A single ion gel polymer electrolyte, its preparation and application

By using in-situ thermally induced deep eutectic solvents to polymerize single-ion gel polymer electrolytes in lithium batteries, the problems of low lithium ion migration numbers and environmental pollution in lithium batteries are solved, achieving high lithium ion conductivity and safety sexual enhancement.

CN115117442BActive Publication Date: 2024-10-22HUAZHONG UNIV OF SCI & TECH
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202210898619.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-07-28
Publication Date
2024-10-22
Estimated Expiration
2042-07-28

AI Technical Summary

Technical Problem

Existing single-ion gel polymer electrolytes have problems such as low ionic conductivity, concentration polarization and lithium dendrite growth in lithium batteries, and the use of a large amount of organic solvents in the preparation process of traditional pouring methods leads to environmental pollution.

Method used

By in-situ thermally initiating the free radical polymerization of single-ion monomers in deep eutectic solvents, the deep eutectic solvent is used to increase the lithium ion migration number, inhibit the growth of lithium dendrites, reduce the use of organic solvents, and improve the contact between the electrolyte and the electrode. .

Benefits of technology

It improves the lithium ion conductivity, inhibits the generation and growth of lithium dendrites, improves the rate performance and safety of lithium batteries, and reduces environmental pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115117442B_ABST
    Figure CN115117442B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of polymer electrolytes, and more specifically, relates to a single ion gel polymer electrolyte, its preparation and application. The single ion gel polymer electrolyte is prepared by in-situ thermal initiation of free radical polymerization of single ion monomers in a deep eutectic solvent, wherein the deep eutectic solvent is obtained by Lewis acid-base interaction between single ion monomers and Lewis bases. When the polymer electrolyte is applied to a lithium battery, the ionic conductivity of the single ion gel polymer electrolyte is improved due to the introduction of the deep eutectic solvent; the in-situ polymerization method improves the contact between the electrolyte and the positive and negative electrode materials; the polymerized single ion network fixes the anions, increases the lithium ion migration number, thereby inhibiting the growth of lithium dendrites, while reducing the concentration polarization during battery operation and improving the battery's rate performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of polymer electrolytes, and more specifically, relates to a single ion gel polymer electrolyte, and its preparation and application. Background Art

[0002] With the development of society and the progress of science and technology, the consumption of non-renewable fossil resources is increasing. On the other hand, as people's awareness of environmental protection gradually increases, the call for protecting the natural environment and developing renewable resources is increasing. Renewable natural resources such as solar energy and wind energy are greatly affected by weather, region and other environmental factors, so energy storage equipment is required to store and integrate the electric energy before it can be connected to the power grid. Therefore, convenient and efficient energy storage equipment is very necessary. Lithium batteries have been widely used in mobile electronic devices, new energy vehicles and large energy storage equipment due to their advantages such as high energy density, long cycle life and high operating voltage.

[0003] With the popularity of new energy vehicles, car mileage anxiety has become more and more serious, and people are increasingly eager for lithium batteries with high energy density and fast charging speed. Although traditional commercial electrolytes have good electrochemical properties, their inherent volatility and flammability limit their further development and application. All-solid-state polymer electrolytes have good safety and easy processing, but there is concentration polarization when the battery is working, resulting in a low lithium ion migration number and lithium dendrite growth. Single-ion polymer electrolytes that connect anions to the polymer backbone through chemical bonds can only allow lithium ions to move in the battery system, ensuring stable and uniform transmission of lithium ions, effectively inhibiting the growth of lithium dendrites, and thus improving battery safety. However, all-solid-state single-ion polymer electrolytes have the defect of low lithium ion conductivity, making them difficult to commercialize.

[0004] Patent CN114665149A discloses a single-ion gel polymer electrolyte material, which first polymerizes monomers to obtain single-ion polymers, further prepares polymer electrolyte membranes by a casting method, and then prepares single-ion gel polymer electrolyte materials by adding organic solvents; the organic solvent introduced in this patent document increases the ionic conductivity of the single-ion electrolyte material, but a large amount of organic solvent is used in the casting process, and the organic solvent needs to be added later, which has defects such as environmental pollution and organic solvent volatilization. Summary of the invention

[0005] In view of the defects of the prior art, the present invention provides a single ion gel polymer electrolyte, its preparation and application. The single ion gel polymer electrolyte is prepared by in-situ thermal initiation of free radical polymerization of single ion monomers in a deep eutectic solvent, wherein the deep eutectic solvent is obtained by Lewis acid-base interaction between single ion monomers and Lewis bases. When the polymer electrolyte is applied to a lithium battery, the ionic conductivity of the single ion gel polymer electrolyte is improved due to the introduction of the deep eutectic solvent; and the in-situ polymerization method improves the contact between the electrolyte and the positive and negative electrode materials; the polymerized single ion network fixes the anions, increases the lithium ion migration number, thereby inhibiting the growth of lithium dendrites, and at the same time reduces the concentration polarization when the battery is working, and improves the rate performance of the battery. At the same time, it also solves the technical problem that the prior art first polymerizes the monomer to obtain a single ion polymer, and further prepares the polymer electrolyte membrane by a casting method, and a large amount of organic solvent needs to be added later, resulting in environmental pollution.

[0006] To achieve the above object, the present invention provides a method for preparing a single ion gel polymer electrolyte, comprising the following steps:

[0007] (1) using 3-sulfonyl propyl acrylate metal salt or 3-sulfonyl propyl methacrylate metal salt as a raw material, first subjecting it to a sulfonylation treatment to obtain a crude sulfonyl chloride product, then reacting the crude product with an acid binding agent and an amine in an organic solvent to obtain a sulfonimide salt, and finally reacting the sulfonimide salt with a lithium-containing alkaline solution to obtain a monoionic monomer;

[0008] (2) mixing and stirring the single ion monomer obtained in step (1) and the Lewis base to form a uniform and transparent deep eutectic solvent; and then mixing the deep eutectic solvent with an initiator to obtain a mixed precursor solution;

[0009] (3) Adding the mixed precursor solution obtained in step (2) to the diaphragm, allowing the mixed precursor solution to infiltrate the diaphragm, and heating to induce polymerization of the single-ion monomers infiltrated in the diaphragm to obtain a single-ion gel polymer electrolyte.

[0010] Preferably, the raw material in step (1) is one or more of 3-sulfonate propyl acrylate sodium salt, 3-sulfonate propyl acrylate potassium salt, 3-sulfonate propyl methacrylate sodium salt, and 3-sulfonate propyl methacrylate potassium salt.

[0011] Preferably, the Lewis base in step (2) is one or more of sulfolane, N-methylacetamide and N-methyltrifluoroacetamide;

[0012] The initiator is one of azobisisobutyronitrile, azobisisoheptanenitrile, 4,4'-azobis(4-cyanovaleric acid) and 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile).

[0013] Preferably, the membrane in step (3) is a cellulose membrane or a polyolefin membrane.

[0014] Preferably, step (1) comprises the following sub-steps:

[0015] (1-1) dispersing 3-sulfonyl acrylate metal salt or 3-sulfonyl methacrylate metal salt in an organic solvent, using N,N-dimethylformamide as a catalyst, adding dropwise a sulfonylating agent dissolved in the organic solvent under ice bath conditions, and reacting at room temperature after ice bathing. After the reaction is completed, a crude sulfonyl chloride product is obtained;

[0016] (1-2) mixing the crude sulfonyl chloride product with an acid-binding agent, an amine and an organic solvent, reacting the mixture in an ice bath and then reacting the mixture at room temperature to obtain a sulfonyl imide salt;

[0017] (1-3) The sulfonyl imide salt obtained in step (1-2) is dissolved in an organic solvent, and then slowly added to a lithium-containing alkaline solution under ice bath conditions for reaction. After the reaction is completed, excess alkali and organic solvent are removed, and the monoionic monomer is purified to obtain the monoionic monomer.

[0018] Preferably, the organic solvent is one or more of dichloromethane, tetrahydrofuran, 1,4-dioxane and 1,2-dichloroethane;

[0019] The sulfonylating agent is one or more of thionyl chloride and oxalyl chloride;

[0020] The acid binding agent is one or more of triethylamine, trimethylamine, pyridine, pyrrolidine and bipyridine;

[0021] The amine is one or more of cyanamide, trifluoromethylsulfonamide, methylsulfonamide, trifluoromethoxybenzenesulfonamide, benzenesulfonamide, nitrobenzenesulfonamide and trifluoromethylbenzenesulfonamide;

[0022] The lithium-containing base is one or more of lithium carbonate, lithium hydroxide and lithium hydride.

[0023] Preferably, the molar ratio of the monoionic monomer to the Lewis base in step (2) is 1:3 to 1:80; more preferably 1:5 to 1:40; and even more preferably 1:10:1:20.

[0024] The mass ratio of the monoionic monomer to the initiator is 100:0.5 to 100:5.

[0025] Preferably, in step (2), the monoionic monomer obtained in step (1) and the Lewis base are mixed, heated to 60-80° C., and stirred to form a deep eutectic solvent;

[0026] The heating in step (3) triggers the polymerization reaction of the monoionic monomers infiltrated in the diaphragm, and the heating temperature is 60° C. to 80° C.; the polymerization reaction time is 12 hours to 48 hours.

[0027] According to another aspect of the present invention, a single ion gel polymer electrolyte prepared by the preparation method is provided.

[0028] According to another aspect of the present invention, there is provided an application of the polymer electrolyte as a polymer electrolyte for a lithium ion battery.

[0029] In general, the above technical solution conceived by the present invention has the following beneficial effects compared with the prior art:

[0030] 1. The preparation method of the single-ion gel polymer electrolyte provided by the present invention is obtained by further thermally initiating polymerization of single-ion monomers in a deep eutectic solvent. The deep eutectic solvent formed by the single-ion monomers serves as both a solvent for the polymerization reaction and a monomer, thereby reducing the introduction of organic solvents in the preparation process of the electrolyte membrane and reducing pollution to the environment.

[0031] 2. The present invention prepares a single ion gel polymer electrolyte by an in-situ polymerization method, which increases the contact between the electrolyte and the electrode, reduces the interface contact impedance, and can improve the cycle and rate performance of the battery.

[0032] 3. The preparation method of the single-ion gel polymer electrolyte provided by the present invention introduces a Lewis base that interacts with the single-ion monomer, and through the interaction between the two, the interaction between lithium ions and anions is weakened, thereby improving the ionic conductivity of the single-ion gel polymer electrolyte.

[0033] 4. In the preparation method of the single-ion gel polymer electrolyte provided by the present invention, the interaction between the Lewis base and the lithium salt on the polymer chain inhibits the leakage and volatilization of the Lewis base, thereby improving the safety of the battery.

[0034] 5. When the single-ion gel polymer electrolyte prepared by the single-ion gel polymer electrolyte preparation method provided by the present invention is applied to a lithium battery, it exhibits a lithium ion migration number higher than 0.8, which can inhibit the concentration polarization inside the battery, and further inhibit the generation and growth of lithium dendrites.

[0035] 6. The single-ion gel polymer electrolyte material prepared by the preparation method of the single-ion gel polymer electrolyte provided by the present invention has good interface stability when applied to lithium batteries, thereby extending the battery service life. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 It is a schematic diagram of the preparation process of the single ion monomer of the present invention.

[0037] Figure 2 This is a flow chart of preparing a single ion gel polymer electrolyte in Example 1 of the present invention.

[0038] Figure 3 The differential scanning calorimetry (DSC) curves of the deep eutectic solvent, the single ion monomer and the Lewis base prepared in Example 1 of the present invention are shown.

[0039] Figure 4 1 is a curve diagram showing the change of conductivity of the single ion gel polymer electrolyte prepared in Example 1 of the present invention with temperature.

[0040] Figure 5 It is a linear sweep voltammetry curve diagram of the single ion gel polymer electrolyte prepared in Example 1 of the present invention and Comparative Examples 1-4.

[0041] Figure 6 It is the chronoamperometry and electrochemical impedance spectroscopy of the single ion gel polymer electrolyte prepared in Example 1 of the present invention.

[0042] Figure 7 It is a cycle performance diagram of batteries assembled with single ion gel polymer electrolytes prepared in Example 1 of the present invention and Comparative Examples 1-4. DETAILED DESCRIPTION

[0043] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0044] The present invention provides a method for preparing a single ion gel polymer electrolyte, comprising the following steps:

[0045] (1) using 3-sulfonyl propyl acrylate metal salt or 3-sulfonyl propyl methacrylate metal salt as a raw material, first subjecting it to a sulfonylation treatment to obtain a crude sulfonyl chloride product, then reacting the crude product with an acid binding agent and an amine in an organic solvent to obtain a sulfonimide salt, and finally reacting the sulfonimide salt with a lithium-containing alkaline solution to obtain a monoionic monomer;

[0046] (2) mixing and stirring the single ion monomer obtained in step (1) and the Lewis base to form a uniform and transparent deep eutectic solvent; and then mixing the deep eutectic solvent with an initiator to obtain a mixed precursor solution;

[0047] (3) Adding the mixed precursor solution obtained in step (2) to the diaphragm, allowing the mixed precursor solution to infiltrate the diaphragm, and heating to induce polymerization of the single-ion monomers infiltrated in the diaphragm to obtain a single-ion gel polymer electrolyte.

[0048] During the experiment of the present invention, a single-ion monomer prepared with 3-sulfonate propyl acrylate metal salt or 3-sulfonate propyl methacrylate metal salt as raw material was mixed with a Lewis base and then fully stirred. It was found that the powdered single-ion monomer and the solid Lewis base could form a uniform and transparent liquid deep eutectic solvent (or called deep eutectic solvent or low eutectic solvent) after being fully mixed and stirred, possibly due to hydrogen bonding or Lewis acid-base action. Considering that the deep eutectic solvent formed by the single-ion monomer and the Lewis base can serve as a solvent for the polymerization reaction and contain monomers, it can reduce the introduction of organic solvents in the preparation process of the electrolyte membrane and reduce pollution to the environment. Therefore, the deep eutectic solvent is further heated to induce polymerization of the monomers therein to obtain the single-ion gel polymer electrolyte of the present invention.

[0049] By mixing the single-ion monomer of the present invention with a Lewis base, a deep eutectic solvent can be formed within a wide range of molar ratios. At the same time, experiments have also found that if the molar ratio of Lewis base to single-ion monomer is too small, the Lewis base is insufficient and the lithium salt is difficult to dissociate; if the ratio is too large, too much Lewis base will dilute the lithium ion concentration, resulting in insufficient lithium ions being transmitted, which will also cause battery performance to decline. In a preferred embodiment, the molar ratio of the single-ion monomer to the Lewis base in step (2) is 1:3 to 1:80; more preferably 1:5-1:40; and optimally 1:10:1:20. The mass ratio of the single-ion monomer to the initiator is 100:0.5 to 100:5. The single-ion monomer and the Lewis base mixed in the above ratio can form a deep eutectic solvent. And after adding the initiator thereto, due to the good solubility of the deep eutectic solvent, the initiator can also be dissolved in the deep eutectic solvent.

[0050] For the single ion monomer and Lewis base of the present invention, sufficient stirring at room temperature, such as magnetic stirring or mechanical stirring for a sufficient period of time, such as 1-2 hours, can form a deep eutectic solvent; in a preferred embodiment, heating can also be used to promote the formation of the deep eutectic solvent, such as heating to 60-80°C and stirring to form a deep eutectic solvent, which can shorten the formation time of the deep eutectic solvent. After heating the single ion monomer and Lewis base to form a deep eutectic solvent, the temperature is lowered to room temperature, and then the initiator is added.

[0051] In some embodiments, the 3-sulfonate propyl (meth)acrylate metal salt in step (1) is one or more of 3-sulfonate propyl acrylate sodium salt, 3-sulfonate propyl acrylate potassium salt, 3-sulfonate propyl methacrylate sodium salt, and 3-sulfonate propyl methacrylate potassium salt.

[0052] The Lewis base used in the present invention can be any Lewis base that can form a deep eutectic solvent with the above-mentioned single ion monomer. In some embodiments, the Lewis base in step (2) is one or more of sulfolane, N-methylacetamide, and N-methyltrifluoroacetamide.

[0053] The present invention can use any initiator that can initiate the polymerization of the above-mentioned monoionic monomer. In some embodiments, the initiator is one of azobisisobutyronitrile, azobisisoheptanenitrile, 4,4'-azobis(4-cyanovaleric acid), and 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile).

[0054] The separator of the present invention is a separator commonly used in lithium-ion batteries, including but not limited to a cellulose separator or a polyolefin separator.

[0055] In some embodiments, the preparation method of the monoionic monomer in step (1) is as follows: Figure 1 As shown, it includes the following sub-steps:

[0056] (1-1) dispersing 3-sulfopropyl (meth)acrylate metal salt in an organic solvent, using N,N-dimethylformamide as a catalyst, adding dropwise a sulfonylating agent dissolved in the organic solvent under ice bath conditions, reacting at room temperature after ice bathing, and obtaining a crude sulfonyl chloride product after post-treatment after the reaction;

[0057] (1-2) mixing the crude sulfonyl chloride product with an acid-binding agent, an amine and an organic solvent, reacting the mixture in an ice bath and then reacting the mixture at room temperature, and after the reaction is completed, performing post-treatment to obtain a sulfonyl imide salt;

[0058] (1-3) The sulfonyl imide salt obtained in step (1-2) is dissolved in an organic solvent, and slowly added to a lithium-containing alkaline solution under ice bath conditions for reaction. After the reaction is completed, excess alkali and organic solvent are removed, and the lithium single ion monomer is purified to obtain the lithium single ion monomer.

[0059] In a preferred embodiment, the organic solvent is one or more of dichloromethane, tetrahydrofuran, 1,4-dioxane, and 1,2-dichloroethane; the sulfonylating agent is one or more of dichlorothionyl chloride and oxalyl chloride; the acid binding agent is one or more of triethylamine, trimethylamine, pyridine, pyrrolidine, and bipyridine; the amine is one or more of cyanamide, trifluoromethylsulfonamide, methylsulfonamide, trifluoromethoxybenzenesulfonamide, benzenesulfonamide, nitrobenzenesulfonamide, and trifluoromethylbenzenesulfonamide; the lithium-containing base is one or more of lithium carbonate, lithium hydroxide, and lithium hydride.

[0060] In some embodiments, the heating in step (3) to initiate the polymerization reaction of the monoionic monomers has a heating temperature of 60° C. to 80° C.; and the polymerization reaction time is 12 hours to 48 hours.

[0061] In some embodiments, in step (3) of the present invention, the mixed precursor solution obtained in step (2) is added to the separator located between the positive electrode and the negative electrode, so that the mixed precursor solution infiltrates the separator, and heating is used to induce the in-situ polymerization reaction of the single-ion monomer infiltrated in the separator to obtain a single-ion gel polymer electrolyte. The positive electrode and the negative electrode can be conventional positive electrode materials and negative electrode materials of lithium-ion batteries. The mixed precursor solution is added to the separator, and can be slowly poured or dripped onto the separator to make the separator infiltrated.

[0062] The single-ion gel polymer electrolyte prepared by the preparation method of the present invention can be used as a polymer electrolyte for lithium-ion batteries. By introducing a Lewis base that interacts with the single-ion monomer structure, the interaction between lithium ions and anions is weakened through the interaction between the two, thereby improving the ionic conductivity of the single-ion gel polymer electrolyte; when the single-ion gel polymer electrolyte is applied to a lithium battery, it exhibits a high lithium ion migration number, can inhibit concentration polarization inside the battery, and further inhibits the generation and growth of lithium dendrites, has good interface stability, and prolongs the battery service life.

[0063] The polymer electrolyte of the present invention can be applied to lithium-ion batteries. The thickness of the single-ion gel polymer electrolyte membrane prepared by in-situ polymerization in the present invention can be flexibly adjusted according to actual needs. Of course, polymer electrolytes in non-film shapes can also be prepared according to actual application requirements.

[0064] The following are specific embodiments:

[0065] Example 1

[0066] This embodiment provides a method for preparing a single ion gel polymer electrolyte, and the preparation method is as follows:

[0067] 12.38 g of 3-sulfonic acid propyl methacrylate potassium salt was added to 20 mL of tetrahydrofuran, 1.4 mL of N, N-dimethylformamide was added dropwise as a catalyst, and magnetic stirring was carried out at room temperature for 0.5 h. 20 mL of dichlorothionyl (dissolved in 10 mL) was added, and the reaction was carried out in an ice bath for 1 h. The temperature was further raised to room temperature and the reaction was carried out overnight. The mixture after the reaction was completed was added dropwise to ice water, extracted with dichloromethane, washed with ice distilled water, dried over anhydrous magnesium sulfate, and concentrated by vacuum distillation to obtain a crude product of 3-sulfonyl chloride propyl methacrylate; 2.11 g of cyanamide and 14 mL of triethylamine were dissolved in 20 mL of tetrahydrofuran, and the obtained crude sulfonyl chloride product was dissolved in 15 mL of tetrahydrofuran. The mixture was added dropwise to the above mixed solution under ice bath conditions, reacted for 5 hours, the triethylamine salt was filtered out, the organic solvent was removed by distillation under reduced pressure, dichloromethane was added and washed with water four times, dried over anhydrous magnesium sulfate, and concentrated by distillation under reduced pressure to obtain a monoionic triethylamine salt; the monoionic triethylamine salt was dissolved in 20 mL of tetrahydrofuran, and added dropwise to a tetrahydrofuran suspension of 0.5 g of lithium hydride under ice bath conditions, reacted for 3 hours, the excess lithium hydride was removed by filtration, concentrated under reduced pressure, washed three times with n-hexane, and recrystallized from dichloromethane to obtain a cyano monoionic monomer (LiCSAPMA).

[0068] Under an argon atmosphere, 0.0725 g of LiCSAPMA and 0.51 g of cyclopentane sulfone were weighed in a molar ratio of 1:14, and magnetic stirring was performed for 0.5 h to form a deep eutectic solvent. 0.001 g of azobisisobutyronitrile was added and stirred to dissolve the azobisisobutyronitrile. The obtained mixed solution was dropped on the separator between the negative electrode and the positive electrode, and the mixture was heated to 60 ° C and reacted for 48 hours to completely polymerize the single-ion monomer, thereby obtaining a single-ion gel polymer electrolyte (LiCSAPMA / SL-1) prepared by in situ polymerization.

[0069] like Figure 2 As shown, firstly, a single-ion monomer is synthesized by a three-step method, then mixed with a Lewis base to form a deep eutectic solvent, an initiator is added and stirred thoroughly to obtain a precursor solution, the uniformly mixed precursor solution is dropped onto a diaphragm, and a battery is formed by buckling it with the negative and positive electrode materials of a lithium battery, and a single-ion gel polymer electrolyte is obtained by further thermal initiation polymerization.

[0070] Figure 3 That is, the differential scanning calorimetry (DSC) curves of the LiCSAPMA / SL complex, the single-ion monomer LiCSAPMA and the Lewis base SL prepared in Example 1. It can be seen that the melting point of the prepared LiCSAPMA / SL complex is significantly lower than that of the single-ion monomer LiCSAPMA and the Lewis base SL, indicating that the two are composited to form a deep eutectic solvent.

[0071] Figure 4 This is the single ion gel polymer electrolyte prepared in Example 1, which has a conductivity of 2.6×10-5 S cm -1 ionic conductivity.

[0072] Example 2

[0073] The other conditions were the same as those in Example 1, except that the molar ratio of LiCSAPMA to sulfolane was changed to 1:5, i.e., 0.1 g of LiCSAPMA and 0.25 g of sulfolane were weighed, and the subsequent steps were the same as those in Example 1 to obtain a single ion gel polymer electrolyte (LiCSAPMA / SL-2) prepared by in situ polymerization.

[0074] Example 3

[0075] The other conditions were the same as those in Example 1, but the molar ratio of LiCSAPMA to sulfolane was changed to 1:7, that is, 0.1 g of LiCSAPMA and 0.36 g of sulfolane were weighed, and the subsequent steps were the same as those in Example 1 to obtain a single ion gel polymer electrolyte (LiCSAPMA / SL-3) prepared by in situ polymerization.

[0076] Example 4

[0077] The other conditions were the same as those in Example 1, but the molar ratio of LiCSAPMA to sulfolane was changed to 1:10, that is, 0.1 g of LiCSAPMA and 0.5 g of sulfolane were weighed, and the subsequent steps were the same as those in Example 1 to obtain a single ion gel polymer electrolyte (LiCSAPMA / SL-4) prepared by in situ polymerization.

[0078] Example 5

[0079] The other conditions were the same as those in Example 1, except that the molar ratio of LiCSAPMA to sulfolane was changed to 1:28, i.e., 0.05 g of LiCSAPMA and 0.72 g of sulfolane were weighed, and the subsequent steps were the same as those in Example 1 to obtain a single ion gel polymer electrolyte (LiCSAPMA / SL-5) prepared by in situ polymerization.

[0080] Figure 5 That is, the linear sweep voltammetry curve of the electrolyte prepared in Example 1 to Example 5. It can be seen that the single-ion gel polymer electrolyte prepared in Example 1 to Example 5 has no obvious oxidation current before 7V, has a wide electrochemical stability window, and can meet the use requirements of high-voltage batteries.

[0081] Figure 6 That is, the chronoamperometric curve and the electrochemical impedance spectrum before and after polarization of the single ion gel polymer electrolyte prepared in Example 1. Based on this, it can be calculated that the migration number of the single ion gel electrolyte is 0.92.

[0082] Figure 7That is, the cycle performance of the button cell using the single ion gel polymer electrolyte prepared in Example 1 and Example 5 as the solid electrolyte at 1C rate. It can be seen that the lithium batteries prepared with these single ion gel polymer electrolytes have good cycle performance. At the same time, compared with the gel polymer electrolytes prepared in Examples 2 to 5, it is found that the best electrochemical performance is achieved when the molar ratio of LiCSAPMA to sulfolane is 1:14 under the experimental conditions of Example 1.

[0083] Example 6

[0084] This embodiment provides a method for preparing a single ion gel polymer electrolyte, and the preparation method is as follows:

[0085] 11.77g of 3-sulfonic acid propyl acrylate potassium salt was added to 20mL of dichloromethane, 1.4mL of N,N-dimethylformamide was added dropwise as a catalyst, magnetic stirring was carried out at room temperature for 0.5h, 20mL of oxalyl chloride (dissolved in 10mL) was added, and the reaction was carried out in an ice bath for 1h, and the temperature was further raised to room temperature and the reaction was carried out overnight. The mixture after the reaction was completed was added dropwise to ice water, extracted with 1,2-dichloroethane, washed with ice distilled water, dried over anhydrous magnesium sulfate, and concentrated by vacuum distillation to obtain a crude sulfonyl chloride product; 7.89g of benzenesulfonamide and 14mL of trimethylamine were dissolved in 20mL of 1,2-dichloroethane, and the obtained crude sulfonyl chloride product was dissolved in 15mL 1,2-dichloroethane was added dropwise to the mixed solution under ice bath conditions, reacted for 5 hours, trimethylamine salt was filtered off, the organic solvent was removed by reduced pressure distillation, 1,2-dichloroethane was added and washed with water four times, dried over anhydrous magnesium sulfate, and concentrated by reduced pressure distillation to obtain mono-ion trimethylamine salt; the mono-ion trimethylamine salt was dissolved in 20 mL of 1,4-dioxane, and added dropwise to a suspension of 1.51 g of lithium hydroxide in 1,4-dioxane under ice bath conditions, reacted for 3 hours, excess lithium hydroxide was filtered off, concentrated under reduced pressure, washed three times with n-hexane, and recrystallized from dichloromethane to obtain benzenesulfonyl imide mono-ion monomer (LiBSAPMA).

[0086] Under argon atmosphere, 0.1 g LiBSAPMA and 0.49 g N-methylacetamide were weighed in a molar ratio of 1:20, and magnetic stirring was performed to form a deep eutectic solvent. 0.005 g azobisisoheptanitrile was added and stirred thoroughly to dissolve the azobisisoheptanitrile. The mixed solution was dropped on the separator, and the obtained mixed solution was dropped on the separator between the negative electrode and the positive electrode, and heated to 80 ° C for 24 hours to completely polymerize the single ion monomer, that is, to obtain a single ion gel polymer electrolyte prepared by in situ polymerization, which has a thermal conductivity of 3.0×10 -5 S cm -1 ionic conductivity.

[0087] Example 7

[0088] This embodiment provides a method for preparing a single ion gel polymer electrolyte, and the preparation method is as follows:

[0089] 11.56 g of 3-sulfonic acid propyl methacrylate sodium salt was added to 20 mL of tetrahydrofuran, 1.4 mL of N, N-dimethylformamide was added dropwise as a catalyst, magnetically stirred at room temperature for 0.5 h, 20 mL of dichlorothionyl (dissolved in 10 mL) was added, and the reaction was carried out in an ice bath for 1 h, and the temperature was further raised to room temperature and the reaction was carried out overnight. The mixture after the reaction was completed was added dropwise to ice water, extracted with dichloromethane, washed with ice distilled water, dried over anhydrous magnesium sulfate, and concentrated by vacuum distillation to obtain a crude sulfonyl chloride product; 7.48 g of trifluoromethylsulfonamide and 20 mL of pyridine were dissolved in 20 mL of tetrahydrofuran, and the obtained crude sulfonyl chloride product was dissolved in 15 mL of tetrahydrofuran and added dropwise under ice bath conditions; Add to the above mixed solution, react for 5 hours, filter to remove the pyridinium salt, remove the organic solvent by distillation under reduced pressure, add dichloromethane and wash with water four times, dry over anhydrous magnesium sulfate, and concentrate by distillation under reduced pressure to obtain a monoionic pyridinium salt; dissolve the monoionic pyridinium salt in 20 mL of tetrahydrofuran, add dropwise to a tetrahydrofuran suspension of 2.32 g of lithium carbonate under ice bath conditions, react for 3 hours, filter to remove excess lithium carbonate, concentrate under reduced pressure, wash three times with n-hexane, and recrystallize from dichloromethane to obtain a trifluoromethylsulfonyl imide monoionic monomer (LiTFMSAPMA).

[0090] Under argon atmosphere, 0.27 g LiTFMSAPMA and 0.24 g N-methyltrifluoroacetamide were weighed in a molar ratio of 1:3, and stirred thoroughly to form a deep eutectic solvent. 0.001 g 4,4'-azobis(4-cyanovaleric acid) was added and stirred thoroughly to dissolve 4,4'-azobis(4-cyanovaleric acid). The obtained mixed solution was dropped on the separator between the negative electrode and the positive electrode, and heated to 60 ° C for 36 hours to completely polymerize the single ion monomer, thereby obtaining a single ion gel polymer electrolyte prepared by in situ polymerization, which has a carbonyl content of 3.5×10 -5 S cm -1 ionic conductivity.

[0091] Example 8

[0092] This embodiment provides a method for preparing a single ion gel polymer electrolyte, and the preparation method is as follows:

[0093] 10.95 g of 3-sulfonic acid propyl acrylate sodium salt was added to 20 mL of tetrahydrofuran, 1.4 mL of N, N-dimethylformamide was added dropwise as a catalyst, and magnetic stirring was carried out at room temperature for 0.5 h. 20 mL of dichlorothionyl (dissolved in 10 mL) was added, and the reaction was carried out in an ice bath for 1 h. The temperature was further raised to room temperature and the reaction was carried out overnight. The mixture after the reaction was completed was added dropwise to ice water, extracted with dichloromethane, washed with ice distilled water, dried over anhydrous magnesium sulfate, and concentrated by vacuum distillation to obtain a crude sulfonyl chloride product; 5.73 g of methylsulfonamide and 16 mL of pyrrolidine were dissolved in 20 mL of tetrahydrofuran, and the obtained crude sulfonyl chloride product was dissolved in 15 mL of tetrahydrofuran under ice bath conditions. The mixture was added dropwise to the above mixed solution, reacted for 5 h, the pyrrolidine salt was filtered off, the organic solvent was removed by distillation under reduced pressure, dichloromethane was added and washed with water four times, dried over anhydrous magnesium sulfate, and concentrated by distillation under reduced pressure to obtain a monoionic pyrrolidine salt; the monoionic pyrrolidine salt was dissolved in 20 mL of tetrahydrofuran, and added dropwise to a tetrahydrofuran suspension of 0.5 g of lithium hydride under ice bath conditions, reacted for 3 h, the excess lithium hydride was removed by filtration, concentrated under reduced pressure, washed three times with n-hexane, and recrystallized from dichloromethane to obtain a monoionic methylsulfonyl imide monomer (LiMSAPMA).

[0094] Under argon atmosphere, 0.1 g LiMSAPMA and 2.39 g N-methylacetamide were weighed in a molar ratio of 1:80, stirred thoroughly to form a deep eutectic solvent, 0.003 g 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile) was added, and stirred thoroughly to dissolve 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile); the obtained mixed solution was dropped on the separator between the negative electrode and the positive electrode, heated to 70 ° C for 30 hours to completely polymerize the single ion monomer, and a single ion gel polymer electrolyte prepared by in situ polymerization was obtained, which had a thermal conductivity of 3.1×10 -5 S cm -1 ionic conductivity.

[0095] Example 9

[0096] 10.95 g of 3-sulfonic acid propyl acrylate sodium salt was added to 20 mL of tetrahydrofuran, and 1.4 mL of N, N-dimethylformamide was added dropwise as a catalyst. The mixture was stirred magnetically at room temperature for 0.5 h, and 20 mL of dichlorothionyl (dissolved in 10 mL) was added. The mixture was reacted in an ice bath for 1 h, and then the temperature was further raised to room temperature and the reaction was allowed to proceed overnight. The mixture after the reaction was completed was added dropwise to ice water, extracted with dichloromethane, washed with ice distilled water, dried over anhydrous magnesium sulfate, and concentrated by vacuum distillation to obtain a crude sulfonyl chloride product. 11.30 g of trifluoromethylbenzenesulfonamide and 10 mL of bipyridine were dissolved in 20 mL of tetrahydrofuran, and the obtained crude sulfonyl chloride product was dissolved in 15 mL of tetrahydrofuran and added dropwise under ice bath conditions. Add to the above mixed solution, react for 5 hours, filter to remove the bipyridyl salt, remove the organic solvent by vacuum distillation, add dichloromethane and wash with water four times, dry over anhydrous magnesium sulfate, and concentrate by vacuum distillation to obtain a monoionic bipyridyl salt; dissolve the monoionic bipyridyl salt in 20 mL of tetrahydrofuran, add dropwise to a tetrahydrofuran suspension of 0.5 g of lithium hydride under ice bath conditions, react for 3 hours, filter to remove excess lithium hydride, concentrate under reduced pressure, wash three times with n-hexane, and recrystallize from dichloromethane to obtain a trifluoromethylbenzenesulfonyl imide monoionic monomer (LiTFBSAPMA).

[0097] Under argon atmosphere, 0.1 g LiTFBSAPMA and 0.41 g N-methylacetamide were weighed in a molar ratio of 1:20, stirred thoroughly to form a deep eutectic solvent, 0.004 g azobisisobutyronitrile was added, and stirred thoroughly to dissolve the azobisisobutyronitrile; the obtained mixed solution was dropped on the separator between the negative electrode and the positive electrode, heated to 70 ° C for 30 hours to completely polymerize the single ion monomer, and a single ion gel polymer electrolyte prepared by in situ polymerization was obtained. The electrolyte has a thermal conductivity of 2.9×10 -5 Scm -1 ionic conductivity.

[0098] Example 10

[0099] 12.38g of 3-sulfonic acid propyl methacrylate potassium salt was added to 20mL of tetrahydrofuran, 1.4mL of N,N-dimethylformamide was added dropwise as a catalyst, magnetically stirred at room temperature for 0.5h, 20mL of dichlorothionyl (dissolved in 10mL) was added, and the reaction was carried out in an ice bath for 1h, and the temperature was further raised to room temperature and the reaction was carried out overnight. The mixture after the reaction was added dropwise to ice water, extracted with dichloromethane, washed with ice distilled water, dried over anhydrous magnesium sulfate, and concentrated by vacuum distillation to obtain a crude sulfonyl chloride product; 12.11g of trifluoromethoxybenzenesulfonamide and 15mL of triethylamine were dissolved in 20mL of tetrahydrofuran, and the obtained crude sulfonyl chloride product was dissolved in 15mL of tetrahydrofuran and added dropwise under ice bath conditions. Add to the above mixed solution, react for 5 hours, filter to remove triethylamine salt, remove organic solvent by vacuum distillation, add dichloromethane and wash with water four times, dry over anhydrous magnesium sulfate, and concentrate by vacuum distillation to obtain monoionic triethylamine salt; dissolve the monoionic triethylamine salt in 20 mL of tetrahydrofuran, add dropwise to a tetrahydrofuran suspension of 0.5 g of lithium hydride under ice bath conditions, react for 3 hours, filter to remove excess lithium hydride, concentrate under reduced pressure, wash three times with n-hexane, and recrystallize from dichloromethane to obtain trifluoromethoxybenzenesulfonyl imide monoionic monomer (LiTFOBSAPMA).

[0100] Under argon atmosphere, 0.1 g LiTFOBSAPMA and 0.3 g cyclopentane sulfone were weighed in a molar ratio of 1:11, stirred thoroughly to form a deep eutectic solvent, 0.003 g azobisisobutyronitrile was added, stirred thoroughly to dissolve the azobisisobutyronitrile; the obtained mixed solution was dropped on the separator between the negative electrode and the positive electrode, heated to 60 ° C for 32 hours to completely polymerize the single ion monomer, and a single ion gel polymer electrolyte prepared by in situ polymerization was obtained. The electrolyte has a thermal conductivity of 3.3×10 -5 S cm -1 ionic conductivity.

[0101] Embodiment 11

[0102] 12.38g of 3-sulfonic acid propyl methacrylate potassium salt was added to 20mL of tetrahydrofuran, 1.4mL of N,N-dimethylformamide was added dropwise as a catalyst, and magnetic stirring was carried out at room temperature for 0.5h. 20mL of dichlorothionyl (dissolved in 10mL) was added, and the reaction was carried out in an ice bath for 1h. The temperature was further raised to room temperature and the reaction was carried out overnight. The mixture after the reaction was completed was added dropwise to ice water, extracted with dichloromethane, washed with ice distilled water, dried over anhydrous magnesium sulfate, and concentrated by vacuum distillation to obtain a crude sulfonyl chloride product; 12.11g of nitrobenzenesulfonamide and 15mL of triethylamine were dissolved in 20mL of tetrahydrofuran, and the obtained crude sulfonyl chloride product was dissolved in 15mL of tetrahydrofuran under ice bath conditions. The mixture was added dropwise to the above mixed solution, reacted for 5 h, the triethylamine salt was filtered off, the organic solvent was removed by distillation under reduced pressure, dichloromethane was added and washed with water four times, dried over anhydrous magnesium sulfate, and concentrated by distillation under reduced pressure to obtain a monoionic triethylamine salt; the monoionic triethylamine salt was dissolved in 20 mL of tetrahydrofuran, and added dropwise to a tetrahydrofuran suspension of 0.5 g of lithium hydride under ice bath conditions, reacted for 3 h, the excess lithium hydride was removed by filtration, concentrated under reduced pressure, washed three times with n-hexane, and recrystallized from dichloromethane to obtain a nitrobenzenesulfonyl imide monoionic monomer (LiNBSAPMA).

[0103] Under argon atmosphere, 0.1 g LiNBSAPMA and 0.32 g cyclopentane sulfone were weighed in a molar ratio of 1:8, stirred thoroughly to form a deep eutectic solvent, 0.003 g azobisisobutyronitrile was added, stirred thoroughly to dissolve the azobisisobutyronitrile; the obtained mixed solution was dropped on the separator between the negative electrode and the positive electrode, heated to 70 ° C for 30 hours to completely polymerize the single ion monomer, and a single ion gel polymer electrolyte prepared by in situ polymerization was obtained. The electrolyte has a thermal conductivity of 2.8×10 -5 S cm -1 ionic conductivity.

[0104] Example 12

[0105] 12.38 g of 3-sulfonic acid propyl methacrylate potassium salt was added to 20 mL of tetrahydrofuran, 1.4 mL of N, N-dimethylformamide was added dropwise as a catalyst, magnetically stirred at room temperature for 0.5 h, 20 mL of dichlorothionyl (dissolved in 10 mL) was added, and the reaction was carried out in an ice bath for 1 h, and the temperature was further raised to room temperature and the reaction was carried out overnight. The mixture after the reaction was completed was added dropwise to ice water, extracted with dichloromethane, washed with ice distilled water, dried over anhydrous magnesium sulfate, and concentrated by vacuum distillation to obtain a crude sulfonyl chloride product; 7.48 g of trifluoromethylsulfonamide and 15 mL of triethylamine were dissolved in 20 mL of tetrahydrofuran, and the obtained crude sulfonyl chloride product was dissolved in 15 mL of tetrahydrofuran and added dropwise under ice bath conditions; Add to the above mixed solution, react for 5 hours, filter to remove triethylamine salt, remove organic solvent by vacuum distillation, add dichloromethane and wash with water four times, dry over anhydrous magnesium sulfate, and concentrate by vacuum distillation to obtain monoionic triethylamine salt; dissolve the monoionic triethylamine salt in 20 mL of tetrahydrofuran, add dropwise to a tetrahydrofuran suspension of 0.5 g of lithium hydride under ice bath conditions, react for 3 hours, filter to remove excess lithium hydride, concentrate under reduced pressure, wash three times with n-hexane, and recrystallize from dichloromethane to obtain trifluoromethylsulfonyl imide monoionic monomer (LiTFSAPMA).

[0106] Under argon atmosphere, 0.02 g LiTFSAPMA and 0.56 g cyclopentane sulfone were weighed in a molar ratio of 1:80, stirred thoroughly to form a deep eutectic solvent, 0.001 g azobisisobutyronitrile was added, and stirred thoroughly to dissolve the azobisisobutyronitrile; the obtained mixed solution was dropped on the separator between the negative electrode and the positive electrode, heated to 70 ° C for 30 hours to completely polymerize the single ion monomer, and a single ion gel polymer electrolyte prepared by in situ polymerization was obtained. The electrolyte has a thermal conductivity of 5.1×10 -6 S cm -1 ionic conductivity.

[0107] The single-ion gel polymer electrolyte prepared by in-situ polymerization in the embodiment has a higher lithium ion migration number than the traditional polymer electrolyte, and compared with the previous single-ion polymer electrolyte, the interface contact and conductivity are improved.

[0108] Comparative Example 1

[0109] The other conditions are the same as those in Example 1, except that the Lewis base is replaced by succinonitrile. The experiment first mixed the cyano monoion monomer (LiCSAPMA) and succinonitrile and stirred for 12 hours, and it was found that a uniform and transparent deep eutectic solvent could not be obtained; then it was heated to 80°C and stirred vigorously for 0.5 hours to obtain a milky white turbid liquid, but after the temperature dropped to room temperature, it solidified into a white opaque solid, indicating that succinonitrile and the cyano monoion monomer could not form a deep eutectic solvent.

[0110] Comparative Example 2

[0111] The other conditions are the same as those in Example 1, except that the Lewis base is replaced by 18-crown-6 ether. The experiment first mixes the cyano monoion monomer (LiCSAPMA) and 18-crown-6 ether and stirs for 12 hours, and it is found that a uniform and transparent deep eutectic solvent cannot be obtained; then, it is heated to 80°C and stirred vigorously for 0.5 hours to obtain a uniform and transparent liquid, but after the temperature drops to room temperature, it solidifies into a white opaque solid, indicating that 18-crown-6 ether and the cyano monoion monomer cannot form a deep eutectic solvent.

[0112] It will be easily understood by those skilled in the art that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a single ion gel polymer electrolyte, characterized in that: The steps include: (1) 3-sulfonyl propyl acrylate metal salt or 3-sulfonyl propyl methacrylate metal salt is used as a raw material, firstly subjected to sulfonylation treatment to obtain a crude sulfonyl chloride product, then the crude product is reacted with an acid binding agent and an amine under an organic solvent to obtain a sulfonimide salt, and finally the sulfonimide salt is reacted with a lithium-containing alkaline solution to obtain a monoionic monomer; step (1) comprises the following sub-steps: (1-1) Dispersing 3-sulfopropyl acrylate metal salt or 3-sulfopropyl methacrylate metal salt in an organic solvent to N,N -dimethylformamide is used as a catalyst, and a sulfonylating agent dissolved in an organic solvent is added dropwise under ice bath conditions, and then the reaction is transferred to room temperature after ice bathing. After the reaction is completed, a crude sulfonyl chloride product is obtained; (1-2) mixing the crude sulfonyl chloride product with an acid-binding agent, an amine and an organic solvent, first reacting in an ice bath, then reacting at room temperature, and obtaining a sulfonyl imide salt after the reaction is completed; (1-3) dissolving the sulfonyl imide salt obtained in step (1-2) in an organic solvent, and then slowly adding it to a lithium-containing alkaline solution under ice bath conditions to react, removing excess alkali and organic solvent after the reaction, and purifying to obtain the single ion monomer; (2) mixing and stirring the single ion monomer obtained in step (1) and the Lewis base to form a uniform and transparent deep eutectic solvent; and then mixing the deep eutectic solvent with an initiator to obtain a mixed precursor solution; (3) Adding the mixed precursor solution obtained in step (2) to the separator, allowing the mixed precursor solution to infiltrate the separator, and heating to induce polymerization of the single-ion monomers infiltrated in the separator to obtain a single-ion gel polymer electrolyte.

2. The preparation method according to claim 1, characterized in that The raw materials in step (1) are one or more of 3-sulfonate propyl acrylate sodium salt, 3-sulfonate propyl acrylate potassium salt, 3-sulfonate propyl methacrylate sodium salt, and 3-sulfonate propyl methacrylate potassium salt.

3. The preparation method according to claim 1, characterized in that: The Lewis base in step (2) is sulfolane, N -methylacetamide and N -One or more of methyltrifluoroacetamide; The initiator is one of azobisisobutyronitrile, azobisisoheptanenitrile, 4,4'-azobis(4-cyanovaleric acid) and 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile).

4. The preparation method according to claim 1, characterized in that: The membrane in step (3) is a cellulose membrane or a polyolefin membrane.

5. The preparation method according to claim 1, characterized in that: The organic solvent is one or more of dichloromethane, tetrahydrofuran, 1,4-dioxane and 1,2-dichloroethane; The sulfonylating agent is one or more of thionyl chloride and oxalyl chloride; The acid binding agent is one or more of triethylamine, trimethylamine, pyridine, pyrrolidine and bipyridine; The amine is one or more of cyanamide, trifluoromethylsulfonamide, methylsulfonamide, trifluoromethoxybenzenesulfonamide, benzenesulfonamide, nitrobenzenesulfonamide and trifluoromethylbenzenesulfonamide; The lithium-containing base is one or more of lithium carbonate, lithium hydroxide and lithium hydride.

6. The preparation method according to claim 1, characterized in that: In step (2), the molar ratio of the monoionic monomer to the Lewis base is 1:3 to 1:80; and the mass ratio of the monoionic monomer to the initiator is 100:0.5 to 100:

5.

7. The preparation method according to claim 1, characterized in that: Step (2) mixing the monoionic monomer obtained in step (1) and the Lewis base, heating the mixture to 60-80° C., and stirring the mixture to form a deep eutectic solvent; The heating in step (3) triggers the polymerization reaction of the monoionic monomers infiltrated in the diaphragm, and the heating temperature is 60° C. to 80° C.; the polymerization reaction time is 12 hours to 48 hours.

8. The single ion gel polymer electrolyte prepared by the preparation method according to any one of claims 1 to 7.

9. Use of the polymer electrolyte according to claim 8, characterized in that: Used as polymer electrolyte for lithium-ion batteries.

Citation Information

Cited By

  • A modified pole piece for energy storage, a polymer battery and a preparation method thereof

    CN122868442A