Acrylic resin powder, resin composition, hot melt adhesive composition containing acrylic resin powder, and method for producing the same
Through the combination of multi-stage polymer and polyalkylene glycol, the problems of insufficient bonding strength and short drying time of reactive hot melt adhesive are solved, and hot melt adhesive with high initial strength and long drying time are achieved The adhesive enhances process operability and product performance.
Patent Information
- Application Number
- CN202180010511.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-03-25
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2041-03-25
AI Technical Summary
The existing reactive hot melt adhesives have insufficient bonding strength in the initial stage and have short drying time, making it difficult to take into account both high initial stage strength and long drying time.
Acrylic resin powder composed of multi-stage polymers, by synthesizing a multi-stage polymer containing alkyl methacrylate and methyl methacrylate, adjusting the glass transition temperature and mass average molecular weight, combining polyalkylene glycol and isocyanate, A suitable resin composition is formed to improve initial bonding strength and drying time.
The high initial bonding strength and long drying time of hot melt adhesive are achieved, and the operability of the process and product performance are improved.
Smart Images

Figure BDA0003759424910000081 
Figure BDA0003759424910000091 
Figure BDA0003759424910000301
Abstract
Description
Technical Field
[0001] The present invention relates to an acrylic resin powder, a resin composition, a hot melt adhesive composition containing the acrylic resin powder and a method for producing the same.
[0002] This application claims priority based on Japanese Patent Application No. 2020-061289 filed in Japan on March 30, 2020, the contents of which are incorporated herein by reference. Background Art
[0003] Hot melt adhesives are solid or semi-solid adhesives at room temperature that melt and become fluid when heated. In particular, hot melt adhesives containing polyurethane prepolymers having isocyanate groups at the ends as the main component are called reactive hot melt adhesives, of which moisture-curable polyurethane adhesives are the most common, and are generally products in the form of polyurethane prepolymers containing isocyanate groups obtained by polycondensing a polyol component and an isocyanate component.
[0004] These reactive hot melt adhesives are applied to a substrate in a heated and molten state, and after being cooled and solidified, moisture curing occurs due to a chemical crosslinking reaction between isocyanate groups and water, forming a tough film (adhesive layer) that is resistant to heat and chemicals.
[0005] Existing reactive hot melt adhesives show excellent adhesion when chemical crosslinking is formed by moisture curing. However, reactive hot melt adhesives will not produce chemical crosslinking at that time just after being coated. In addition, since the adhesive temperature just after heating and melting is also high, there is the characteristic fluidity of thermoplastic polymers, so the initial bonding strength to the substrate is insufficient. It is explained that the initial bonding strength refers to the bonding strength before moisture curing after being coated on the substrate. As a method for improving the initial bonding strength, it is known to have a method of allocating thermoplastic resins in hot melt adhesives to improve the initial bonding force. In addition, it is known that if thermoplastic resins are allocated in order to improve the initial strength, the air-drying time becomes shorter. It is explained that the air-drying time refers to the usable time after being coated on the substrate until the adhesive is cooled and solidified.
[0006] Patent Document 1 discloses a polyurethane hot melt adhesive composition using an acrylic resin powder having high solubility in polyalkylene glycol. Furthermore, Patent Document 2 discloses a polyurethane hot melt adhesive composition having a long open time by using an acrylic resin powder containing an acrylic polymer having a low glass transition temperature. However, in the market, in order to shorten the process, it is desired to develop an acrylic resin for polyurethane hot melt adhesive that can achieve both high initial strength and long open time.
[0007] Prior art literature
[0008] Patent Literature
[0009] Patent Document 1: International Publication No. 2018 / 012234
[0010] Patent Document 2: International Publication No. 2019 / 188930 Summary of the invention
[0011] Problems to be solved by the invention
[0012] The present invention is made to solve such problems. That is, an object of the present invention is to provide an acrylic resin powder suitable for a hot-melt adhesive that exhibits higher initial adhesive strength than conventional ones and has a long open time.
[0013] Technical solutions to the problem
[0014] The present invention includes any one of the following aspects [1] to
[33] :
[0015] [1] An acrylic resin powder comprising a multistage polymer (G), wherein the multistage polymer (G) is a multistage polymer of a polymer (A) and a polymer (B), wherein the polymer (A) comprises a monomer unit of an alkyl (meth)acrylate (ma), and the polymer (B) comprises a monomer unit of each of methyl methacrylate and an alkyl (meth)acrylate (mb),
[0016] The multi-stage polymer (G) has a glass transition temperature of 50° C. or higher,
[0017] The softening temperature of the acrylic resin powder measured by a flow tester temperature rising method is 150° C. to 200° C.
[0018] [2] The acrylic resin powder according to [1], wherein the alkyl group in the (meth)acrylic acid alkyl ester (ma) has 4 to 8 carbon atoms, and the alkyl group in the methyl methacrylate and the (meth)acrylic acid alkyl ester (mb) has 4 to 8 carbon atoms.
[0019] [3] An acrylic resin powder comprising a multistage polymer (G) obtained by polymerizing a monomer mixture (b) comprising methyl methacrylate and an alkyl (meth)acrylate (mb) in the presence of a dispersion comprising a polymer (A), wherein the polymer (A) is obtained by polymerizing a monomer mixture (a) comprising an alkyl (meth)acrylate (ma),
[0020] The carbon number of the alkyl group in the (meth)acrylic acid alkyl ester (ma) is 4 to 8,
[0021] The carbon number of the alkyl group in the (meth)acrylic acid alkyl ester (mb) is 4 to 8,
[0022] The multi-stage polymer (G) has a glass transition temperature of 50° C. or higher,
[0023] The mass average molecular weight of the multistage polymer (G) is 10,000 or more and 300,000 or less,
[0024] The softening temperature of the acrylic resin powder measured by the flow tester temperature rising method is 150°C to 200°C.
[0025] The acrylic resin powder is soluble in acetone.
[0026] [4] The acrylic resin powder according to any one of [1] to [3], wherein the volume average particle size of the primary particles of the acrylic resin powder is 0.1 to 10 μm.
[0027] [5] The acrylic resin powder according to any one of [1] to [4], wherein the volume average particle size of secondary particles of the acrylic resin powder is 20 to 100 μm.
[0028] [6] The acrylic resin powder according to [3], wherein the monomer mixture (a) further comprises other copolymerizable monomers,
[0029] In the monomer mixture (a), the content of methyl methacrylate is 0 to 60% by mass, the content of the alkyl (meth)acrylate (ma) is 40 to 100% by mass, and the content of the other copolymerizable monomer is 0 to 10% by mass, based on the total mass of the monomer mixture (a).
[0030] [7] The acrylic resin powder according to any one of [1] to [6], wherein the solubility parameter (SPA) of the polymer (A) is 19.50 (J / cm 3 ) 1 / 2 Above and 20.1(J / cm 3 ) 1 / 2 the following.
[0031] [8] The acrylic resin powder according to [3], wherein the monomer mixture (b) further comprises other copolymerizable monomers,
[0032] In the monomer mixture (b), the content of methyl methacrylate is 50 to 90 mass %, the content of alkyl (meth)acrylate (mb) is 10 to 50 mass %, and the content of the other copolymerizable monomer is 0 to 10 mass % based on the total mass of the monomer mixture (b).
[0033] [9] The acrylic resin powder according to any one of [1] to [8], wherein the content of the monomer units derived from the polymer (A) is 10 to 80% by mass relative to the total mass of the monomer units constituting the multi-stage polymer (G).
[0034]
[10] The acrylic resin powder according to any one of [1] to [9], wherein the glass transition temperature of the multi-stage polymer (G) is preferably 50 to 85°C, more preferably 58 to 80°C, and even more preferably 65 to 75°C.
[0035]
[11] The acrylic resin powder according to any one of [1] to
[10] , wherein the glass transition temperature of the polymer (B) is preferably 55 to 100°C, more preferably 65 to 95°C, and even more preferably 70 to 97°C.
[0036]
[12] The acrylic resin powder according to any one of [1] to
[11] , wherein the solubility parameter (SPA) of the polymer (A) is preferably 19.50 (J / cm 3 ) 1 / 2 Above and 20.1(J / cm 3 ) 1 / 2 Below, more preferably 19.50 (J / cm 3 ) 1 / 2 Above and 20.0(J / cm 3 ) 1 / 2 Below, more preferably 19.60 (J / cm 3 ) 1 / 2 Above and 20.0(J / cm 3 ) 1 / 2 the following.
[0037]
[13] The acrylic resin powder according to any one of [1] to
[12] , wherein the softening temperature of the multi-stage polymer (G) is preferably 150°C to 200°C, more preferably 155°C to 190°C, and even more preferably 155°C to 185°C.
[0038]
[14] The acrylic resin powder according to any one of [1] to
[13] , wherein the acetone-insoluble component is 1% by mass or less when the acetone solubility is evaluated by the method described in the present specification.
[0039]
[15] The acrylic resin powder according to any one of [1] to
[14] , wherein the content of the (meth)acrylic acid alkyl ester (ma) in the monomer mixture (a) is preferably 40 to 100% by mass, more preferably 45 to 100% by mass, and even more preferably 50 to 100% by mass, relative to the total mass of the monomer mixture (a).
[0040]
[16] The acrylic resin powder according to any one of [3] to
[15] , wherein the content of methyl methacrylate in the monomer mixture (b) is preferably 50 to 90% by mass, more preferably 55 to 90% by mass, and even more preferably 65 to 90% by mass, relative to the total mass of the monomer mixture (b).
[0041]
[17] The acrylic resin powder according to any one of [3] to
[16] , wherein the content of the (meth)acrylic acid alkyl ester (mb) in the monomer mixture (b) is preferably 10 to 50% by mass, more preferably 10 to 45% by mass, and even more preferably 10 to 35% by mass, relative to the total mass of the monomer mixture (b).
[0042]
[18] The acrylic resin powder according to any one of [1] to
[17] , wherein the content of the monomer units derived from the polymer (A) is preferably 10 to 80% by mass, and more preferably 20 to 70% by mass, when the monomer units constituting the multi-stage polymer (G) are taken as 100% by mass.
[0043]
[19] The acrylic resin powder according to any one of [1] to
[18] , wherein the volume average particle size of the primary particles is preferably 0.1 to 10 μm, more preferably 0.1 to 5 μm, and even more preferably 0.1 to 2 μm.
[0044]
[20] The acrylic resin powder according to any one of [1] to
[19] , wherein the volume average particle size of the secondary particles of the acrylic resin powder is preferably 20 to 100 μm, more preferably 20 to 80 μm.
[0045]
[21] The acrylic resin powder according to any one of [1] to
[21] , wherein the acrylic resin powder is dissolved in polyalkylene glycol to form a resin composition, and when a hot melt adhesive containing the resin composition is prepared, the initial bonding strength x (kPa) and the open time y (minutes) measured under the following conditions preferably satisfy the following relations (3) and (4):
[0046] y>-0.325x+124···(Formula (3))
[0047] y>10····(Formula (4)),
[0048] The initial adhesive strength x is preferably 200 kPa or more, more preferably 300 kPa or more, and even more preferably 400 kPa or more.
[0049] In formula (3), preferably y>-0.325x+130, more preferably y>-0.325x+140, further preferably y>-0.325x+150,
[0050] In formula (4), 60>y>10 is preferred, 40>y>10 is more preferred, and 20>y>10 is further preferred.
[0051]
[22] A resin composition obtained by dissolving the acrylic resin powder according to any one of [1] to
[21] in polyalkylene glycol.
[0052]
[23] The resin composition according to
[22] , wherein the number average molecular weight of the polyalkylene glycol is 200 to 5,000.
[0053]
[24] The resin composition according to
[22] or
[23] , further comprising a polyester polyol.
[0054]
[25] The resin composition according to any one of
[22] to
[24] , further comprising an isocyanate.
[0055]
[26] A hot-melt adhesive comprising the resin composition according to any one of
[22] to
[25] .
[0056]
[27] A hot melt adhesive, which is a hot melt adhesive formed from a resin composition comprising acrylic resin powder, polyalkylene glycol, polyester polyol and isocyanate, wherein the initial bonding strength x (kPa) measured under the following conditions and the open time y (minutes) measured under the following conditions satisfy the following relations (3) and (4):
[0057] y>-0.325x+124···(Formula (3))
[0058] y>10···(Formula (4)),
[0059] (Initial bonding strength x)
[0060] Prepare two wooden flat bars with a width of 1.7 cm, a length of 7.5 cm, and a thickness of 1.5 mm. On one of the wooden bars, apply hot-melt adhesive heated to melt at 120°C on an area of 1.5 cm × 1.7 cm. Overlap the other wooden flat bar and clamp it with a binder clip. Let it stand for 5 minutes to allow the hot-melt adhesive to cool and solidify. After standing, remove the binder clip and conduct a tensile shear test using the following tensile testing machine and measuring conditions to measure the initial bonding strength x.
[0061] Tensile testing machine: Precision universal testing machine (Product name: AGS-X, manufactured by Shimadzu Corporation)
[0062] Measurement conditions: tensile speed 5.0 mm / min
[0063] The distance between the fixtures is 50mm.
[0064] (Opening time y)
[0065] Apply heated and melted hot-melt adhesive on a dried wooden flat strip with a width of 1.7 cm, a length of 7.5 cm and a thickness of 1.5 mm, and heat it to 120°C in a Gir thermal aging oven; then, at room temperature, repeatedly press and stick kraft paper sheets with fingers and quickly peel off the kraft paper sheets every 1 minute; the time from the time the hot-melt adhesive is applied to the flat strip until no paper fibers remain on the adhesive surface when the kraft paper sheets are peeled off is taken as the air-drying time y.
[0066]
[28] A method for producing acrylic resin powder, comprising:
[0067] Step (I): adding dropwise to a dispersion (A1) containing a polymer (A) obtained by polymerizing a monomer mixture (a) containing methyl methacrylate and an alkyl (meth)acrylate (mb) and 0.1 to 3 parts by mass of a chain transfer agent based on 100 parts by mass of the monomer mixture (b), thereby obtaining a dispersion (G1) containing a multistage polymer (G); and
[0068] Step (II): spray drying the dispersion (G1) of the multi-stage polymer (G) to obtain an acrylic resin powder,
[0069] The carbon number of the alkyl group in the (meth)acrylic acid alkyl ester (ma) is 4 to 8,
[0070] The carbon number of the alkyl group in the (meth)acrylic acid alkyl ester (mb) is 4 to 8,
[0071] The softening temperature of the acrylic resin powder measured by a flow tester temperature rising method is 150° C. to 200° C.
[0072]
[29] The method for producing acrylic resin powder according to
[28] , wherein the monomer mixture (a) further comprises other copolymerizable monomers,
[0073] In the monomer mixture (a), the content of methyl methacrylate is 0 to 60% by mass, the content of the alkyl (meth)acrylate (ma) is 40 to 100% by mass, and the content of the other copolymerizable monomer is 0 to 10% by mass, based on the total mass of the monomer mixture (a).
[0074]
[30] The method for producing acrylic resin powder according to
[28] or
[29] , wherein the monomer mixture (b) further comprises other copolymerizable monomers,
[0075] In the monomer mixture (b), the content of methyl methacrylate is 50-90 mass %, the content of alkyl (meth)acrylate (mb) is 10-50 mass %, and the content of other copolymerizable monomers is 0-10 mass % based on the total mass of the monomer mixture (b).
[0076]
[31] The method for producing an acrylic resin powder according to any one of
[28] to
[30] , wherein the content of the monomer units derived from the polymer (A) is 10 to 80% by mass relative to the total mass of the monomer units constituting the multi-stage polymer (G).
[0077]
[32] A method for producing a resin composition, comprising the step (III) of dissolving an acrylic resin powder obtained by the production method described in any one of
[28] to
[31] in a polyalkylene glycol.
[0078]
[33] A method for producing a hot melt adhesive, comprising step (III): dissolving an acrylic resin powder obtained by the production method described in any one of
[28] to
[31] in polyalkylene glycol and polyester polyol to obtain a resin composition; and step (IV): mixing isocyanate into the resin composition to obtain a polyurethane prepolymer.
[0079] Effects of the Invention
[0080] The acrylic resin powder of the present invention can provide an acrylic resin powder suitable for a hot-melt adhesive which exhibits higher initial adhesive strength than conventional products and has a long open time. BRIEF DESCRIPTION OF THE DRAWINGS
[0081] Figure 1 This is a graph showing the correlation between the initial adhesive strength and the open time in Examples and Comparative Examples. DETAILED DESCRIPTION
[0082] Next, the present invention will be described in detail.
[0083] 《Acrylic resin powder》
[0084] The acrylic resin powder of the present invention is an acrylic resin powder comprising a multistage polymer (G), wherein the multistage polymer (G) is a multistage polymer of a polymer (A) and a polymer (B), wherein the polymer (A) comprises a monomer unit of an alkyl (meth)acrylate (ma), and the polymer (B) comprises monomer units of methyl methacrylate and an alkyl (meth)acrylate (mb), wherein the glass transition temperature of the multistage polymer (G) is 50° C. or higher, and the softening temperature of the acrylic resin powder measured by a flow tester temperature rise method is 150° C. to 200° C.
[0085] The alkyl group in the alkyl (meth)acrylate (ma) preferably has 4 to 8 carbon atoms, and the alkyl group in the methyl methacrylate and the alkyl (meth)acrylate (mb) preferably has 4 to 8 carbon atoms.
[0086] The acrylic resin powder of the present invention comprises a multi-stage polymer (G), wherein the multi-stage polymer (G) is obtained by polymerizing a monomer mixture (b) comprising methyl methacrylate and an alkyl (meth)acrylate (mb) in the presence of a dispersion comprising a polymer (A), wherein the polymer (A) is obtained by polymerizing a monomer mixture (a) comprising an alkyl (meth)acrylate (ma), wherein the alkyl group in the alkyl (meth)acrylate (ma) has 4 to 8 carbon atoms, and the alkyl group in the alkyl (meth)acrylate (mb) has 4 to 8 carbon atoms, wherein the multi-stage polymer (G) has a glass transition temperature of 50° C. or higher and a mass average molecular weight of 10,000 to 300,000, wherein the softening temperature of the acrylic resin powder measured by a flow tester temperature rise method is 150° C. to 200° C., and the acrylic resin powder is soluble in acetone.
[0087] In this specification, "multi-stage polymer" refers to a resin mixture containing polymer (A) and polymer (B) obtained by synthesizing polymer (B) in the presence of polymer (A). For example, the multi-stage polymer may have a core-shell structure in which polymer (A) forms the core and polymer (B) forms the shell.
[0088] Here, the glass transition temperature (hereinafter also referred to as "Tg") is a value obtained by the FOX formula (formula (1)) as described below. In this specification, the unit of Tg is "°C". Specifically, in the case of a polymer (homopolymer) composed only of a single monomer, the standard analysis value recorded in the "Polymer Data Handbook" compiled by the Japanese Society of Polymer Science can be used. In the case of a copolymer obtained by polymerizing n monomers, it can be regarded as a value calculated from the Tg of the homopolymer of each monomer.
[0089] 1 / (273+Tg)=Σ(W n / (273+Tg n))···(Formula (1))
[0090] Where W n represents the mass fraction of monomer n, Tg n It represents the glass transition temperature (° C.) of the homopolymer of the monomer n. Here, the mass fraction is the ratio of the amount of the monomer n charged to the total amount of all the monomers charged.
[0091] SPA, i.e., the solubility parameter (SP value) of the polymer (A), is a value obtained by substituting the Sp value (Sp(ui)) of n monomer units i (i=1 to n) constituting the polymer (A) into the following formula (2). Sp(ui) can be obtained by the Fedors method described in Polymer Engineering and Science, Vol. 14, 147 (1974).
[0092] [Number 1]
[0093]
[0094] (In formula (2), Mi represents the molar fraction of monomer unit i, ΣMi = 1)
[0095] Table 1 below shows literature values of Tg and Sp values (Sp(ui)) of representative homopolymers.
[0096] [Table 1]
[0097]
[0098] The abbreviations in the table represent the following monomers:
[0099] "MMA": Methyl methacrylate
[0100] "n-BMA": n-butyl methacrylate
[0101] "i-BMA": isobutyl methacrylate
[0102] "t-BMA": tert-butyl methacrylate
[0103] "n-BA": n-butyl acrylate
[0104] "MAA": methacrylic acid
[0105] "2-HEMA": 2-Hydroxyethyl methacrylate
[0106] The glass transition temperature of the multi-stage polymer (G) of the present invention is 50°C or more, preferably 58°C or more, and more preferably 65°C or more. If the Tg of the multi-stage polymer (G) is 50°C or more, the initial strength of the hot melt adhesive is improved. Specifically, the glass transition temperature of the multi-stage polymer (G) is preferably 50-85°C, more preferably 58-80°C, and further preferably 65-75°C. In addition, the Tg of the polymer (B) obtained by polymerizing the acrylic monomer mixture (b) is 55°C or more, preferably 65°C or more, and more preferably 70°C or more. If the Tg of the polymer (B) is 55°C or more, the initial bonding strength of the hot melt adhesive is improved, and the blocking caused by thermal fusion of acrylic resin powders can be further suppressed. Specifically, the Tg of the polymer (B) is preferably 55-100°C, more preferably 65-95°C, and further preferably 70-97°C.
[0107] The solubility parameter (SPA) of the polymer (A) obtained by polymerizing the acrylic monomer mixture (a) of the present invention is preferably 19.50 (J / cm 3 ) 1 / 2 Above and 20.1(J / cm 3 ) 1 / 2 Below, more preferably 19.50 (J / cm 3 ) 1 / 2 Above and 20.0(J / cm 3 ) 1 / 2 Below, more preferably 19.60 (J / cm 3 ) 1 / 2 Above and 20.0(J / cm 3 ) 1 / 2 By using a polymer having SPA within this range, the solubility in polyalkylene glycol is improved, the open time of the hot melt adhesive is prolonged, and the workability is improved.
[0108] Here, the softening temperature can be measured by a flow tester temperature rise method. The setting conditions of the flow tester include the shape of the nozzle, the load, the temperature rise rate, etc. In the present invention, the flow tester CFT-100 manufactured by Shimadzu Corporation is used for measurement. When the nozzle is subjected to a load of 294 N (30 kgf) and a constant temperature increase rate of 3° C. / min, the temperature at which 1 / 2 of 1.0 g of the sample flows out is taken as the softening temperature.
[0109] The softening temperature of the multistage polymer (G) is preferably 150°C to 200°C, more preferably 155°C to 190°C, and further preferably 155°C to 185°C. If the softening temperature is 150°C or higher, the initial adhesive strength of the hot melt adhesive is improved, and if it is 185°C or lower, the open time of the hot melt adhesive becomes longer and the workability is excellent. If an acrylic resin having a softening temperature of 200°C or higher is used, the open time becomes shorter and handling becomes difficult. The softening temperature can be adjusted by appropriately setting the Tg and mass average molecular weight of the multistage polymer (G) and the content of the monomer unit derived from the polymer (A).
[0110] The acrylic resin powder that can be used in the present invention must be soluble in acetone. The term "acrylic resin powder is soluble in acetone" can be determined by the following method.
[0111] Accurately weigh 1.0 g [W0] of acrylic resin powder in a 50 ml sample bottle, add 40 ml of acetone and disperse for more than 1 day. Then, use a centrifuge (high-speed cooling centrifuge, product name: CR22N / CR21N, manufactured by Hitachi Koki Co., Ltd.) to centrifuge for 60 minutes at a temperature of 2°C and a rotation speed of 12,000 rpm to separate the soluble and insoluble components, add acetone to the insoluble components again to disperse them, and centrifuge in the same way to completely separate the soluble and insoluble components. After centrifugation, the insoluble components are heated to 60°C in an oven under a nitrogen atmosphere to remove acetone, and vacuum dried at 60°C. The insoluble components [W1] are weighed and the result is used as the ratio of the acetone insoluble components, that is, the gel fraction. The gel fraction is calculated by the following formula.
[0112] Gel fraction (mass %) = [W1] / [W0] × 100
[0113] [W1]; Acetone insoluble content (g)
[0114] [W0]: The amount of acrylic resin powder accurately weighed in a 50 ml sample bottle (g)
[0115] In addition, when the gel fraction is 1 mass % or less, it is considered that it is soluble in acetone.
[0116] (Copolymer composition)
[0117] In the (meth)acrylic acid alkyl ester (ma) and (meth)acrylic acid alkyl ester (mb) that may be included in the manufacture of the acrylic resin powder of the present invention, the carbon number of the alkyl group is 4 to 8. Examples of these monomers include: (meth)acrylic acid esters (for example, n-butyl (meth)acrylate, sec-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, hexyl (meth)acrylate, cyclohexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, etc. Among them, in the (meth)acrylic acid alkyl ester (ma), the alkyl group is preferably a primary alkyl group, and more preferably a straight-chain primary alkyl group. In addition, in the (meth)acrylic acid alkyl ester (mb), the alkyl group is preferably a primary alkyl group, and more preferably a branched primary alkyl group. It should be noted that "(meth)acrylic acid" is a general term for acrylic acid and methacrylic acid. It should be noted that the alkyl group may or may not have a substituent. As a substituent, for example, a hydroxyl group, a halogen atom, etc., are mentioned, and it is preferred that there is no alkylamino group or carbonyl group.
[0118] In addition, examples of monomers other than the above-mentioned alkyl (meth)acrylates (ma) and alkyl (meth)acrylates (mb) include: (meth)acrylates having an alkyl chain with 1 to 3 carbon atoms (e.g., methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, etc.); (meth)acrylates having a long alkyl chain with 9 or more carbon atoms (e.g., stearyl (meth)acrylate, etc.); (meth)acrylic acid, itaconic acid, crotonic acid, maleic acid, fumaric acid, methacrylic acid, The present invention also includes monomers containing carboxyl groups, such as 2-succinyloxyethyl (meth)acrylate and 2-hexahydrophthaloyloxyethyl methacrylate; further, (meth)acrylates containing hydroxyl groups, such as 2-hydroxyethyl (meth)acrylate and 2-hydroxypropyl (meth)acrylate; further, (meth)acrylates containing carbonyl groups, such as acetoacetoxyethyl (meth)acrylate; (meth)acrylates containing amino groups, such as N-dimethylaminoethyl (meth)acrylate and N-diethylaminoethyl (meth)acrylate, etc.
[0119] In the monomer mixture (a), the content of methyl methacrylate is preferably 0 to 60% by mass, the content of alkyl (meth)acrylate (ma) is preferably 40 to 100% by mass, and the content of other copolymerizable monomers is preferably 0 to 10% by mass, based on the total mass of the monomer mixture (a).
[0120] When the content is within the above range, it is easy to adjust the Tg and SPA of the polymer (A), and a hot-melt adhesive having a long open time can be obtained.
[0121] In the monomer mixture (a), the content of the alkyl (meth)acrylate (ma) is preferably 40 to 100% by mass, more preferably 45 to 100% by mass, and further preferably 50 to 100% by mass, based on the total mass of the monomer mixture (a).
[0122] In the monomer mixture (a), the content of other copolymerizable monomers is preferably 0 to 10% by mass based on the total mass of the monomer mixture (a).
[0123] The total content of methyl methacrylate, alkyl (meth)acrylate (ma) and other copolymerizable monomers is not more than 100% by mass based on the total mass of the monomer mixture (a).
[0124] In the monomer mixture (b), the content of methyl methacrylate is preferably 50 to 90% by mass, the content of alkyl (meth)acrylate (mb) is preferably 10 to 50% by mass, and the content of other copolymerizable monomers is preferably 0 to 10% by mass, based on the total mass of the monomer mixture (b).
[0125] In the monomer mixture (b), the content of other copolymerizable monomers is preferably 0 to 10% by mass based on the total mass of the monomer mixture (b).
[0126] The total content of methyl methacrylate, alkyl (meth)acrylate (mb) and other copolymerizable monomers is not more than 100% by mass based on the total mass of the monomer mixture (b).
[0127] In the monomer mixture (b), the content of methyl methacrylate is more preferably 55 to 90% by mass, the content of the alkyl (meth)acrylate (mb) is more preferably 10 to 45% by mass, and the content of other copolymerizable monomers is more preferably 0 to 10% by mass, based on the total mass of the monomer mixture (b).
[0128] Furthermore, in the monomer mixture (b), the content of methyl methacrylate is more preferably 65 to 90% by mass, the content of alkyl (meth)acrylate (mb) is more preferably 10 to 35% by mass, and the content of other copolymerizable monomers is more preferably 0 to 10% by mass, relative to the total mass of the monomer mixture (b).
[0129] When the content is within the above range, the glass transition temperature of the polymer (B) can be easily adjusted to 55° C. or higher, the initial bonding strength of the hot melt adhesive can be improved, and blocking caused by thermal fusion of acrylic resin powders can be suppressed.
[0130] When the monomer units constituting the multi-stage polymer (G) are counted as 100% by mass, the content of the monomer units derived from the polymer (A) is preferably 10 to 80% by mass, and more preferably 20 to 70% by mass. If the content of the monomer units derived from the polymer (A) is 10% by mass or more, the open time of the hot melt adhesive becomes longer. If the content of the monomer units derived from the polymer (A) is 80% by mass or less, the initial bonding strength is improved, and the adhesion caused by the thermal fusion of the acrylic resin powders can be further suppressed. The content of the monomer units derived from the polymer (B) is preferably 20 to 90% by mass, and more preferably 30 to 80% by mass.
[0131] The acrylic resin powder of the present invention comprises a multi-stage polymer (G) obtained by polymerizing a monomer mixture (b) in the presence of a dispersion of a polymer (A) obtained by polymerizing a monomer mixture (a). In this case, the multi-stage polymer (G) may be a multi-stage polymer obtained by adding another monomer mixture to the monomer mixture (a) or the monomer mixture (b) and polymerizing the monomer mixture (a) within the range that the functions of the polymer (A) and the polymer (B) are not impaired.
[0132] In addition, before the polymerization of the above-mentioned monomer mixture (a), polymerization of other monomer mixtures (s) may also be carried out within the range that the functions of the above-mentioned polymers (A) and polymers (B) are not impaired. Specifically, polymer (A) is obtained by polymerizing monomer mixture (a) in the presence of a polymer dispersion (S) obtained by polymerizing monomer mixture (s). As other monomer mixtures (s), (meth) acrylic acid esters obtained by esterification of alcohols having 1 to 4 carbon atoms with (meth) acrylic acid are preferred as the main component because of the appropriate balance of hydrophobicity / hydrophilicity. In addition, the amount (input amount) of other monomer mixtures (s) is preferably 0 to 10% by mass relative to the amount of all monomers used in the synthesis of multi-stage polymers (G). However, the total amount of monomer mixtures (a), monomer mixtures (b) and monomer mixtures (s) used in the synthesis of multi-stage polymers (G) does not exceed 100% by mass.
[0133] (Mass average molecular weight)
[0134] The mass average molecular weight of the multistage polymer (G) usable in the present invention is a value calculated in terms of standard polystyrene which can be determined by GPC (gel permeation chromatography). The mass average molecular weight of the multistage polymer (G) contained in the acrylic resin powder of the present invention is 10,000 to 300,000.
[0135] The mass average molecular weight of the multi-stage polymer (G) is preferably 20,000 or more and 200,000 or less. If the mass average molecular weight of the multi-stage polymer (G) is 10,000 or more, the initial bonding strength of the adhesive tends to be good. If the mass average molecular weight of the multi-stage polymer (G) is 300,000 or less, the viscosity of the resin composition and the adhesive is suppressed, and the open time of the hot melt adhesive is further prolonged.
[0136] (Volume average particle size of primary particles (primary particle size))
[0137] The volume average particle size (primary particle size) of primary particles of the acrylic resin powder that can be used in the present invention is preferably 0.1 to 10 μm, more preferably 0.1 to 5 μm, and even more preferably 0.1 to 2 μm.
[0138] Here, the primary particles refer to the polymer particles that are the smallest units constituting the acrylic resin powder. If the volume average particle size of the primary particles is 10 μm or less, the surface area of the particles increases, and the solubility in solvents such as polyalkylene glycol becomes better. In addition, if it is 0.1 μm or more, the thermal fusion of the volume average particle size of the secondary particles in the powder can be suppressed, and the dispersibility in solvents such as polyalkylene glycol becomes better.
[0139] In the present invention, the volume average particle size of the primary particles is the average value obtained by measuring the particle sizes of the multistage polymer (G) dispersion using a laser diffraction / scattering particle size distribution analyzer (manufactured by Horiba, Ltd., product name: LA-960).
[0140] (Volume average particle size of secondary particles)
[0141] The volume average particle size of the secondary particles of the acrylic resin powder that can be used in the present invention is preferably 20 to 100 μm, more preferably 20 to 80 μm.
[0142] Secondary particles refer to aggregated particles formed by agglomeration of a plurality of primary particles. If the particle size is 20 μm or larger, the particle size can be easily handled because powder scattering can be suppressed. If the particle size is 100 μm or smaller, the particle size has good solubility in polyalkylene glycol.
[0143] In the present invention, the volume average particle size of the secondary particles is the average value obtained by measuring the particle size of the acrylic resin powder using a laser diffraction / scattering particle size distribution analyzer (manufactured by Horiba, Ltd., product name: LA-960).
[0144] (Contents in acrylic resin powder)
[0145] The acrylic resin powder that can be used in the present invention may contain additives such as a defoaming agent as necessary.
[0146] The acrylic resin powder of the present invention is prepared by dissolving the acrylic resin powder of the present invention in polyalkylene glycol to prepare a resin composition. When a hot melt adhesive containing the resin composition is prepared, the initial bonding strength x (kPa) and the open time y (minutes) measured under the following conditions preferably satisfy the following relations (3) and (4):
[0147] y>-0.325x+124···(Formula (3))
[0148] y>10····(Formula (4)),
[0149] For formula (3), within this range, an acrylic resin powder suitable for a hot melt adhesive can be provided, wherein the hot melt adhesive exhibits high initial bonding strength and has a long open time. In addition, the initial bonding strength x is preferably 200 kPa or more, more preferably 300 kPa or more, and further preferably 400 kPa or more.
[0150] In formula (3), y>-0.325x+130 is preferred, y>-0.325x+140 is more preferred, and y>-0.325x+150 is further preferred.
[0151] Regarding formula (4), the air-standing time y is preferably longer than 10 minutes because the operation time can be guaranteed. In addition, the air-standing time y is preferably less than 60 minutes because the process time can be shortened.
[0152] In formula (4), 60>y>10 is preferred, 40>y>10 is more preferred, and 20>y>10 is further preferred.
[0153] (Initial bonding strength x)
[0154] Prepare two wooden flat strips with a width of 1.7 cm, a length of 7.5 cm, and a thickness of 1.5 mm. Apply a hot melt adhesive heated and melted at 120°C to an area of 1.5 cm × 1.7 cm on one of the strips. Overlap the other wooden flat strip and clamp it with a binder clip. Let it stand for 5 minutes to allow the hot melt adhesive to cool and solidify. After standing, remove the binder clip and perform a tensile shear test using the following tensile testing machine and measurement conditions to measure the initial bonding strength x.
[0155] Tensile testing machine: Precision universal testing machine (product name: AGS-X, manufactured by Shimadzu Corporation)
[0156] Measurement conditions: tensile speed 5.0 mm / min
[0157] Distance between fixtures: 50mm
[0158] (Opening time y)
[0159] A hot melt adhesive was applied to a dried wooden flat strip of 1.7 cm in width, 7.5 cm in length, and 1.5 mm in thickness, and heated to 120°C in a Gill heat aging oven. Then, the kraft paper was repeatedly pressed and quickly peeled off at room temperature every 1 minute. The time from the time the hot melt adhesive was applied to the flat strip until no paper fibers remained on the adhesive surface when the kraft paper was peeled off was taken as the air-drying time y.
[0160] 《Resin composition》
[0161] The resin composition of the present invention is obtained by dissolving the acrylic resin powder of the present invention in polyalkylene glycol. The resin composition of the present invention may be contained in a hot melt adhesive.
[0162] (Polyalkylene glycol)
[0163] Examples of the polyalkylene glycol component include polyalkylene glycols having two or more diol units such as polymethylene glycol, polyethylene glycol, polypropylene glycol, polyethylene glycol, and copolymers of ethylene oxide and propylene oxide; and branched polyalkylene glycols using polyfunctional alcohols such as glycerol. These may be used alone or in combination of two or more.
[0164] The number average molecular weight of the polyalkylene glycol is preferably 200 to 5000, more preferably 400 to 3000. If the number average molecular weight of the polyalkylene glycol is 200 or more, the adhesive strength of the hot melt adhesive after curing becomes good. If the number average molecular weight of the polyalkylene glycol is 5000 or less, the viscosity of the resin composition is low and the coating property becomes good.
[0165] In this specification, the number average molecular weight can be measured by GPC (gel permeation chromatography) method.
[0166] When the resin composition of the present invention is prepared into a hot melt adhesive containing the resin composition of the present invention, the initial bonding strength x (kPa) and the open time y (minutes) measured under the above conditions preferably satisfy the following relations (3) and (4):
[0167] y>-0.325x+124···(Formula (3))
[0168] y>10····(Formula (4)),
[0169] For formula (3), within this range, an acrylic resin powder suitable for a hot melt adhesive can be provided, wherein the hot melt adhesive exhibits high initial bonding strength and has a long open time. In addition, the initial bonding strength x is preferably 200 kPa or more, more preferably 300 kPa or more, and further preferably 400 kPa or more.
[0170] In formula (3), y>-0.325x+130 is preferred, y>-0.325x+140 is more preferred, and y>-0.325x+150 is further preferred.
[0171] Regarding formula (4), the air-standing time y is preferably longer than 10 minutes because the operation time can be guaranteed. In addition, the air-standing time y is preferably less than 60 minutes because the process time can be shortened.
[0172] In formula (4), 60>y>10 is preferred, 40>y>10 is more preferred, and 20>y>10 is further preferred.
[0173] (Polyester polyol)
[0174] The resin composition of the present invention may further contain a polyester polyol. As polyester polyols, crystalline polyester polyols and amorphous polyester polyols are known, and specific examples thereof include aliphatic polyester polyols and aromatic polyester polyols. Crystalline polyester polyols and amorphous polyester polyols can be easily distinguished by DSC. The melting point of the crystalline polyester polyol is measured by DSC, and an endothermic peak can be observed when the temperature is increased, and an exothermic peak can be observed when the temperature is decreased.
[0175] When the melting point of the amorphous polyester polyol is measured by DSC, no endothermic peak or exothermic peak is clearly observed, and thus the amorphous polyester polyol can be distinguished from the crystalline polyester polyol.
[0176] Aliphatic polyester polyols can be obtained by reacting aliphatic dicarboxylic acids with diols. Examples of aliphatic dicarboxylic acids include adipic acid, sebacic acid, azelaic acid, and dodecanedioic acid. These can be used alone or in combination of two or more.
[0177] The diol includes low molecular weight diols having 2 to 12 carbon atoms, such as ethylene glycol, 1-methylethylene glycol, 1-ethylethylene glycol, propylene glycol, butanediol, pentanediol, hexanediol, heptanediol, octanediol, nonanediol, decanediol, dodecanediol, neopentyl glycol, 2-methyl-1,3-propanediol, cyclohexanedimethanol, and 2,4-dimethyl-1,5-pentanediol. Among them, at least one selected from ethylene glycol, butanediol, hexanediol, octanediol, and decanediol is preferred. These diols may be used alone or in combination of two or more.
[0178] Examples of the aliphatic polyester polyol include polyhexanediol adipate, polyhexanediol sebacate, polyhexanediol dodecanoate, and polybutylene adipate.
[0179] The aromatic polyester polyol is preferably obtained by reacting an aromatic poly (or di) carboxylic acid with the above-mentioned diol. Examples of the aromatic poly (or di) carboxylic acid include phthalic acid, isophthalic acid, and terephthalic acid. These may be used alone or in combination of two or more. Examples of the aromatic polyester polyol include polyalkylene phthalates, polyalkylene isophthalates, and polyalkylene terephthalates.
[0180] Polyether polyol has low viscosity and good workability, and is suitable for dissolving acrylic resin powder. In addition, polyester polyol has high heat resistance and solvent resistance and high strength, so it is preferable to use polyalkylene glycol and polyester polyol together.
[0181] (isocyanate)
[0182] The resin composition of the present invention may further contain an isocyanate. Examples of the isocyanate include 1,2-ethylene diisocyanate, 1,1-ethylene diisocyanate, propylene diisocyanate, butylene diisocyanate, hexamethylene diisocyanate, toluene diisocyanate, cyclopentylene-1,3-diisocyanate, cyclohexylene-1,4-diisocyanate, cyclohexylene-1,2-diisocyanate, 4,4'-diphenylmethane diisocyanate, 2,2-diphenylpropane-4,4'-diisocyanate, p-phenylene diisocyanate, m-phenylene diisocyanate, xylylene diisocyanate, 1 ,4-naphthylene diisocyanate, 1,5-naphthylene diisocyanate, diphenyl-4,4'-diisocyanate, azobenzene-4,4'-diisocyanate, diphenyl sulfone-4,4'-diisocyanate, dichlorohexamethylene diisocyanate, furfurylidene diisocyanate, 1-chlorobenzene-2,4-diisocyanate, 4,4',4"-triisocyanate-triphenylmethane, 1,3,5-triisocyanate-benzene, 2,4,6-triisocyanate-toluene and 4,4'-dimethyldiphenylmethane-2,2',5,5'-tetraisocyanate.
[0183] As isocyanate, it is preferred that the number of isocyanate groups contained in each molecule is 1 to 3 on average, and in particular, difunctional isocyanate, i.e., diisocyanate, is preferred. One isocyanate may be used alone, or two or more is used in combination. Among them, 4,4'-diphenylmethane diisocyanate is preferred from the perspective of high bonding strength after moisture curing.
[0184] Although monools or monoisocyanates, trifunctional polyols and trifunctional isocyanates may be used, difunctional polyols (diols) and difunctional isocyanates (diisocyanates) are preferred from the viewpoint of the viscosity of the resin composition.
[0185] In addition, it is preferable to use 2 mol of difunctional isocyanate compared to 1 mol of difunctional polyol because the target polyurethane prepolymer can be produced relatively easily.
[0186] Hot Melt Adhesives
[0187] The adhesive formed from the resin composition of the present invention can also be used as a hot-melt adhesive.
[0188] The hot melt adhesive of the present invention is formed from the resin composition of the present invention. The polyol in the resin composition can react with isocyanate to form a polyurethane polymer. That is, the hot melt adhesive of the present invention contains a polyurethane polymer.
[0189] The content of the acrylic resin powder is preferably 1 to 50% by mass, more preferably 5 to 30% by mass, based on the total mass of the hot-melt adhesive.
[0190] When the hot melt adhesive of the present invention contains acrylic resin powder, polyol and isocyanate, the acrylic resin powder is preferably 1 to 50% by mass, and the total amount of polyol and isocyanate is preferably 50 to 99% by mass, relative to the total amount of acrylic resin powder, polyol and isocyanate being 100% by mass. Furthermore, it is more preferred that the acrylic resin powder is 5 to 30% by mass, and the total amount of polyol and isocyanate is 70 to 95% by mass. However, the total amount of acrylic resin powder, polyol and isocyanate does not exceed 100% by mass.
[0191] When the acrylic resin powder is 1% by mass or more relative to 100% by mass of the total amount of the acrylic resin powder, polyol and isocyanate, the initial bonding strength tends to be good, and when it is 50% by mass or less, the bonding strength after curing tends to be improved.
[0192] Other additives may be added within a range that does not impair the effects of the present invention.
[0193] The amount of addition is preferably 0 to 5% by mass. Other additives for the hot melt adhesive of the present invention include: plasticizers such as dioctyl phthalate, dibutyl phthalate, and dioctyl adipate; antioxidants such as phenolic antioxidants, phosphite antioxidants, thioether antioxidants, and amine antioxidants; pigments such as titanium oxide and carbon black; light stabilizers such as benzotriazole, hindered amine, benzoate, and benzotriazole; flame retardants such as halogen flame retardants, phosphorus flame retardants, antimony flame retardants, and metal hydroxide flame retardants; metal catalysts such as tin; The present invention can be used as a curing catalyst such as trimethyltin laurate, trimethyltin hydroxide, dibutyltin dilaurate, dibutyltin maleate, etc., lead catalysts (lead oleate, lead naphthenate, lead octenate, etc.), other metal catalysts (metal salts of naphthenate such as cobalt naphthenate, etc.), and amine catalysts, such as curing catalysts such as triethylenediamine, tetramethylethylenediamine, tetramethylhexanediamine, diazabicycloolefins, dialkylaminoalkylamines, bis(2-dimethylaminoethyl)ether, dimorpholinodiethylether, etc.; waxes such as paraffin wax and microcrystalline wax. In addition, wetting agents, thickeners, defoamers, rheology modifiers, etc. can also be added as needed.
[0194] The initial bonding strength x (kPa) and the open time y (minutes) of the hot melt adhesive of the present invention measured under the above conditions preferably satisfy the following relations (3) and (4):
[0195] y>-0.325x+124···(Formula (3))
[0196] y>10····(Formula (4)),
[0197] For formula (3), within this range, an acrylic resin powder suitable for a hot melt adhesive can be provided, wherein the hot melt adhesive exhibits high initial bonding strength and has a long open time. In addition, the initial bonding strength x is preferably 200 kPa or more, more preferably 300 kPa or more, and further preferably 400 kPa or more.
[0198] In formula (3), y>-0.325x+130 is preferred, y>-0.325x+140 is more preferred, and y>-0.325x+150 is further preferred.
[0199] Regarding formula (4), the air-standing time y is preferably longer than 10 minutes because the operation time can be guaranteed. In addition, the air-standing time y is preferably less than 60 minutes because the process time can be shortened.
[0200] In formula (4), 60>y>10 is preferred, 40>y>10 is more preferred, and 20>y>10 is further preferred.
[0201] 《Method for producing acrylic resin powder》
[0202] The method for producing acrylic resin powder of the present invention uses a polymer (A) obtained by polymerizing a monomer mixture (a) containing an alkyl (meth)acrylate (ma) by dropping 0.1 to 3 parts by mass of a chain transfer agent relative to 100 parts by mass of the monomer mixture (a). In the polymerization of the monomer mixture (a), for example, emulsion polymerization, seed polymerization, soap-free polymerization, dispersion polymerization, microsuspension polymerization, etc. can be used. In the obtained dispersion of the polymer (A), a chain transfer agent is dropped in an amount of 0.1 to 3 parts by mass relative to 100 parts by mass of the monomer mixture (b) containing a monomer mixture (b) containing methyl methacrylate and an alkyl (meth)acrylate (mb), and polymerization is performed to form a dispersion (G1) containing a multi-stage polymer (G). Then, the dispersion (G1) containing the multi-stage polymer (G) can be powdered by spray drying, acid coagulation or salt coagulation and subsequent drying process, freeze drying, centrifugal separation, etc. to obtain acrylic resin powder. In particular, the spray drying method is preferred because the primary particles of the agglomerated particles are not relatively strongly bonded to each other, and thus the structure of the polymerized particles can be broken by weak shearing, and the particles can be uniformly dispersed as primary particles.
[0203] In the method for producing an acrylic resin powder of the present invention, a monomer mixture (b) is polymerized in the presence of a dispersion of a polymer (A) obtained by polymerizing a monomer mixture (a) to form a dispersion (G1) containing a multistage polymer (G). At this time, after the polymerization of the monomer mixture (a) or after the polymerization of the monomer mixture (b), another monomer mixture may be added and polymerized to produce a dispersion (G1) containing a multistage polymer (G) within the range that does not impair the functions of the polymer (A) and the polymer (B).
[0204] In addition, before the polymerization of the above-mentioned monomer mixture (a), other monomer mixtures (s) may be polymerized within the range that the functions of the above-mentioned polymers (A) and (B) are not impaired. Among the other monomer mixtures (s), (meth)acrylates of alcohols having 1 to 4 carbon atoms as the main component are preferred because of the appropriate balance of hydrophobicity / hydrophilicity. In addition, the amount (input amount) of the other monomer mixture (s) is preferably used in the range of 1 to 10% by mass relative to the amount of all monomers used in the synthesis of the multi-stage polymer (G).
[0205] The monomer mixture (a) contains an alkyl (meth)acrylate (ma), and the monomer mixture (b) contains methyl methacrylate and an alkyl (meth)acrylate (mb). As other copolymerizable monomers, the same monomers as those described above may be contained.
[0206] In the monomer mixture (a), the content of methyl methacrylate is preferably 0 to 60% by mass, more preferably 0 to 55% by mass, and even more preferably 0 to 50% by mass, based on the total mass of the monomer mixture (a).
[0207] In the monomer mixture (a), the content of the alkyl (meth)acrylate (ma) is preferably 40 to 100% by mass, more preferably 45 to 100% by mass, and further preferably 50 to 100% by mass, based on the total mass of the monomer mixture (a).
[0208] In the monomer mixture (a), the content of other copolymerizable monomers is preferably 0 to 10% by mass based on the total mass of the monomer mixture (a).
[0209] The total content of methyl methacrylate, alkyl (meth)acrylate (ma) and other copolymerizable monomers is not more than 100% by mass based on the total mass of the monomer mixture (a).
[0210] In the monomer mixture (b), the content of methyl methacrylate is preferably 50 to 90% by mass, more preferably 55 to 90% by mass, and even more preferably 65 to 90% by mass, based on the total mass of the monomer mixture (b).
[0211] In the monomer mixture (b), the content of the alkyl (meth)acrylate (mb) is preferably 10 to 50% by mass, more preferably 10 to 45% by mass, and even more preferably 10 to 35% by mass, based on the total mass of the monomer mixture (b).
[0212] In the monomer mixture (b), the content of other copolymerizable monomers is preferably 0 to 10% by mass based on the total mass of the monomer mixture (b).
[0213] The total content of methyl methacrylate, alkyl (meth)acrylate (mb) and other copolymerizable monomers is not more than 100% by mass based on the total mass of the monomer mixture (b).
[0214] When the monomer units constituting the multistage polymer (G) are taken as 100% by mass, the content of the monomer units derived from the polymer (A) is preferably 10 to 80% by mass, more preferably 20 to 70% by mass.
[0215] When the monomer units constituting the multistage polymer (G) are taken as 100% by mass, the content of the monomer units derived from the monomer mixture (b) is preferably 20 to 90% by mass, more preferably 30 to 80% by mass.
[0216] However, the total content of the monomer units derived from the polymer (A) and the monomer units derived from the monomer mixture (b) does not exceed 100% by mass.
[0217] (Chain transfer agent)
[0218] In order to adjust the molecular weight of the obtained polymer, a chain transfer agent is preferably used. Examples of the chain transfer agent include: mercaptans such as n-dodecyl mercaptan; thioglycolates such as octyl thioglycolate; α-methylstyrene dimer, terpinolene. Among them, a primary or secondary mercapto compound is preferred because the physical properties of the hot melt adhesive using the acrylic resin powder obtained by polymerization become good.
[0219] Examples of primary or secondary mercapto compounds include alkyl mercaptans such as n-butyl mercaptan, sec-butyl mercaptan, n-octyl mercaptan, n-dodecyl mercaptan, and n-octadecyl mercaptan; mercaptoacetic acid esters such as 2-ethylhexyl mercaptoacetate, methoxybutyl mercaptoacetate, and trimethylolpropane tris(mercaptoacetate); and mercaptopropionic acid esters such as β-mercaptopropionic acid-2-ethylhexyl ester, β-mercaptopropionic acid-3-methoxybutyl ester, and trimethylolpropane tris(β-mercaptopropionate). These may be used alone or in combination of two or more. Among them, n-octyl mercaptan, n-dodecyl mercaptan, and 2-ethylhexyl mercaptoacetate having a large chain transfer constant are preferred.
[0220] The amount of the chain transfer agent used is preferably in the range of 0.1 to 3 parts by mass, more preferably in the range of 0.3 to 2 parts by mass, relative to 100 parts by mass of the monomer mixture (a) or the monomer mixture (b). If the amount of the chain transfer agent used is 0.1 parts by mass or more, the molecular weight of the copolymer is reduced by chain transfer of free radicals, and the physical properties of the hot melt adhesive are improved. In addition, if the amount of the chain transfer agent used is 3 parts by mass or less, the residual amount of unreacted monomers and chain transfer agents is reduced, and the odor is reduced.
[0221] (Emulsifier)
[0222] When the polymerization is carried out in water, it is desirable to use an emulsifier. As the emulsifier, an anionic surfactant or a nonionic surfactant can be used. Specific examples of anionic surfactants include: alkylbenzene sulfonates, alkyl sulfonates, alkyl sulfate ester salts, fatty acid metal salts, polyoxyalkyl ether sulfate ester salts, polyoxyethylene carboxylate sulfate ester salts, polyoxyethylene alkylphenyl ether sulfate ester salts, dialkyl succinate sulfonates (e.g., sodium dioctyl sulfosuccinate, etc.). These can be used alone or in combination of two or more.
[0223] Specific examples of nonionic surfactants include: polyoxyethylene alkylphenyl ether, polyoxyethylene alkyl ether, polyoxyethylene fatty acid ester, polyoxyethylene sorbitan fatty acid ester, polyoxyethylene alkyl ether glycerol borate, polyoxyethylene alkyl ether phosphate, polyoxyethylene and other compounds having polyoxyethylene chains in the molecule and having surface activity; compounds in which the polyoxyethylene chains of these compounds are replaced by copolymers of oxyethylene and oxypropylene, sorbitan fatty acid ester, fatty acid glyceride, glycerol fatty acid ester, pentaerythritol fatty acid ester. These may be used alone or in combination of two or more.
[0224] (Polymerization initiator)
[0225] When the polymerization is carried out in water, it is desirable to use a water-soluble free radical polymerization initiator. Examples of water-soluble free radical polymerization initiators include: persulfates such as potassium persulfate, ammonium persulfate, and sodium persulfate; water-soluble azo compounds such as 2,2'-azobis(2-amidinopropane) trihydrochloride and 4,4'-azobis(4-cyanovaleric acid); thermal decomposition polymerization initiators such as hydrogen peroxide; redox polymerization initiators such as hydrogen peroxide and ascorbic acid, tert-butyl hydroperoxide and Rongalite, potassium persulfate and metal salts, ammonium persulfate and sodium bisulfite, etc. These polymerization initiators may be used alone or in combination of two or more.
[0226] 《Method for producing resin composition》
[0227] The method for producing the resin composition of the present invention comprises step (III): dissolving the acrylic resin powder obtained in the above production method in polyalkylene glycol. For example, the acrylic resin powder can be added to polyalkylene glycol, dispersed, and then heated and mixed to dissolve.
[0228] The heating temperature is not particularly limited as long as it is a temperature at which the acrylic resin powder dissolves, but it can be dissolved at a lower temperature or in a shorter time than when using acrylic resin powder obtained by suspension polymerization. It is also possible to add acrylic resin powder and polyester polyol at the same time to dissolve them. Then, it is preferred to add a defoamer as needed, and use a vacuum pump or the like to heat and stir under reduced pressure to fully remove moisture from the resin composition.
[0229] As the polyalkylene glycol used, the same polyalkylene glycol as exemplified in the polyalkylene glycol part that can be included in the resin composition of the present invention can be used. Polyester polyol can also be used in combination. As the polyester polyol, the same polyester polyol as exemplified in the polyester polyol part that can be included in the resin composition of the present invention can be used.
[0230] The polyurethane prepolymer can be obtained by dissolving the acrylic resin powder obtained in the above production method in polyalkylene glycol, adding isocyanate and heating and mixing. As for the polyester polyol, the acrylic resin powder can be added to the polyalkylene glycol and heated and mixed to dissolve it, or it can be added together with isocyanate and heated and mixed.
[0231] Other additives may be included within the range that they do not adversely affect the reaction of the polyol and isocyanate to form the polyurethane prepolymer. There is no particular restriction on the time of addition, for example, it may be added together with the polyol and isocyanate when synthesizing the polyurethane prepolymer, or it may be added after the polyol and isocyanate are reacted to synthesize the polyurethane prepolymer. As additives, the same substances as those exemplified as other additives for hot melt adhesives may be used.
[0232] The heating temperature is preferably 80 to 140° C., more preferably 90 to 110° C. Within this heating temperature range, each component dissolves well, the viscosity decreases, and the workability becomes good. Furthermore, the reaction of isocyanate and polyalkylene glycol proceeds sufficiently. The heating time is not particularly limited, but is preferably 30 to 300 minutes, more preferably 60 to 180 minutes.
[0233] 《Application of resin composition》
[0234] The obtained resin composition of the present invention can be suitably used as a hot melt adhesive. In the present invention, "hot melt adhesive" refers to an adhesive that is melted and reused by applying heat of 80 to 150°C. The hot melt adhesive of the present invention can be used in fields where hot melt adhesives can be used conventionally, such as the building interior field (or construction field), the electronic material field, and the automobile interior field.
[0235] 《Method for producing hot melt adhesive》
[0236] The method for producing a hot melt adhesive comprises a step (III) of dissolving the acrylic resin powder obtained in the above production method in polyalkylene glycol to obtain a resin composition; and a step (IV) of mixing isocyanate with the resin composition to obtain a polyurethane prepolymer.
[0237] In step (III), the same conditions as those described in the "Method for producing resin composition" can be employed.
[0238] The (IV) may further contain a curing catalyst. Examples of the curing catalyst include 2,2'-dimorpholinodiethyl ether and the like.
[0239] The hot melt adhesive is preferably used for bonding automobile interior parts and bonding decorative materials to building interior parts, but is not particularly limited and may be used for woodworking, paper processing, fiber processing, or general use.
[0240] Hot-melt adhesive of the present invention can be used by the same method as conventional hot-melt adhesive, and its method of use is not particularly limited. In addition, for example, when an adherend is pasted on a substrate, the hot-melt adhesive can be applied to the substrate side and / or the adherend side.
[0241] The adherend and the substrate may be commonly used materials, for example, molding materials, film sheets, and fibrous materials formed into sheets by weaving synthetic fibers or natural fibers using a textile machine.
[0242] The molding material, film and sheet are not particularly limited, but thermoplastic resins are preferred. Examples thereof include polyolefin resins, polyester resins, acetate resins, polystyrene resins, ABS resins, vinyl chloride resins, polycarbonate resins, etc. Examples of the polyolefin resins include polyethylene and polypropylene, and examples of the polyester resins include polyethylene terephthalate.
[0243] The laminated product obtained by pasting adherend and base material with hot-melt adhesive of the present invention can be specifically used for various purposes such as building, electronic materials and automobile field. It is not necessary to use special device for manufacturing laminated product, and the commonly known manufacturing device including conveyor, coating machine, pressurizing machine, heater and cutting machine can be used to manufacture. For example, laminated product can be manufactured as follows. While conveying base material and adherend with conveyor, hot-melt adhesive of the present invention is applied to base material or adherend with coating machine. The temperature during coating is controlled to a specified temperature with a heater. Press adherend to base material gently with a pressurizing machine, and paste adherend and base material with the help of hot-melt adhesive. Then the adherend and base material after pasting are placed for cooling, and directly conveyed with conveyor, so that hot-melt adhesive is solidified. Then, the base material with adherend pasted with a cutting machine is cut and processed into appropriate size.
[0244] Since the hot melt adhesive of the present invention has high initial bonding strength, these laminated products have excellent heat resistance after moisture curing, so the substrate and the adherend are not easy to peel off even in summer. It should be noted that the laminated products can also be manufactured by applying the adhesive without using a coating machine.
[0245] Example
[0246] The present invention will be described in more detail below with reference to Examples, but it should be noted that the present invention is not limited to these Examples.
[0247] Various measurement and evaluation methods are described below.
[0248] (Mass average molecular weight)
[0249] The polystyrene-equivalent value measured by GPC (gel permeation chromatography) under the following conditions was defined as the mass average molecular weight of the polymer.
[0250] High-efficiency GPC device (manufactured by Tosoh Corporation, product name: HLC-8220GPC)
[0251] ·· Four columns (manufactured by Tosoh Corporation, product name: TSKgel SuperHZM-M) were used in series
[0252] Column box temperature: 40℃
[0253] ··Eluent: tetrahydrofuran
[0254] ··Sample concentration: 0.1 mass%
[0255] Flow rate: 0.35mL / min
[0256] ··Injection volume: 1μL
[0257] Detector: RI (differential refractometer)
[0258] (Volume average particle size)
[0259] The particle sizes of the obtained polymer dispersion and acrylic resin powder were measured using a laser diffraction / scattering particle size distribution measuring device (manufactured by Horiba, Ltd., product name: LA-960). The particle sizes in this specification use the median particle size (volume average particle size). The relative refractive index of the resin particles and the dispersion solvent was set to 1.12. Ion-exchanged water was used as the dispersion solvent.
[0260] (Softening temperature)
[0261] The flow tester CFT-100 manufactured by Shimadzu Corporation was used for the measurement. When the load was 294N (30Kgf) and the temperature was increased at a constant rate of 3°C / min, the flow rate was 0.1% and the flow rate was 0.2%. The temperature at which 1 / 2 of 1.0 g of the sample flows out of the nozzle is taken as the softening temperature.
[0262] (Solubility in acetone)
[0263] Accurately weigh 1.0 g of acrylic resin powder in a 50 ml sample bottle as [W0], add 40 ml of acetone and disperse for more than 1 day. Then, use a centrifuge (high-speed cooling centrifuge, product name: CR22N / CR21N, manufactured by Hitachi Koki Co., Ltd.) to centrifuge at 2°C and 12,000 rpm for 60 minutes to separate the soluble and insoluble components. Add acetone to the insoluble components again to disperse them, and use a centrifuge (high-speed cooling centrifuge, product name: CR22N / CR21N, manufactured by Hitachi Koki Co., Ltd.) to centrifuge at 2°C and 12,000 rpm for 60 minutes to completely separate the soluble and insoluble components. After centrifugation, the insoluble components are heated to 60°C in an oven under a nitrogen atmosphere to remove acetone, and vacuum dried at 60°C to weigh the insoluble components [W1]. The result is the ratio of the acetone insoluble components, that is, the gel fraction. The gel fraction was calculated by the following formula.
[0264] Gel fraction (mass %) = {[W1] / [W0]}×100
[0265] [W1]: Acetone insoluble content
[0266] [W0]: The amount of acrylic resin powder accurately weighed into a 50ml sample bottle
[0267] When the gel fraction is 1 mass % or less, the compound is judged to be soluble in acetone.
[0268] (Initial bonding strength)
[0269] Prepare two flat strips (wooden, 1.7 cm wide, 7.5 cm long, 1.5 mm thick), apply a hot melt adhesive melted at 120°C to one of them over an area of 1.5 cm x 1.7 cm, overlap the other wooden flat strip, clamp it with a binder clip, and let it stand for 5 minutes to cool and solidify the hot melt adhesive. After standing, remove the binder clip, and perform a tensile shear test using the following tensile testing machine and measurement conditions to measure the initial bonding strength.
[0270] Tensile testing machine: Precision universal testing machine (product name: AGS-X, manufactured by Shimadzu Corporation)
[0271] Measurement conditions: tensile speed 5.0 mm / min
[0272] Distance between fixtures: 50mm
[0273] The initial bonding strength was determined based on the measured values according to the following criteria: If the initial bonding strength was 340 kPa or more, it was considered good.
[0274] A: Above 400kPa;
[0275] B: 250kPa or more and less than 400kPa;
[0276] C: Less than 250kPa.
[0277] (Opening time)
[0278] Apply the heated and melted hot melt adhesive on the dried flat strip (wooden, 1.7 cm wide, 7.5 cm long, 1.5 mm thick), and heat it to 120°C in a Gill heat aging oven. Then, press and stick the kraft paper with your fingers and quickly peel off the kraft paper at 1 minute intervals at room temperature. The time from when the hot melt adhesive is applied to the flat strip until there is no paper fiber remaining on the adhesive surface when the kraft paper is peeled off is taken as the air-drying time. Based on the measured values obtained, determine the air-drying time according to the following standards. If the air-drying time is more than 15 minutes, it is considered good.
[0279] A: More than 15 minutes;
[0280] B: more than 10 minutes and less than 15 minutes;
[0281] C: Less than 10 minutes.
[0282] <Example 1> Acrylic resin powder (P-1)
[0283] [Step I (1)]
[0284] 583 g of ion exchange water was added to a 2-liter four-necked flask equipped with a thermometer, a nitrogen conduit, a stirring rod, a dropping funnel and a condenser, and nitrogen was introduced for 30 minutes to replace the dissolved oxygen in the ion exchange water. Then, the introduction of nitrogen was stopped and the temperature was raised to 80° C. under stirring at 200 rpm. When the internal temperature reached 80° C., a monomer mixture (s-1) consisting of 14.72 g of methyl methacrylate and 31.28 g of isobutyl methacrylate was added, and 0.80 g of potassium persulfate and 20 g of ion exchange water were added, and the mixture was kept for 45 minutes to obtain a polymer dispersion (S-1).
[0285] [Step I (2)]
[0286] 0.32 g of Pelex OT-P (sodium dioctyl sulfosuccinate, active ingredient (emulsifier) 70%, manufactured by Kao Corporation), 0.4 g of potassium persulfate and 44 g of ion exchange water were added to the polymer dispersion (S-1) obtained in [Step I (1)]. After 15 minutes, an acrylic acid monomer mixture (a-1) consisting of 48.48 g of methyl methacrylate, 58.24 g of n-butyl methacrylate, 87.28 g of n-butyl acrylate, 2.24 g of Pelex OT-P, 1.92 g of n-octyl mercaptan and 184 g of ion exchange water was added dropwise over 1.5 hours. After the addition was completed, the mixture was maintained at 80° C. for 1 hour to terminate the polymerization, thereby obtaining a polymer dispersion (A-1). The polymerization was carried out under an environment in which 25 ml of nitrogen was introduced per minute.
[0287] [Step I (3)]
[0288] To the polymer dispersion (A-1) obtained in [Step I (2)], an acrylic monomer mixture (b-1) consisting of 448.96 g of methyl methacrylate, 103.92 g of isobutyl methacrylate, 3.6 g of methacrylic acid, 3.6 g of hydroxyethyl methacrylate, 4.16 g of Pelex OT-P, 4.48 g of n-octyl mercaptan and 280 g of ion exchange water was added dropwise over 3.5 hours. After the addition was completed, the mixture was maintained at 80° C. for 1 hour to terminate the polymerization, thereby obtaining a multi-stage polymer dispersion (G-1). The polymerization was carried out under an environment in which 25 ml of nitrogen was introduced per minute.
[0289] [Step (II)]
[0290] The multi-stage polymer dispersion (G-1) was spray dried using a spray dryer (manufactured by Ohkawara Chemical Industry Co., Ltd., product name: L-8i model) under the conditions of inlet temperature / outlet temperature = 120 / 60°C and a disk rotation speed of 20,000 rpm to obtain an acrylic resin powder (P-1).
[0291] The mass average molecular weight of the acrylic resin powder (P-1) was 42,000, the volume average particle size of the primary particles was 0.53 μm, and the volume average particle size of the secondary particles was 69 μm.
[0292] <Example 2> Acrylic resin powder (P-2)
[0293] An acrylic resin powder (P-2) was produced in the same manner as in Example 1 except that the monomer mixture (a) and the monomer mixture (b) had the compositions shown in Table 2. The results are shown in Table 5.
[0294] <Example 3> Acrylic resin powder (P-3)
[0295] An acrylic resin powder (P-3) was produced in the same manner as in Example 1 except that the monomer mixture (a) and the monomer mixture (b) had the compositions shown in Table 2. The results are shown in Table 5.
[0296] <Example 4> Acrylic resin powder (P-4)
[0297] An acrylic resin powder (P-4) was produced in the same manner as in Example 1 except that the monomer mixture (a) and the monomer mixture (b) had the compositions shown in Table 2. The results are shown in Table 5.
[0298] <Example 5> Acrylic resin powder (P-5)
[0299] An acrylic resin powder (P-5) was produced in the same manner as in Example 1 except that the monomer mixture (a) and the monomer mixture (b) had the compositions shown in Table 2. The results are shown in Table 5.
[0300] <Example 6> Acrylic resin powder (P-6)
[0301] Except that the monomer mixture (a) and the monomer mixture (b) had the compositions shown in Table 3, and the dropping time in [Step I (2)] was 2.5 hours and the dropping time in [Step I (3)] was 2.5 hours, an acrylic resin powder (P-6) was produced in the same manner as in Example 1. The results are shown in Table 6.
[0302] <Example 7> Acrylic resin powder (P-7)
[0303] Except that the monomer mixture (a) and the monomer mixture (b) had the compositions shown in Table 3, and the dropping time in [Step I (2)] was 2.5 hours and the dropping time in [Step I (3)] was 2.5 hours, an acrylic resin powder (P-6) was produced in the same manner as in Example 1. The results are shown in Table 6.
[0304] <Example 8> Acrylic resin powder (P-8)
[0305] Except that the monomer mixture (a) and the monomer mixture (b) had the compositions shown in Table 3, the dropping time in [Step I (2)] was 1 hour, and the dropping time in [Step I (3)] was 4 hours, an acrylic resin powder (P-8) was produced in the same manner as in Example 1. The results are shown in Table 6.
[0306] <Example 9> Acrylic resin powder (P-9)
[0307] Except that the monomer mixture (a) and the monomer mixture (b) had the compositions shown in Table 3, the dropping time in [Step I (2)] was 4 hours, and the dropping time in [Step I (3)] was 1 hour, an acrylic resin powder (P-9) was produced in the same manner as in Example 1. The results are shown in Table 6.
[0308] <Example 10> Acrylic resin powder (P-10)
[0309] Except that the monomer mixture (a) and the monomer mixture (b) had the compositions shown in Table 3, the dropping time in [Step I (2)] was 3 hours, and the dropping time in [Step I (3)] was 2 hours, an acrylic resin powder (P-8) was produced in the same manner as in Example 1. The results are shown in Table 6.
[0310] <Comparative Example 1> Acrylic resin powder (P-11)
[0311] An acrylic resin powder (P-11) was produced in the same manner as in Example 6 except that the monomer mixture (s), the monomer mixture (a), and the monomer mixture (b) had the compositions shown in Table 4. The results are shown in Table 7.
[0312] <Comparative Example 2> Acrylic resin powder (P-12)
[0313] The acrylic resin powder (P-12) was produced in the same manner as in Example 1 except that the acrylic monomer mixture (b) had the composition shown in Table 4 and the [Step I (2)] was not performed. The results are shown in Table 7.
[0314] <Comparative Example 3> Acrylic resin powder (P-13)
[0315] Except that the monomer mixture (a) and the monomer mixture (b) had the compositions shown in Table 4, the dropping time in [Step I (2)] was 3.5 hours, and the dropping time in [Step I (3)] was 1.5 hours, an acrylic resin powder (P-13) was produced in the same manner as in Example 1. The results are shown in Table 7.
[0316] The acetone solubility of the resin powders obtained in Examples 1 to 10 and Comparative Examples 1 to 3 was confirmed, and it was found that the gel fractions of the resin powders were all 1% by mass or less, and the resin powders were all soluble in acetone.
[0317] [Table 2]
[0318]
[0319] [Table 3]
[0320]
[0321] [Table 4]
[0322]
[0323] The compounds in the table represent the following compounds.
[0324] "MMA": Methyl methacrylate (manufactured by Mitsubishi Chemical Corporation)
[0325] · "n-BMA": n-butyl methacrylate (manufactured by Mitsubishi Chemical Corporation)
[0326] · "i-BMA": isobutyl methacrylate (manufactured by Mitsubishi Chemical Corporation)
[0327] · "t-BMA": tert-butyl methacrylate (manufactured by Mitsubishi Chemical Corporation)
[0328] "n-BA": n-butyl acrylate (manufactured by Mitsubishi Chemical Corporation)
[0329] · "MAA": Methacrylic acid (manufactured by Mitsubishi Chemical Corporation)
[0330] · "2-HEMA": 2-hydroxyethyl methacrylate (manufactured by Mitsubishi Chemical Corporation)
[0331] "n-OM": n-octyl mercaptan (manufactured by Wako Pure Chemical Industries, Ltd.)
[0332] "KPS": Potassium persulfate (manufactured by Mitsubishi Gas Chemical Co., Ltd.)
[0333] "OT-P": Pelex OT-P, sodium dioctyl sulfosuccinate, active ingredient (emulsifier) 70% (manufactured by Kao Corporation)
[0334] [Table 5]
[0335]
[0336] [Table 6]
[0337]
[0338] [Table 7]
[0339]
[0340] <Example 11>
[0341] [Dissolution process]
[0342] Into a 300-ml four-necked flask equipped with a thermometer, a stirring rod and a condenser, 41.1 g of polypropylene glycol with a mass average molecular weight of about 2000 (trade name: ADEKA polyether P-2000, manufactured by ADEKA) as a polyol, 3.0 g of polypropylene glycol with a mass average molecular weight of about 400 (trade name: ADEKA polyether P-400, manufactured by ADEKA), 0.3 g of "Modaflow 2100" (manufactured by Allnex) as a defoaming agent, and 23.7 g of acrylic resin powder (P-1) were added, the internal temperature was heated to 100°C, and stirred for 1 hour to obtain a uniform solution-like resin composition.
[0343] [Decompression dehydration process]
[0344] The resin composition was heated and stirred at 15 kPa and 100° C. for 1 hour, and dehydrated under reduced pressure.
[0345] 24.5 g of polyester polyol "HS 2H-351A" (produced by Toyokuni Oil, polyester polyol of hexanediol and adipic acid, molecular weight 3500, melting point 55°C, OHV = 32 mgKOH / g) as a polyol, 14.0 g of 4,4'-diphenylmethane diisocyanate as an isocyanate, and 0.2 g of 2,2'-dimorpholinodiethyl ether (produced by Mitsui Fine Chemicals Co., Ltd.) as a curing catalyst were added, and stirred at 15 kPa and 100°C for 3 hours. Then, the mixture was cooled, and the obtained hot melt adhesive was recovered and sealed for storage.
[0346] <Examples 12 to 20>
[0347] Hot melt adhesives were obtained in the same manner as in Example 11 except that the types of acrylic resin powder were changed as shown in Tables 8 to 20. The results of initial adhesive strength and open time are shown in Tables 8 to 20.
[0348] <Comparative Examples 4 to 6>
[0349] Hot melt adhesives were obtained in the same manner as in Example 11 except that the types of acrylic resin powder were changed as shown in Tables 8 to 20. The results of initial adhesive strength and open time are shown in Tables 8 to 10.
[0350] [Table 8]
[0351]
[0352] [Table 9]
[0353]
[0354] [Table 10]
[0355]
[0356] The results of Examples 11 to 20 and Comparative Examples 4 to 6 were plotted into a graph. Figure 1 Examples 11 to 20 are within the region of y>-0.325x+124 and 60>y>10.
[0357] In Examples 11 to 20, it was determined that they had an appropriate open time and had a high initial adhesive strength.
[0358] In Comparative Example 4, it was determined that the air-standing time was too long, workability was poor, and initial adhesive strength was low.
[0359] In Comparative Example 5, although the initial adhesive strength was large, the open time was too short and the workability was poor.
[0360] In Comparative Example 6, although it had an appropriate open time, it was judged that the initial adhesive strength was small.
[0361] Industrial Applicability
[0362] The acrylic resin powder of the present invention can provide an acrylic resin powder suitable for a hot-melt adhesive that exhibits good initial adhesive strength and has a longer open time than conventional products.
Claims
1. An acrylic resin powder, comprising a multi-stage polymer G, wherein the multi-stage polymer G is a multi-stage polymer of a polymer A and a polymer B, wherein the polymer A comprises a monomer unit of an alkyl (meth)acrylate ma, and the polymer B comprises a monomer unit of each of methyl methacrylate and an alkyl (meth)acrylate mb, When the monomer units constituting the multistage polymer G are taken as 100% by mass, the content of the monomer units derived from the polymer A is 10 to 80% by mass, and the content of the monomer units derived from the polymer B is 20 to 90% by mass. The mass average molecular weight of the multi-stage polymer G is greater than or equal to 10,000 and less than or equal to 300,000. The glass transition temperature of the multi-stage polymer G is above 50°C, The solubility parameter SPA of the polymer A is 19.50 (J / cm 3 ) 1 / 2 Above and 20.1 (J / cm 3 ) 1 / 2 The glass transition temperature of polymer B is 55 to 100°C. The softening temperature of the acrylic resin powder measured by the flow tester temperature rising method is 150°C to 200°C. The acrylic resin powder is soluble in acetone.
2. The acrylic resin powder according to claim 1, in, The alkyl group in the (meth)acrylic acid alkyl ester ma has 4 to 8 carbon atoms, and the alkyl group in the (meth)acrylic acid methyl ester and the (meth)acrylic acid alkyl ester mb has 4 to 8 carbon atoms.
3. An acrylic resin powder, comprising a multistage polymer G, wherein the multistage polymer G is obtained by polymerizing a monomer mixture b comprising methyl methacrylate and an alkyl (meth)acrylate mb in the presence of a dispersion comprising a polymer A, wherein the polymer A is obtained by polymerizing a monomer mixture a comprising an alkyl (meth)acrylate ma, The carbon number of the alkyl group in the (meth)acrylic acid alkyl ester ma is 4 to 8, The carbon number of the alkyl group in the (meth)acrylic acid alkyl ester mb is 4 to 8. When the monomer units constituting the multistage polymer G are taken as 100% by mass, the content of the monomer units derived from the polymer A is 10 to 80% by mass, and the content of the monomer units derived from the polymer B is 20 to 90% by mass. The glass transition temperature of the multi-stage polymer G is above 50°C, The mass average molecular weight of the multi-stage polymer G is greater than or equal to 10,000 and less than or equal to 300,000. The solubility parameter SPA of the polymer A is 19.50 (J / cm 3 ) 1 / 2 Above and 20.1 (J / cm 3 ) 1 / 2 The glass transition temperature of polymer B is 55 to 100°C. The softening temperature of the acrylic resin powder measured by the flow tester temperature rising method is 150°C to 200°C. The acrylic resin powder is soluble in acetone.
4. The acrylic resin powder according to any one of claims 1 to 3, in, The volume average particle size of the primary particles of the acrylic resin powder is 0.1 to 10 μm.
5. The acrylic resin powder according to claim 4, in, The volume average particle size of the secondary particles of the acrylic resin powder is 20 to 100 μm.
6. The acrylic resin powder according to claim 3, in, The monomer mixture a further comprises other copolymerizable monomers, In the monomer mixture a, the content of methyl methacrylate is 0 to 60 mass %, the content of the alkyl (meth)acrylate ma is 40 to 100 mass %, and the content of the other copolymerizable monomer is 0 to 10 mass % relative to the total mass of the monomer mixture a.
7. The acrylic resin powder according to claim 3, in, The monomer mixture b further comprises other copolymerizable monomers, In the monomer mixture b, the content of methyl methacrylate is 50-90 mass %, the content of alkyl (meth)acrylate mb is 10-50 mass %, and the content of the other copolymerizable monomer is 0-10 mass % based on the total mass of the monomer mixture b. 8 . A resin composition obtained by dissolving the acrylic resin powder according to claim 1 in polyalkylene glycol.
9. The resin composition according to claim 8, in, The number average molecular weight of the polyalkylene glycol is 200-5000. 10 . The resin composition according to claim 8 , further comprising a polyester polyol. 11 . The resin composition according to claim 8 , further comprising isocyanate. 12 . A hot-melt adhesive comprising the resin composition according to claim 8 .
13. The hot melt adhesive according to claim 12, wherein the hot melt adhesive is formed from a resin composition comprising acrylic resin powder, polyalkylene glycol, polyester polyol and isocyanate, wherein the initial bonding strength x in kPa measured under the following conditions and the open time y in minutes measured under the following conditions satisfy the following relations (3) and (4): y>-0.325x+124 ···Formula (3) y>10···Formula (4), Initial bonding strength x Prepare two wooden flat strips with a width of 1.7 cm, a length of 7.5 cm, and a thickness of 1.5 mm. On one of the strips, apply a hot-melt adhesive melted at 120°C to an area of 1.5 cm × 1.7 cm. Overlap the other wooden flat strip and clamp it with a binder clip. Let it stand for 5 minutes to allow the hot-melt adhesive to cool and solidify. After standing, remove the binder clip and perform a tensile shear test using the following tensile testing machine and measurement conditions to measure the initial bonding strength x. Tensile testing machine: precision universal testing machine; product name: AGS-X, made by Shimadzu Corporation Measurement conditions: tensile speed 5.0 mm / min The distance between the fixtures is 50mm; Open time Apply heated and melted hot-melt adhesive on a dried wooden flat strip with a width of 1.7 cm, a length of 7.5 cm and a thickness of 1.5 mm, and heat it to 120°C in a Gir thermal aging oven; then, at room temperature, repeatedly press and stick kraft paper sheets with fingers and quickly peel off the kraft paper sheets every 1 minute; the time from the time the hot-melt adhesive is applied to the flat strip until no paper fibers remain on the adhesive surface when the kraft paper sheets are peeled off is taken as the air-drying time y.
14. A method for producing acrylic resin powder, wherein include: Step I: adding dropwise and polymerizing a monomer mixture b containing methyl methacrylate and an alkyl (meth)acrylate mb and 0.1 to 3 parts by mass of a chain transfer agent based on 100 parts by mass of the monomer mixture b to a dispersion A1 containing a polymer A, wherein the polymer A is obtained by polymerizing a monomer mixture a containing an alkyl (meth)acrylate ma and 0.1 to 3 parts by mass of a chain transfer agent based on 100 parts by mass of the monomer mixture a, to obtain a dispersion G1 containing a multistage polymer G; and Step II: spray drying the dispersion G1 of the multi-stage polymer G to obtain acrylic resin powder; The carbon number of the alkyl group in the (meth)acrylic acid alkyl ester ma is 4 to 8, The carbon number of the alkyl group in the (meth)acrylic acid alkyl ester mb is 4 to 8. When the monomer units constituting the multistage polymer G are taken as 100% by mass, the content of the monomer units derived from the polymer A is 10 to 80% by mass, and the content of the monomer units derived from the polymer B is 20 to 90% by mass. The mass average molecular weight of the multi-stage polymer G is 10,000 or more and 300,000 or less, and the glass transition temperature of the multi-stage polymer G is 50° C. or more. The solubility parameter SPA of the polymer A is 19.50 (J / cm 3 ) 1 / 2 Above and 20.1 (J / cm 3 ) 1 / 2 The glass transition temperature of polymer B is 55 to 100°C. The softening temperature of the acrylic resin powder measured by the flow tester temperature rising method is 150°C to 200°C. The acrylic resin powder is soluble in acetone.
15. The method for producing acrylic resin powder according to claim 14, in, The monomer mixture a further comprises other copolymerizable monomers, In the monomer mixture a, the content of methyl methacrylate is 0 to 60 mass %, the content of the alkyl (meth)acrylate ma is 40 to 100 mass %, and the content of the other copolymerizable monomers is 0 to 10 mass % relative to the total mass of the monomer mixture a.
16. The method for producing acrylic resin powder according to claim 14 or 15, in, The monomer mixture b further comprises other copolymerizable monomers, In the monomer mixture b, the content of methyl methacrylate is 50 to 90% by mass, the content of alkyl (meth)acrylate mb is 10 to 50% by mass, and the content of methyl methacrylate mb is 10 to 50% by mass, relative to the total mass of the monomer mixture b. The content of the other copolymerizable monomers is 0 to 10% by mass.
17. The method for producing acrylic resin powder according to claim 14 or 15, in, The content of the monomer units derived from the polymer A is 10 to 80% by mass relative to the total mass of the monomer units constituting the multi-stage polymer G. 18 . A method for producing a resin composition, comprising step III of dissolving an acrylic resin powder obtained by the production method according to claim 14 in a polyalkylene glycol.
19. A method for producing a hot melt adhesive, comprising step III: dissolving an acrylic resin powder obtained by the production method according to any one of claims 14 to 17 in polyalkylene glycol and polyester polyol to obtain a resin composition; and step IV: mixing isocyanate with the resin composition to obtain a polyurethane prepolymer.
Citation Information
Patent Citations
Enamel wire and method for producing enamel wire
JP2020061289A
Acrylic resin powder and resin composition for hot melt adhesives, and method for producing same
WO2018012234A1
Acrylic resin powder, resin composition, hot melt adhesive composition containing acrylic resin powder and method for producing same
WO2019188930A1