000 to 400,000), a first ultra-high molecular weight PE (Y, viscosity average molecular weight 400,000 to 800,000) and a second ultra-high molecular weight PE (Z, viscosity average molecular weight 800,000 to 9,000,000) or a composition in which two or three selected from the group consisting of X, Y and Z are mixed in any proportion. It should be noted that a polyolefin consisting only of a hydrocarbon skeleton, such as a low-density polyethylene (LDPE), a linear low-density polyethylene (LLDPE), a polypropylene (PP), an olefin-based thermoplastic elastomer, etc., can be added to the mixed composition.
[0127] On the other hand, the gel fraction of the polyolefin resin microporous membrane having a crosslinked structure such as a silane crosslinked structure is preferably 30% or more, more preferably 70% or more.
[0128] (Physical properties of polyolefin resin microporous membrane)
[0129] The weight average molecular weight of the entire polyolefin resin microporous membrane is preferably 100,000 or more and 1,200,000 or less, and more preferably 150,000 or more and 800,000 or less.
[0130] The porosity of the microporous film made of polyolefin resin is preferably 20% or more, more preferably 30% or more, and further preferably 32% or more or 35% or more. By making the porosity 20% or more, there is a tendency to further improve the followability of the rapid movement of lithium ions. On the other hand, the porosity is preferably 90% or less, more preferably 80% or less, and further preferably 50% or less. By making the porosity 90% or less, there is a tendency to further improve the membrane strength and further suppress the self-discharge. The porosity can be measured by the method described in the examples, and can also be controlled by changing the stretching ratio of the microporous film made of polyolefin resin.
[0131] The air permeability of the polyolefin resin microporous film is preferably 1 sec / 100 cm 3 More preferably, 50 seconds / 100 cm 3 More preferably, 55 seconds / 100 cm 3 More preferably, 70 seconds / 100 cm 3 Above, 90 seconds / 100cm 3 Above or 110 seconds / 100cm 3 By making the air permeability 1 second / 100cm 3 The balance between the film thickness, the porosity and the average pore size tends to be further improved. On the other hand, the air permeability is preferably 400 sec / 100 cm 3Less than 300 sec / 100 cm, more preferably less than 300 sec / 100 cm 3 , more preferably 270 sec / 100 cm 3 By making the air permeability 400 seconds / 100cm 3 The ion permeability tends to be further improved. The air permeability can be measured by the method described in the Examples, and can be controlled by changing the stretching temperature and / or stretching ratio of the polyolefin resin microporous film.
[0132] The film thickness of the polyolefin resin microporous film is preferably 1.0 μm or more, more preferably 2.0 μm or more, and further preferably 3.0 μm or more, 4.0 μm or more, or 5.5 μm or more. By making the film thickness 1.0 μm or more, there is a tendency for the film strength to be further improved. On the other hand, the film thickness is preferably 500 μm or less, more preferably 100 μm or less, and further preferably 80 μm or less, 22 μm or less, or 19 μm or less. By making the film thickness 500 μm or less, there is a tendency for the ion permeability to be further improved. The film thickness can be measured by the method described in the examples, and can also be controlled by changing the stretching ratio of the polyolefin resin microporous film.
[0133] When using a polyolefin resin microporous film as a constituent material of a LIB separator, the film thickness of the polyolefin resin microporous film is preferably 25 μm or less, more preferably 22 μm or less or 20 μm or less, further preferably 18 μm or less, and particularly preferably 16 μm or less. By making the film thickness 25 μm or less, there is a tendency for the permeability to be further improved. In this case, the lower limit of the film thickness can be 1.0 μm or more, 3.0 μm or more, 4.0 μm or more, or 5.5 μm or more.
[0134] <Inorganic porous layer>
[0135] As the film thickness of the inorganic porous layer, there is no particular limitation, preferably 0.01 μm or more, more preferably 0.05 μm or more, and further preferably 1.0 μm or more. On the other hand, the film thickness is preferably 15 μm or less, more preferably 10 μm or less, and further preferably 5 μm or less. From the viewpoint of improving mechanical strength, it is preferred that the film thickness is set to 0.01 μm or more. On the other hand, setting the film thickness to 15 μm or less has a tendency to be more favorable from the viewpoint of reducing the volume occupied by the separator in the power storage device and the high capacity of the power storage device. In addition, from the viewpoint of preventing the air permeability of the separator from rising excessively, it is also preferred that the film thickness of the inorganic porous layer is 15 μm or less. The film thickness can be measured based on the method described in the embodiment, and can also be controlled by changing the coating amount of the slurry (slurry for inorganic porous layer) used to form the inorganic porous layer on the polyolefin resin microporous membrane.
[0136] The air permeability of the inorganic porous layer can be any value that does not excessively increase the air permeability of the separator. The air permeability of the inorganic porous layer is equivalent to the increase in the air permeability of the separator caused by forming the inorganic porous layer on the polyolefin resin microporous membrane. The increase is preferably 200 seconds / 100cm 3 Less than 150 sec / 100 cm 3 Below, more preferably 130 seconds / 100cm 3 From the viewpoint of allowing ions to permeate appropriately in a non-aqueous electrolyte (hereinafter also referred to as "electrolyte") during charge and discharge of the power storage device, it is preferred that the increase amount be set to 200 seconds / 100 cm 3 The amount of increase can be measured according to the method described in the Examples, and can be controlled by changing various structures of the inorganic porous layer or various production conditions.
[0137] <Cross-linked structure>
[0138] In the inorganic porous layer, the cross-linked structure is preferably formed by at least one selected from the group consisting of nucleophilic substitution reaction, nucleophilic addition reaction, electrophilic addition reaction and silane coupling reaction. By making such a cross-linked structure present in the inorganic porous layer, it becomes easy to play the effect of the present invention. From the same viewpoint, when the inorganic porous layer includes a cross-linking agent, it is preferred that: in the inorganic porous layer, there is a polar functional group on the surface of the inorganic particles, there is a cross-linking agent between the polar functional group and the resin binder, and the cross-linked structure is formed by the covalent bond between the polar functional group and the cross-linking agent and the resin binder.
[0139] This cross-linked structure can be formed (i) in the film-making process or immediately after the process, or (ii) after being accommodated in the power storage device, using the surrounding environment or the chemical substances inside the power storage device to form. According to the degree of progress of the above-mentioned cross-linking reaction (i) in the film-making process of the inorganic porous layer or immediately after the process, the environment in the power storage device that accommodates the inorganic porous layer, the composition of the microporous film of the stacked inorganic porous layer, the cross-linking opportunity when the microporous film has cross-linking property, etc., there is the possibility that the cross-linking reaction in the inorganic porous layer is further carried out after the separator containing the inorganic porous layer is accommodated in the power storage device. Therefore, the inorganic porous layer is preferably constituted in a manner that can carry out the above-mentioned cross-linking reaction (i) and / or (ii).
[0140] It should be noted that a layer (other layer) not equivalent to either of the two may be sandwiched between the inorganic porous layer and the polyolefin resin microporous film, but such other layers are preferably not sandwiched. That is, it is preferred to directly configure the inorganic porous layer on the polyolefin resin microporous film. Thus, it is easy to control the composition or characteristics of the inorganic porous layer by the composition of the polyolefin resin microporous film (e.g., the surface roughness of the region of the polyolefin resin microporous film opposite to the inorganic porous layer).
[0141] As the cross-linked structure (cross-linking reaction) based on a covalent bond, for example, at least one selected from the group consisting of the following reactions (I) or (II) is preferred:
[0142] (I) Reaction between multiple heterogeneous functional groups
[0143] (II) Chain condensation reaction between the functional group and the cross-linking agent.
[0144] The functional group or combination of reactants that forms a crosslinked structure by covalent bonding in reaction (I) is not particularly limited, but is preferably:
[0145] Hydroxyl and carboxyl (esterification);
[0146] Carbonyl and alkyl (aldol condensation);
[0147] Halogen and carboxyl group (intramolecular condensation);
[0148] Alkoxy and alkyl (Claisen condensation);
[0149] Carbonyl and anhydride (Perkin reaction);
[0150] Amino and halogen;
[0151] Isocyanate groups and hydroxyl groups (forming urethane bonds); and
[0152] Oxazoline and hydroxyl groups, etc.
[0153] As a combination of functional groups that form a cross-linked structure by covalent bonds based on reaction (II), it is not particularly limited, for example, preferably the reaction (including ring-opening reaction) of inorganic particles and / or resin binder with a cross-linking agent. When inorganic particles and / or resin binder are cross-linked by means of a cross-linking agent, the cross-linking agent preferably has more than two active groups. As long as multiple active groups can react with inorganic particles and / or resin binder, they can be any structure or group, can be substituted or non-substituted, can contain heteroatoms or inorganic substances, and can be the same or different from each other.
[0154] (Inorganic particles)
[0155] The inorganic particles of the present embodiment form a cross-linked structure by covalent bonds with other inorganic particles and / or by covalent bonds with a resin binder. The material that can be used as such inorganic particles is not particularly limited, and examples thereof include inorganic oxides (oxide-based ceramics) such as aluminum oxide, silicon dioxide, titanium dioxide, zirconium oxide, magnesium oxide, cerium oxide, yttrium oxide, zinc oxide, and iron oxide; inorganic nitrides (nitride-based ceramics) such as silicon nitride, titanium nitride, and boron nitride; silicon carbide, calcium carbonate, magnesium sulfate, aluminum sulfate, aluminum hydroxide, aluminum hydroxide, potassium titanate, talc, kaolinite, dickite, pearl clay, halloysite, pyrophyllite, montmorillonite, sericite, mica, magnesia chlorite, bentonite, asbestos, zeolite, calcium silicate, magnesium silicate, diatomaceous earth, and quartz sand; and glass fiber. These can be used alone or in combination of two or more.
[0156] From the viewpoint of ensuring heat resistance, the mass ratio of the inorganic particles in the inorganic porous layer (100×mass of inorganic particles / mass of inorganic porous layer) is preferably 30 mass % or more, more preferably 50 mass % or more. On the other hand, from the viewpoint of ensuring that there is room for the inorganic porous layer to contain a binder, the mass ratio is preferably 99.5 mass % or less, more preferably 99.0 mass % or less, and further preferably 98 mass % or less.
[0157] Examples of the shape of the inorganic particles include plate-like, flaky, needle-like, columnar, spherical, polyhedral, and block-like. A plurality of inorganic particles having these shapes may be used in combination.
[0158] The number average particle size of the inorganic particles is, for example, 0.01 μm or more, 0.1 μm or more, or 0.3 μm or more. In addition, the number average particle size is 10.0 μm or less, 9.0 μm or less, or 6.0 μm or less. As a method for adjusting the particle size, for example, a method of crushing the inorganic particles using a suitable crushing device such as a ball mill, a bead mill, or a jet mill to reduce the particle size can be cited.
[0159] Here, preferably there is polar functional group on the surface of inorganic particles. That is, inorganic particles preferably have polar functional groups on their surface. Thus, the reactivity to other compounds (resin binder, other inorganic particles and crosslinking agent included as required, etc.) can be improved. Thus, it is easy to form a suitable crosslinked structure by the covalent bond of inorganic particles and resin binder, and in addition, when inorganic particles are multiple, it is easy to form a suitable crosslinked structure by the covalent bond between multiple inorganic particles. From the same viewpoint, the polar functional group is preferably at least one selected from the group consisting of carboxyl, hydroxyl and amino.
[0160] In addition, it is also preferred that there are silicon-containing functional groups on the surface of the inorganic particles. That is, the inorganic particles preferably have silicon-containing functional groups on their surfaces. Thus, the reactivity to other compounds (resin binder, other inorganic particles and cross-linking agents included as required, etc.) can be improved. Thus, it is easy to form a suitable cross-linked structure by the covalent bond of the inorganic particles and the resin binder. In addition, when the inorganic particles are multiple, it is easy to form a suitable cross-linked structure by the covalent bond between the multiple inorganic particles. From the same viewpoint, the silicon-containing functional group is preferably at least one selected from the group consisting of alkoxysilyl, halogen-substituted silyl and silazane.
[0161] (resin binder)
[0162] The resin binder forms a cross-linked structure through covalent bonds with other resin binders and / or covalent bonds with inorganic particles. The material that can be used as such a resin binder is not particularly limited, and for example, a single resin or a combination of two or more resins that are insoluble in the electrolyte of a power storage device represented by LIB and electrochemically stable within the use range of the power storage device can be used.
[0163] Specific examples of materials that can be used as resin binders include polyolefins such as polyethylene and polypropylene; fluorine-containing resins such as polyvinylidene fluoride (PVdF) and polytetrafluoroethylene; fluorine-containing rubbers such as vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene copolymer and ethylene-tetrafluoroethylene copolymer; rubbers such as styrene-butadiene copolymer and its hydride, acrylonitrile-butadiene copolymer and its hydride, acrylonitrile-butadiene-styrene copolymer and its hydride, methacrylate-acrylate copolymer, styrene-acrylate copolymer, acrylonitrile-acrylate copolymer, ethylene-propylene rubber, polyvinyl alcohol, and polyvinyl acetate; cellulose derivatives such as ethyl cellulose, methyl cellulose, hydroxyethyl cellulose, and carboxymethyl cellulose; and resins having a melting point and / or glass transition temperature of 180° C. or above, such as polyphenylene ether, polysulfone, polyethersulfone, polyphenylene sulfide, polyetherimide, polyamideimide, polyamide, and polyester. One or more of these can be used alone or in combination.
[0164] Specific examples of the resin binder include the following 1) to 7).
[0165] 1) Polyolefins: such as polyethylene, polypropylene, ethylene-propylene rubber and their modified bodies;
[0166] 2) Conjugated diene polymers: for example, styrene-butadiene copolymers and their hydrides, acrylonitrile-butadiene copolymers and their hydrides, acrylonitrile-butadiene-styrene copolymers and their hydrides;
[0167] 3) Acrylic polymers: such as methacrylate-acrylate copolymers, styrene-acrylate copolymers and acrylonitrile-acrylate copolymers;
[0168] 4) Polyvinyl alcohol resins: such as polyvinyl alcohol and polyvinyl acetate;
[0169] 5) Fluorine-containing resins: such as PVdF, polytetrafluoroethylene, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene copolymer and ethylene-tetrafluoroethylene copolymer;
[0170] 6) Cellulose derivatives: such as ethyl cellulose, methyl cellulose, hydroxyethyl cellulose and carboxymethyl cellulose; and
[0171] 7) Resins having a melting point and / or glass transition temperature of 180°C or higher or polymers having no melting point but a decomposition temperature of 200°C or higher: for example, polyphenylene ether, polysulfone, polyethersulfone, polyphenylene sulfide, polyetherimide, polyamideimide, polyamide and polyester.
[0172] These types of resin binders can be obtained by using desired monomers as raw materials according to known manufacturing methods such as emulsion polymerization or solution polymerization. In the polymerization, the polymerization temperature, the pressure during polymerization, the method of adding monomers, and the additives used (polymerization initiator, molecular weight modifier, pH modifier, etc.) are not particularly limited.
[0173] The above-mentioned resin binder and / or the cross-linking agent described later are preferably in the form of an emulsion, a suspension or a colloid. Among them, from the viewpoints of film-forming properties and the strength of the obtained inorganic porous layer, for the emulsion, it is preferably formed by a core composed of prescribed particles and a shell containing a prescribed polymer compound located around the core. The particles forming the core can be organic polymer compounds or inorganic particles. From the viewpoint of further imparting flexibility through the inorganic porous layer finally obtained, organic polymer compounds are more preferred. For example, a suspension refers to a system in which solid particles are dispersed in a solvent to a degree visible under a microscope, and a colloid refers to a system in which giant molecules are dispersed to a degree that can be confirmed by the naked eye.
[0174] Resin binder preferably has a functional group (nucleophilic substitution reactive functional group) or a functional group (nucleophilic addition reactive functional group) that undergoes nucleophilic substitution reaction with the polar functional group and / or the silicon-containing functional group present on the surface of the above-mentioned inorganic particles. Thus, the reactivity between other compounds (such as inorganic particles, resin binder and the crosslinking agent included as required) can be improved. Thus, it is easy to form a suitable crosslinked structure by the covalent bond of inorganic particles and resin binder. In addition, when the resin binder is multiple, it is easy to form a suitable crosslinked structure by the covalent bond between multiple resin binders. From the same viewpoint, the nucleophilic substitution reactive functional group or the nucleophilic addition reactive functional group of the resin binder are preferably at least one selected from the group consisting of carboxyl, hydroxyl and amino.
[0175] From the viewpoint of ensuring heat resistance, the mass ratio of the resin binder in the inorganic porous layer (100×mass of the resin binder / mass of the inorganic porous layer) is preferably 0.5 mass % or more, more preferably 1.0 mass % or more. On the other hand, from the viewpoint of ensuring that the inorganic porous layer contains inorganic particles in a sufficient amount, the mass ratio is preferably 50 mass % or less, more preferably 20 mass % or less.
[0176] (Crosslinking agent)
[0177] The inorganic porous layer preferably contains a crosslinking agent in addition to the above-mentioned inorganic particles and the above-mentioned resin binder. Thus, it is easier to form a suitable crosslinked structure in the inorganic porous layer. The mass ratio of the crosslinking agent in the inorganic porous layer (100×the mass of the crosslinking agent / the mass of the inorganic porous layer) can be appropriately selected within the range of 0.01 mass % to 5 mass %. The mass ratio of the crosslinking agent in the inorganic porous layer is more preferably 0.1 mass % to 5 mass %, and further preferably 0.1 mass % to 3 mass %.
[0178] The cross-linking agent preferably comprises a reactive action group with the above-mentioned inorganic particles and / or the above-mentioned resin binder. For example, the cross-linking agent preferably has a functional group (nucleophilic substitution reactive functional group) and / or a functional group (electrophilic addition reactive functional group) that undergoes a nucleophilic substitution reaction between the above-mentioned inorganic particles and / or the above-mentioned resin binder. It is particularly preferred that the cross-linking agent has a nucleophilic substitution reactive functional group and an electrophilic addition reactive functional group. Thus, it is easier to form a suitable cross-linked structure in the inorganic porous layer. Wherein, as the nucleophilic substitution reactive functional group of the cross-linking agent, preferably oxazoline and / or epoxy. In addition, as the electrophilic addition reactive functional group of the cross-linking agent, it is particularly preferred to be selected from at least one of the group consisting of isocyanate, thioisocyanate, carbodiimide, allenyl, oxime and carbonyl.
[0179] As the crosslinking agent that can be used, for example, as an oxazoline crosslinking agent, the EPOCROS series (K-2010E, K-2020E, K-2030, WS-300, WS-500, WS-700) manufactured by Nippon Shokubai Co., Ltd. can be cited; as a carbodiimide crosslinking agent, the CARBODILITE series (V-02, V-02-L2, SV-02, V-04, V-10, SW-12G, E-02, E-03A) manufactured by Nisshinbo Chemical Inc. can be cited; as an isocyanate crosslinking agent, the DURANATE series (WB40-100, WB40-80D, WT20-100, WT30-100, WL70-100, WR80-70P, WE50-100) manufactured by Asahi Kasei Corporation can be cited; as an epoxy crosslinking agent, the Nagase ChemteX As the alkoxysilane, there are triethoxysilane (X-12-1273ES), dimethyldimethoxysilane, methyltrimethoxysilane, tetraethoxysilane, etc. manufactured by Shin-Etsu Chemical Co., Ltd.; as the crosslinking agent of the alkoxysilane compound containing various functional groups, there are the KBM series (3-aminopropyltrimethoxysilane KBM-903, etc.), KBE series) manufactured by Shin-Etsu Chemical Co., Ltd., etc.
[0180] The crosslinking agent may be, for example, a substance also used as a silane coupling agent. The silane coupling agent is an organic silicon compound having a hydrolyzable reactive group, which is a reactive group capable of bonding to inorganic particles having silicon dioxide or the like after hydrolysis.
[0181] <Other additives>
[0182] The polyolefin resin microporous membrane and / or the inorganic porous layer may contain any additives. The additives are not particularly limited, and examples thereof include phenolic, phosphorus, and sulfur antioxidants; metal soaps such as calcium stearate and zinc stearate; ultraviolet absorbers; light stabilizers; antistatic agents; antifogging agents; and coloring pigments.
[0183] <Method for manufacturing separator>
[0184] (Method for producing a polyolefin resin microporous film)
[0185] The method for manufacturing a polyolefin resin microporous membrane can adopt a known manufacturing method, for example, any of a wet porosification method and a dry porosification method can be adopted. If examples of the wet porosification method are listed, for example: a method of melt-kneading a polyolefin resin composition and a plasticizer, forming a sheet, and then stretching it according to the situation to extract the plasticizer to make it porous; a method of melt-kneading a polyolefin resin composition containing a polyolefin resin as a main component and extruding it at a high stretch ratio, and then making it porous by heat treatment and stretching to peel off the interface of the polyolefin crystal; a method of melt-kneading a polyolefin resin composition and an inorganic filler material and forming it into a sheet, and then stretching to peel off the interface between the polyolefin and the inorganic filler material to make it porous; and a method of dissolving a polyolefin resin composition, immersing it in a solvent that is poor for polyolefin to solidify the polyolefin, and removing the solvent to make it porous.
[0186] Hereinafter, as an example of a method for manufacturing a polyolefin microporous membrane, a method for extracting a plasticizer after a polyolefin resin composition and a plasticizer are melt-mixed and formed into a sheet is described. First, a polyolefin resin composition and a plasticizer are melt-mixed. As a melt-mixing method, for example, a polyolefin resin and other additives used as needed are put into a resin mixing device such as an extruder, a kneader, a small sand mill, a mixing roller and a Banbury mixer, and a method for mixing the resin component while heating and melting the resin component and introducing a plasticizer at an arbitrary ratio. At this time, it is preferred that a Henschel mixer or the like is used in advance to mix in a specified ratio before the polyolefin resin, other additives and the plasticizer are put into the resin mixing device. More preferably, only a part of the plasticizer is put into the pre-mixing, and the remaining plasticizer is mixed while the resin mixing device is side-fed.
[0187] As a plasticizer, a non-volatile solvent that can form a uniform solution above the melting point of polyolefin can be used. Specific examples of such non-volatile solvents include hydrocarbons such as liquid paraffin and paraffin; esters such as dioctyl phthalate and dibutyl phthalate; and higher alcohols such as oleyl alcohol and stearyl alcohol. Among these, liquid paraffin is preferred.
[0188] The ratio of the polyolefin resin composition to the plasticizer is as long as it is a range that can uniformly melt-mix and form them into sheets. For example, the mass percentage of the plasticizer in the composition consisting of the polyolefin resin composition and the plasticizer is preferably 30 mass % or more and 80 mass % or less, more preferably 40 mass % or more and 70 mass % or less. By setting the mass percentage of the plasticizer to this range, the melt tension during melt molding and the formation of uniform and fine pore structure can be taken into account, which is preferred from this viewpoint.
[0189] Then, the molten kneaded product obtained by heating, melting and kneading is formed into a sheet as described above. As a method for manufacturing a sheet-like molded body, for example, the following method can be cited: the molten kneaded product is extruded into a sheet by means of a T-die, etc., and it is cooled to a temperature sufficiently lower than the crystallization temperature of the resin component to solidify it by contacting a heat conductor. As the heat conductor used in cooling and solidification, metals, water, air and plasticizers themselves can be cited, and metal rollers are preferred due to their high thermal conductivity. In this case, when in contact with metal rollers, if the molten kneaded product is sandwiched between the rollers, the thermal conductivity efficiency is further improved, the sheet is oriented, the film strength is increased, and the surface smoothness of the sheet is also improved, so it is more preferred. When extruded into a sheet from a T-die, the die lip spacing is preferably 400 μm or more and 3000 μm or less, and more preferably 500 μm or more and 2500 μm or less.
[0190] Preferably, the sheet-like molded body thus obtained is then stretched. As a stretching treatment, any one of uniaxial stretching or biaxial stretching can be suitably used. From the viewpoints of the strength of the obtained microporous film, biaxial stretching is preferred. When the sheet-like molded body is stretched in two directions at a high ratio, the molecules are oriented along the surface direction, and the polyolefin microporous film finally obtained becomes difficult to break, becoming a film with high puncture strength. As a stretching method, methods such as simultaneous biaxial stretching, successive biaxial stretching, multistage stretching and multiple stretching can be cited. From the viewpoints of improved puncture strength, uniformity of stretching, and closure, simultaneous biaxial stretching is preferred.
[0191] The stretching ratio is preferably in the range of 20 times or more and 100 times or less in terms of surface ratio, and more preferably in the range of 25 times or more and 50 times or less. The stretching ratio in each direction is preferably in the range of 4 times or more and 10 times or less in MD and 4 times or more and 10 times or less in TD, and more preferably in the range of 5 times or more and 8 times or less in MD and 5 times or more and 8 times or less in TD. By setting the stretching ratio to a ratio within this range, it is possible to impart more sufficient strength and prevent film breakage in the stretching process, which is preferred from the perspective of obtaining high productivity.
[0192] It should be noted that MD refers to, for example, a machine direction when a polyolefin microporous membrane is continuously molded, and TD refers to a direction forming an angle of 90° with MD.
[0193] The sheet-like molded body obtained as described above can be further calendered. Calendering can be implemented, for example, by an extrusion method using a double-belt extruder or the like. By calendering, the orientation of the surface layer of the sheet-like molded body can be particularly increased. The calendering ratio is preferably greater than 1 times and less than 3 times, more preferably greater than 1 times and less than 2 times. By setting the calendering ratio within this range, the film strength of the polyolefin microporous membrane finally obtained can be increased and a more uniform porous structure can be formed in the film thickness direction, which is preferred from this point of view.
[0194] Next, the plasticizer is removed from the sheet-like molded body to obtain a polyolefin microporous membrane. As a method for removing the plasticizer, for example, a method in which the sheet-like molded body is immersed in an extraction solvent to extract the plasticizer and fully dried can be cited. The method for extracting the plasticizer can be any of an intermittent method and a continuous method. In order to suppress the shrinkage of the polyolefin microporous membrane, it is preferred to constrain the end of the sheet-like molded body in a series of steps of immersion and drying. In addition, the residual amount of plasticizer in the polyolefin microporous membrane is preferably less than 1% by mass.
[0195] As the extraction solvent, it is preferred to use a solvent that is a poor solvent for the polyolefin resin and a good solvent for the plasticizer, and has a boiling point lower than the melting point of the polyolefin resin. Examples of such extraction solvents include hydrocarbons such as n-hexane and cyclohexane; halogenated hydrocarbons such as dichloromethane and 1,1,1-trichloroethane; non-chlorine halogenated solvents such as hydrofluoroethers and hydrofluorocarbons; alcohols such as ethanol and isopropanol; ethers such as diethyl ether and tetrahydrofuran; and ketones such as acetone and methyl ethyl ketone. It should be noted that these extraction solvents can be recovered and reused by operations such as distillation.
[0196] In order to suppress shrinkage of the polyolefin microporous membrane, after the stretching step or after the polyolefin microporous membrane is formed, a heat treatment such as heat setting or heat relaxation may be performed. The polyolefin microporous membrane may also be subjected to post-treatment such as hydrophilization treatment using a surfactant or the like, crosslinking treatment using ionizing radiation or the like.
[0197] (Method for producing a polyolefin resin microporous membrane comprising a silane-grafted modified polyolefin)
[0198] As a method for producing a polyolefin resin microporous membrane including a silane-graft-modified polyolefin, the case of a microporous membrane (flat membrane) will be described below, but forms other than the flat membrane are not intended to be excluded.
[0199] The method for producing a microporous membrane comprising a silane-grafted modified polyolefin comprises the following steps:
[0200] (1) Sheet forming process;
[0201] (2) Stretching process;
[0202] (3) a porous body forming step; and
[0203] (4) Heat treatment process.
[0204] The method for producing a microporous membrane comprising a silane-grafted modified polyolefin may include a kneading step before the sheet forming step (1) and / or a winding / slitting step after the heat treatment step (3) as desired, but preferably does not include a silane crosslinking treatment step from the viewpoint of maintaining the silane crosslinking property until contact with the electrolyte. The silane crosslinking treatment step is generally a step of contacting the treated article comprising a silane-grafted modified polyolefin with a mixture of an organic metal catalyst and water or immersing it in an alkaline solution or an acid solution to carry out a silane dehydration condensation reaction to form an oligosiloxane bond.
[0205] The metal of the catalyst containing an organic metal is, for example, at least one selected from the group consisting of scandium, titanium, vanadium, copper, zinc, aluminum, zirconium, palladium, gallium, tin and lead. Examples of the catalyst containing an organic metal include dibutyltin dilaurate, dibutyltin diacetate, dibutyltin dioctoate, etc. It is known that the reaction rate can be greatly accelerated by the reaction mechanism proposed by Weij et al. (FW van. der. Weij: Macromol. Chem., 181, 2541, 1980.). In addition, in recent years, in order to avoid the harm of organic tin to the environment and human health, it is known that the Lewis function of the chelate complex of copper or titanium can be used to accelerate the reaction of alkoxysilyl groups to form siloxane bonds with each other in the same way as the organic tin complex by combining with an organic base.
[0206] The pH of the alkaline solution exceeds 7, and may contain, for example, alkali metal hydroxides, alkaline earth metal hydroxides, alkali metal carbonates, alkali metal phosphates, ammonia, amine compounds, etc. Among these, alkali metal hydroxides or alkaline earth metal hydroxides are preferred, alkali metal hydroxides are more preferred, and sodium hydroxide is further preferred from the viewpoint of the safety of the power storage device and the silane crosslinking property.
[0207] The pH of the acid solution is less than 7, and may contain, for example, an inorganic acid, an organic acid, etc. Preferred acids are hydrochloric acid, sulfuric acid, carboxylic acids, or phosphoric acids.
[0208] In the kneading process, a kneading machine can be used to knead the silane grafted modified polyolefin, the plasticizer or inorganic material used as desired, and other polyolefins. From the viewpoint of preventing the generation of resin agglomerates in the manufacturing process and maintaining the silane crosslinking property until contact with the electrolyte, it is preferred not to add a masterbatch resin containing a dehydration condensation catalyst to the kneaded product.
[0209] As a plasticizer, there is no particular limitation, and examples thereof include organic compounds that can form a uniform solution with polyolefin at a temperature below the boiling point. More specifically, examples thereof include: decalin, xylene, dioctyl phthalate, dibutyl phthalate, stearyl alcohol, oleyl alcohol, decanol, nonanol, diphenyl ether, n-decane, n-dodecane, paraffin oil, etc. Among these, paraffin oil and dioctyl phthalate are preferred. One type of plasticizer can be used alone, or two or more types can be used in combination. The proportion of the plasticizer is not particularly limited. Regarding the proportion of polyolefin and silane grafted modified polyolefin, from the viewpoint of the porosity of the obtained microporous membrane, it is preferably 20% by mass or more relative to the total mass of the microporous membrane as required, and from the viewpoint of the viscosity during melt kneading, it is preferably 90% by mass or less.
[0210] The sheet forming step is a step of extruding the obtained kneaded product, or the mixture of the silane grafted modified polyolefin, the ultrahigh molecular weight polyolefin and the plasticizer, cooling and solidifying, and molding into a sheet to obtain a sheet. The sheet forming method is not particularly limited, and for example, a method of solidifying the melt kneaded and extruded melt by compression cooling can be cited. As the cooling method, there can be cited: a method of directly contacting the melt with a cooling medium such as cold air or cooling water; a method of contacting the melt with a roller or a press cooled with a refrigerant, etc. Among them, the method of contacting the roller or press cooled with a refrigerant is preferred from the aspect of excellent film thickness controllability.
[0211] From the viewpoint of the resin agglomerates or the maximum internal heat release rate in the microporous membrane, the mass ratio of the silane grafted modified polyolefin to the ultra-high molecular weight polyethylene (mass of the silane grafted modified polyolefin / mass of the ultra-high molecular weight polyethylene) in the sheet forming process is preferably 0.05 / 0.95 to 0.4 / 0.6, and more preferably 0.06 / 0.94 to 0.38 / 0.62.
[0212] From the viewpoint of having low-temperature shutdown property below 150°C and film rupture resistance at high temperatures above 180°C of the separator, and suppressing thermal runaway when the power storage device is destroyed to improve safety, in the sheet forming process, the silane-grafted modified polyolefin is preferably not a masterbatch resin containing a dehydration condensation catalyst that crosslinks the silane-grafted modified polyolefin before the sheet forming process. Preferably, the film rupture resistance can be ensured at 190°C or above, 200°C or above, 210°C or above, 220°C or above, 230°C or above, 240°C or above, or 250°C or above. In addition, it should be understood that the upper limit of the film rupture temperature of the separator is not limited, and in the technical field of the present invention, the film rupture phenomenon may also occur at a high temperature above 250°C.
[0213] The stretching process is to extract plasticizer or inorganic material as required from the obtained sheet, and then the sheet is stretched in one or more directions. As the stretching method of the sheet, the MD uniaxial stretching based on the roller stretching machine, the TD uniaxial stretching based on the stenter, the successive biaxial stretching based on the combination of the roller stretching machine and the stenter or the stenter and the stenter, the biaxial stretching based on the simultaneous biaxial stenter or the inflation molding, etc. can be listed. From the viewpoint of obtaining a more uniform film, it is preferably biaxially stretched simultaneously. From the viewpoint of the balance of the uniformity of the film thickness, the tensile elongation and the porosity and the average pore size, the total surface ratio is preferably more than 8 times, more preferably more than 15 times, and further preferably more than 20 times or more than 30 times. By making the total surface ratio more than 8 times, there is a tendency to easily obtain a film with high strength and good thickness distribution. In addition, from the viewpoints of preventing fracture, the surface ratio can be less than 250 times.
[0214] The porous body forming process is a process of extracting the plasticizer from the stretched product after the stretching process and making the stretched product porous. There is no particular limitation on the method for extracting the plasticizer, and examples thereof include: a method of immersing the stretched product in an extraction solvent, a method of spraying the stretched product with an extraction solvent, and the like. There is no particular limitation on the extraction solvent, and for example, a solvent that is a poor solvent for polyolefins and a good solvent for plasticizers or inorganic materials, and has a boiling point lower than the melting point of polyolefins is preferred. There is no particular limitation on such an extraction solvent, and examples thereof include: hydrocarbons such as n-hexane and cyclohexane; halogenated hydrocarbons such as dichloromethane or 1,1,1-trichloroethane, and fluorocarbons; alcohols such as ethanol and isopropanol; ketones such as acetone and 2-butanone; alkaline water, and the like. One extraction solvent may be used alone, or two or more may be used in combination.
[0215] The heat treatment process is a process for extracting plasticizer from the sheet as needed after the stretching process, and further heat treating to obtain a microporous film. As a method of heat treatment, there is no particular limitation, and examples include heat setting methods such as stretching and relaxation operations using a stenter or a roller stretching machine. Relaxation operation refers to a shrinking operation performed at a specified temperature and relaxation rate along the mechanical direction (MD) and / or width direction (TD) of the film. The relaxation rate refers to the value obtained by dividing the MD size of the film after the relaxation operation by the MD size of the film before the operation; or the value obtained by dividing the TD size of the film after the relaxation operation by the TD size of the film before the operation; or in the case of relaxing both MD and TD, it refers to the value obtained by multiplying the relaxation rate of MD by the relaxation rate of TD. In addition, in the winding process, the obtained microporous film can be cut and wound on a specified core as needed.
[0216] (Method for producing inorganic porous layer)
[0217] As a method for manufacturing an inorganic porous layer, there is no particular limitation, and a known manufacturing method can be used, for example: regardless of whether the polyolefin resin microporous film contains a silane-grafted modified polyolefin resin, a coating solution (inorganic porous layer slurry) containing inorganic particles and a resin binder is applied to a polyolefin resin microporous film. According to expectations, the inorganic porous layer slurry may include a crosslinking agent. The raw material containing inorganic particles and a resin binder and the raw material of the polyolefin resin microporous film containing a polyolefin resin can be stacked and extruded by a coextrusion method, or the polyolefin resin microporous film and the inorganic porous layer (film) can be made separately and then bonded.
[0218] The solvent of the coating liquid is preferably a solvent that can uniformly and stably disperse or dissolve the inorganic particles and the resin binder, and examples thereof include N-methylpyrrolidone (NMP), N,N-dimethylformamide, N,N-dimethylacetamide, water, ethanol, toluene, hot xylene, dichloromethane and hexane.
[0219] The above crosslinking agent may be added to the coating liquid. In addition, various additives such as dispersants such as surfactants, thickeners, wetting agents, defoaming agents, and pH adjusters including acids and alkalis may be added to the coating liquid.
[0220] Examples of methods for dispersing or dissolving the inorganic particles and the resin binder in the coating liquid medium include mechanical stirring using a ball mill, a bead mill, a planetary ball mill, a vibration ball mill, a sand mill, a colloid mill, an attritor, a roller mill, a high-speed impeller dispersion, a disperser, a homogenizer, a high-speed impact mill, an ultrasonic dispersion, and a stirring blade.
[0221] As for the method of applying the coating liquid to the polyolefin resin microporous membrane, for example, a gravure coater method, a small diameter gravure coater method, a reverse roll coater method, a transfer roll coater method, a kiss coater method, a dip coater method, a knife coater method, an air knife coater method, a blade coater method, a rod coater method, an extrusion coater method, a cast coater method, a die coater method, a screen printing method and a spray coating method can be listed.
[0222] There is no particular limitation on the method of removing the solvent from the coating film after coating, as long as it is a method that does not adversely affect the polyolefin resin microporous membrane. Examples include: a method of drying at a temperature below the melting point of the material constituting the polyolefin resin microporous membrane while fixing the polyolefin resin microporous membrane, a method of drying under reduced pressure at a low temperature, and a method of immersing in a poor solvent for a resin binder to solidify the resin binder and extracting the solvent at the same time. In addition, a portion of the solvent may remain within a range that does not significantly affect the characteristics of the device.
[0223] <Electricity storage device>
[0224] The separators of embodiments 1 and 2 can be used in an electrical storage device. The electrical storage device comprises a positive electrode, a negative electrode, a separator of embodiment 1 or 2 disposed between the positive and negative electrodes, and an electrolyte. As an electrical storage device, specifically, a lithium battery, a lithium secondary battery, a lithium ion secondary battery (LIB), a sodium secondary battery, a sodium ion secondary battery, a magnesium secondary battery, a magnesium ion secondary battery, a calcium secondary battery, a calcium ion secondary battery, an aluminum secondary battery, an aluminum ion secondary battery, a nickel-hydrogen battery, a nickel-cadmium battery, an electric double layer capacitor, a lithium ion capacitor, a redox flow battery, a lithium-sulfur battery, a lithium-air battery, a zinc-air battery, etc. Among these, from the viewpoint of practicality, preferably a lithium battery, a lithium secondary battery, a LIB, a nickel-hydrogen battery or a lithium ion capacitor, more preferably a lithium battery or a LIB.
[0225] The electrolyte in the battery may contain water, and the water contained in the system after the battery is manufactured may be the water contained in the electrolyte or the water contained in the components such as electrodes or separators and brought in. The electrolyte may contain a non-aqueous solvent. As the solvent contained in the non-aqueous solvent of this embodiment, for example, alcohols such as methanol and ethanol; aprotic solvents, etc. Among them, as the non-aqueous solvent, aprotic solvents are preferred.
[0226] Examples of aprotic solvents include cyclic carbonates, fluoroethylene carbonate, lactones, organic compounds having sulfur atoms, chain fluorinated carbonates, cyclic ethers, mononitriles, alkoxy-substituted nitriles, dinitriles, cyclic nitriles, short-chain fatty acid esters, chain ethers, fluorinated ethers, ketones, and compounds in which a part or all of the H atoms of the above aprotic solvents are substituted with halogen atoms.
[0227] Examples of the cyclic carbonate include ethylene carbonate, propylene carbonate, 1,2-butylene carbonate, trans-2,3-butylene carbonate, cis-2,3-butylene carbonate, 1,2-pentylene carbonate, trans-2,3-pentylene carbonate, cis-2,3-pentylene carbonate, vinylene carbonate, 4,5-dimethylvinylene carbonate, and vinylethylene carbonate.
[0228] Examples of the fluoroethylene carbonate include 4-fluoro-1,3-dioxolane-2-one, 4,4-difluoro-1,3-dioxolane-2-one, cis-4,5-difluoro-1,3-dioxolane-2-one, trans-4,5-difluoro-1,3-dioxolane-2-one, 4,4,5-trifluoro-1,3-dioxolane-2-one, 4,4,5,5-tetrafluoro-1,3-dioxolane-2-one, and 4,4,5-trifluoro-5-methyl-1,3-dioxolane-2-one.
[0229] Examples of the lactone include γ-butyrolactone, α-methyl-γ-butyrolactone, γ-valerolactone, γ-caprolactone, δ-valerolactone, δ-caprolactone, and ε-caprolactone.
[0230] Examples of the organic compound having a sulfur atom include ethylene sulfite, propylene sulfite, butylene sulfite, pentenyl sulfite, sulfolane, 3-sulfolane, 3-methylsulfolane, 1,3-propane sultone, 1,4-butane sultone, 1-propylene 1,3-sultone, dimethyl sulfoxide, tetramethylene sulfoxide, and ethylene glycol sulfite.
[0231] Examples of the chain carbonate include ethyl methyl carbonate, dimethyl carbonate, diethyl carbonate, methyl propyl carbonate, methyl isopropyl carbonate, dipropyl carbonate, methyl butyl carbonate, dibutyl carbonate, and ethyl propyl carbonate.
[0232] Examples of the cyclic ether include tetrahydrofuran, 2-methyltetrahydrofuran, 1,4-dioxane, and 1,3-dioxane.
[0233] Examples of the mononitrile include acetonitrile, propionitrile, butyronitrile, valeronitrile, benzonitrile, and acrylonitrile.
[0234] Examples of the alkoxy-substituted nitrile include methoxyacetonitrile and 3-methoxypropionitrile.
[0235] Examples of the dinitriles include malononitrile, succinonitrile, methylsuccinonitrile, glutaronitrile, dimethylglutaronitrile, adiponitrile, 1,4-dicyanoheptane, 1,5-dicyanopentane, 1,6-dicyanohexane, 1,7-dicyanoheptane, 2,6-dicyanoheptane, 1,8-dicyanooctane, 2,7-dicyanooctane, 1,9-dicyanononane, 2,8-dicyanononane, 1,10-dicyanodecane, 1,6-dicyanodecane, 2,4-dimethylglutaronitrile, and ethylene glycol bis(propionitrile)ether.
[0236] Examples of the cyclic nitrile include benzonitrile and the like.
[0237] Examples of the short-chain fatty acid esters include methyl acetate, methyl propionate, methyl isobutyrate, methyl butyrate, methyl isovalerate, methyl valerate, methyl pivalate, methyl hydrogenated angelate, methyl caproate, ethyl acetate, ethyl propionate, ethyl isobutyrate, ethyl butyrate, ethyl isovalerate, ethyl valerate, ethyl pivalate, ethyl hydrogenated angelate, ethyl caproate, propyl acetate, propyl propionate, propyl isobutyrate, propyl butyrate, propyl isovalerate, propyl valerate, propyl pivalate, propyl hydrogenated angelate, propyl caproate, isopropyl acetate, isopropyl propionate, isopropyl isobutyrate, isopropyl butyrate, isopropyl isovalerate, propyl valerate, propyl pivalate, propyl hydrogenated angelate, propyl caproate, isopropyl acetate, isopropyl propionate, isopropyl isobutyrate, isopropyl butyrate, isopropyl isovalerate, Isopropyl valerate, isopropyl neopentanoate, isopropyl hydrogenated angelate, isopropyl caproate, butyl acetate, butyl propionate, butyl isobutyrate, butyl butyrate, butyl isovalerate, butyl valerate, butyl neopentanoate, butyl hydrogenated angelate, butyl caproate, isobutyl acetate, isobutyl propionate, isobutyl isobutyrate, isobutyl butyrate, isobutyl isovalerate, isobutyl valerate, isobutyl neopentanoate, isobutyl hydrogenated angelate, isobutyl caproate, tert-butyl acetate, tert-butyl propionate, tert-butyl isobutyrate, tert-butyl butyrate, tert-butyl isovalerate, tert-butyl valerate, tert-butyl neopentanoate, tert-butyl hydrogenated angelate and tert-butyl caproate, etc.
[0238] Examples of the chain ether include dimethoxyethane, diethyl ether, 1,3-dioxolane, diglyme, triglyme, and tetraglyme.
[0239] Examples of the fluorinated ether include: aa -OR bb (Where Rf aa is an alkyl group containing a fluorine atom, and R bb is an organic group which may contain fluorine atoms), etc.
[0240] Examples of the ketone include acetone, methyl ethyl ketone, and methyl isobutyl ketone.
[0241] Examples of the compound in which a part or all of the H atoms of the aprotic solvent are substituted with halogen atoms include compounds in which the halogen atom is fluorine.
[0242] Here, as the fluorinated compound of the chain carbonate, for example, methyl trifluoroethyl carbonate, trifluorodimethyl carbonate, trifluorodiethyl carbonate, trifluoroethyl methyl carbonate, methyl 2,2-difluoroethyl carbonate, methyl 2,2,2-trifluoroethyl carbonate, methyl 2,2,3,3-tetrafluoropropyl carbonate can be cited. The above-mentioned fluorinated chain carbonate can be represented by the following general formula:
[0243] R cc -OC(O)OR dd
[0244] {In the formula, R cc and Rdd is selected from CH3, CH2CH3, CH2CH2CH3, CH(CH3)2 and CH2Rf ee (Where Rf ee is at least one of the group consisting of a group represented by an alkyl group having 1 to 3 carbon atoms in which a hydrogen atom is substituted by at least one fluorine atom, and R cc and / or R dd Contains at least one fluorine atom.}.
[0245] In addition, examples of fluorinated short-chain fatty acid esters include fluorinated short-chain fatty acid esters represented by 2,2-difluoroethyl acetate, 2,2,2-trifluoroethyl acetate, and 2,2,3,3-tetrafluoropropyl acetate. The fluorinated short-chain fatty acid ester can be represented by the following general formula:
[0246] R ff -C(O)OR gg
[0247] {In the formula, R ff is selected from CH3, CH2CH3, CH2CH2CH3, CH(CH3)2, CF3CF2H, CFH2, CF2H, CF2Rf hh CFHRf hh and CH2Rf ii At least one of the group consisting of R gg is selected from the group consisting of CH3, CH2CH3, CH2CH2CH3, CH(CH3)2 and CH2Rf ii At least one of the group consisting of hh is an alkyl group having 1 to 3 carbon atoms in which a hydrogen atom is optionally substituted by at least one fluorine atom, Rf ii is an alkyl group having 1 to 3 carbon atoms in which a hydrogen atom is replaced by at least one fluorine atom, and R ff and / or R gg Contains at least one fluorine atom, in R ff In the case of CF2H, R gg Not CH3}.
[0248] LIB, a representative example of an electrical storage device, is a storage battery that uses lithium transition metal oxides such as lithium cobalt oxide and lithium cobalt composite oxide as a positive electrode, a carbon material such as graphite as a negative electrode, and a non-aqueous organic solvent containing a fluorine-containing lithium salt such as LiPF6 as an electrolyte. When LIB is charged / discharged, ionized Li (lithium) travels back and forth between the electrodes. In addition, since it is necessary to suppress the contact between the electrodes while allowing the ionized Li to migrate relatively quickly between the electrodes, a separator is configured between the electrodes.
[0249] <Method for manufacturing power storage device>
[0250] The method for manufacturing an electrical storage device using a separator is not particularly limited, and for example, the following method can be illustrated. First, a longitudinal separator with a width of 10 to 500 mm (preferably 80 to 500 mm) and a length of 200 to 4000 m (preferably 1000 to 4000 m) is manufactured. Next, the positive electrode-separator-negative electrode-separator or negative electrode-separator-positive electrode-separator are stacked in the order of positive electrode-separator-negative electrode-separator, and wound into a circular or flat spiral to obtain a wound body. The wound body can be housed in a device can (such as a battery can) and further injected with an electrolyte to thereby manufacture. Alternatively, it can also be manufactured by placing a wound body made by folding electrodes and separators into a device container (such as an aluminum film) and injecting an electrolyte.
[0251] At this time, the wound body may be pressed. Specifically, a method in which a separator and an electrode including a current collector and an active material layer formed on at least one surface of the current collector are stacked and pressed can be exemplified.
[0252] Regarding the pressing temperature, as a temperature at which adhesion can be effectively exhibited, for example, it is preferably above 20°C. In addition, from the perspective of suppressing the clogging or thermal shrinkage of the pores in the separator caused by hot pressing, the pressing temperature is preferably lower than the melting point of the material contained in the microporous membrane made of polyolefin resin, and is further preferably below 120°C. From the perspective of suppressing the clogging of the pores in the separator, the pressing pressure is preferably below 20MPa. Regarding the pressing time, when roller pressing is used, it can be less than 1 second, or it can be a surface pressure of several hours. From the perspective of productivity, it is preferably less than 2 hours. When the separator for the storage device using embodiment 1 or 2 is subjected to the above-mentioned manufacturing process, it is possible to suppress the push back (press back) when the winding body composed of the electrode and the separator is pressed and formed. Therefore, it is possible to suppress the reduction in the yield in the device assembly process and shorten the production process time, which is preferred.
[0253] Since the power storage device, particularly the LIB, manufactured as described above includes the separator of the first or second embodiment, its performance (for example, cycle characteristics and safety evaluated by device destruction or heating test) can be further improved.
[0254] From the viewpoint of reliably carrying out the silane crosslinking reaction of the polyolefin resin microporous membrane containing the silane grafted modified polyolefin in the manufactured power storage device, it is preferred to carry out the following steps: a step of connecting a lead terminal to at least one pair of electrodes of the power storage device to connect to a power source; and a step of carrying out at least one charge and discharge cycle. Through the charge and discharge cycle, a substance that catalyzes the silane crosslinking reaction is generated in the electrolyte or on the electrode surface, thereby achieving the silane crosslinking reaction.
[0255] Although it is not desired to be bound by theory, it is speculated that the methoxysilane grafted portion is converted into silanol and undergoes a cross-linking reaction to become a siloxane bond due to the trace amount of water contained in the storage device (water contained in components such as electrodes, separators, and electrolytes). It is also believed that if the electrolyte or electrolyte contacts the electrode, a substance that catalyzes the silane cross-linking reaction will be generated in the electrolyte or on the surface of the electrode. They will enter the electrolyte and swell and diffuse uniformly in the amorphous part of the polyolefin where the silane-modified grafted portion is located, thereby uniformly promoting the cross-linking reaction of the laminate or winding body containing the separator. The substance that catalyzes the silane cross-linking reaction can be in the form of an acid solution or a film. When the electrolyte contains lithium hexafluorophosphate (LiPF6), it can be hydrogen fluoride (HF) generated by the reaction of LiPF6 with water, or a fluorine-containing organic substance from hydrogen fluoride (HF).
[0256] When the separator for the storage device of embodiment 1 or 2 is assembled into the storage device, the silane-grafted modified polyolefin in the polyolefin resin microporous membrane is cross-linked, and / or a cross-linked structure is formed through covalent bonds between multiple components in the inorganic porous layer. Therefore, it is considered to be suitable for the manufacturing process of the previous storage device and improve the cycle characteristics and / or safety of the storage device.
[0257] Example
[0258] The present invention is specifically described below with reference to Examples and Comparative Examples, but the present invention is not limited to these Examples and Comparative Examples. The physical properties in the Examples were measured by the following methods.
[0259] (Detection method of silane-modified polyolefin contained in separator)
[0260] The silane-modified polyolefin contained in the separator is insoluble or insufficiently soluble in an organic solvent when cross-linked, so it is sometimes difficult to directly measure the content of the silane-modified polyolefin by the separator. In this case, as a pre-treatment of the sample, methyl orthoformate, which does not cause side reactions, is used to decompose the siloxane bonds into methoxysilanols, and then a solution NMR measurement is performed, thereby detecting the silane-modified polyolefin contained in the separator, or a GPC measurement can be performed on it. The pre-treatment experiment can be performed with reference to Japanese Patent Gazette No. 3529854 and Japanese Patent Gazette No. 3529858.
[0261] Specifically, the method for detecting the silane-modified polyolefin contained in the separator can effectively utilize the silane-modified polyolefin as a raw material used in the manufacture of the separator. 1 H or 13 C NMR identification. 1 H and 13 An example of the measurement method of C NMR is described below.
[0262] (1 H NMR determination)
[0263] The sample was dissolved in o-dichlorobenzene-d4 at 140°C to obtain a proton resonance frequency of 600 MHz. 1 H-NMR spectrum. 1 The measurement conditions of H-NMR are as follows.
[0264] Equipment: AVANCE NEO 600 manufactured by Bruker
[0265] Sample tube diameter:
[0266] Solvent: o-dichlorobenzene-d4
[0267] Measuring temperature: 130℃
[0268] Pulse angle: 30°
[0269] Pulse waiting time: 1sec
[0270] Cumulative times: more than 1000 times
[0271] Sample concentration: 1wt / vol%
[0272] ( 13 C NMR determination)
[0273] The sample was dissolved in o-dichlorobenzene-d4 at 140°C to obtain 13 C-NMR spectroscopy. 13 The measurement conditions of C-NMR are as follows.
[0274] Equipment: AVANCE NEO 600 manufactured by Bruker
[0275] Sample tube diameter:
[0276] Solvent: o-dichlorobenzene-d4
[0277] Measuring temperature: 130℃
[0278] Pulse angle: 30°
[0279] Pulse waiting time: 5sec
[0280] Cumulative times: more than 10,000 times
[0281] Sample concentration: 10wt / vol%
[0282] pass 1 H and / or 13C NMR measurement can confirm the amount of silane units in the silane-modified polyolefin in the polyolefin raw material, the amount of alkyl modification of the polyolefin, etc., and can identify the content of (-CH 2 -Si: 1 H, 0.69ppm, t; 13 C, 6.11ppm,s).
[0283] (1) Weight average molecular weight
[0284] Using ALC / GPC 150C (trademark) manufactured by Waters, standard polystyrene was measured under the following conditions to prepare a calibration curve. In addition, chromatograms were measured for each of the following polymers under the same conditions, and the weight average molecular weight of each polymer was calculated based on the calibration curve by the following method.
[0285] Chromatographic columns: 2 GMH6-HT (trademark) + 2 GMH6-HTL (trademark) manufactured by Tosoh Corporation
[0286] Mobile phase: o-dichlorobenzene
[0287] Detector: Differential Refractometer
[0288] Flow rate: 1.0ml / min
[0289] Column temperature: 140°C
[0290] Sample concentration: 0.1wt%
[0291] (Weight average molecular weight of polyethylene)
[0292] The molecular weight distribution curve in terms of polyethylene was obtained by multiplying each molecular weight component in the obtained calibration curve by 0.43 (Q factor of polyethylene / Q factor of polystyrene=17.7 / 41.3), and the weight average molecular weight was calculated.
[0293] (Weight average molecular weight of resin composition)
[0294] The weight average molecular weight was calculated in the same manner as in the case of polyethylene, except that the Q factor value of the polyolefin having the largest mass fraction was used.
[0295] (2) Viscosity average molecular weight (Mv)
[0296] The intrinsic viscosity [η] at 135° C. in a decalin solvent was determined based on ASTM-D4020. The Mv of polyethylene was calculated according to the following formula.
[0297] [η] = 6.77 × 10 -4 Mv 0.67
[0298] (3) Melt flow rate (MFR) (g / 10min)
[0299] The weight of a resin product extruded for 10 minutes at 190° C. and a load of 2.16 kg was determined as an MFR value using a melt flow rate measuring instrument (MELT INDEXER F-F01) manufactured by Toyo Seiki Co., Ltd.
[0300] (4) Thickness of microporous membrane and inorganic porous layer (μm)
[0301] The thickness of the microporous film was measured at room temperature 23±2°C and relative humidity 60% using a micro thickness gauge, KBM (trademark), manufactured by Toyo Seiki Co., Ltd. Specifically, the film thickness was measured at five points at substantially equal intervals along the entire width in the TD direction, and the average value thereof was obtained.
[0302] The thickness of the separator was measured in the same manner, and the thickness of the microporous membrane was subtracted from the thickness of the separator to obtain the thickness of the inorganic porous layer.
[0303] (5) Porosity of microporous membrane (%)
[0304] A 10 cm × 10 cm square sample was cut from the microporous membrane and its volume (cm 3 ) and mass (g), and based on these and density (g / cm 3 ), the porosity is calculated using the following formula. It should be noted that the density of the mixed composition is a value calculated based on the density of each raw material used and the mixing ratio. For example, in the case of a polyolefin microporous membrane composed of polyethylene, it is assumed that the density of the mixed composition is 0.95 (g / cm 3 ) to perform the calculation.
[0305] Porosity (%) = (volume-mass / density of mixed composition) / volume×100
[0306] (6) Air permeability of microporous membrane and air permeability increase (sec / 100 cm 3 )
[0307] The air permeability of the microporous membrane was measured using a Gurley type air permeometer, G-B2 (trademark), manufactured by Toyo Seiki Co., Ltd., in accordance with JIS P-8117 (2009).
[0308] The air permeability of the separator was measured in the same manner, and the value obtained by subtracting the air permeability of the separator from the air permeability of the microporous membrane was used as the increase in air permeability.
[0309] (7) Surface roughness of microporous membrane (μm)
[0310] The surface roughness (μm) of the microporous membrane was calculated using VK-X200 manufactured by KEYENCE Corporation in accordance with JIS B0671-2002 under the conditions of surface profile measurement mode, measurement interval of 0.2 μm, and surface roughness calculation area of 216 μm×287 μm (observation magnification 50 times).
[0311] (8) Safety test 1 against battery destruction (battery destruction test 1)
[0312] The safety test is a test in which an iron nail is driven into a battery charged to 4.5V at a speed of 20mm / second to penetrate the battery to cause an internal short circuit. This test can clarify the phenomenon of internal short circuit by measuring the time change behavior of the battery voltage drop caused by the internal short circuit and the battery surface temperature rise caused by the internal short circuit. In addition, due to the insufficient closing function of the separator or the rupture of the membrane at low temperature during the internal short circuit, the battery sometimes releases heat rapidly, and the electrolyte sometimes catches fire, and the battery smokes and / or explodes.
[0313] (Preparation of Batteries Used in Safety Tests)
[0314] a. Preparation of positive electrode
[0315] 92.2% by mass of lithium cobalt composite oxide LiCoO2 as a positive electrode active material, 2.3% by mass of flaky graphite and acetylene black as conductive materials, and 3.2% by mass of PVdF as a resin binder were dispersed in NMP to prepare a slurry. The slurry was applied to one side of a 20 μm thick aluminum foil constituting a positive electrode current collector using a die coater, dried at 130°C for 3 minutes, and then compression molded using a roll press. At this time, the amount of active material applied to the positive electrode was adjusted to 250 g / m 2 , the volume density of the active material is adjusted to 3.00 g / cm 3 .
[0316] b. Preparation of negative electrode
[0317] 96.9% artificial graphite as negative electrode active material, 1.4% ammonium salt of carboxymethyl cellulose as resin binder and 1.7% styrene-butadiene copolymer latex as resin binder were dispersed in purified water to prepare slurry. The slurry was applied to one side of a copper foil with a thickness of 12 μm constituting the negative electrode current collector using a die coater, dried at 120°C for 3 minutes, and then compression molded using a roller press. At this time, the amount of negative electrode active material applied was adjusted to 106 g / m 2 , the volume density of the active material was adjusted to 1.35 g / cm 3 .
[0318] c. Preparation of non-aqueous electrolyte
[0319] The catalyst was prepared by dissolving LiPF6 as a solute in a mixed solvent of ethylene carbonate:ethyl methyl carbonate=1:2 (volume ratio) so as to give a concentration of 1.0 mol / L.
[0320] d.Battery assembly
[0321] The separator is cut into 60 mm in the width (TD) direction and 1000 mm in the length (MD) direction, and the separator is folded repeatedly, and the positive electrode and the negative electrode (12 positive electrodes and 13 negative electrodes) are alternately stacked between the separators. It should be noted that the positive electrode uses an area of 30 mm × 50 mm and the negative electrode uses an area of 32 mm × 52 mm. After the repeatedly folded stack is put into a laminated bag, the non-aqueous electrolyte obtained in the above c. is injected and sealed. After being placed at room temperature for 1 day, the battery voltage is charged to 4.2V at a current value of 3mA (0.5C) in an atmosphere of 25°C. After reaching 4.2V, the current value is reduced from 3mA to maintain 4.2V. This method is used for the initial charge after the battery is made for a total of 6 hours. Then, the battery voltage is discharged to 3.0V at a current value of 3mA (0.5C).
[0322] (Maximum heat release rate)
[0323] After an iron nail was driven into the obtained battery at a speed of 20 mm / sec and penetrated, the temperature change rate at which the temperature rise per 1 sec was the largest was determined as the maximum heat release rate based on the temperature change graph obtained by measuring the battery surface temperature for 300 sec using a thermocouple.
[0324] (Voltage drop time)
[0325] After an iron nail was driven into the obtained battery at a speed of 20 mm / sec and penetrated, the time required for the voltage to drop from 4.5 V to 3 V was determined as the voltage drop time (time to drop to 3 V).
[0326] (9) Evaluation of cycle characteristics 1 (battery cycle stability 1) and method for manufacturing the battery
[0327] A battery for evaluating cycle characteristics was prepared in the same manner as a. to c. of the method for preparing the battery used in the above item "(8) Battery destruction test 1", except that the assembly was in accordance with d. below.
[0328] The charge and discharge of the obtained battery were carried out for 100 cycles in an atmosphere of 60°C. The battery voltage was charged to 4.2V at a current value of 6.0mA (1.0C). After reaching the current value, the current value was reduced from 6.0mA to maintain 4.2V, and the charging was carried out for a total of 3 hours in this way. The battery voltage was discharged to 3.0V at a current value of 6.0mA (1.0C). The capacity retention rate (%) was calculated from the discharge capacity of the 100th cycle and the discharge capacity of the 1st cycle. When the capacity retention rate in the battery cycle stability is high, it is evaluated as having good cycle characteristics.
[0329] d.Battery assembly
[0330] Cut the separator into a circle with a diameter of 18 mm, cut the positive electrode and the negative electrode into a circle with a diameter of 16 mm, and stack the positive electrode, separator, and negative electrode in order so that the active material surfaces of the positive electrode and the negative electrode face each other, and place them in a stainless steel metal container with a lid. The container and the lid are insulated, the container is in contact with the copper foil of the negative electrode, and the lid is in contact with the aluminum foil of the positive electrode. The non-aqueous electrolyte obtained in c. of the above-mentioned item "(8) Battery Destruction Test 1" is injected into the container and sealed. After being placed at room temperature for 1 day, charge at a current value of 3mA (0.5C) to a battery voltage of 4.2V in an atmosphere of 25°C. After reaching 4.2V, the current value is reduced from 3mA to maintain the current value. This method is used for the initial charge after the battery is made for a total of 6 hours. Next, discharge at a current value of 3mA (0.5C) to a battery voltage of 3.0V.
[0331] (10) Determination of closing and rupture temperature 1
[0332] (Fusing / Melting (F / MD) Characteristics 1)
[0333] The positive electrode, separator and negative electrode are cut into a circular shape with a diameter of 200 mm and stacked. The electrolyte is added to the obtained stack and infiltrated into the whole. The stack is clamped in the center of a circular aluminum heater with a diameter of 600 mm, and the aluminum heater is pressurized to 0.5 MPa from the top and bottom with a hydraulic jack to complete the preparation for the measurement. While heating the stack with an aluminum heater at a heating rate of 2°C / min, the resistance (Ω) between the electrodes is measured. The temperature at which the separator melts and the resistance between the electrodes rises and the resistance exceeds 1000Ω for the first time is taken as the melting temperature (shutdown temperature). In addition, further heating is continued, and the temperature at which the resistance is reduced to less than 1000Ω is taken as the melting temperature (film rupture temperature). It should be noted that the measurement uses a wire for resistance measurement bonded to the back of the aluminum foil of the positive electrode made in the item "a. Preparation of positive electrode" of the above-mentioned "(8) Battery destruction test". In addition, the measurement used a wire for resistance measurement bonded to the back of the copper foil of the negative electrode produced in the item "b. Production of negative electrode" of the above "(8) Battery destruction test" using a conductive silver paste. Furthermore, the electrolyte prepared in the item "c. Preparation of non-aqueous electrolyte" of the above "(8) Battery destruction test" was also used in the F / MD characteristic test.
[0334] (11) Solvent immersion test
[0335] The microporous membrane having the inorganic porous layer formed thereon was cut into a 5.0×5.0 cm square and immersed in acetone at 25° C. in a glass sample jar. The entire glass sample jar was vibrated at a frequency of 40 Hz for 10 minutes using an ultrasonic cleaner.
[0336] The microporous membrane with the inorganic porous layer formed thereon was then taken out from the acetone, air-dried, and then the inorganic porous layer side was read as a monochrome image using a scanner manufactured by EPSON at 8 bit shades and 600 dpi resolution (see Figure 3 ).
[0337] The read image was subjected to image processing according to the following methods (I) to (IV), and the ratio of the area of the peeled portion (peeled area (%)) was derived.
[0338] (I) The read image is defined as an evaluation image P, and the length of one side of the evaluation image P is defined as X and Y. X and Y may correspond to the length of one side of the cut microporous film. Therefore, X=5 cm and Y=5 cm are defined here.
[0339] (II) In the evaluation image P, when the direction along the X side is defined as the X axis and the direction along the Y side is defined as the Y axis, the pixel density value at the coordinate position (x, y) constituting the evaluation image P is defined as P(x, y). Then, a histogram is created for all Xp×Yp density values P(x, y) included in the evaluation image P.
[0340] An example of a histogram obtained by evaluation of Example 15 is shown below. Figure 1 . Figure 1 In the figure, the vertical axis (logarithmic representation) represents the frequency value, and the horizontal axis represents the lightness and darkness value. Figure 1 The peaks representing the bright part (peaks with small shading values) and the peaks representing the dark part (peaks with large shading values) are confirmed. Then, the shading value corresponding to the top of the peak representing the bright part is determined as the shading value Pb of the bright part, and the shading value corresponding to the top of the peak representing the dark part is determined as the shading value Pd of the dark part. Figure 1 In FIG. 1 , the frequency value that gives the gradation value Pb of the bright portion and the frequency value that gives the gradation value Pd of the dark portion are shown by “×” symbols, respectively.
[0341] When the number of pixels corresponding to the bright part or the number of pixels corresponding to the dark part is relatively small, the peak of the side with fewer pixels may not be clearly confirmed. In this case, the light and dark values Pb of the bright part and the light and dark values Pd of the dark part can be determined as follows based on the shape of the obtained histogram.
[0342] (II-1)
[0343] Another example of a histogram is shown in Figure 2 The vertical and horizontal axes are Figure 1 The same example. When the number of pixels in the dark area is relatively small, such as Figure 2 As shown, there is a case where a peak indicating a bright part is confirmed, but a peak indicating a dark part cannot be clearly confirmed. In this case, within the range where the shading value is greater than the peak corresponding to the brightness, the frequency value on the histogram is kept substantially constant, but as the shading value increases, the frequency value decreases sharply, and the shading value of the portion that begins to decrease sharply (corresponding to the right shoulder of the histogram) can be determined as the shading value Pd of the dark part. Figure 2 In FIG. 1 , the frequency value giving the gradation value Pb of the bright portion and the frequency value giving the gradation value Pd of the dark portion are shown by “×” symbols, respectively.
[0344] (II-2)
[0345] When the number of pixels corresponding to the bright part is relatively small, although not shown in the figure, there is a case where a peak indicating the dark part is confirmed, but a peak indicating the bright part cannot be clearly confirmed. In this case, within the range of the shading value less than the corresponding dark part, the frequency value on the histogram is kept substantially constant, but as the shading value decreases, the frequency value decreases sharply, and the shading value of the part that starts to decrease sharply (the part of the left shoulder of the histogram) can be determined as the shading value Pb of the bright part.
[0346] (III) The light portion shading value Pb and the dark portion shading value Pd determined as described above are used to calculate their average value by the following equation, and the obtained value is determined as the threshold value Ps. Figure 1 and Figure 2 In FIG. 1 , the frequency value giving the threshold value Ps is shown by an “×” symbol.
[0347] Threshold value Ps = (bright part shading value Pb + dark part shading value Pd) / 2
[0348] (IV) Prepare a sequence BW(x, y) as a binary image of the same size as the evaluation image P. For pixels P(x, y) in the evaluation image P with a shading value greater than a threshold value Ps, substitute 1 into the BW(x, y) corresponding to the pixel P(x, y) and treat it as a bright portion. For pixels P(x, y) with a shading value less than or equal to the threshold value Ps, substitute 0 into the BW(x, y) corresponding to the pixel P(x, y) and treat it as a dark portion. Thus, a binary image BW (see FIG. 1 ) in which the bright and dark portions of the evaluation image P are distinguished is obtained. Figure 4 ).
[0349] (V) The number of BW(x, y) with a value of 1 in the binary image BW is determined as the number of bright pixels Br. Similarly, the number of BW(x, y) with a value of 0 in the binary image BW is determined as the number of dark pixels Dk. Br, Dk, Xp, and Yp satisfy the equation Br+Dk=Xp×Yp.
[0350] (VI) The ratio of the bright part Brp is calculated by the formula Brp = Br / (Xp × Yp), and the ratio of the dark part Dkp is calculated by the formula Dkp = Dk / (Xp × Yp). The obtained ratio of the bright part Brp is determined as the ratio (%) of the area of the peeling part, and the obtained ratio of the dark part Dkp is determined as the ratio (%) of the area of the normal part.
[0351] [Production Example of Silane Graft-Modified Polyolefin]
[0352] Polyethylene with a viscosity average molecular weight of 20,000 is used as the raw polyethylene. An organic peroxide (di-tert-butyl peroxide) is added while the raw polyethylene is melt-kneaded by an extruder. After free radicals are generated in the polymer chain of the α-olefin, trimethoxyalkoxylate-substituted vinyl silane is injected, and alkoxysilyl groups are introduced into the α-olefin polymer through an addition reaction to form a silane grafted structure. In addition, in order to simultaneously adjust the free radical concentration in the reaction system, an antioxidant (pentaerythritol tetra[3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate]) is added in an appropriate amount to inhibit the chain reaction (gelation) in the α-olefin. The obtained silane-grafted polyolefin molten resin is cooled in water, pelletized, and then heated and dried at 80°C for 2 days to remove moisture or unreacted trimethoxyalkoxylate-substituted vinyl silane. It should be noted that the residual concentration of unreacted trimethoxyalkoxylate-substituted vinyl silane in the pellets is about 1500ppm or less.
[0353] By the modification reaction using trimethoxyalkoxylate instead of vinylsilane as described above, a silane-grafted polyethylene having an MFR (190° C.) of 0.24 g / min (represented as “silane-modified polyethylene (B)” in Tables 1, 2, 5, or 6) was obtained.
[0354] [Example 1]
[0355] (Manufacturing of Silane Crosslinkable Polyolefin Microporous Membrane)
[0356] 19.8% by mass of the silane-modified polyethylene (B) obtained above was added to 79.2% by mass of polyethylene (A) as a homopolymer having a weight average molecular weight of 700,000 (represented as "polyethylene (A)" in Tables 1, 2, 5 or 6) to form a resin complex having resin compositions of 0.8 and 0.2 for polyethylene (A) and (B), respectively, and 1% by mass of pentaerythritol-tetrakis-[3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate] as an antioxidant was added to the complex, and dry blending was performed using a drum mixer to obtain a mixture. The obtained mixture was supplied to a twin-screw extruder from a feeder under a nitrogen atmosphere. In addition, liquid paraffin (kinematic viscosity at 37.78°C was 7.59×10 -5 m 2 / s) is injected into the extruder drum through a plunger pump.
[0357] The mixture and liquid paraffin were melt-kneaded in an extruder, and the feeder and pump were adjusted so that the amount of liquid paraffin in the extruded polyolefin composition was 70% by mass (i.e., the polymer concentration was 30% by mass). The melt-kneading conditions were a set temperature of 220° C., a screw speed of 240 rpm, and a discharge of 18 kg / h.
[0358] Next, the melt-kneaded product was extruded through a T-die onto a cooling roll whose surface temperature was controlled to be 25° C. and cast, thereby obtaining a gel sheet (sheet-like molded product) having a green film thickness of 1100 μm.
[0359] Then, the sheet-shaped molded body was introduced into a simultaneous biaxial stretching machine and biaxially stretched to obtain a stretched product. The stretching conditions were set to MD ratio 7.0 times, TD ratio 6.2 times, and biaxial stretching temperature 120°C.
[0360] Then, the stretched gel sheet was introduced into a dichloromethane tank, fully immersed in dichloromethane to extract and remove the liquid paraffin, and then dried to remove the dichloromethane, thereby obtaining a porous body.
[0361] Then, the porous body was introduced into a TD stenter for heat setting (HS), and HS was performed at a heat setting temperature of 133° C. and a stretching ratio of 2.1 times, and then a relaxation operation was performed to 2.0 times in the TD direction.
[0362] Then, the end of the obtained microporous membrane was cut and wound into a mother roll having a width of 1100 mm and a length of 5000 m.
[0363] In the above evaluation, the microporous membrane unwound from the mother roll was cut as necessary and used as a microporous membrane for evaluation.
[0364] The film thickness, air permeability, porosity, surface roughness, etc. of the obtained microporous film for evaluation were measured and the results are shown in Table 1.
[0365] (Manufacturing of Inorganic Porous Layer)
[0366] (Method for producing acrylic latex)
[0367] The acrylic latex used as the resin binder is produced by the following method.
[0368] Into a reaction vessel equipped with a stirrer, a reflux condenser, a dropping tank, and a thermometer, 70.4 parts by mass of ion exchange water, 0.5 parts by mass of "Aquaron KH1025" (registered trademark, 25% aqueous solution manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) as an emulsifier, and 0.5 parts by mass of "ADEKA REASOAP SR1025" (registered trademark, 25% aqueous solution manufactured by ADEKA Co., Ltd.) were added. Next, the temperature inside the reaction vessel was raised to 80°C, and 7.5 parts by mass of a 2% aqueous solution of ammonium persulfate was added while maintaining the temperature at 80°C to obtain an initial mixture. Five minutes after the addition of the ammonium persulfate aqueous solution was completed, the emulsion was dropped from the dropping tank into the reaction vessel over 150 minutes.
[0369] It should be noted that the above-mentioned emulsion was prepared by mixing the following substances for 5 minutes using a homomixer: 70 parts by mass of butyl acrylate; 29 parts by mass of methyl methacrylate; 1 part by mass of methacrylic acid; 3 parts by mass of "Aquaron KH1025" (registered trademark, 25% aqueous solution manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) and 3 parts by mass of "ADEKA REASOAPSR1025" (registered trademark, 25% aqueous solution manufactured by ADEKA Co., Ltd.) as emulsifiers; 7.5 parts by mass of a 2% aqueous solution of ammonium persulfate; and a mixture of 52 parts by mass of ion-exchanged water.
[0370] After the dropwise addition of the emulsion was completed, the temperature inside the reaction vessel was maintained at 80°C for 90 minutes, and then cooled to room temperature. The obtained emulsion was adjusted to pH = 8.0 with a 25% aqueous ammonium hydroxide solution, and a small amount of water was added to obtain an acrylic latex with a solid content of 40%. The obtained acrylic latex had a number average particle size of 145 nm and a glass transition temperature of -23°C.
[0371] (Formation of Inorganic Porous Layer)
[0372] 94.6 parts by weight of aluminum hydroxide (average particle size 1.4 μm) as inorganic particles and 0.4 parts by weight (solid content conversion) of an aqueous solution of ammonium polycarboxylate (SN Dispersant 5468 manufactured by SANOPCO LIMITED, solid content concentration 40%) as an ionic dispersant were uniformly dispersed in 100 parts by weight of water to prepare a dispersion. The obtained dispersion was crushed using a bead mill (tank volume 200 cc, zirconia bead diameter 0.1 mm, filling amount 80%) to adjust the particle size distribution of the inorganic particles to D50 = 1.0 μm. 2.0 parts by weight (solid content conversion) of acrylic latex (solid content concentration 40%, average particle size 145 nm, glass transition temperature -23°C, constituent monomers: butyl acrylate, methyl methacrylate, methacrylic acid) as a resin binder were added to the dispersion with adjusted particle size distribution. Then, 3.0 parts by mass (in terms of solid content) of EPOCROS K-2010E manufactured by Nippon Shokubai Co., Ltd. was added as a crosslinking agent to prepare a slurry containing inorganic particles.
[0373] Then, the microporous membrane is continuously unwound from the microporous membrane mother roll, and a slurry containing inorganic particles is coated on one side of the microporous membrane using a gravure reverse coater, and then dried in a drier at 60° C. to remove water, and wound up to obtain a separator mother roll.
[0374] During the evaluation, the separators unwound from the mother roll were cut as necessary and used as separators for evaluation.
[0375] [Examples 2-14, Comparative Examples 1-18]
[0376] Separators with various physical properties were prepared by the same method as in Example 1, except that the presence or absence of silane-modified polyethylene (B), various raw material compositions, HS ratios, stretching temperatures, etc. were adjusted as shown in Table 1 or 2. It should be noted that the crosslinking agent used in Examples 2, 3, 11-14, and Comparative Examples 1-3 was EPOCROS K-2010E manufactured by Nippon Shokubai Co., Ltd., the crosslinking agent used in Example 4 was CARBODILITE V-02 manufactured by Nisshinbo Chemical Inc., the crosslinking agent used in Example 5 was duranate WB40-100 manufactured by Asahi Kasei Corporation, and the crosslinking agent used in Example 6 was Denacol EX-61B manufactured by Nagase ChemteX Corporation, which is an epoxy crosslinking agent. Examples 7, 9, and 10 used tetraethoxysilane manufactured by Shin-Etsu Chemical Co., Ltd., Example 8 used 3-aminopropyltrimethoxysilane KBM-903 manufactured by Shin-Etsu Chemical Co., Ltd., Comparative Examples 9 and 14 used HARDENER 12A manufactured by Asahi Kasei Corporation, Comparative Examples 10, 12, 15, and 17 used ethylenediaminetetraacetic acid (EDTA) manufactured by SIGAM-ALDRICH, and Comparative Examples 11, 13, 16, and 18 used 1,4,7,10-tetraazacyclododecane-1,4,7,10-tetraacetic acid (DOTA) manufactured by SIGAM-ALDRICH.
[0377] The above-mentioned various measurements and tests were performed using the separators obtained in the above-mentioned Examples and Comparative Examples. The test results are shown in Tables 1 and 2.
[0378] [Table 1-1]
[0379]
[0380] [Table 1-2]
[0381]
[0382] [Table 1-3]
[0383]
[0384] [Table 2-1]
[0385]
[0386] [Table 2-2]
[0387]
[0388] [Table 2-3]
[0389]
[0390] [Table 2-4]
[0391]
[0392] [Table 2-5]
[0393]
[0394] [Example 15]
[0395] (Manufacturing of polyolefin microporous membrane)
[0396] 99% by mass of polyethylene (PE(A)) as a homopolymer having a weight average molecular weight of 700,000 and 1% by mass of pentaerythritol-tetrakis-[3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate] as an antioxidant were added and dry-mixed again with a drum mixer to obtain a polymer mixture. The obtained polymer mixture was replaced with nitrogen and then supplied to a twin-screw extruder from a feeder under a nitrogen atmosphere. In addition, liquid paraffin (kinematic viscosity at 37.78°C was 7.59×10 - 5 m 2 / s) is injected into the extruder drum through a plunger pump.
[0397] Melt mixing was performed, and the feeder and pump were adjusted so that the amount of liquid paraffin in the total mixture extruded was 70% by mass (i.e., the polymer concentration was 30% by mass). The melt mixing conditions were a set temperature of 230° C., a screw speed of 240 rpm, and a discharge rate of 18 kg / h.
[0398] Next, the molten kneaded product is extruded through a T die onto a cooling roller whose surface temperature is controlled to be 25°C and cast, thereby obtaining a gel sheet with a blank film thickness of 1400 μm. Then, it is guided to a simultaneous biaxial stretching machine for biaxial stretching. The stretching conditions are set to MD ratio 7.0 times, TD ratio 6.0 times (i.e., 7×6 times), and biaxial stretching temperature 125°C. Then, it is guided to a methyl ethyl ketone tank, fully immersed in methyl ethyl ketone to extract and remove liquid paraffin, and then dried to remove methyl ethyl ketone. Then, in order to perform heat setting (sometimes simply referred to as "HS"), it is guided to a TD stenter, HS is performed at a heat setting temperature of 125°C and a stretching ratio of 1.8 times, and then a relaxation operation is performed until 1.2 times. Then, for the obtained microporous membrane, the ends are cut off and rolled into a mother roll with a width of 1100 mm and a length of 5000 m to obtain a microporous membrane. For the obtained membrane, the film thickness, air permeability, porosity and surface roughness were measured, as shown in Table 3.
[0399] (Manufacturing of Inorganic Porous Layer)
[0400] (Method for producing acrylic latex)
[0401] The acrylic latex used as the resin binder is produced by the following method.
[0402] Into a reaction vessel equipped with a stirrer, a reflux condenser, a dropping tank, and a thermometer, 70.4 parts by mass of ion exchange water, 0.5 parts by mass of "Aquaron KH1025" (registered trademark, 25% aqueous solution manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) as an emulsifier, and 0.5 parts by mass of "ADEKA REASOAP SR1025" (registered trademark, 25% aqueous solution manufactured by ADEKA Co., Ltd.) were added. Next, the temperature inside the reaction vessel was raised to 80°C, and 7.5 parts by mass of a 2% aqueous solution of ammonium persulfate was added while maintaining the temperature at 80°C to obtain an initial mixture. Five minutes after the addition of the ammonium persulfate aqueous solution was completed, the emulsion was dropped from the dropping tank into the reaction vessel over 150 minutes.
[0403] The emulsion was prepared by mixing the following for 5 minutes using a homomixer: 70 parts by mass of butyl acrylate; 29 parts by mass of methyl methacrylate; 1 part by mass of methacrylic acid; 3 parts by mass of "Aquaron KH1025" (registered trademark, 25% aqueous solution manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) and 3 parts by mass of "ADEKAREASOAP SR1025" (registered trademark, 25% aqueous solution manufactured by ADEKA Co., Ltd.) as emulsifiers; 7.5 parts by mass of a 2% aqueous solution of ammonium persulfate; and a mixture of 52 parts by mass of ion-exchanged water.
[0404] After the dropwise addition of the emulsion was completed, the temperature inside the reaction vessel was maintained at 80°C for 90 minutes, and then cooled to room temperature. The obtained emulsion was adjusted to pH = 8.0 with a 25% aqueous ammonium hydroxide solution, and a small amount of water was added to obtain an acrylic latex with a solid content of 40%. The obtained acrylic latex had a number average particle size of 145 nm and a glass transition temperature of -23°C.
[0405] (Formation of Inorganic Porous Layer)
[0406] 94.6% by mass of aluminum hydroxide (average particle size 1.4 μm) as inorganic particles and 0.40% by mass (solid content conversion) of polycarboxylic acid ammonium aqueous solution (SN Dispersant 5468 manufactured by SANOPCO LIMITED, solid content concentration 40%) as an ionic dispersant are uniformly dispersed in 100% by mass of water to prepare a dispersion. The obtained dispersion is crushed using a bead mill (tank volume 200cc, zirconia bead diameter 0.1mm, filling amount 80%) to adjust the particle size distribution of the inorganic particles to D50 = 1.0 μm. 2.0% by mass (solid content conversion) of acrylic latex (solid content concentration 40%, average particle size 145nm, glass transition temperature -23°C, constituent monomers: butyl acrylate, methyl methacrylate, methacrylic acid) as a resin binder is added to the dispersion with adjusted particle size distribution. Then, 3.0% by mass (solid content conversion) of EPOCROS K-2010E manufactured by Nippon Shokubai Co., Ltd. was added as a crosslinking agent to prepare a slurry containing inorganic particles.
[0407] Then, the microporous membrane is continuously unwound from the microporous membrane mother roll, and a slurry containing inorganic particles is coated on one side of the microporous membrane using a gravure reverse coater, and then dried in a drier at 60° C. to remove water, and wound up to obtain a separator mother roll.
[0408] During the evaluation, the separators unwound from the mother roll were cut as necessary and used as separators for evaluation.
[0409] [Examples 16-27, Comparative Examples 19-29]
[0410] Separators with various physical properties were prepared by adjusting the HS ratio and the stretching temperature in the same manner as in Example 15. It should be noted that the crosslinking agent used in Examples 16, 24-27, and Comparative Examples 19-21 was EPOCROS K-2010E manufactured by Nippon Shokubai Co., Ltd., the crosslinking agent used in Example 17 was CARBODILITE V-02 manufactured by Nisshinbo Chemical Inc., the crosslinking agent used in Example 18 was duranate WB40-100 manufactured by Asahi Kasei Corporation, and the crosslinking agent used in Example 19 was Denacol EX-61B manufactured by Nagase ChemteX Corporation, which is an epoxy crosslinking agent. Examples 20, 22, and 23 used an alkoxy oligomer (KR-500) manufactured by Shin-Etsu Chemical Co., Ltd., Example 21 used 3-aminopropyltrimethoxysilane KBM-903 manufactured by Shin-Etsu Chemical Co., Ltd., Comparative Example 25 used HARDENER 12A manufactured by Asahi Kasei Corporation, Comparative Examples 26 and 28 used ethylenediaminetetraacetic acid (EDTA) manufactured by SIGAM-ALDRICH, and Comparative Examples 27 and 29 used 1,4,7,10-tetraazacyclododecane-1,4,7,10-tetraacetic acid (DOTA) manufactured by SIGAM-ALDRICH.
[0411] The above-mentioned various tests were conducted using the separators obtained in the above-mentioned Examples and Comparative Examples. The test results are shown in Tables 3 and 4. In the tables, the unit "mass %" is described as "wt %".
[0412] [Table 3-1]
[0413]
[0414] [Table 3-2]
[0415]
[0416] [Table 4-1]
[0417]
[0418] [Table 4-2]
[0419]
[0420] [Example 28]
[0421] (Manufacturing of Silane Crosslinkable Polyolefin Microporous Membrane)
[0422] 19.8% by mass of the silane-modified polyethylene (B) obtained above was added to 79.2% by mass of polyethylene (A) as a homopolymer having a weight average molecular weight of 800,000 to form a resin complex having a resin composition of 0.8 and 0.2 for polyethylene (A) and (B), respectively. 1% by mass of pentaerythritol-tetrakis-[3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate] as an antioxidant was added to the complex and dry-mixed using a drum mixer to obtain a mixture. The obtained mixture was supplied to a twin-screw extruder from a feeder under a nitrogen atmosphere. In addition, liquid paraffin (kinematic viscosity at 37.78°C is 7.59×10 -5 m 2 / s) is injected into the extruder drum through a plunger pump.
[0423] The mixture and liquid paraffin were melt-kneaded in an extruder, and the feeder and pump were adjusted so that the amount of liquid paraffin in the extruded polyolefin composition was 70% by mass (i.e., the polymer concentration was 30% by mass). The melt-kneading conditions were a set temperature of 220° C., a screw speed of 300 rpm, and a discharge of 18 kg / h.
[0424] Next, the melt-kneaded product was extruded through a T-die onto a cooling roll whose surface temperature was controlled to be 25° C. and cast, thereby obtaining a gel sheet (sheet-like molded product) having a green film thickness of 1150 μm.
[0425] Then, the sheet-shaped molded body was introduced into a simultaneous biaxial stretching machine and biaxially stretched to obtain a stretched product. The stretching conditions were set to MD ratio 7.0 times, TD ratio 6.7 times, and biaxial stretching temperature 119°C.
[0426] Then, the stretched gel sheet was introduced into a dichloromethane tank, fully immersed in dichloromethane to extract and remove the liquid paraffin, and then dried to remove the dichloromethane, thereby obtaining a porous body.
[0427] Then, the porous body was introduced into a TD stenter for heat setting (HS), HS was performed at a heat setting temperature of 132° C. and a stretching ratio of 2.1 times, and then a relaxation operation was performed to 1.7 times in the TD direction.
[0428] Then, the end of the obtained microporous membrane was cut and wound into a mother roll having a width of 1100 mm and a length of 5000 m.
[0429] In the above evaluation, the microporous membrane unwound from the mother roll was cut as necessary and used as a microporous membrane for evaluation.
[0430] The film thickness, surface roughness, air permeability, porosity, etc. of the obtained microporous film for evaluation were measured. The results are shown in Table 5.
[0431] (Manufacturing of Inorganic Porous Layer)
[0432] (Method for producing acrylic latex)
[0433] The acrylic latex used as the resin binder is produced by the following method.
[0434] Into a reaction vessel equipped with a stirrer, a reflux condenser, a dropping tank, and a thermometer, 70.4 parts by mass of ion exchange water, 0.5 parts by mass of "Aquaron KH1025" (registered trademark, 25% aqueous solution manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) as an emulsifier, and 0.5 parts by mass of "ADEKA REASOAP SR1025" (registered trademark, 25% aqueous solution manufactured by ADEKA Co., Ltd.) were added. Next, the temperature inside the reaction vessel was raised to 80°C, and 7.5 parts by mass of a 2% aqueous solution of ammonium persulfate was added while maintaining the temperature at 80°C to obtain an initial mixture. Five minutes after the addition of the aqueous ammonium persulfate solution was completed, the emulsion was dropped from the dropping tank into the reaction vessel over 150 minutes.
[0435] It should be noted that the above-mentioned emulsion was prepared by mixing the following substances for 5 minutes using a homomixer: 70 parts by mass of butyl acrylate; 29 parts by mass of methyl methacrylate; 1 part by mass of methacrylic acid; 3 parts by mass of "Aquaron KH1025" (registered trademark, 25% aqueous solution manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) and 3 parts by mass of "ADEKA REASOAPSR1025" (registered trademark, 25% aqueous solution manufactured by ADEKA Co., Ltd.) as emulsifiers; 7.5 parts by mass of a 2% aqueous solution of ammonium persulfate; and a mixture of 52 parts by mass of ion-exchanged water.
[0436] After the dropwise addition of the emulsion was completed, the temperature inside the reaction vessel was maintained at 80°C for 90 minutes, and then cooled to room temperature. The obtained emulsion was adjusted to pH = 8.0 with a 25% aqueous ammonium hydroxide solution, and a small amount of water was added to obtain an acrylic latex with a solid content of 40%. The obtained acrylic latex had a number average particle size of 145 nm and a glass transition temperature of -20°C.
[0437] (Formation of Inorganic Porous Layer)
[0438] 94.60 parts by weight of aluminum hydroxide (average particle size 1.4 μm) as inorganic particles and 0.40 parts by weight (solid content conversion) of polycarboxylic acid ammonium aqueous solution (SN Dispersant 5468 manufactured by SANOPCO LIMITED, solid content concentration 40%) as an ionic dispersant were uniformly dispersed in 100 parts by weight of water to prepare a dispersion. The obtained dispersion was crushed using a bead mill (tank volume 200 cc, zirconia bead diameter 0.1 mm, filling amount 80%) to adjust the particle size distribution of the inorganic particles to D50 = 0.8 μm. 2 parts by weight (solid content conversion) of acrylic latex (solid content concentration 40%, average particle size 145 nm, glass transition temperature -20°C, constituent monomers: butyl acrylate, methyl methacrylate, methacrylic acid) as a resin binder were added to the dispersion with adjusted particle size distribution. Then, 3 parts by mass (in terms of solid content) of EPOCROS K-2010E manufactured by Nippon Shokubai Co., Ltd. was added as a crosslinking agent to prepare a slurry containing inorganic particles.
[0439] Then, the microporous membrane is continuously unwound from the microporous membrane mother roll, and a slurry containing inorganic particles is coated on one side of the microporous membrane using a gravure reverse coater, and then dried in a drier at 60° C. to remove water, and wound up to obtain a separator mother roll.
[0440] During the evaluation, the separators unwound from the mother roll were cut as necessary and used as separators for evaluation.
[0441] [Examples 29-41, Comparative Examples 30-44]
[0442] Separators with various physical properties were prepared by the same method as in Example 28, except that the presence or absence of silane-modified polyethylene (B), various raw material compositions, HS ratios, stretching temperatures, etc. were adjusted as shown in Table 5 or Table 6. It should be noted that the crosslinking agent used in Examples 29, 30, 38-41 was EPOCROS K-2010E manufactured by Nippon Shokubai Co., Ltd., the crosslinking agent used in Example 31 was CARBODILITE V-02 manufactured by Nisshinbo Chemical Inc., the crosslinking agent used in Example 32 was duranate WB40-100 manufactured by Asahi Kasei Corporation, and the crosslinking agent used in Example 33 was Denacol EX-61B manufactured by Nagase ChemteX Corporation, which is an epoxy crosslinking agent. Examples 34, 36, and 37 use tetraethoxysilane manufactured by Shin-Etsu Chemical Co., Ltd., Example 35 uses 3-aminopropyltrimethoxysilane KBM-903 manufactured by Shin-Etsu Chemical Co., Ltd., Comparative Examples 35 and 40 use HARDENER 12A manufactured by Asahi Kasei Corporation, Comparative Examples 36, 38, 41, and 43 use ethylenediaminetetraacetic acid (EDTA) manufactured by SIGAM-ALDRICH, and Comparative Examples 37, 39, 42, and 44 use 1,4,7,10-tetraazacyclododecane-1,4,7,10-tetraacetic acid (DOTA) manufactured by SIGAM-ALDRICH.
[0443] The separators obtained in the above-mentioned embodiments and the above-mentioned comparative examples were used to carry out the above-mentioned various measurements or tests, especially the solvent immersion test, F / MD measurement, measurement of the increase in air permeability after coating, battery cycle test, battery destruction test, etc. The test results are shown in Tables 5 to 6. It should be noted that in Examples 28 to 41 and Comparative Examples 30 to 44, the positive electrode active material was changed to LiNi which has a poorer thermal stability than LiCoO2 as shown below. 3 / 5 Mn 1 / 5 Co 1 / 5 O2 and the speed of hammering the iron nail into the battery is changed from 20mm / sec to 30mm / sec, thus becoming a more stringent evaluation system than the above-mentioned "Battery Cycle Stability 1" and "Battery Destruction Test 1", and is therefore represented as "Battery Cycle Stability 2" and "Battery Destruction Test 2" in Tables 5 and 6.
[0444] (12) Battery cycle stability 2 (cycle test 2), battery destruction test 2 (nail penetration test 2)
[0445] a. Preparation of positive electrode
[0446] LiNi as the positive electrode active material 3 / 5 Mn 1 / 5 Co 1 / 5O2, carbon black as a conductive aid, and polyvinylidene fluoride solution as a binder were mixed at a solid content mass ratio of 91:5:4, and N-methyl-2-pyrrolidone as a dispersion solvent was added to make the solid content 68% by mass, and further mixed to prepare a slurry solution. The slurry solution was applied to one side of an aluminum foil with a thickness of 15 μm so that a part of the aluminum foil was exposed, and then dried to remove the solvent, so that the coating amount was 175 g / m 2 The positive electrode mixture was then rolled using a roller press to a density of 2.8 g / cm 3 Then, the coated portion was cut into 30 mm×50 mm including the exposed portion of the aluminum foil to obtain a positive electrode.
[0447] b. Preparation of negative electrode
[0448] Artificial graphite as a negative electrode active material, styrene butadiene rubber as a binder, and a carboxymethyl cellulose aqueous solution were mixed at a solid content mass ratio of 96.4:1.9:1.7, and water was added as a dispersion solvent to make the solid content 50% by mass, and further mixed to prepare a slurry solution. The slurry solution was applied to one side of a copper foil with a thickness of 10 μm so that a part of the copper foil was exposed, and then dried to remove the solvent, so that the coating amount was 86 g / m 2 The negative electrode mixture was then rolled using a roller press to a density of 1.45 g / cm 3 Then, the coated portion was cut into 32 mm×52 mm including the copper foil exposed portion to obtain a negative electrode.
[0449] c. Preparation of non-aqueous electrolyte
[0450] A non-aqueous electrolyte was prepared by dissolving LiPF6 as a solute in a mixed solvent of ethylene carbonate:ethyl methyl carbonate=1:2 (volume ratio) to a concentration of 1.0 mol / L, and further adding vinylene carbonate to a concentration of 1.0 wt%.
[0451] d.Battery assembly
[0452] A 60 mm x 40 mm square was cut out from the separator to prepare a sample.
[0453] While folding a 55mm wide strip separator in a manner that the active material surface of the positive electrode and the negative electrode is opposite and sandwiched between the positive electrode and the negative electrode, a laminate consisting of 15 double-sided negative electrodes and 14 double-sided positive electrodes is made. At this time, the inorganic porous layer of the sample is configured in a manner relative to the positive electrode. After welding an aluminum lead sheet with a sealant to the exposed portion of 14 positive aluminum foils of the laminate, and welding a nickel lead sheet with a sealant to the exposed portion of 15 negative copper foils, insert it into the aluminum laminated outer shell, and laminate and seal the exposed edge of the positive / negative lead sheet and the other 2 edges in total. 3 edges. Next, the above-mentioned non-aqueous electrolyte is injected into the outer shell, and then the opening is sealed, thereby making 28 relative laminated batteries. The obtained battery was placed at room temperature for 1 day, and then charged at a constant current of 330 mA (0.3C) to a battery voltage of 4.2 V in an atmosphere of 25°C. After reaching the voltage, the battery was kept at 4.2 V and charged at a constant voltage. This method was used for the initial charge after the battery was made for a total of 8 hours. Then, the battery was discharged at a current value of 330 mA (0.3C) to a battery voltage of 3.0 V.
[0454] Evaluation of battery cycle stability 2
[0455] The battery obtained in the above "d. Battery assembly" was charged and discharged for 1000 cycles in an atmosphere of 25°C. Regarding charging, the battery voltage was charged to 4.2V at a constant current of 1A (1.0C), and after reaching 4.2V, constant voltage charging was performed. The battery was charged for a total of 3 hours using this method. Regarding discharging, the battery was discharged to a battery voltage of 3.0V at a current value of 1A (1.0C). The capacity retention rate was calculated from the discharge capacity of the 1000th cycle and the discharge capacity of the 1st cycle. When the capacity retention rate is high, it is evaluated as having good cycle characteristics.
[0456] Safety test 2 for battery destruction (battery destruction test 2)
[0457] The safety test is a test in which an iron nail is driven into a battery charged to 4.5V at a speed of 30mm / second to penetrate the battery to cause an internal short circuit. This test can clarify the phenomenon of internal short circuit by measuring the time change behavior of the battery voltage drop caused by the internal short circuit and the battery surface temperature rise caused by the internal short circuit. In addition, due to the insufficient closing function of the separator or the rupture of the membrane at low temperature during the internal short circuit, the battery sometimes releases heat rapidly, and the electrolyte sometimes catches fire, and the battery smokes and / or explodes.
[0458] (13) Determination of closing and rupture temperature 2
[0459] (Fusing / Melting (F / MD) Characteristics 2)
[0460] In Examples 28 to 41 and Comparative Examples 30 to 44, the F / MD characteristics were measured as follows.
[0461] The positive electrode, separator and negative electrode are cut into a circular shape with a diameter of 200 mm and stacked, and the electrolyte is added to the obtained stack to penetrate the whole. The stack is clamped in the center of a circular aluminum heater with a diameter of 600 mm, and the aluminum heater is pressurized to 0.5 MPa from the top and bottom with a hydraulic jack to complete the preparation for the measurement. While heating the stack with an aluminum heater at a heating rate of 2°C / min, the resistance (Ω) between the electrodes is measured. The temperature at which the separator melts and the resistance between the electrodes rises and the resistance exceeds 1000Ω for the first time is taken as the melting temperature (shutdown temperature). In addition, further heating is continued, and the temperature at which the resistance is reduced to less than 1000Ω is taken as the melting temperature (film rupture temperature). It should be noted that the measurement uses a wire for resistance measurement bonded to the back of the aluminum foil of the positive electrode made by the item "a. Preparation of positive electrode" of the above "(12)" with conductive silver paste. In addition, the measurement used a wire for resistance measurement bonded to the back of the copper foil of the negative electrode prepared in the item "b. Preparation of negative electrode" of the above "(12)" with a conductive silver paste. Furthermore, the electrolyte prepared in the item "c. Preparation of non-aqueous electrolyte" of the above "(12)" was also used in the F / MD characteristic test.
[0462] [Table 5-1]
[0463]
[0464] [Table 5-2]
[0465]
[0466] [Table 5-3]
[0467]
[0468] [Table 6-1]
[0469]
[0470] [Table 6-2]
[0471]
[0472] [Table 6-3]
[0473]
[0474] [Table 6-4]
[0475]
Claims
1. A separator for a power storage device, comprising a polyolefin resin microporous film and an inorganic porous layer disposed on at least one surface of the polyolefin resin microporous film, The inorganic porous layer has at least one selected from the group consisting of (i) covalent bonds between inorganic particles, (ii) covalent bonds between resin binders, and (iii) covalent bonds between inorganic particles and resin binders, The inorganic porous layer uses a crosslinking agent, the crosslinking agent has a nucleophilic substitution reactive functional group and / or an electrophilic addition reactive functional group, wherein the mass ratio of the crosslinking agent in the inorganic porous layer is in the range of 0.1 mass % to 5 mass %, The polyolefin resin microporous film includes a silane-grafted modified polyolefin, and a silane crosslinking reaction of the silane-grafted modified polyolefin is initiated when the power storage device separator comes into contact with an electrolyte solution.
2. The separator for a power storage device according to claim 1, in, The electrolyte is non-aqueous and contains a fluorine (F)-containing lithium salt.
3. The separator for a power storage device according to claim 1, in, The polyolefin resin microporous membrane contains a polyolefin other than the silane-graft-modified polyolefin.
4. The separator for an electric storage device according to claim 1, in, The inorganic porous layer includes a cross-linked structure.
5. A separator for a power storage device, comprising a polyolefin resin microporous film and an inorganic porous layer disposed on at least one surface of the polyolefin resin microporous film, The inorganic porous layer uses a crosslinking agent, the crosslinking agent has a nucleophilic substitution reactive functional group and / or an electrophilic addition reactive functional group, wherein the mass ratio of the crosslinking agent in the inorganic porous layer is in the range of 0.1 mass % to 5 mass %, In the solvent immersion test, the area of the inorganic porous layer peeled off from the polyolefin resin microporous membrane is 0 to 35% based on the area of the inorganic porous layer before the test.
6. The separator for an electric storage device according to claim 5, in, The area of the inorganic porous layer peeled off from the polyolefin resin microporous film is 0 to 8%.
7. The separator for a power storage device according to claim 5, in, The inorganic porous layer has at least one selected from the group consisting of (i) covalent bonds between inorganic particles, (ii) covalent bonds between resin binders, and (iii) covalent bonds between inorganic particles and resin binders.
8. The separator for a power storage device according to claim 7, in, The inorganic porous layer includes a cross-linked structure formed by at least one selected from the group consisting of the covalent bonds (i) to (iii).
9. The separator for a power storage device according to claim 5, in, The polyolefin resin microporous membrane includes a silane-graft-modified polyolefin.
10. The separator for a power storage device according to claim 9, in, When the separator for a power storage device comes into contact with an electrolyte, a silane cross-linking reaction of the silane-graft-modified polyolefin starts.
11. The separator for a power storage device according to claim 10, in, The electrolyte is non-aqueous and contains a fluorine (F)-containing lithium salt.
12. The separator for an electric storage device according to any one of claims 9 to 11, in, The polyolefin resin microporous membrane contains a polyolefin other than the silane-graft-modified polyolefin.
13. The separator for an electric storage device according to any one of claims 5 to 11, in, The surface roughness of a region of the polyolefin resin microporous membrane facing the inorganic porous layer is 0.2 to 3.0 μm.
14. The separator for a power storage device according to claim 4 or 8, in, In the inorganic porous layer, the cross-linked structure is formed by at least one selected from the group consisting of a nucleophilic substitution reaction, a nucleophilic addition reaction, an electrophilic addition reaction, and a silane coupling reaction.
15. The separator for an electric storage device according to any one of claims 1 to 4, 7 and 8, in, The resin binder is in the form of emulsion, suspension or colloid.
16. The separator for an electric storage device according to any one of claims 1 to 4, 7 and 8, in, The resin binder has a nucleophilic substitution reactive functional group or a nucleophilic addition reactive functional group.
17. The separator for an electric storage device according to any one of claims 1 to 4, 7 and 8, in, The nucleophilic substitution reactive functional group or the nucleophilic addition reactive functional group of the resin binder is at least one selected from the group consisting of a carboxyl group, a hydroxyl group, and an amino group.
18. The separator for an electric storage device according to any one of claims 1 to 11, in, The inorganic porous layer includes inorganic particles, and polar functional groups exist on the surfaces of the inorganic particles.
19. The separator for an electric storage device according to claim 18, in, The polar functional group is at least one selected from the group consisting of a carboxyl group, a hydroxyl group, and an amino group.
20. The separator for an electric storage device according to any one of claims 1 to 11, in, The inorganic porous layer includes inorganic particles, and silicon-containing functional groups exist on surfaces of the inorganic particles.
21. The separator for an electric storage device according to claim 20, in, The silicon-containing functional group is at least one selected from the group consisting of an alkoxysilyl group, a halogen-substituted silyl group, and a silazane group.
22. The separator for an electric storage device according to any one of claims 1 to 11, in, The cross-linking agent has a nucleophilic substitution reactive functional group and an electrophilic addition reactive functional group.
23. The separator for an electric storage device according to any one of claims 1 to 11, in, The nucleophilic substitution reactive functional group of the cross-linking agent is an oxazoline group and / or an epoxy group.
24. The separator for an electric storage device according to any one of claims 1 to 11, in, The electrophilic addition-reactive functional group of the cross-linking agent is at least one selected from the group consisting of an isocyanate group, a thioisocyanate group, a carbodiimide group, an allene group, an oxime group, and a carbonyl group.
25. The separator for an electric storage device according to any one of claims 1 to 11, in, The inorganic porous layer contains inorganic particles and a resin binder. Polar functional groups exist on the surface of the inorganic particles. The crosslinking agent exists between the polar functional groups and the resin binder, and a crosslinking structure is formed by covalent bonds between the polar functional groups, the crosslinking agent and the resin binder.
26. The separator for an electric storage device according to any one of claims 1 to 11, in, The cross-linking agent is in the form of emulsion, suspension or colloid.
27. The separator for an electric storage device according to any one of claims 1 to 11, in, The content of the polyolefin resin in the polyolefin resin microporous membrane is 75% by mass or more based on the total mass of the polyolefin resin microporous membrane.
28. The separator for an electric storage device according to any one of claims 1 to 11, in, The polyolefin resin microporous membrane contains a polyolefin having a weight average molecular weight of less than 1,200,000.
29. The separator for an electric storage device according to any one of claims 1 to 11, in, The porosity of the polyolefin resin microporous film is 20% or more and 90% or less.
30. The separator for an electric storage device according to any one of claims 1 to 11, in, The air permeability of the polyolefin resin microporous membrane is 1 second / 100 cm 3 Above and 400 seconds / 100cm 3 the following.
31. The separator for an electric storage device according to any one of claims 1 to 11, in, The air permeability increase of the separator for power storage device is 200 seconds / 100 cm 3 The following is the increase in air permeability obtained as follows: According to JIS P-8117:2009, the air permeability of the microporous membrane is measured using a GURLEY type air permeability meter with the trademark G-B2 manufactured by Toyo Seiki Co., Ltd., and the air permeability of the separator is measured by the same method. The air permeability of the separator is then subtracted from the air permeability of the microporous membrane, and the obtained value is used as the increase in air permeability.
32. The separator for an electric storage device according to any one of claims 1 to 11, in, The cross-linked structure is formed (i) during or immediately after the film forming process or (ii) after being housed in the power storage device, using the surrounding environment or chemical substances inside the power storage device.
33. The separator for an electric storage device according to any one of claims 1 to 11, in, The mass ratio of the resin binder in the inorganic porous layer is 0.5 mass % or more and 50 mass % or less. 34 . An electricity storage device comprising an electrode, an electrolyte, and the separator for an electricity storage device according to claim 1 . 35 . A secondary battery comprising an electrode, an electrolyte, and the separator for an electrical storage device according to claim 1 .