Semiconductor manufacturing methods and semiconductor devices
By replacing the silicon film with a conductive film containing different concentrations of suppressing substances at different temperatures, the problem of wiring voids in the recess was solved, and the electrical properties and mechanical strength were improved.
Patent Information
- Application Number
- CN202110923490.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-03-15
- Filing Date
- 2021-08-12
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2041-08-12
AI Technical Summary
During the manufacturing process of semiconductor devices, voids can easily form in the wiring within the recesses, resulting in poor electrical properties and mechanical strength.
By exposing the silicon film to metal raw material gas and suppressing gas at different temperatures, a first conductive film and a second conductive film containing different concentrations of suppressing substances are formed, thereby inhibiting metal growth and avoiding the formation of voids.
It effectively suppressed voids in the wiring layer, ensuring electrical properties and mechanical strength, and improving the filling effect of the wiring layer.
Smart Images

Figure CN115084005B_ABST
Abstract
Description
[0001] This application enjoys priority based on Japanese Patent Application No. 2021-041724 (filed on March 15, 2021). This application incorporates the entire contents of that basic application by reference. Technical Field
[0002] This embodiment relates to a semiconductor manufacturing method and a semiconductor device. Background Technology
[0003] In the manufacture of semiconductor devices, wiring is sometimes embedded within recesses in an insulating layer. In this case, voids may be created within the wiring. Summary of the Invention
[0004] The problem to be solved by the present invention is to provide a semiconductor manufacturing method and a semiconductor device capable of forming wiring in a recess.
[0005] According to one embodiment, a semiconductor manufacturing method includes the step of forming a recess downward from the upper surface of a layer having at least a partial insulating layer disposed above a substrate. The method further includes the step of forming a silicon film on the inner surface of the recess. The method also includes the step of exposing the silicon film to a metal-containing feed gas and a metal-inhibiting gas at a first temperature to replace a first portion of the silicon film located at the upper end of the recess with a first conductive film containing metal. The method further includes the step of exposing the silicon film to a feed gas and a metal-inhibiting gas at a second temperature lower than the first temperature to replace a second portion of the silicon film, different from the first portion, with a second conductive film containing metal. Attached Figure Description
[0006] Figure 1 This is a cross-sectional view illustrating an embodiment of a semiconductor device.
[0007] Figure 2 This is a cross-sectional view illustrating an embodiment of a semiconductor manufacturing method.
[0008] Figure 3 Is it connected to Figure 2 The following is a cross-sectional view illustrating the semiconductor manufacturing method of an embodiment.
[0009] Figure 4 Is it connected to Figure 3 The following is a cross-sectional view illustrating the semiconductor manufacturing method of an embodiment.
[0010] Figure 5 Is it connected to Figure 4 The following is a cross-sectional view illustrating the semiconductor manufacturing method of an embodiment.
[0011] Figure 6 Is it connected to Figure 5The following is a cross-sectional view illustrating the semiconductor manufacturing method of an embodiment.
[0012] Figure 7 Is it connected to Figure 6 The following is a cross-sectional view illustrating the semiconductor manufacturing method of an embodiment.
[0013] Figure 8 This is a cross-sectional view showing the semiconductor device of the first modified example.
[0014] Figure 9 This is a cross-sectional view showing the semiconductor device of the second modified example.
[0015] Figure 10 This is a cross-sectional view showing the semiconductor manufacturing method of the second variation.
[0016] Figure 11 Is it connected to Figure 10 The following is a cross-sectional view showing the semiconductor manufacturing method of the second variation.
[0017] Label Explanation
[0018] 3: Interlayer insulating film, 31: Upper surface, 32: Recess, 5: Silicon film, 42: First conductive film, 43: Second conductive film. Detailed Implementation
[0019] Hereinafter, embodiments of the present invention will be described with reference to the accompanying drawings. Figures 1 to 7 In this context, identical or similar structures are labeled with the same number, and redundant descriptions are omitted. Figure 1 This is a diagram illustrating the semiconductor device 1 according to an embodiment.
[0020] like Figure 1 As shown, the semiconductor device 1 of the embodiment includes a semiconductor substrate 2, an interlayer insulating film 3, and a wiring layer 4.
[0021] An interlayer insulating film 3 is disposed above the semiconductor substrate 2. A recess 32 is formed on the interlayer insulating film 3, extending downwards from its upper surface 31. The lateral width w of the recess 32 is maximum at a first position P1 between its upper and lower ends. Furthermore, the width w of the recess 32 increases from its upper end toward the first position P1. Conversely, the width w of the recess 32 decreases from its first position P1 toward its lower end. In other words, the cross-section of the recess 32 has a roughly barrel-shaped, or roughly hexagonal, shape. This shape, where the recess 32 has its maximum width at the first position P1, is one that, even if the width w of the recess 32 were designed uniformly, would still be obtained due to process requirements. As a process consideration, for example, when the recess 32 is formed by RIE (Reactive Ion Etching), it is advantageous to minimize the adsorption of etching byproducts near P1 of the recess 32, which protects the sidewalls from the effects of etching gases, and to facilitate the incidence of the oblique component of etching ions. Additionally, the cross-section of the recess 32 may also have rounded corners. The height h of the recess 32 is greater than its width w. The recess 32 can be a hole. Alternatively, the recess 32 can also be a groove or slot extending in a depth direction orthogonal to the width direction. The interlayer insulating film 3 is, for example, a silicon oxide film.
[0022] The wiring layer 4 is disposed inside the recess 32 in a manner that fills the recess 32. The wiring layer 4 has a barrier metal film 41, a first conductive film 42, a second conductive film 43 and a conductive layer 44.
[0023] A barrier metal film 41 is provided covering the entire inner surface of the recess 32. The barrier metal film 32 is, for example, a titanium nitride film.
[0024] A first conductive film 42 is disposed on a first region R1 on the upper end side of the inner surface of the recess 32, separated by a blocking metal film 41. The first region R1 is the range on the inner surface of the recess 32 from the upper end to a second position P2, which is higher than the first position P1. The first conductive film 42 contains a metal and an inhibitory substance that inhibits the growth of the metal. The metal is, for example, tungsten. The inhibitory substance is, for example, nitrogen.
[0025] The second conductive film 43 is disposed on a second range R2, different from the first range R1, on the inner surface of the recess 32, separated from the first range R1, by the blocking metal film 41. Figure 1 In the example shown, the second range R2 is the entire range outside the first range R1 on the inner surface of the recess 32. The second conductive film 43 contains the same metal as the metal contained in the first conductive film 42 (e.g., tungsten). In addition, the second conductive film 43 contains the same suppressing substance as the suppressing substance contained in the first conductive film 42 (e.g., nitrogen).
[0026] A conductive layer 44 is disposed on the first conductive film 42 and the second conductive film 43. The conductive layer 44 contains the same metal as the metal contained in the first conductive film 42 (e.g., tungsten).
[0027] The concentration of the suppressing substance in the first conductive film 42 is higher than that in the second conductive film 43. The higher concentration of the suppressing substance in the first conductive film 42 helps to suppress the formation of voids within the conductive layer 44.
[0028] Next, refer to Figures 2-7 The manufacturing method of the semiconductor device 1 configured as described above will be explained.
[0029] Figure 2 This is a cross-sectional view illustrating a semiconductor manufacturing method according to an embodiment. First, as... Figure 2 As shown, for the interlayer insulating film 3 disposed on the semiconductor substrate 2, a recess 32 is formed from the upper surface 31 of the interlayer insulating film 3 downwards. The recess 32 is formed, for example, by photolithography or RIE. After the recess 32 is formed, as... Figure 2 As shown, a barrier metal film 41 is formed on the inner surface of the recess 32. The barrier metal film 41 is formed, for example, by forming a titanium nitride film using CVD (Chemical Vapor Deposition). By forming the barrier metal film 41, the tightness of the wiring layer 4 to the recess 32 can be ensured, and the diffusion of metal contained in the wiring layer 4 into the interlayer insulating film 3 can be suppressed.
[0030] Figure 3 Is it connected to Figure 2 The following is a cross-sectional view illustrating the semiconductor manufacturing method of the embodiment. After the barrier metal film 41 is formed, as... Figure 3 As shown, a silicon film 5 is formed on the inner surface of the recess 32 through a barrier metal film 41. The silicon film 5 is formed, for example, by a CVD method. From the viewpoint of properly replacing the silicon film 5 with conductive films 42 and 43, the thickness of the silicon film 5 is preferably 0.5 to 10 nm.
[0031] Figure 4 yes Figure 3 The following is a cross-sectional view illustrating the semiconductor manufacturing method of an embodiment. After the silicon film 5 is formed, as... Figure 4As shown, at a first temperature, the silicon film 5 is exposed to a raw material gas containing a metal (e.g., tungsten) and an inhibiting gas that inhibits the growth of the metal contained in the first conductive film 42. The first temperature is 400°C or higher, for example, 500°C. By setting the first temperature to 400°C or higher, the concentration of nitrogen, as an example of an inhibiting substance, in the first conductive film 42 can be made to be a high concentration of 6 [atomic%] or higher. The raw material gas is, for example, tungsten hexafluoride (WF6) gas. The inhibiting gas is the gas of the aforementioned inhibiting substance, for example, nitrogen. By exposing the silicon film 5 to the raw material gas and the inhibiting gas at the first temperature, such as... Figure 4 As shown, a first portion of the silicon film 5 located on the upper end side of the recess 32, i.e., the first region R1, is replaced with the first conductive film 42. At this time, the time the silicon film 5 is exposed to the raw material gas and the suppressing gas is set to a relatively short time, so that only the first portion is replaced with the first conductive film 42. The exposure time at the first temperature can be, for example, a few seconds. The localized replacement of the silicon film 5 with the first conductive film 42 is performed, for example, by a CVD method.
[0032] Figure 5 Is it connected to Figure 4 The following is a cross-sectional view illustrating the semiconductor manufacturing method of the embodiment. After partially replacing the silicon film 5 with the first conductive film 42, as... Figure 5 As shown, the silicon film 5 is exposed to the aforementioned raw material gas and suppressing gas at a second temperature lower than the first temperature. The second temperature is below 400°C, for example, it can be 300°C. By setting the second temperature below 400°C, the concentration of nitrogen in the second conductive film 43 can be made to be a low concentration of less than 6 [atomic %]. By exposing the silicon film 5 to the raw material gas and suppressing gas at the second temperature, such as... Figure 5 As shown, a second portion of the silicon film located on the second region R2 of the recess 32 is replaced with a second conductive film 43. The time for which the silicon film 5 is exposed to the feed gas and the suppressing gas is set to be longer than the exposure time at the first temperature, so that the second portion is properly replaced with the second conductive film 43. The exposure time at the second temperature can be, for example, tens of seconds. The localized replacement of the silicon film 5 with the second conductive film 43 is performed, for example, by a CVD method.
[0033] Thus, a first conductive film 42 with a high concentration of inhibitory substance and a second conductive film 43 with a low concentration of inhibitory substance are formed.
[0034] Figure 6 Is it connected to Figure 5 The following is a cross-sectional view illustrating the semiconductor manufacturing method of the embodiment. After replacing the silicon film 5 with the first conductive film 42 and the second conductive film 43, as... Figure 6 As shown, a raw material gas is used to form the conductive layer 44 of the buried recess 32. The conductive layer 44 is formed, for example, by a CVD method.
[0035] Here, assuming that the conductive layer 44 is formed on the first conductive film 42 and the second conductive film 43 at a uniform growth rate, before the recess 32 at the first position P1, where the width w is the largest, is filled by the conductive layer 44, the recess 32 at the opening side above the first position P1 will be filled by the conductive layer 44. That is, the opening of the recess 32 used to introduce the raw material gas into the recess 32 will be blocked by the conductive layer 44. Because the opening of the recess 32 is blocked, the subsequent growth of the conductive layer 44 is hindered, resulting in a void in the conductive layer 44 at the first position P1 side.
[0036] In contrast, according to the embodiment, the first conductive film 42 contains a high concentration of an inhibitory substance that suppresses the growth of the metal (e.g., tungsten) constituting the conductive layer 44. Therefore, as... Figure 6 As shown, the conductive layer 44 is preferentially formed on the second conductive film 43. That is, the formation of the conductive layer 44 on the first conductive film 42 located on the opening side at the upper end of the recess 32 is suppressed. By suppressing the formation of the conductive layer 44 on the first conductive film 42, it is possible to prevent the opening of the recess 32 from being blocked by the conductive layer 44 before it is filled in the recess 32.
[0037] Furthermore, the conductive layer 44 can also be formed by continuing the process of exposing the silicon film 5 to the raw material gas and the suppressing gas at the second temperature. By doing so, the processing time can be reduced.
[0038] Figure 7 Is it connected to Figure 6 The following is a cross-sectional view illustrating an embodiment of the semiconductor manufacturing method. (By relative to...) Figure 6 Further, the conductive layer 44 is formed, such as... Figure 7 As shown, a conductive layer 44 is formed on the first conductive film 42 and the second conductive film 43. By inhibiting the formation of the conductive layer 44 on the first conductive film 42, the opening at the upper end of the recess 32 is prevented from being blocked by the conductive layer 44, as shown. Figure 7 As shown, voids within the conductive layer 44 are suppressed.
[0039] As described above, according to this embodiment, by exposing the silicon film to a raw material gas and a suppressing gas at a first temperature, the first portion of the silicon film 5 located on the upper end side of the recess 32 is replaced with a first conductive film 42. Then, by exposing the silicon film 5 to the raw material gas and the suppressing gas at a second temperature lower than the first temperature, the second portion of the silicon film 5, which is different from the first portion, is replaced with a second conductive film 43. This suppresses voids in the conductive layer 44. Consequently, a wiring layer 4 can be suitably formed within the recess 32. By forming a wiring layer 4 with suppressed voids, the electrical characteristics (resistance value) and mechanical strength of the wiring layer 4 can be suitably ensured.
[0040] The above-described embodiments can be adapted to several variations as shown below.
[0041] Figure 8 This is a cross-sectional view showing the semiconductor device 1 of the first modified example. Figure 1 In this paper, a semiconductor device 1 with a blocking metal film 41 between the inner surface of the recess 32 and the first conductive film 42 and the second conductive film 43 is described. In contrast, as... Figure 8 As shown, the blocking metal film 41 can also be omitted. According to the first variation, manufacturing time and cost can be reduced.
[0042] Figure 9 This is a cross-sectional view showing the semiconductor device 1 of the second modified example. Figure 1 In this paper, a semiconductor device 1 in which a wiring layer 4 is disposed within a recess 32 of an interlayer insulating film 3 is described. In contrast, as... Figure 9 As shown, the wiring layer 4 can also be disposed in the gap 320 disposed from the upper surface of the laminate 30 of the insulating layer 301 and the conductive layer 302 downward. Figure 9 The semiconductor device 1 shown is a three-dimensional semiconductor memory. The insulating layer 301 is, for example, a silicon oxide film. The conductive layer 302 contains, for example, tungsten.
[0043] The semiconductor device 1 of the second modification includes a pillar-shaped memory cell 6 extending through the laminate 30. The memory cell 6 has a memory film (not shown) and silicon pillars (not shown) inside the memory film. The memory film, for example, has a block insulating film, a charge storage layer, and a tunnel insulating film in sequence from the outside. The wiring layer 4 is used to connect the source line (not shown) connected to the lower end of the wiring layer 4 to the upper wiring (not shown). In addition, the gap 320 is used to replace the sacrificial layer 303 between the insulating layers 301 described later with a conductive layer 302.
[0044] Figure 10 This is a cross-sectional view illustrating the semiconductor manufacturing method of the second modification. To manufacture the semiconductor substrate 1 of the second modification, as follows... Figure 10 As shown, a laminate 300 consisting of an insulating layer 301 and a sacrificial layer 303 is formed on a semiconductor substrate 2, for example, by a CVD method. The sacrificial layer 303 is, for example, a silicon nitride film. Then, after a memory via 61 is formed through the laminate 300, for example, by a RIE method, a memory cell 6 is formed within the memory via 61. The memory cell 6 can also be formed in two stages: the formation of the lower layer and the formation of the upper layer. Furthermore, a gap 320 is formed through the laminate 300, for example, by a RIE method.
[0045] Figure 11 Is it connected to Figure 10 The following is a cross-sectional view showing the semiconductor manufacturing method of the second modified example. After the gap 320 is formed, as... Figure 11As shown, the sacrificial layer 303 is selectively removed from the laminate 300 by wet etching through the gap 320.
[0046] After removing the sacrificial layer 303, a conductive layer 302 is formed within the void created by removing the sacrificial layer 303, for example, by CVD. Additionally, a conductive layer 302 is formed within the gap 320 by... Figures 1 to 8 The same method is used to form wiring layer 4.
[0047] According to the second variation, in the manufacturing process of a three-dimensional semiconductor memory, a wiring layer 4 can be appropriately formed within the gap 320.
[0048] The above describes some embodiments, but these embodiments are merely illustrative and not intended to limit the scope of the invention. The novel apparatus and methods described in this specification can be implemented in a wide variety of other ways. Furthermore, various omissions, substitutions, and modifications can be made to the apparatus and methods described in this specification without departing from the spirit of the invention. The appended claims and their equivalents are intended to include such embodiments and modifications as contained within the scope and spirit of the invention.
Claims
1. A semiconductor manufacturing method, comprising: A recess is formed downward from the upper surface of a layer having at least a partial insulating layer disposed above the substrate; A silicon film is formed on the inner surface of the recess; At a first temperature, the silicon film is exposed to a metal-based raw material gas and an inhibitory gas that inhibits the growth of the metal, thereby replacing the first portion of the silicon film located on the upper end side of the recess with a first conductive film containing the metal; and At a second temperature lower than the first temperature, the silicon film is exposed to the raw material gas and the suppressing gas, and a second portion of the silicon film, different from the first portion, is replaced with a second conductive film containing the metal. The time during which the silicon film is exposed to the raw material gas and the suppressing gas at the first temperature is shorter than the time during which the silicon film is exposed to the raw material gas and the suppressing gas at the second temperature.
2. The semiconductor manufacturing method according to claim 1, further comprising: A conductive layer containing the metal is formed on the first conductive film and the second conductive film.
3. The semiconductor manufacturing method according to claim 1, By exposing the silicon film to the raw material gas and the suppressing gas at the second temperature, the second portion is replaced by the second conductive film, and a conductive layer containing the metal is formed on the first conductive film and the second conductive film.
4. The semiconductor manufacturing method according to claim 1, The concentration of the suppressing gas component in the first conductive film is higher than that in the second conductive film.
5. The semiconductor manufacturing method according to claim 2, The concentration of the suppressing gas component in the first conductive film is higher than that in the second conductive film.
6. The semiconductor manufacturing method according to claim 3, The concentration of the suppressing gas component in the first conductive film is higher than that in the second conductive film.
7. The semiconductor manufacturing method according to claim 1, further comprising: Before forming the silicon film, a metal film is formed on the inner surface of the recess.
8. The semiconductor manufacturing method according to claim 1, The metal is tungsten.
9. The semiconductor manufacturing method according to claim 8, The raw material gas is tungsten hexafluoride gas. The suppressing gas is nitrogen.
10. The semiconductor manufacturing method according to claim 1, The first temperature is above 400°C. The second temperature is below 400°C.
11. The semiconductor manufacturing method according to claim 1, The silicon film is formed to a thickness of 0.5~10nm.
12. The semiconductor manufacturing method according to claim 1, The width of the recess is at a first position between the upper and lower ends of the recess, increases from the upper end toward the first position, and decreases from the first position toward the lower end.
13. The semiconductor manufacturing method according to claim 12, The first portion is a portion of the silicon film formed on the range from the upper end of the recess to a second position that is higher than the first position.
14. A semiconductor device manufactured using the semiconductor manufacturing method according to any one of claims 1 to 13, comprising: A layer having an insulating layer at least partially disposed above a substrate and having a recessed portion extending from the upper surface toward the lower surface; The first conductive film is disposed on the upper end side of the inner surface of the recess in a first region, and contains a metal and an inhibitory substance that inhibits the growth of the metal. A second conductive film, disposed on a second region different from the first region on the inner surface of the recess, contains the metal and the inhibitory substance; and A conductive layer, disposed on the first conductive film and the second conductive film, contains the metal. The concentration of the inhibitory substance in the first conductive film is higher than that in the second conductive film.
15. The semiconductor device according to claim 14, The metal is tungsten. The inhibitory substance is nitrogen.
16. The semiconductor device according to claim 14, The layer having the insulating layer is a stack of the insulating layer and the conductive layer.
Citation Information
Patent Citations
Interior member for vehicle and method of manufacturing the same
JP2021041724A
Conductive plug and method of forming the same
US20170011960A1