A method for preparing metallographic samples for inspecting inclusions on the surface of thin steel plates

Preparation of L-shaped samples by right-angle bending and grinding and polishing solves the randomness and missed detection of inclusions on the surface or subcutaneous inclusions, and realizes accurate positioning and efficient detection of inclusions.

CN114942166BActive Publication Date: 2024-11-29ANGANG STEEL CO LTD +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202210322868.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-03-30
Publication Date
2024-11-29
Estimated Expiration
2042-03-30

AI Technical Summary

Technical Problem

The prior art is difficult to accurately detect and locate the surface of extremely thin steel plates or subcutaneous non-metallic inclusions, and conventional sampling methods have problems such as high randomness and serious missed detection.

Method used

The thin steel plate is bent into an L-shaped sample by right angle bending method and prepared by mechanical polishing and polishing to ensure that the inclusions are located on the outer bottom surface of the right angle bottom edge of the sample, and metallographic microscopy is observed to locate the inclusions.

Benefits of technology

Effectively display surface or subcutaneous non-metallic inclusions, reduce sampling randomness, avoid inclusion shedding and missing inspection, and is simple and suitable for surface inspection of extremely thin steel plates or steel strips.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114942166B_ABST
    Figure CN114942166B_ABST
Patent Text Reader

Abstract

This invention relates to the field of material testing in metallurgical analysis, and more particularly to a method for preparing metallographic specimens for inspecting inclusions on the surface of thin steel plates. The method includes the following steps: 1) Cutting a plate-shaped specimen of the thin steel plate to detect macroscopic inclusion defects; 2) Bending the plate-shaped sample into a right-angled L-shaped metallographic specimen: With the surface containing the inclusion facing down, along the longitudinal direction of the plate-shaped sample, take 1 / 3 of the length from the end furthest from the inclusion, and mechanically bend the plate-shaped sample laterally to approximately a 90-degree angle to form an L-shaped metallographic specimen; ensuring that the inclusion area is located on the outer bottom surface of the right-angled base of the L-shaped metallographic specimen; 3) Grinding and polishing the L-shaped specimen; 4) Metallographic microscopic observation and inspection. This invention can grind and polish the Z-axis surface of the steel plate, thereby effectively displaying surface or subcutaneous non-metallic inclusions. It can accurately locate inclusion defects on the surface of thin steel plates, solving the problems of high randomness in traditional inclusion sampling and missed detection of serious inclusion areas.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to material inspection in the field of metallurgical analysis, and in particular to a method for preparing a metallographic sample for inspecting inclusions on the surface of a thin steel plate. Background Art

[0002] The surface inclusion defect of low-carbon cold-rolled steel plate is one of the more common surface quality defects of ultra-thin steel plates; it is a type of steel plate defect that is more harmful, especially for some cold-rolled thin plate products with high surface quality requirements such as automotive steel. The presence of surface inclusions greatly affects the surface quality of the product and has a serious impact on the deep processing and production of subsequent products. The inclusions on the surface of ultra-thin steel plates are generally caused by the more serious strip-shaped or large particle inclusions inside the hot-rolled plate after multiple hot rolling and cold rolling, which gradually approach or are exposed to the surface as the steel plate widens, stretches, deforms, breaks, stretches, and thins.

[0003] The presence of inclusions destroys the continuity of the steel matrix and reduces the plasticity, toughness and fatigue properties of the steel. Currently, there are two methods for testing non-metallic inclusions in steel: macroscopic testing and microscopic testing. Macroscopic testing methods include corrosion, fracture, step and magnetic methods, which can detect large particle inclusions on large area samples, but are not suitable for detecting inclusions less than 0.4 mm. The type of inclusions cannot be distinguished.

[0004] The microscopic inspection method is to take a longitudinal metallographic sample of the steel plate, grind and polish it, and then measure the size, distribution, quantity and type of inclusions on the test surface under an optical microscope. Since the sample is a longitudinal section of the steel plate, the sample size is generally 20mm×20mm, and a limited number of fields of view are used to evaluate the longitudinal section inclusions. For the case where the thickness is thin and the inclusions have been exposed to the surface of the steel plate, this conventional sampling and sample preparation method is bound to have a certain degree of contingency. On the one hand, the inclusions on the surface of the steel plate are located at the edge of the test surface in the longitudinal section. When preparing the sample, the inclusions are easily ground off or fall off; on the other hand, due to the limitation of the sample section, it is difficult for the inspector to accurately obtain the actual size, distribution, quantity and other information of the inclusions on the steel plate.

[0005] Therefore, it is necessary to target the characteristics of strip-like exposure on the surface of thin steel plates (often accompanied by subcutaneous inclusions) and, during microscopic inspection, start with sample preparation and select a sample surface that directly captures the exposed inclusion position for inspection and analysis. However, due to the thinness of the steel plate, conventional sample grinding and polishing preparation methods are not feasible and it is difficult to obtain microscopic observation results. Summary of the invention

[0006] In order to overcome the shortcomings of the prior art, the present invention provides a method for preparing metallographic samples for inspecting surface inclusions of thin steel plates, which can effectively display surface or subcutaneous non-metallic inclusions, accurately locate surface inclusion defects of thin steel plates, and solve the problems of large randomness of traditional inclusion sampling and missed detection of seriously included areas.

[0007] In order to achieve the above object, the present invention adopts the following technical solutions:

[0008] A method for preparing a metallographic sample for inspecting inclusions on the surface of a thin steel plate, wherein the thickness of the thin steel plate is less than 3 mm, specifically comprising the following steps:

[0009] 1) Cutting the thin steel plate macroscopic inclusion defect plate specimen:

[0010] Chamfer the edges of the plate specimen. For thin steel plate samples with exposed inclusion defects on the surface that need metallographic inspection, first select the area where macroscopic inclusions are distributed, take a rectangular plate specimen with a length of 30 to 70 mm and a width of 10 to 30 mm along the extension line of the inclusion distribution, and make the most serious inclusion position on the plate specimen tend to the 1 / 2-2 / 3 length range in the length direction.

[0011] 2) Bend the plate sample into a right-angle L-shaped metallographic sample:

[0012] With the surface where the inclusions are located facing downward, take 1 / 3 of the length along the longitudinal direction of the plate sample at the end away from the inclusions, and fold the plate sample horizontally to approximately 90 degrees using a mechanical bending method to make an L-shaped metallographic sample; ensure that the inclusion area is located on the outer bottom surface of the right-angle bottom edge of the L-shaped metallographic sample.

[0013] 3) Grinding and polishing preparation operation of L-type samples:

[0014] ① Use the mechanical polishing method, first use water sandpaper to coarsely grind the sample on the metallographic pre-grinder; hold the right-angled vertical edge of the L-shaped sample, press the outside of the palm to the bottom surface where the inclusions exist, and apply uniform and moderate pressure to the bottom surface, so that the bottom surface where the inclusions exist is in contact with the rotating sandpaper grinding disc of the pre-grinder as a whole, select sandpaper from coarse to fine, add water and grind until the finest sandpaper is polished.

[0015] ② Mechanically polish the sample. Place the sandpaper-polished sample surface on a mechanical polisher for polishing. Hold the plate-shaped sample L by the right-angled vertical edge and use the outside of your palm to evenly press the bottom surface of the inclusions and polish it on the polishing disc.

[0016] During this process, the hand gesture of holding the sample at a right angle should follow the rotation of the polishing disk to bring the ground surface into even contact with the polishing disk, and at the same time make slight reciprocating movements in the normal direction of the rotation of the polishing disk.

[0017] Replenish abrasive or add water for lubrication at any time. The ideal lubrication state is that the water film on the surface evaporates within 1s to 5s after the grinding surface leaves the throwing disc.

[0018] After polishing, the scratches left by the finest sandpaper are evenly removed, and the surface of the sample reaches a smooth mirror state.

[0019] 4) Metallographic microscopic observation and inspection:

[0020] Place the prepared smooth and bright test surface on the stage of an inverted optical metallographic microscope, press the test surface with a pressure clamp, and then observe the morphology and distribution of more serious inclusions on the test surface; locate the position of the inclusions.

[0021] Compared with the existing method, the present invention has the following beneficial effects:

[0022] The present invention adopts a right-angle bending method to take an L-shaped sample, grinds and polishes the Z-direction surface of the steel plate, and then effectively displays the surface or subcutaneous non-metallic inclusions. It can accurately locate the surface inclusion defects of the thin steel plate, and solve the problem of large randomness of traditional inclusion sampling and missed detection of serious inclusion areas.

[0023] 1) It can directly find the location of inclusions in a large range and determine the properties, form and distribution of representative inclusions. This greatly reduces the randomness of conventional inclusion inspection methods.

[0024] 2) It can realize direct grinding, observation and analysis of the surface of extremely thin steel plates or steel strips, avoiding the phenomenon of missing detection due to the edge effect when longitudinal sampling caused by the steel plate being too thin, which causes the inclusions to fall off.

[0025] 3) The sample preparation method is simple and convenient for grinding and polishing operations. As long as the pressure is properly controlled, an ideal inclusion inspection test surface can be obtained. In particular, it provides a feasible solution for the inspection of inclusions on the surface of extremely thin steel strips that are not suitable for inlaying. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 It is the microscopic morphology of inclusions in the transverse section of the steel plate;

[0027] Figure 2 This is a microscopic morphology of inclusions on the Z-direction surface of the steel plate in Example 1;

[0028] Figure 3 This is a microscopic morphology of inclusions on the Z-direction surface of the steel plate in Example 2. DETAILED DESCRIPTION

[0029] The present invention discloses a method for preparing a metallographic sample for inspecting inclusions on the surface of a thin steel plate. A person skilled in the art can refer to the content of this article and appropriately improve the process parameters to achieve the same. It should be particularly noted that all similar substitutions and modifications are obvious to a person skilled in the art and are considered to be included in the present invention. The method and application of the present invention have been described through preferred embodiments, and relevant personnel can obviously modify or appropriately change and combine the method and application described herein without departing from the content, spirit and scope of the present invention to implement and apply the technology of the present invention.

[0030] A method for preparing a metallographic sample for inspecting surface inclusions on a thin steel plate comprises the following steps:

[0031] 1. Cutting thin plate inclusion defect specimens:

[0032] For thin steel plate samples with exposed inclusion defects on the surface that need to be metallographically inspected, first select the area where the macroscopic inclusions are distributed, and take a rectangular plate specimen with a length of 30 to 70 mm and a width of 10 to 30 mm along the extension line of the inclusion distribution. On the plate specimen, try to make the severe inclusion position tend to the 1 / 2-2 / 3 length range in the length direction.

[0033] 2. Bend the plate sample into a right-angle L-shaped metallographic sample:

[0034] Chamfer the edges of the plate sample to avoid scratches during subsequent sample preparation. Then, place the surface with inclusions downward, take 1 / 3 of the length from the end away from the inclusions along the longitudinal direction of the plate sample, and fold the plate sample horizontally to approximately 90 degrees using a mechanical bending method. Make an L-shaped metallographic sample. Make sure that the inclusion area is located on the outer bottom surface of the right-angle bottom edge of the L-shaped metallographic sample.

[0035] 3. Grinding and polishing preparation operation of L-type samples:

[0036] (1) Use mechanical polishing method, first use water sandpaper to coarsely grind the sample on a metallographic pre-grinder: hold the right-angled vertical edge of the L-shaped sample, press the outside of the palm onto the bottom surface where the inclusions are located, and apply uniform and moderate pressure to the bottom surface so that the bottom surface where the inclusions are located is in contact with the rotating sandpaper grinding disc of the pre-grinder. Select sandpaper from coarse to fine and add water to grind until the finest sandpaper is polished.

[0037] (2) Mechanical polishing of the sample: Place the sandpaper-polished sample surface on a mechanical polisher for polishing. Similarly, hold the plate-shaped sample L at a right angle and use the outside of your palm to evenly press the bottom surface of the inclusion on the polishing disc. During this process, the hand gesture of holding the sample at a right angle should follow the rotation of the polishing disc to evenly contact the grinding surface with the polishing disc, and at the same time, move back and forth slightly in the normal direction of the rotation of the polishing disc. Replenish abrasives or add water for lubrication at any time to prevent the grinding surface from being damaged. The ideal lubrication state is that the water film on the surface evaporates within 1s-5s after the grinding surface leaves the polishing disc. After polishing, the scratches left by the finest sandpaper are evenly polished away, and the sample surface reaches a smooth mirror state.

[0038] 4. Metallographic microscopic observation and inspection:

[0039] Place the prepared smooth and bright test surface on the stage of an inverted optical metallographic microscope, press the test surface with a pressure clip, and observe the morphology and distribution of the more serious inclusions on the test surface. Locate the position of the inclusions for further qualitative and quantitative analysis.

[0040] Embodiment 1:

[0041] A 0.9 mm thick cold-rolled annealed steel strip with the chemical composition of C 0.11 wt%, Si 0.014 wt%, Mn 0.45 wt%, P 0.0021 wt%, S 0.0031 wt% and the remainder being Fe, and an inspection method for inclusion defects existing on the surface and under the surface of a thin steel plate.

[0042] Conventional longitudinal section metallographic samples cannot accurately capture the location of inclusions, and the detection is accidental. Transverse section samples can only observe part of the sample, and the overall distribution of inclusions cannot be seen. Figure 1 .

[0043] The preparation method of the metallographic sample for inspecting the surface inclusions of the thin steel plate specifically comprises the following steps:

[0044] 1. Cutting plate specimens with surface inclusion defects:

[0045] Select a representative position from the steel strip with macroscopically visible strip-shaped inclusion defects on the surface, and take a 60mm long and 30mm wide rectangular plate specimen along the extension line of the inclusion distribution. On the plate specimen, try to make the severe inclusion position tend to the 1 / 2-2 / 3 length range of the 60mm length direction.

[0046] 2. Bend the plate sample into an L-shaped right-angle metallographic sample:

[0047] First, chamfer the four corners of the plate sample to avoid scratches during subsequent sample preparation. Then turn the surface where the inclusions exist downward, take 1 / 3 of the length from the end away from the inclusions along the longitudinal direction of the plate sample, and fold the plate sample horizontally by mechanical bending to an angle of approximately 90 degrees. Make an L-shaped metallographic sample. Make sure that the inclusion area is located on the outer bottom surface of the right-angle bottom edge of the L-shaped metallographic sample.

[0048] 3. Preparation of L-shaped right-angle metallographic samples:

[0049] (1) Grind the test surface on a metallographic sample pre-grinding machine: Hold the vertical edge of the right-angle plate-shaped sample, and make the bottom surface with inclusions contact the rotating water sandpaper grinding disc as a whole. Apply uniform and moderate pressure to the bottom surface and grind it with water. After grinding with sandpaper from coarse to fine, an initial smooth test surface is obtained.

[0050] (2) Place the sample surface with fine scratches that has been ground with sandpaper on a metallographic sample polishing machine and polish it in the same way as the polishing preparation: hold the vertical edge of the right-angle plate sample, and make the bottom surface with inclusions contact the rotating polishing disk as a whole, and apply uniform and moderate pressure to the bottom surface for polishing. At the same time, move the sample along the normal direction of the rotating disk, so that the sample surface moves relative to the rotating disk under a certain pressure, remove the scratches on the sample surface, and make the polished surface reach a smooth and flawless mirror surface.

[0051] 4. Microscopic observation to locate inclusions:

[0052] Place the prepared sample surface on the stage of an inverted optical microscope, press the right-angle bottom edge with a pressure clip, and observe the morphology of inclusions on the sample to locate the morphology and distribution of typical inclusions at the most serious location. Carry out qualitative and quantitative analysis of inclusions, see Figure 2 .

[0053] Embodiment 2:

[0054] Used for inspection of surface warping and crack defects of 1.4mm thick low carbon steel cold rolled thin plate containing C 0.03wt%, Si 0.02wt%, Mn 0.20wt%, P 0.01wt%, S 0.008wt%, Al 0.03% and balance Fe.

[0055] The preparation method of the metallographic sample for inspecting the surface inclusions of the thin steel plate specifically comprises the following steps:

[0056] 1. Cut the plate specimen with inclusion defects on the macro surface:

[0057] Select a representative area at the warping position on the steel plate surface, take a 60mm long and 30mm wide rectangular plate specimen along the extension line of the inclusion distribution, and try to make the severe inclusion position on the plate specimen tend to the 1 / 2-2 / 3 length range of the 60mm length direction.

[0058] 2. Bend the plate sample into an L-shaped right-angle metallographic sample:

[0059] First, chamfer the four corners of the plate sample to avoid scratches during subsequent sample preparation. Then turn the surface where the inclusions exist downward, take 1 / 3 of the length from the end away from the inclusions along the longitudinal direction of the plate sample, and fold the plate sample horizontally by mechanical bending to an angle of approximately 90 degrees. Make an L-shaped metallographic sample. Make sure that the inclusion area is located on the outer bottom surface of the right-angle bottom edge of the L-shaped metallographic sample.

[0060] 3. Preparation of L-shaped right-angle metallographic samples:

[0061] (1) Grind the test surface on a metallographic sample pre-grinding machine: Hold the vertical edge of the right-angle plate-shaped sample, and make the bottom surface with inclusions contact the rotating water sandpaper grinding disc as a whole. Apply uniform and moderate pressure to the bottom surface and grind it with water. After grinding with sandpaper from coarse to fine, an initial smooth test surface is obtained.

[0062] (2) Place the sample surface with fine scratches after sandpaper grinding on a metallographic sample polishing machine and polish it in the same way as the polishing preparation: hold the vertical edge of the right-angle plate sample, and make the bottom surface with inclusions contact the rotating polishing disk as a whole, and apply uniform and moderate pressure to the bottom surface for polishing. At the same time, move the sample back and forth along the normal direction of the rotating disk, so that the sample grinding surface moves relative to the rotating disk under a certain pressure, remove the scratches on the sample surface, and make the polished surface reach a smooth and flawless mirror surface.

[0063] 4. Microscopic observation to locate inclusions:

[0064] Place the prepared sample surface on the stage of an inverted optical microscope, press the right-angle bottom edge with a pressure clip, and observe the morphology of inclusions on the sample to locate the morphology and distribution of typical inclusions at the most serious location. Carry out qualitative and quantitative analysis of inclusions, see Figure 3 .

[0065] The present invention adopts a right-angle bending method to take an L-shaped sample, grinds and polishes the Z-direction surface of the steel plate, and then effectively displays the surface or subcutaneous non-metallic inclusions. The surface inclusion defects of thin steel plates can be accurately located, solving the problem that the traditional inclusion sampling is highly random and misses the serious inclusion area. The location of the inclusion can be directly found within a large range, and the nature, morphology, and distribution state of the representative inclusion can be determined. The randomness of the conventional inclusion inspection method is greatly reduced. The surface of extremely thin steel plates or steel strips can be directly ground, observed and analyzed, avoiding the phenomenon of inclusions falling off and missing detection due to the edge effect when longitudinal sampling due to the excessive thinness of the steel plate. The sample preparation method is simple and convenient for grinding and polishing operations. As long as the pressure is properly controlled, an ideal inclusion inspection test surface can be obtained. In particular, it provides a feasible solution for the surface inclusion inspection of extremely thin steel strips that are not suitable for inlay.

[0066] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A method for preparing a metallographic sample for inspecting inclusions on the surface of a thin steel plate, wherein the thickness of the thin steel plate is less than 3 mm, characterized in that: The specific steps include: 1) Cutting thin steel plate macroscopic inclusion defect plate specimen: For thin steel plate samples with surface exposed inclusion defects that need metallographic inspection, first select the area where the macroscopic inclusions are distributed, take a rectangular plate sample with a length of 30~70mm and a width of 10~30mm along the extension line of the inclusion distribution, and make the most serious inclusion position on the plate sample tend to the 1 / 2-2 / 3 length range in the length direction; 2) Bend the plate sample into a right-angle L-shaped metallographic sample: With the surface where the inclusions are located facing downward, take 1 / 3 of the length from the end away from the inclusions along the longitudinal direction of the plate-shaped sample, and fold the plate-shaped sample horizontally to approximately 90 degrees using a mechanical bending method to make an L-shaped metallographic sample; ensure that the inclusion area is located on the outer bottom surface of the right-angle bottom edge of the L-shaped metallographic sample; 3) Grinding and polishing preparation operation of L-type samples: ① Use mechanical polishing method, first use water sandpaper to coarsely grind the sample on the metallographic pre-grinding machine; Hold the right-angled vertical edge of the L-shaped sample, press the outer side of your palm onto the bottom surface where the inclusions are located, apply even and moderate pressure to the bottom surface, so that the bottom surface where the inclusions are located is in contact with the rotating sandpaper grinding disc of the pre-grinder as a whole, and grind with sandpaper from coarse to fine, adding water, until the finest sandpaper is polished; ② Mechanically polish the sample, place the sandpaper-polished sample surface on a mechanical polisher for polishing; Hold the plate-shaped sample L by its right-angled vertical edge and apply uniform pressure to the bottom surface of the inclusion with the outside of the palm to polish it on the polishing disc; During this process, the hand gesture of holding the sample at a right angle should follow the rotation of the polishing disk to evenly contact the grinding surface with the polishing disk, and at the same time, slightly reciprocate in the normal direction of the polishing disk's rotation; Replenish abrasives or add water for lubrication at any time. The ideal lubrication state is that the water film on the surface evaporates within 1s to 5s after the grinding surface leaves the throwing disc. After polishing, the scratches left by the finest sandpaper are evenly removed, and the surface of the sample reaches a smooth mirror state; 4) Metallographic microscopic observation and inspection: Place the prepared smooth and bright test surface on the stage of an inverted optical metallographic microscope, press the test surface with a pressure clamp, and then observe the morphology and distribution of more serious inclusions on the test surface; locate the position of the inclusions.

2. A method for preparing a metallographic sample for inspecting inclusions on the surface of a thin steel plate according to claim 1, characterized in that: In the step 2), the four sides of the plate-shaped sample are chamfered.

Citation Information

Patent Citations

  • Method for measuring ultratrace calcium content of cold and hot rolled sheets

    CN101995401A

  • Metallographic test sample preparation method

    CN107941582A