Nanocellulose dispersion compositions containing carbon black for tire applications
By adding a separator during the drying process of nanocellulose, the problem of poor dispersion in polymer is solved, and good dispersion and performance improvement in tire preparations are achieved, the fatigue life of the material is extended and the hysteresis and heat accumulation are reduced. .
Patent Information
- Application Number
- CN202180015844.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-02-19
- Filing Date
- 2021-02-18
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2041-02-18
AI Technical Summary
The poor dispersion of nanocellulose in hydrophobic, non-polar solvents and substrates leads to the formation of large nanocellulose aggregates in the polymer composite structure, affecting the performance and sustainability of the material.
During or before the nanocellulose drying process, the addition of separators such as carbon black fillers, elastomer latex or wax prevents the binding between the nanocellulose crystals and the fibrils, thereby forming a nanocellulose dispersion composition, improving its in-depth analysis of the nanocellulose sequential tissues. Dispersibility in polymers.
The good dispersion of nanocellulose in tire preparations is achieved, the performance of polymer composites is improved, the fatigue life is extended, and the hysteresis and heat accumulation is reduced.
Smart Images

Figure GDA0004979874110000231 
Figure GDA0004979874110000241 
Figure GDA0004979874110000251
Abstract
Description
[0001] Citation of Related Applications
[0002] This application was filed as a PCT international application on February 18, 2021, and claims priority to U.S. Provisional Application No. 62 / 978,397 filed on February 19, 2020, the disclosure of which is incorporated herein by reference in its entirety. Technical Field
[0003] The present invention relates to nanocellulose dispersion compositions for use in polymer formulations, and more particularly, nanocellulose dispersion compositions for use in elastomer formulations intended for tire applications. Background Art
[0004] Recently, as the nano material with many different potential uses (such as in plastics and elastomers), nano cellulose has received much attention. The use of nano cellulose in these applications is intended to improve the performance of the resulting composite material and the sustainability of the material in the future, because nano cellulose is derived from biomass rather than hydrocarbon materials. However, a problem of nano cellulose is its dispersibility in hydrophobicity, non-polar solvents and matrix (comprising plastics and elastomers), no matter nano cellulose is crystalline form or fibril form, usually in drying process, nano cellulose is combined with itself, thereby produces large nano cellulose aggregates in polymer composite structures.
[0005] For example, when mixing nanocellulose in an elastomeric compound, good dispersion of the nanocellulose is desired so that large aggregates are eliminated and the full benefit of incorporating the nanocellulose into the elastomeric matrix is achieved. Large aggregates can lead to stress concentrators that can cause premature failure of the polymer composite.
[0006] Therefore, it has become important to devise methods to greatly improve the dispersibility of nanocellulose in polymer formulations, which remains a key issue facing the development, growth and commercialization of nanocellulose in tires and other end-use applications. It is to these ends that the present invention is generally directed. Summary of the invention
[0007] This summary is provided to introduce a selection of concepts in a simplified form that are further described in the detailed description below. This summary is not intended to identify required or essential features of the claimed subject matter. This summary is also not intended to be used to limit the scope of the claimed subject matter.
[0008] In accordance with the purposes of the present invention, as specifically demonstrated and broadly described herein, in one aspect, the present invention relates to a method of adding a separator during or prior to the drying of nanocellulose so that the separator remains intact and prevents the nanocellulose crystals and nanocellulose fibrils from bonding to each other. The result is a nanocellulose dispersion composition that can be easily dispersed in tire formulations, such as in elastomers and plastics, for use in tires and other end-use applications.
[0009] Nanocellulose dispersion compositions (NDCs) are described herein and the NDCs may include (i) a separator including a carbon black filler, an elastomer latex, a wax, or any combination thereof, and (ii) nanocellulose. Such NDCs may be used in tire compositions, whereby the tire compositions may include (I) a polymer, (II) any of the nanocellulose dispersion compositions disclosed herein, and (III) a carbon black additive. In some aspects, the tire compositions may be characterized by a dispersion index of at least about 90% as measured by interferometric microscopy (IFM), while in other aspects, the tire compositions may be characterized by a fatigue life of at least about 300,000 cycles at 100% tensile strain. The tire compositions disclosed herein may be used to produce a variety of articles, such as tires for passenger vehicles as well as trucks and buses.
[0010] The preceding summary and the following detailed description all provide examples and are illustrative only. Therefore, the preceding summary and the following detailed description should not be considered as restrictive. In addition, in addition to those features or variants set forth herein, features or variants may also be provided. For example, certain aspects and embodiments may relate to the various feature combinations and sub-combinations described in the detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0011] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate several aspects and, together with the description, serve to explain certain principles of the invention.
[0012] Figure 1A and 1B Backscattered and secondary scanning electron microscope (SEM) images of a model passenger tire tread compound compounded using reference carbon black grade N234, respectively. Figure 1A and 1B The scale is the same (scale bar = 300 μm).
[0013] Figure 2A and 2B Backscattered and secondary SEM images, respectively, of the size dispersion of Example 2 according to various aspects of the present invention, wherein a portion of the carbon black was replaced by dried lignin coated nanocellulose fibrils (LCNF). Figure 2A and 2B The scale is the same (scale bar = 300 μm).
[0014] Figure 3A and 3B Backscattered and secondary SEM images, respectively, of the size dispersion of Example 3 according to various aspects of the present invention, wherein a portion of the carbon black was replaced by LCNFs as part of a nanocellulose dispersion composition (NDC) containing LCNFs, surface modified carbon black (SMCB) and TDAE oil. Figure 3A and 3B The scale is the same (scale bar = 300 μm).
[0015] Figure 4A and 4B ] are backscattered and secondary SEM images, respectively, of the model truck tire tread compound dispersion of Example 4 according to various aspects of the present invention. Figure 4A and 4B The scale is the same (scale bar = 300 μm).
[0016] Figure 5A and 5B Backscattered and secondary SEM images, respectively, of the size dispersion of Example 5 according to various aspects of the present invention, wherein a portion of the carbon black was replaced by dry LCNFs. Figure 5A and 5B The scale is the same (scale bar = 300 μm).
[0017] Fig. 6A and 6B Backscattered and secondary SEM images, respectively, of the rubber dispersion of Example 6 according to various aspects of the present invention, wherein a portion of the carbon black was replaced by LCNFs as part of the NDC containing LCNFs and natural rubber latex. Fig. 6A and 6B The scale is the same (scale bar = 300 μm).
[0018] Fig. 7A and 7B 7C and 7C are backscattered SEM images (scrape cut surface with the grain) at 100 μm, 40 μm and 10 μm scales, respectively, of the size dispersion of Example 11 according to various aspects of the present invention, wherein a portion of the carbon black is replaced by LCNFs as part of a nanocellulose dispersion composition (NDC) containing LCNFs, surface modified carbon black (SMCB) and TDAE oil.
[0019] Fig. 8A and 8B100 μm and 40 μm scale backscattered SEM images of the size dispersion (scrape cut against the grain / against the grain) of Example 11 according to various aspects of the present invention, respectively, wherein a portion of the carbon black is replaced by LCNFs as part of a nanocellulose dispersion composition (NDC) containing LCNFs, surface modified carbon black (SMCB) and TDAE oil.
[0020] Figure 9-12 Bar graphs summarizing the MDR T90 cure time, Mooney T5 scorch time, Mooney viscosity, and Shore A hardness of the size dispersions of Examples 7-11, respectively.
[0021] Fig.13 is a bar graph summarizing the static modulus (with the grain) at 100%, 200% and 300% elongation for the size dispersions of Examples 7-11.
[0022] Fig.14 is a graph showing the change in tensile strength versus percent elongation for the size dispersions of Examples 7 and 11.
[0023] Fig.15 is a graph showing with-grain and against-grain grinding directions and with-grain and against-grain tensile testing.
[0024] Fig.16 is a bar graph summarizing the static modulus (with and against the grain) at 100%, 200% and 300% elongation for the size dispersions of Examples 7-11.
[0025] Fig.17 is a bar graph summarizing the mechanical anisotropy of the size dispersions of Examples 7-11 at 100%, 200% and 300% elongation.
[0026] Figure 18-20 Bar graphs summarizing the tensile strength (with and against the grain), elongation at break, and critical tear strength of the size dispersions of Examples 7-11, respectively.
[0027] Figure 21-25 The DIN wear, rebound at 60°C, interferometer heat accumulation, tan δ at 60°C of the rubber dispersions of Examples 7-11 are summarized respectively. 最大 and ΔG' at 60 °C.
[0028] Other aspects of the invention will be described in part in the following description, and will be apparent in part from the description, or may be learned through the practice of the invention. The advantages of the invention will be realized and achieved by means of the elements and combinations specifically pointed out in the appended claims. It should be understood that the foregoing general description and the following detailed description are merely exemplary and illustrative, and are not restrictive of the claimed invention. DETAILED DESCRIPTION
[0029] The present invention may be understood more readily by reference to the following detailed description of the invention and the Examples included therein.
[0030] Before disclosing and describing the compounds, compositions, articles, systems, devices and / or methods of the present invention, it should be understood that, unless otherwise stated, they are not limited to specific synthetic methods, or, unless otherwise stated, are not limited to specific reagents, and therefore can certainly vary. It should also be understood that the terms used herein are only for the purpose of describing specific aspects and are not intended to be limiting. Although any methods and materials similar or comparable to those described herein can be used in the practice or testing of the present invention, exemplary and representative methods and materials are now described.
[0031] All publications mentioned herein are incorporated herein by reference to disclose and describe the methods and / or materials in connection with which the publications are cited.
[0032] Unless defined otherwise, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention belongs.
[0033] The testing method used herein is known and understood by those skilled in the art. Where appropriate, reference is provided to specific testing methods. For example, using ASTM D2663, the dispersion (Standard Test Methods for Carbon Black-Dispersion in Rubber) in the standard test method of carbon black-rubber, method D carries out interferometric microscopic analysis (IFM) (for example, to measure the dispersion index and the area fraction of undispersed material-filler such as carbon black and nanocellulose).
[0034] As used herein, the singular forms "a", "an", and "the" include plural alternatives unless expressly stated to the contrary. Thus, for example, reference to "a polymer" or "a separator" includes a mixture or combination of two or more polymers or separators, respectively, unless otherwise stated.
[0035] Although compositions and methods are described herein in terms of "comprising" various components or steps, unless otherwise specified, these compositions and methods may also "consist essentially of" or "consist of" various components or steps. For example, a nanocellulose dispersion composition (NDC) consistent with aspects of the present invention may include (i) a separator and (ii) nanocellulose; alternatively, may consist essentially of (i) a separator and (ii) nanocellulose; or alternatively, may consist of (i) a separator and (ii) nanocellulose.
[0036] Ranges can be expressed herein as from "about" a particular value and / or to "about" another particular value. When such a range is expressed, another aspect includes from a particular value and / or to another particular value. Similarly, when a value is expressed as an approximation by using the antecedent "about", it is understood that the particular value forms another aspect. It is further understood that the endpoints of each range are meaningful relative to the other endpoint and are independent of the other endpoint. It is also understood that there are a large number of values disclosed herein, and in addition to the value itself, each value is also disclosed herein as "about" the particular value. For example, if the value "10" is disclosed, "about 10" is also disclosed. It is also understood that each unit between two specific units is also disclosed. For example, if 10 and 15 are disclosed, 11, 12, 13 and 14 are also disclosed.
[0037] As used herein, the terms "optional" and "optionally" mean that the subsequently described event or circumstance may or may not occur, and that the description includes instances where said event or circumstance occurs and instances where it does not occur.
[0038] Components used in methods for preparing compositions of the present invention and the compositions themselves are disclosed. These and other materials are disclosed herein, and it should be understood that when combinations, subsets, interactions, groups, etc. of these materials are disclosed, although it is not possible to explicitly disclose specific references to various individual and collective combinations and arrangements of these compounds, each is specifically considered and described herein. For example, if a specific compound is disclosed and discussed, and many modifications that can be made to many molecules including the compound are discussed, then unless there is a clear statement to the contrary, each and every combination and arrangement of the compound and possible modifications are specifically considered. Therefore, if a class of molecules A, B and C and a class of molecules D, E and F are disclosed, and an example of a combined molecule AD is disclosed, then even if each is not listed individually, each is considered individually and collectively, meaning that combinations AE, AF, BD, BE, BF, CD, CE and CF are considered to be disclosed. Similarly, any subset or combination of these is also disclosed. Therefore, for example, it will be considered that a subgroup of AE, BF and CE is disclosed. This conception applies to all aspects of the present application, including but not limited to steps in the method for preparing and using the composition of the present invention. Thus, if there are a variety of additional steps that can be performed it is understood that each of these additional steps can be performed using any specific aspect or combination of aspects of the methods of the invention.
[0039] As briefly described above, the present invention provides a method for separating nanocellulose, as if the nanocellulose is present in an aqueous system in a single fibril or crystalline state, wherein a separator remains stable and is spaced between nanocellulose particles when dry to prevent binding-and aggregation between individual nanocellulose fibrils and / or crystals. In one aspect, the present invention provides a method for separating nanocellulose, and in another aspect, the present invention provides a nanocellulose composition compatible with a variety of polymers and elastomeric compounds to improve the nanocellulose dispersion in these polymers and elastomeric compounds so that the full benefits of nanocellulose addition can be achieved. For example, the benefits of the improved nanocellulose dispersion in the elastomeric material can include, but are not limited to, lower hysteresis or heat accumulation of the tire compound, lower compound weight and other performance characteristics for both tread and non-tread compounds, which may be important in terms of the overall performance of the tire.
[0040] It should be noted that nanocellulose of the present invention can include any nanocellulose, no matter it is crystalline form or fibril form, and whether it has been processed or modified in some other way.The source of nanocellulose can be any suitable source, no matter it is prepared by wood pulp or other biomass materials, and can be prepared by any industrial method.Biomass fiber is made up of cellulose structure constituent units, and it can be extracted industrially with various shapes and sizes, and this includes cellulose nanocrystals (NC) and cellulose nanofibrils (NF).In addition, the specific size and shape of nanocellulose can be in the scope of nanometer level until micrometer level (no matter in width and / or length).NF is typically of a size of 5-20nm width and 500-2000nm length, and contains amorphous domain and crystalline domain of cellulose.NC typically has a width of 5-8nm and a length of 100-300nm, and is mainly crystalline.Although these scopes and sizes are typical, the present invention encompasses all NC and NF materials, and has nothing to do with particle shape or particle size / size.
[0041] For nearly all non-aqueous applications in which nanocellulose is used, improving its dispersibility and therefore improving its practicality and benefit to these applications has been the major obstacle to implementing this technology. Therefore, improving dispersibility and finding economical and practical methods and techniques become important, and these methods and techniques make nanocellulose highly dispersible in polymers such as elastomeric compounds. Using a separator in or before the nanocellulose drying process itself (rather than post-processing technology) can help achieve this goal.
[0042] With regard to improving the dispersibility of nanocellulose, multiple chemical surface modification methods have been tried after drying, and although some methods may eventually succeed, these methods usually require extreme measures, which will prove to be difficult to expand to commercial scale, and are uneconomical. Usually, these methods are based on the freeze-drying (freeze drying) of nanocellulose, which is a mature laboratory method for preventing the irreversible interparticle binding of nanocellulose. Freeze drying is neither economical nor scalable for the commercial production of nanofibers.
[0043] Therefore, a simpler and more economical method is desired.Thus, a method is provided for separating nanocellulose before or during drying to prevent inter-nanocellulose bonding, thereby resulting in improved dispersion of nanocellulose in polymers such as plastics and elastomers.
[0044] Nanocellulose dispersion composition
[0045] Nanocellulose can be produced by, for example, decomposing biomass into submicron cellulose nanofibrils or nanocrystals using chemical means, mechanical means, or a combination of chemical and mechanical means. Other methods for providing nanocellulose, such as, for example, bacterial nanocellulose and membrane-nanocellulose, can also be used. Typically, the production of nanocellulose occurs in two main stages. The first stage is the purification of biomass to remove most of the non-cellulose components in the biomass, such as lignin, hemicellulose, extractives, and inorganic pollutants. This is typically accomplished by conventional pulping and bleaching. In order to produce cellulose nanofibrils, the second stage typically requires mechanical refining of the purified biomass fibers. For cellulose nanocrystals, the second stage typically requires acid hydrolysis of the purified fibers, followed by high shear mechanical treatment. New production processes such as the general Technology can be by using SO2 and ethanol (different degrees) to carry out chemical fractionation to biomass, then carry out mechanical treatment to produce cellulose nano crystals or cellulose nano fibrils.No matter what kind of nano cellulose, after the final mechanical treatment stage, nano cellulose is usually suspended in aqueous solution as stable gel to be higher than threshold concentration (typically greater than 2 % by weight solid).After drying and removing water, nano cellulose particles will usually be irreversibly combined and gathered, thereby causing the poor dispersibility in polymer system.
[0046] As described herein, in order to reduce or prevent the nanocellulose from self-binding during the drying process, a separator can be added to the aqueous nanocellulose dispersion, which separator will fully interact with the surface of the nanocellulose and / or be evenly distributed between the nanocellulose particles to reduce or prevent the aggregation of the nanocellulose.
[0047] A first method for separating nanocellulose in an aqueous system to improve dispersibility in a polymer may include (a) combining an aqueous dispersion of the nanocellulose with a separator to form a mixture, and (b) drying the mixture to form a nanocellulose dispersion composition (NDC). A second method for separating nanocellulose in an aqueous system using a separator may include (A) combining an aqueous dispersion of the nanocellulose with the separator to form a mixture, and (B) drying the mixture to form a nanocellulose dispersion composition (NDC). The separator may be stable in the NDC and may form a spacer between the nanocellulose particles to reduce or prevent the aggregation of the nanocellulose particles in the NDC. The present invention also encompasses a nanocellulose dispersion composition produced by any of the methods disclosed herein. The nanocellulose dispersion composition (NDC) may contain at least a separator and nanocellulose - and the separator may include a carbon black filler, an elastomer latex or a wax, and any combination of these materials.
[0048] In step (a) and step (A) of the first and second methods, an aqueous dispersion of nanocellulose can be combined with a separator to form a mixture. The aqueous dispersion of nanocellulose can contain any suitable amount of nanocellulose, but is typically at least about 2 wt % solids and up to 10 wt % solids (e.g., about 2 wt % to about 5 wt % solids).
[0049] Any suitable container and conditions can be used to combine the aqueous nanocellulose dispersion with the separator, and this can be done batchwise or continuously. As an example, the nanocellulose dispersion and separator can be combined at atmospheric pressure, optionally under stirring or mixing, and at any suitable temperature (generally in the range of about 15° C. to about 60° C.) in a suitable container (e.g., a tank).
[0050] There is no particular limitation on the amount of separator relative to nanocellulose used, but the weight ratio of separator to nanocellulose in the nanocellulose dispersion composition is generally in the range of about 0.1:1 to about 25:1. In some aspects, the weight ratio of separator to nanocellulose can fall within the range of about 0.1:1 to about 10:1, about 0.1:1 to about 5:1, about 0.1:1 to about 2:1, about 0.1:1 to about 1:1, about 0.25:1 to about 25:1, about 0.25:1 to about 15:1, about 0.3:1 to about 10:1, about 0.5:1 to about 25:1, about 0.7:1 to about 15:1, about 0.75:1 to about 15:1, about 1:1 to about 10:1, about 1.2:1 to about 12:1, about 1.8:1 to about 8:1, about 1.5:1 to about 10:1, about 1, 24: 1, 25: 1, 26: 1, 27: 1, 28: 1, 29: 1, 30: 1, 31: 1, 32: 1, 33: 1, 34: 1, 35: 1, 36: 1, 37: 1, 38: 1, 39: 20: 1, 40: 1, 41: 1, 42: 1, 43: 1, 44: 1, 45: 1, 46: 1, 47: 1, 48: 1, 49: 20: 1, 50: 1, 51: 1, 52: 1, 53: 1, 54: 1, 55: 1, 56: 1, 57: 1, 58: 1, 59: 22: 1, 60: 1, 61: 1, 62: 1, 63: 1, 64: 1, 65: 1
[0051] In aqueous nanocellulose dispersion or nanocellulose dispersion composition (NDC), the type of nanocellulose is not particularly limited either. In one aspect, for example, nanocellulose can include nanocellulose crystal (NC), nanocellulose fibril (NF) or a combination thereof. Nanocellulose can further contain lignin, as surface lignin and / or as the lignin contained in bulk particles. In another aspect, nanocellulose can include nanocellulose crystal (LCNC) coated with lignin, nanocellulose fibril (LCNF) coated with lignin or a combination thereof. Usually, the materials coated with these lignins are more hydrophobic. In yet another aspect, nanocellulose can include hydrophilic cellulose nanocellulose crystal (CNC), hydrophilic cellulose nanocellulose fibril (CNF) or a combination thereof.
[0052] Typically, suitable separators and polymers (for example, elastomers, tire formulations) are compatible and reduce the nanocellulose aggregation in the NDC, and reduce the aggregation in the polymer formulations.Usually, the separator in the nanocellulose dispersion composition, or the separator used to form the nanocellulose dispersion composition, can contain carbon black filler, elastomer latex, wax or their combination in any.Any suitable rubber latex can be used, and its illustrative examples can include but are not limited to natural rubber (NR), isoprene rubber (IR), emulsion polystyrene butadiene rubber (ESBR) etc.Can use mixture or the combination of two or more rubber latex materials.
[0053] The wax component may include, but is not limited to, non-branched paraffin wax, microcrystalline wax (natural mineral, petroleum-refined or lignin-refined) including branched paraffin wax and ozokerite wax, polyethylene wax, functionalized polyethylene wax, etc., or any combination thereof.
[0054] When present, the carbon black of the present invention may include any carbon black suitable for use with the NDC and / or elastomeric material employed. In one aspect, the carbon black may include furnace carbon black (or substantially consisting of or consisting of). Additionally or alternatively, the carbon black may include furnace carbon black (or substantially consisting of or consisting of) surface-modified, such as oxidized furnace carbon black. In other aspects, the carbon black may include carbon black suitable for rubber, such as for tires. In another aspect, the carbon black may include carbon black suitable for tire treads or tire carcasses. In various aspects, the carbon black may include N900 series carbon black, N800 series carbon black, N700 series carbon black, N600 series carbon black, N500 series carbon black, N400 series carbon black, N300 series carbon black, N200 series carbon black, N100 series carbon black, or mixtures thereof. The various physical properties of exemplary carbon blacks that may be used in the present invention are described below. It should be understood that these values and ranges are intended to be exemplary and the present invention is not limited to any specific range, value, or combination.
[0055] The nitrogen surface area of carbon black, as measured by, for example, ASTM method D6556-14, may be about 8 m 2 / g to about 140m 2 / g; about 20m 2 / g to about 140m 2 / g; about 45m 2 / g to about 140m 2 / g; about 60m 2 / g to about 140m 2 / g; about 90m 2 / g to about 140m 2 / g; about 95m 2 / g to about 135m 2 / g; about 100m 2 / g to about 130m 2 / g; about 105m 2 / g to about 125m 2 / g; about 110m 2 / g to about 125m 2 / g; about 115m 2 / g to about 125m 2 / g; about 110m 2 / g to about 120m 2 / g; about 115m 2 / g to about 120m 2 / g; about 115m 2 / g to about 121m 2 / g; or about 116m 2 / g to about 120m 2 In another aspect, the carbon black may have a nitrogen surface area of about 90, 92, 94, 96, 98, 100, 102, 104, 106, 108, 110, 112, 114, 116, 118, 120, 122, 124, 126, 128, 130, 132, 134, 136, 138, or 140 m 2 In another aspect, the carbon black may have a nitrogen surface area of about 8, 10, 12, 14, 16, 18, 20, 22, 24, 26, 28, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 80, 85, 90, 95, 100, 105, 110, 115, 120, 125, 130, 135, or 140 m2. 2 / g. In yet another aspect, the nitrogen surface area of the carbon black may be about 118 m 2In other aspects, the carbon blacks of the present invention may have a nitrogen surface area greater than or less than any value specifically recited herein, and the present invention is not intended to be limited to any particular nitrogen surface area value.
[0056] Based on the statistical thickness method (STSA, ASTM D6556-14), the external surface area of carbon black can be about 8 m 2 / g to about 125m 2 / g; about 20m 2 / g to about 125m 2 / g; about 45m 2 / g to about 125m 2 / g; about 60m 2 / g to about 125m 2 / g; about 80m 2 / g to about 125m 2 / g; about 85m 2 / g to about 120m 2 / g; about 90m 2 / g to about 115m 2 / g; about 95m 2 / g to about 110m 2 / g; about 95m 2 / g to about 105m 2 / g; about 98m 2 / g to about 104m 2 / g; or about 99m 2 / g to about 103m 2 / g. In another aspect, the external surface area of the carbon black can be about 101m 2 In another aspect, the carbon black can have an external surface area of about 8, 10, 12, 14, 16, 18, 20, 22, 24, 26, 28, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 80, 85, 90, 95, 100, 105, 110, 115, 120, or 125 m2 based on the statistical thickness method. 2 / g. In many aspects, the external surface area of carbon black is the specific surface area that the rubber compound can contact. In other aspects, the carbon black of the present invention can have an external surface area greater than or less than any value specifically set forth herein, and the present invention is not intended to be limited to any specific external surface area value.
[0057] The carbon black of the present invention (e.g., furnace carbon black) may have a pH of about 2.5 to about 9, about 2.5 to about 7, or about 4 to about 7, as measured by, for example, ASTM Method D1512-15, using Test Method A or Test Method B. In one aspect, the carbon black may be an oxidized carbon black, typically having a pH of about 2.5 to about 4; alternatively, about 2.8 to about 3.6; alternatively, about 3 to about 3.4; alternatively, about 3.2. In other aspects, the carbon black of the present invention may have a pH greater than or less than any value specifically set forth herein, and the present invention is not intended to be limited to any particular pH value.
[0058] The pore volume of the carbon black of the present invention may be about 55 cm 3 / 100g to about 67cm 3 / 100g(50GM); about 60cm 3 / 100g to about 65cm 3 / 100g(50GM); about 25cm 3 / 100g to about 60cm 3 / 100g; about 30cm 3 / 100g to 60cm 3 / 100g; about 35cm 3 / 100g to 60cm 3 / 100g; about 40cm 3 / 100g to 60cm 3 / 100g; about 45cm 3 / 100g to 60cm 3 / 100g; about 50cm 3 / 100g to about 60cm 3 / 100g(75GM); Approx. 53cm 3 / 100g to about 58cm 3 / 100g(75GM); about 45cm 3 / 100g to about 55cm 3 / 100g(100GM); or about 47cm 3 / 100g to about 53cm 3 / 100g (100GM). In another aspect, the 50GM pore volume of the carbon black may be about 62.2cm 3 / 100g; 75GM pore volume can be about 55.3cm 3 / 100g; and / or 100GM pore volume can be about 50.4cm 3In other aspects, the pore volume of the carbon black can be greater or less than any value specifically recited herein, and the present invention is not intended to be limited to any particular pore volume.
[0059] As measured by, for example, ASTM method D1509-15, the moisture content of the carbon black of the present invention can be from about 2.5 weight % to about 4.5 weight %; from about 3 weight % to about 4 weight %; or from about 3.2 weight % to about 3.8 weight %. In another aspect, the moisture content of the carbon black of the present invention can be about 3.5 weight %. It should be understood that, depending on, for example, environmental and / or storage conditions, the moisture content of the carbon black material can vary, and therefore, the specific moisture content of a given carbon black sample can vary. In other aspects, the carbon black of the present invention can have a moisture content greater than or less than any value specifically set forth herein, and the present invention is not intended to be limited to any specific moisture content value.
[0060] In one aspect, the carbon black of the present invention is an oxidized carbon black, such as an oxidized furnace black. There are a variety of methods to oxidize carbon black, such as, for example, ozonation, and if there are multiple desired oxygen-containing functional groups on the surface of the carbon black, the specific method for oxidizing the carbon black can vary. Typical oxygen-containing functional groups that can be present on the surface of the oxidized carbon black can include, for example, carboxyl, hydroxyl, phenol, lactone, aldehyde, ketone, quinone and hydroquinone groups. In many aspects, depending on the intensity and type of the oxidation treatment, the amount and type of functional groups present on the surface of the oxidized carbon black can vary. In one aspect, the carbon black has been oxidized by treatment with ozone.
[0061] The volatile content of the carbon black of the present invention can be from about 0.5% by weight to about 6.5% by weight; from about 1% by weight to about 6.5% by weight; from about 1.5% by weight to about 6.5% by weight; from about 2% by weight to about 6.5% by weight; from about 2.5% by weight to about 6.5% by weight; from about 3% by weight to about 6.5% by weight; from about 3.5% by weight to about 6.5% by weight; from about 4% by weight to about 6.5% by weight; from about 4.5% by weight to about 6.5% by weight; from about 5% by weight to about 6% by weight; or from about 5.2% by weight to about 5.8% by weight. In another aspect, the volatile content of the carbon black of the present invention can be at least about 4.5% by weight, at least about 5% by weight, at least about 5.5% by weight or more. In another aspect, the volatile content of the carbon black of the present invention can be about 5.5% by weight. In yet another aspect, the volatile content of the carbon black can be greater than or less than any value specifically set forth herein, and the present invention is not intended to be limited to any particular volatile content value.
[0062] The oxygen content of the carbon black of the present invention can be from about 0.25% by weight to about 5.5% by weight; from about 0.5% by weight to about 5.5% by weight; from about 1% by weight to about 5.5% by weight; from about 1.5% by weight to about 5.5% by weight; from about 2% by weight to about 5.5% by weight; from about 2.5% by weight to about 5.5% by weight; from about 3% by weight to about 5% by weight; from about 3.5% by weight to about 4.5% by weight; or from about 3.7% by weight to about 4.3% by weight. In another aspect, the oxygen content of the carbon black of the present invention can be at least about 3.5% by weight, at least about 4% by weight or more. In another aspect, the oxygen content of the carbon black of the present invention can be about 4% by weight. In yet another aspect, the oxygen content of the carbon black can be greater than or less than any value specifically set forth herein, and the present invention is not intended to be limited to any particular oxygen content value.
[0063] Optionally, hydrocarbon oil can be used together with one or more separators. For example, in step (a) or step (A), the aqueous dispersion of nanocellulose can merge with one or more separators and hydrocarbon oil to form a mixture. In one aspect, hydrocarbon oil can include aliphatic hydrocarbons, and in another aspect, hydrocarbon oil can include aromatic hydrocarbons. However, in another aspect, hydrocarbon oil can include a mixture or a combination of aliphatic hydrocarbons and aromatic hydrocarbons. Any suitable aliphatic and / or aromatic hydrocarbons can be used, but it is beneficial that these hydrocarbons are liquid phases under the conditions that the aqueous dispersion of nanocellulose and separators merge. An illustrative and non-limiting example of a suitable hydrocarbon oil that can be used as a separator is distillate aromatic extract (TDAE) oil after processing.
[0064] Optionally, the aqueous nanocellulose dispersion, separator and optional hydrocarbon oil can be mixed under high shear to ensure uniform distribution of the individual components. High shear mixing techniques include, but are not limited to, homogenization, sigma blade mixing, rotor-stator mixing and static in-line mixing.
[0065] In the first and second method steps (b) and step (B), the mixture can be dried to form a nanocellulose dispersion composition (NDC). Any suitable equipment and drying techniques can be used. In one aspect, the aqueous mixture can be exposed to a suitable drying step to remove water. Drying techniques can include but are not limited to evaporation, spray drying, freeze drying, spin flash drying, high shear mixing, drying and drum drying. The nanocellulose dispersion composition of the gained - containing separator and nanocellulose - usually contains less than 1.5 weight % water / moisture.
[0066] During the drying step and in the dry state, one or more coupling chemicals may optionally be introduced into the NDC composition, for example to modify the surface of the nanocellulose and enable subsequent coupling of the cellulose surface to the rubber matrix during vulcanization of a rubber compound prepared using the NDC. Coupling agents are well known to those skilled in the art, and in various aspects may include monofunctional and / or difunctional silanes based on mercapto, alkoxy, vinyl, amino, and methacryloxy chemistry, including, for example, common difunctional sulfur-containing coupling silanes such as 3,3'-bis-(triethoxysilylpropyl)-tetrasulfide.
[0067] Advantageously, the nanocellulose dispersion composition (NDC) (which may comprise (i) a separator and (ii) nanocellulose) has excellent nanocellulose dispersibility in the polymer formulation as measured by interferometry microscopy (IFM) that is superior to the dispersibility of the nanocellulose in the absence of the separator, typically by more than 25% or more than 50%. For example, if the amount of undispersed material (based on area) of the nanocellulose via IFM in the absence of the separator is 12%, a 25% increase would be an area fraction of undispersed material of 9%, and a 50% increase would be an area fraction of undispersed material of 6%.
[0068] Tire composition and manufactured product
[0069] In some variations, the present invention also relates to and encompasses any composition, formulation, and manufactured article containing any nanocellulose dispersion composition disclosed herein (and its corresponding properties or characteristics, such as the relative amounts of separator and nanocellulose, the type of separator, and the type of nanocellulose, etc.). In a particular aspect of the present invention, a tire composition is disclosed, and in this regard, the tire composition may include any suitable polymer (one or more than one), any nanocellulose dispersion composition disclosed herein, and a carbon black additive. Tire compositions are generally referred to as tire formulations or tire rubbers, etc.
[0070] There is no particular limitation on the amount of nanocellulose dispersion composition used in the tire composition, but the weight ratio of polymer to nanocellulose dispersion composition (polymer:NDC) is generally about 100:1 to about 1:1, about 80:1, about 10:1, about 75:1 to about 2:1, about 60:1 to about 5:1, about 50:1 to about 1:1, about 40:1 to about 4:1, about 75:1 to about 25:1, about 90:1 to about 10:1, about 15:1 to about 20:1, about 10:1 to about 25:1, about 15:1 to about 20:1, about 10:1 to about 25:1, about 15:1 to about 25 ... 1, 8: 1, 6: 1, 4: 1, 2: 1, or 1: 1. In some aspects, the weight ratio of polymer: NDC can fall within the range of about 75: 1 to about 1.5: 1 or about 50: 1 to about 2: 1.
[0071] In one aspect, the polymer in the tire composition can include a thermoplastic polymer, while in another aspect, the polymer can include a thermosetting polymer. In another aspect, the polymer can include a single or any combination of epoxy resins, acrylics, esters, polyurethanes, silicones, and / or phenols. In yet another aspect, the polymer can include a single or any combination of polyethylene (e.g., ethylene homopolymers or ethylene-based copolymers), polypropylene, polybutylene terephthalate, acrylonitrile butadiene styrene (ABS), polyamides, polyimides, polystyrene, polycarbonates, ethylene-vinyl acetate (EVA) copolymers, and / or polyolefin-styrenes (e.g., ethylene-styrene).
[0072] In another aspect, the polymer used in the tire formulation / composition / compound may include any suitable rubber or elastomer (single or in any combination), and non-limiting examples may include natural rubber (NR), epoxidized natural rubber (ENR), synthetic cis-polyisoprene (IR), emulsion-polymerized styrene-butadiene rubber (ESBR), solution-polymerized styrene-butadiene rubber (SSBR), polybutadiene rubber (BR), butyl rubber (IIR / CIIR / BIIR), chloroprene rubber (CR), nitrile elastomer (NBR), hydrogenated nitrile elastomer (HNBR), carboxylated nitrile elastomer (XNBR), ethylene-propylene rubber (EPM / EPDM), fluoroelastomer (FPM / FKM), polyurethane rubber (AU / EU / PU), etc., and any combination of these.
[0073] There is no particular limitation on the total amount of carbon black present in the tire composition, but it is typically in the range of about 20 to about 150 phr. This includes any carbon black additives present in the formulation and any carbon black fillers present in the NDC. In one aspect, for example, the total amount of carbon black can be in the range of about 25 to about 125 phr, in another aspect in the range of about 30 to about 100 phr, in another aspect in the range of about 35 to about 85 phr, and in yet another aspect in the range of about 40 to about 80 phr. In other aspects, the total amount of carbon black can be in the range of any minimum carbon black content to any maximum carbon black content specifically recited herein, and the present invention is not intended to be limited to any particular phr amount of carbon black.
[0074] Equally, the total amount of the nanocellulose in the tire composition is not particularly limited, but typically in the scope of about 1 to about 15phr.In some respects, the amount of nanocellulose can be in the scope of about 1 to about 10phr, about 1 to about 8phr, about 1 to about 7phr or about 1 to about 6phr, and in other aspects, the amount of nanocellulose can be in the scope of about 2 to about 15phr, about 2 to about 10phr, about 2 to about 7.5phr or about 2 to about 5phr.In addition, the amount of nanocellulose can be in the scope of any minimum nanocellulose content to any maximum nanocellulose content specifically cited herein, and the present invention is not intended to be limited to the nanocellulose of any specific phr amount.
[0075] Similarly, the total amount of hydrocarbon oil (e.g., TDAE oil) present in the tire composition is not particularly limited, but is typically in the range of about 1 to about 15 phr. This includes any hydrocarbon oil present in the formulation as well as any hydrocarbon oil present in the NDC. In one aspect, for example, the total amount of hydrocarbon oil can be in the range of about 2 to about 12 phr, in another aspect in the range of about 2 to about 10 phr, in another aspect in the range of about 3 to about 9 phr, and in yet another aspect, in the range of about 4 to about 8 phr. In other aspects, the total amount of hydrocarbon oil can be in the range of any minimum hydrocarbon oil content to any maximum hydrocarbon oil content specifically recited herein, and the present invention is not intended to be limited to any particular phr amount of hydrocarbon oil such as TDAE.
[0076] Beneficially, the disclosed tire compositions - which contain a polymer such as a suitable rubber or elastomer, a nanocellulose dispersion composition (NDC) (which contains a partitioning agent and nanocellulose), and a carbon black additive - have excellent dispersibility of both the carbon black additive and the nanocellulose. In one aspect, for example, the tire compositions disclosed herein may be characterized in that the area fraction of undispersed material measured by interferometric microscopy (IFM) is less than or equal to about 8%, less than or equal to about 6%, less than or equal to about 4%, less than or equal to about 3%, or less than or equal to about 2%. Additionally or alternatively, the tire compositions disclosed herein may be characterized in that the dispersion index measured by interferometric microscopy (IFM) is at least about 90%, at least about 92%, at least about 93%, at least about 94%, at least about 95%, at least about 96%, at least about 97%, or at least about 98%.
[0077] Unexpectedly, tire compositions containing NDC have fatigue life values comparable to similar tire formulations without NDC. For example, the tire composition can be characterized by a fatigue life (ASTM D4482) at 100% tensile strain of at least about 300,000 cycles, at least about 325,000 cycles, at least about 350,000 cycles, at least about 375,000 cycles, or at least about 400,000 cycles.
[0078] In one aspect, at equivalent total filler loading, the tan δ of the disclosed tire compositions (containing nanocellulose via NDC) is 最大 The tan delta (at 60°C) may be less than or equal to that of an otherwise equivalent tire composition without NDC (or nanocellulose) 最大 On the other hand, the tan δ of the N234-based tire composition (50 phr N234) in which 10 phr N234 was replaced by LCNF 最大 The tan delta may be equivalent to that of an otherwise equivalent composition in which 10 phr of N234 is replaced by N660. 最大 For example, the tan δ of a tire composition with 40 phr N234 and 10 phr LCNF is 最大 The tan delta of an otherwise identical composition containing 40 phr N234 and 10 phr N660 can be 最大 similar, and both may have a lower tan δ than an otherwise equivalent composition containing 50 phr N234 最大 .
[0079] Articles may be formed from and / or may include tire formulations (tire compositions, tire compounds) of the present invention, and are accordingly encompassed herein. For example, articles that may include formulations of the present invention may include, but are not limited to, pneumatic tires, passenger tires, truck and bus radial (TBR) tires, or tire treads, etc. In one aspect, any of the compositions described herein may be used in one or more tire compounds. In various aspects, such tire compounds may be uncured elastomeric compounds or cured elastomeric compounds. In another aspect, any of the compositions described herein may be used in one or more parts of a tire, including, for example, tire treads, sidewalls, sub-treads, beads, inner liners, etc. In other aspects, such tires may include passenger tires, truck or bus radial tires, or any other tire suitable for containing compositions described herein. It should be understood that individual components of the compositions as described herein may be added to any elastomer formulation, in addition to or in place of any one or more conventional components of such formulations. It should also be understood that individual components of such compositions may interact with other components of conventional elastomer formulations.
[0080] Example
[0081] The present invention is further illustrated by the following examples, which are not to be construed in any way as limiting the scope of the invention. Various other aspects, embodiments, modifications and equivalents thereof may be proposed to one of ordinary skill in the art after reading the description herein without departing from the spirit of the present invention or the scope of the appended claims.
[0082] Furthermore, these examples should in no way limit the scope or limits of available spacers or available nanocellulose materials that can be used to prepare nanocellulose dispersion compositions for polymer formulations, and serve merely as examples for the purpose of demonstrating the concept of combining spacers and nanocellulose into highly dispersible NDCs.
[0083] The nanocellulose crystals or nanocellulose fibrils in these embodiments are prepared using the above The invention is produced by a process and a proprietary method that deposits lignin on the surface of fibrils or crystals to make them more hydrophobic and more compatible with polymers and elastomers.
[0084] In Example 1, a reference carbon black grade N234 was used to mix a model passenger tire tread compound. This compound was included as a reference to demonstrate typical carbon black dispersion levels. N234 constituted 100% of the filler in the compound, equivalent to 75 phr in the compound formulation. Tables 1-2 summarize representative compound formulations (values in phr) and details of the standard mixing procedure. Figure 1A and 1B As shown in the SEM photos, N234 carbon black has excellent dispersibility. Figure 1A is a backscattered electron image of the rubber surface cut by the scraper, and Figure 1B is a secondary electron image of the same area. Dispersion as quantified by interferometric microscopy (IFM) is typically in the range of 98% to 100% dispersion index with an area fraction of undispersed carbon black of 0.8%.
[0085] Example 2 was prepared using the same mixing procedure as Example 1; however, a small fraction (6.7 wt%) of N234 was replaced with dried lignin-coated nanocellulose fibrils (LCNF). LCNF accounted for 6.7 wt% of the total filler loading, which was equivalent to 5 phr in the size formulation. The remaining filler loading consisted of N234 (93.3 wt%), which was equivalent to 70 phr in the size formulation. Figure 2A and 2B The dispersion of nanocellulose is very poor, which is shown by backscattering ( Figure 2A ) and quadratic ( Figure 2B ) SEM imaging revealed large aggregates of nanocellulose fibrils throughout the cross section of the compound. The area fraction of undispersed material, as quantified by interferometric microscopy (IFM), was 9.11%.
[0086] Use the same procedure as Example 2 to produce Example 3.Replace the independent LCNF of adding drying in Example 2, Example 3 has used NDC, and it contains the LCNF processed as separator with surface-modified carbon black (SMCB, N234), and TDAE oil and natural rubber latex.The weight ratio of LCNF, SMCB, TDAE oil and NR latex is 1:1:1:1.By mixing the aqueous dispersion of nano-cellulose with SMCB, TDAE oil and NR latex, then carry out high shear homogenization and be dried to the water lower than 1.5 % by weight, to prepare NDC.The total loading of NDC is 20phr, makes the LCNF added in the final sizing compound be 6.7 % by weight of total filler loading, and this is equivalent to 5phr in the sizing compound formulation.
[0087] Figure 3A and 3B Shown is the nanocellulose dispersion obtained when LCNF / SMCB / TDAE / NR NDC is added to a rubber compound mixer. Figure 3A is a backscattered electron image of the rubber surface cut by the scraper, and Figure 3B is a secondary electron image of the same area. The area fraction of undispersed material is 2.78% (as quantified by IFM) and is Figure 2A and2B ) is a significant improvement, where there are fewer and smaller nanocellulose aggregates in the cross section. Dispersibility is similar to Example 1 ( Figure 1A and 1B ) is more similar to the N234 carbon black in which there are some undispersed areas.
[0088] In Example 4, a reference carbon black grade N234 was used to mix a model truck tire tread compound. This compound was included as a reference to demonstrate typical carbon black dispersion levels. N234 accounted for 100% of the filler in this compound, which is equivalent to 50 phr in the compound formulation. Tables 1 and 3 summarize representative compound formulations (values in phr) and detailed descriptions of the standard mixing procedure. Figure 4A and 4B As shown in the figure, N234 carbon black has excellent dispersibility. Figure 4A is a backscattered electron image of the rubber surface cut by the scraper, and Figure 4B is a secondary electron image of the same area. Dispersion as quantified by interferometric microscopy (IFM) is typically in the range of 98% to 100% dispersion index with an area fraction of undispersed carbon black of 0.15%.
[0089] Example 5 was produced using the same mixing procedure as Example 4; however, a small fraction (10 wt%) of N234 was replaced with dried lignin-coated nanocellulose fibrils (LCNF). LCNF accounted for 10 wt% of the total filler loading, which was equivalent to 5 phr in the size formulation. The remaining filler loading consisted of N234 (90 wt%), which was equivalent to 45 phr in the size formulation. Figure 5A and 5B The dispersion of nanocellulose was shown by backscattering ( Figure 5A ) and quadratic ( Figure 5B ) SEM imaging showed very poor dispersion, as evidenced by large aggregates of nanocellulose fibrils throughout the compound cross section. The area fraction of undispersed material, as quantified by interferometric microscopy (IFM), was 11.52%.
[0090] Example 6 was produced using the same mixing procedure as Example 1. Instead of adding dry, separate LCNFs as in Example 5, Example 6 used the same NDC as in Example 3. In this particular example, NR latex was used in the NDC because this is a common material in truck tread formulations; however, other latex elastomeric materials can be used. The weight ratio of LCNF, SMCB, TDAE oil, and NR was 1:1:1:1. The NDC was prepared in a similar manner to Example 3. The total loading of NDC was 20 phr, so that the LCNF added to the final compound was 10 wt% of the total filler loading, which is equivalent to 5 phr in the compound formulation. Fig. 6A and 6B Shown is the nanocellulose dispersion obtained when LCNF / SMCB / TDAE / NR NDC is added to a rubber compound. Fig. 6A is a backscattered electron image of the rubber surface cut by the scraper, and Figure 6B is a secondary electron image of the same area. The area fraction of undispersed material is 2.44% (quantified by IFM) and is Figure 5A and 5B ) is significantly improved. Note that the less undispersed area in this SEM cross section is Figure 5A and 5B The dispersion level of nanocellulose in this compound was similar to that in Example 4.
[0091] In Examples 7-11, model TBR (truck and bus radial) tire tread compounds were produced using reference carbon black grade N234 and with or without LCNF as summarized in Table 4. Example 7 is a reference formulation for demonstrating typical carbon black performance, and N234 constitutes 100% of the filler, which is equivalent to 50 phr in the compound formulation. Example 8 contains 2.5 phr less carbon black than Example 7, and Example 9 contains 5 phr less carbon black than Example 7. Examples 10-11 replace some of the carbon black with LCNF, but use the same NDC described in Examples 3 and 6. The LCNF amount is 2.5 phr in Example 10 and 5 phr in Example 11. The standard mixing procedure is summarized in Tables 5 and 6. Although Examples 7-11 utilize representative TBR tire tread formulations, the disclosed NDC can be incorporated into a variety of non-tread formulations (e.g., sidewall, subtread, bead / apex, etc.) using any suitable elastomer or elastomers.
[0092] Due to shear, LCNFs are typically aligned in the grinding direction, so the properties of polymer formulations and LCNF dispersions can vary based on direction (e.g., along or against the grain). Regarding the dispersion of carbon black, ASTM D3053 defines macroscopic dispersion as the degree of distribution of fillers in the rubber compound, typically a value of 2 μm to 100 μm. Macroscopic dispersion can be analyzed by IFM (interference measurement microscopy, ASTM D2663 method D), which measures surface roughness to quantify the macroscopic dispersion of fillers with a diameter of at least 5 μm. This test method was developed for carbon black, but the analytical data can be used to evaluate the macroscopic dispersion of LCNFs. For along and against grain scans, the dispersion results of Examples 7-11 are summarized in Table 7. Although the macroscopic dispersion by IFM is calibrated for carbon black, the data in Table 7 can be used to estimate the relative change in the amount of undispersed filler. It is believed that the area fraction measurement is the most accurate presentation of the amount of undispersed filler. Example 11 contains 5 phr LCNF and has unexpectedly good dispersion results; the area fraction of undispersed filler for Example 11 (0.51 with the grain and 0.83 against the grain) is similar to that of Examples 7-9 containing only carbon black.
[0093] Figures 7A-7C is a backscattered SEM image of a knife cut surface with the grain, which demonstrates the excellent dispersion of both the N234 carbon black and the LCNF in Example 11. Evidence of aligned discrete fibers is shown at high magnifications, and overall unexpectedly good macroscopic dispersion is shown at all magnifications. Fig. 8A and 8B Similar results for Example 11 are shown in the backscattered SEM image of the reverse-grain scraper cut surface.
[0094] Figure 9-25 Various properties of the corresponding carbon black formulations of Examples 7-11 were compared. The T90 cure time was not affected by the presence of LCNF in Examples 10-11, as Fig. 9 As shown, for Examples 10-11, the scorch time is slightly longer, as shown in FIG. Fig.10 shown. Fig.11 The formulations of Examples 10-11 using NDC containing LCNFs show a slight decrease in Mooney viscosity. Fig.12 The Shore A hardness in the samples decreased with the removal of N234 carbon black and increased slightly with the addition of LCNF.
[0095] Due to the high aspect ratio and anisotropic nature of LCNFs, the stress–strain behaviors show different results based on along-grain or against-grain testing. Fig.13The static modulus of the median of 5 tests at 100%, 200% and 300% elongation for Examples 7-11 is shown. In general, the removal of carbon black results in a lower modulus, while the addition of LCNF results in an increase in modulus (especially at moderate strains). There is no significant reduction in high strain modulus due to the addition of LCNF. Likewise, Fig.14 Similar results are shown in the tensile stress comparison of Examples 7 and 11, where the LCNF formulation has slightly enhanced mid-strain stiffness (and this can translate into potential tire handling benefits) and equivalent high-strain stiffness.
[0096] Fig.15 With-grain and against-grain grinding directions are shown, as well as with-grain and against-grain tensile testing. Fig.16 Including from Fig.13 Based on the median of 5 tests at 100%, 200%, and 300% elongation for Examples 7-11, there is some evidence of mechanical anisotropy, which is more pronounced for the formulations containing LCNF. This is Fig.17 This is more clearly shown in , which shows the mechanical anisotropy introduced by the addition of LCNFs, especially at low and medium strains.
[0097] Fig.18 and Fig.19 The median tensile strength and elongation at break (both with and against the grain) of 5 tests for Examples 7-11 are shown, respectively. The tensile strength with the grain is always greater than the tensile strength against the grain, and the samples containing LCNFs are generally consistent with the control sample of Example 7. There is no obvious anisotropic trend in the elongation at break data, and the samples containing LCNFs generally have slightly lower elongation at break values.
[0098] For the median of 5 tests of Examples 7-11, Fig. 20 The critical tear energy (Tc) data in show no anisotropy for the control samples of Examples 7-9, but exhibit surprisingly larger (about 40% greater) Tc values in the cross-grain tear direction for the samples containing LCNFs.
[0099] Fig.21 , Fig. 22 and Fig.23 DIN wear, rebound at 60°C, and deflectometer heat buildup (average of two tests for Examples 7-11) are summarized separately. The DIN wear data shows a slight increase in DIN wear with the addition of LCNF. Rebound generally increases linearly with the removal of carbon black, and these benefits are maintained with the addition of LCNF in the formulation. The heat buildup data trend with the rebound data.
[0100] Fig.24 and Fig.25 The tan δ from the ARES strain scan data at 60 °C is shown respectively. 最大 and ΔG' (average of two tests for Examples 7-11). Overall, the strain sweep data trend with the rebound and heat accumulation data. There is a small but consistent improvement in hysteresis for Examples 10-11 compared to the control sample of Example 7.
[0101] In summary, these results demonstrate that the disclosed NDC enables efficient incorporation and dispersion of sustainable fillers (LCNFs) with little apparent sacrifice in the resulting properties of carbon black and rubber-based formulations. Unexpectedly, NR-based formulations containing LCNFs (introduced via NDC) maintained or enhanced static stiffness, maintained or enhanced tear resistance, and improved (reduced) hysteresis compared to the N234 carbon black control without LCNFs.
[0102] In Examples 12-15, a reference carbon black grade N660 was used and model innerliner compounds were produced with or without LCNF as summarized in Table 8. Examples 12-13 are reference formulations for demonstrating typical carbon black performance and N660 constitutes 100% of the filler, which is equivalent to 60 phr in the compound formulation. Example 14 contains 5 phr less carbon black than Examples 12-13, and Example 15 contains 10 phr less carbon black than Examples 12-13. Examples 14-15 replace some of the carbon black with LCNF, but the same NDC described in Examples 3 and 6 is used, except that N660 carbon black replaces N234 carbon black. The LCNF amount is 5 phr in Example 14 and 10 phr in Example 15. Since NDC is a NR-based composition, two control samples are used to simulate the replacement of butyl rubber with NR (Example 12 contains 5 phr NR, while Example 13 contains 10 phr FR). Table 9 summarizes the standard mixing procedure.
[0103] Table 10 compares various properties of the corresponding carbon black formulations of Examples 12-15. The T90 cure time is generally not affected by the presence of LCNF, with Example 14 having a longer cure time and Example 15 having a shorter cure time than Control Examples 12-13. The T5 and T35 scorch times of Examples 14-15 containing NDC are slightly longer than Control Examples 12-13. In contrast, Table 10 shows a slight decrease in Mooney viscosity for the formulations of Examples 14-15 using NDC containing LCNF. Shore A hardness decreases slightly with the removal of N660 carbon black and increases slightly with the addition of LCNF.
[0104] The dispersion index (via IFM) is typically reduced by replacing carbon black with NDC, and the resulting dispersion index can depend on the carbon black grade and the loading level of LCNF. However, and unexpectedly, Example 14 (with 5 phr LCNF loading) has excellent dispersion (93.7% dispersion index).
[0105] Table 10 also summarizes the static modulus of the median of 5 tests of Examples 12-15 at 100%, 200% and 300% elongation. Comparable results were found at higher strains, while at 100% elongation, the addition of LCNF resulted in an increase in modulus. Tensile strength and elongation were generally unaffected by replacing carbon black with NDC. Resilience at 60°C generally increased gradually with replacement of N660 carbon black with LCNF.
[0106] Table 10 contains tan δ of RPA strain sweep data at 60°C 最大 and ΔG' (average of two tests from Examples 12-15). Replacing carbon black with LCNF via NDC results in tan δ 最大 and a slight beneficial decrease in ΔG'. Beneficially, the fatigue life values at 100% tensile strain for NDC Examples 14-15 in Table 10 are comparable to those for Control Examples 12-13.
[0107] As described above, these results demonstrate that the disclosed NDC enables efficient incorporation and dispersion of sustainable fillers (LCNFs) with little apparent sacrifice in the resulting properties of carbon black and rubber-based formulations. Unexpectedly, butyl rubber-based formulations containing LCNFs (introduced via NDCs) have comparable performance to the N660 carbon black control without LCNFs.
[0108]
[0109]
[0110]
[0111]
[0112]
[0113]
[0114]
[0115]
[0116]
[0117]
[0118]
[0119]
[0120]
[0121]
[0122] The present invention has been described above with reference to many aspects and specific embodiments. Based on the above detailed description, many variations will provide enlightenment to those skilled in the art. All such obvious variations are within the entire intended scope of the appended claims. Other aspects of the present invention may include, but are not limited to, the following (aspects are described as "comprising...", but alternatively, may be described as "consisting essentially of..." or "consisting of..."):
[0123] Aspect 1. A tire composition comprising: (I) a polymer; (II) a nanocellulose dispersion composition (NDC) comprising (i) a separator comprising a carbon black filler, an elastomer latex, a wax or any combination thereof, and (ii) nanocellulose; and (III) a carbon black additive.
[0124] Aspect 2. The tire composition as defined in aspect 1, wherein the weight ratio of the polymer to the nanocellulose dispersion composition (polymer:NDC) is in the range of about 100:1 to about 1:1.
[0125] Aspect 3. The tire composition as defined in aspect 1, wherein the weight ratio of the polymer to the nanocellulose dispersion composition (polymer:NDC) is in the range of about 50:1 to about 2:1.
[0126] Aspect 4. The tire composition as defined in any one of aspects 1 to 3, wherein the polymer comprises a thermoplastic material.
[0127] Aspect 5. The tire composition as defined in any one of aspects 1 to 3, wherein the polymer comprises an elastomer.
[0128] Aspect 6. The tire composition as defined in any one of Aspects 1-3, wherein the polymer comprises natural rubber (NR), epoxidized natural rubber (ENR), synthetic cis-polyisoprene (IR), emulsion-polymerized styrene-butadiene rubber (ESBR), solution-polymerized styrene-butadiene rubber (SSBR), polybutadiene rubber (BR), butyl rubber (IIR / CIIR / BIIR), chloroprene rubber (CR), nitrile elastomer (NBR), hydrogenated nitrile elastomer (HNBR), carboxylated nitrile elastomer (XNBR), ethylene-propylene rubber (EPM / EPDM), fluorinated elastomer (FPM / FKM), polyurethane rubber (AU / EU / PU), or any combination thereof.
[0129] Aspect 7. The tire composition as defined in any one of aspects 1 to 6, wherein the separator is compatible with the polymer and reduces nanocellulose aggregation.
[0130] Aspect 8. The tire composition as defined in any one of aspects 1 to 7, wherein the nanocellulose dispersion composition has a nanocellulose dispersibility in the tire composition that is greater than the nanocellulose dispersibility in the absence of a separator.
[0131] Aspect 9. The tire composition as defined in any one of aspects 1 to 8, wherein the nanocellulose comprises nanocellulose crystals (NC), nanocellulose fibrils (NF) or a combination thereof.
[0132] Aspect 10. The tire composition as defined in any one of aspects 1 to 9, wherein the nanocellulose comprises lignin-coated nanocellulose crystals (LCNCs), lignin-coated nanocellulose fibrils (LCNFs), or a combination thereof.
[0133] Aspect 11. The tire composition as defined in any one of aspects 1 to 10, wherein the nanocellulose comprises hydrophilic cellulose nanocellulose crystals (CNCs), hydrophilic cellulose nanocellulose fibrils (CNFs), or a combination thereof.
[0134] Aspect 12. The tire composition as defined in any one of aspects 1 to 11, wherein the nanocellulose dispersion composition (NDC) further comprises a hydrocarbon oil.
[0135] Aspect 13. The tire composition as defined in Aspect 12, wherein the hydrocarbon oil comprises an aliphatic hydrocarbon, an aromatic hydrocarbon, or a combination thereof.
[0136] Aspect 14. The tire composition as defined in Aspect 12, wherein the hydrocarbon oil comprises treated distillate aromatic extract (TDAE) oil.
[0137] Aspect 15. The tire composition as defined in any one of aspects 1 to 14, wherein the elastomer latex comprises natural rubber (NR), isoprene rubber (IR), emulsion styrene butadiene rubber (ESBR), or any combination thereof.
[0138] Aspect 16. The tire composition as defined in any one of aspects 1 to 15, wherein the wax comprises a non-branched alkane paraffin wax; a natural mineral, petroleum-refined or lignin-refined branched paraffin wax or ozokerite wax; a polyethylene wax; a functionalized polyethylene wax; or any combination thereof.
[0139] Aspect 17. The tire composition as defined in any one of aspects 1 to 16, wherein the carbon black filler and the carbon black additive independently comprise furnace carbon black and / or surface-modified furnace carbon black.
[0140] Aspect 18. The tire composition defined in any one of aspects 1 to 17, wherein the carbon black filler and the carbon black additive are independently characterized by: a nitrogen surface area of about 90 m 2 / g to about 140m 2 / g; external surface area is about 80m 2 / g to about 125m 2 / g; pH is about 2.5 to about 9; 50GM void volume is about 55cm 3 / 100g to about 67cm 3 / 100g; 75GM void volume is about 50cm 3 / 100g to about 60cm 3 / 100g; 100GM void volume is about 45cm 3 / 100g to about 55cm 3 / 100g; moisture content of about 2.5 wt% to about 4.5 wt%; volatile content of about 4.5 wt% to about 6.5 wt%; oxygen content of about 2.5 wt% to about 5.5 wt%; or any combination of the above.
[0141] Aspect 19. The tire composition as defined in any one of aspects 1 to 18, wherein the separator comprises the carbon black filler, the elastomer latex or wax.
[0142] Aspect 20. The tire composition as defined in any one of aspects 1 to 18, wherein the separator comprises at least two of the carbon black filler, the elastomer latex and wax.
[0143] Aspect 21. The tire composition as defined in any one of aspects 1-20, wherein the weight ratio of the separator to the nanocellulose is in the range of about 0.5:1 to about 25:1.
[0144] Aspect 22. The tire composition as defined in any one of aspects 1-21, wherein the weight ratio of the separator to the nanocellulose is in the range of about 1:1 to about 10:1.
[0145] Aspect 23. The tire composition as defined in any one of Aspects 1-22, wherein the nanocellulose dispersion composition (NDC) is produced by a method comprising the steps of: (a) combining the aqueous dispersion of the nanocellulose with the separator to form a mixture; and (b) drying the mixture to form the nanocellulose dispersion composition (NDC).
[0146] Aspect 24. The tire composition as defined in any one of Aspects 1-22, wherein the nanocellulose dispersion composition (NDC) is produced by a method comprising the following steps: (A) combining an aqueous dispersion of the nanocellulose with the separator to form a mixture; and (B) drying the mixture to form a nanocellulose dispersion composition (NDC); wherein the separator is stable in the NDC and is spaced between the nanocellulose particles to reduce or prevent aggregation of the nanocellulose particles in the NDC.
[0147] Aspect 25. The tire composition as defined in any one of aspects 1 to 24, wherein the tire composition contains any suitable amount of carbon black, for example, from about 20 to about 150 phr, from about 30 to about 100 phr, or from about 40 to about 80 phr.
[0148] Aspect 26. The tire composition as defined in any one of aspects 1-25, wherein the tire composition contains any suitable amount of nanocellulose, for example, from about 1 to about 15 phr, from about 2 to about 10 phr, or from about 2 to about 7.5 phr.
[0149] Aspect 27. The tire composition as defined in any one of aspects 1 to 26, wherein the tire composition contains any suitable amount of hydrocarbon oil, for example, from about 1 to about 15 phr, from about 2 to about 10 phr, or from about 3 to about 9 phr.
[0150] Aspect 28. An article comprising the tire composition defined in any one of aspects 1-27.
[0151] Aspect 29. A pneumatic tire comprising the tire composition defined in any one of aspects 1 to 27.
[0152] Aspect 30. A passenger vehicle tire, comprising the tire composition defined in any one of aspects 1-27.
[0153] Aspect 31. A truck and bus radial (TBR) tire, comprising the tire composition defined in any one of aspects 1-27.
[0154] Aspect 32. A tire tread, comprising the tire composition defined in any one of aspects 1-27.
Claims
1. A tire composition, comprising: (I) polymers; (II) a nanocellulose dispersion composition (NDC), the nanocellulose dispersion composition comprising: (i) a separator comprising at least one of an elastomer latex and / or a wax and a carbon black filler; and (ii) nanocellulose; and (III) carbon black additive; The tire composition described herein is characterized by a dispersion index of at least 90% as determined by interferometric microscopy (IFM).
2. A tire composition, comprising: (I) polymers; (II) a nanocellulose dispersion composition (NDC), the nanocellulose dispersion composition comprising: (i) a separator comprising at least one of an elastomer latex and / or a wax and a carbon black filler; and (ii) nanocellulose; and (III) carbon black additive; The tire composition is characterized by a fatigue life at 100% tensile strain of at least 300,000 cycles.
3. The tire composition of claim 1 or 2, wherein the weight ratio of the polymer to the nanocellulose dispersion composition (polymer:NDC) is in the range of 100:1 to 1:1, 80:1 to 10:1, 75:1 to 2:1, 60:1 to 5:1, 50:1 to 1:1, 40:1 to 4:1, 75:1 to 25:1, 90:1 to 15:1, 75:1 to 1.5:1 or 50:1 to 2:
1.
4. The tire composition according to claim 1 or 2, wherein the polymer comprises an elastomer.
5. The tire composition of claim 1 or 2, wherein the nanocellulose dispersion composition has a dispersibility of nanocellulose in the polymer composition that is greater than the dispersibility of the nanocellulose in the absence of the separator. 6 . The tire composition according to claim 1 , wherein the nanocellulose comprises nanocellulose crystals (NC), nanocellulose fibrils (NF), or a combination thereof.
7. The tire composition according to claim 1 or 2, wherein the nanocellulose comprises lignin coated nanocellulose crystals (LCNCs), lignin coated nanocellulose fibrils (LCNFs), or a combination thereof.
8. The tire composition according to claim 1 or 2, wherein the nanocellulose comprises hydrophilic cellulose nanocellulose crystals (CNC), hydrophilic cellulose nanocellulose fibrils (CNF), or a combination thereof.
9. The tire composition according to claim 1 or 2, wherein the nanocellulose dispersion composition (NDC) further comprises a hydrocarbon oil.
10. The tire composition according to claim 1 or 2, wherein the polymer comprises natural rubber (NR), isoprene rubber (IR), polybutadiene rubber (BR), emulsion styrene butadiene rubber (ESBR), or any combination thereof.
11. The tire composition according to claim 1 or 2, wherein the wax comprises: Non-branched paraffin wax, branched paraffin wax or ozokerite wax refined from natural minerals, petroleum or lignin, polyethylene wax, or any combination thereof.
12. The tire composition of claim 11, wherein the wax comprises a functionalized polyethylene wax.
13. The tire composition according to claim 1 or 2, wherein the carbon black filler and the carbon black additive independently comprise furnace carbon black and / or surface modified furnace carbon black.
14. The tire composition according to claim 1 or 2, wherein the carbon black filler and the carbon black additive are independently characterized by: The surface area of nitrogen is 90m 2 / g to 140m 2 / g; External surface area is 80m 2 / g to 125m 2 / g; pH 2.5 to 9; 50GM void volume is 55cm 3 / 100g to 67cm 3 / 100g; 75GM void volume is 50cm 3 / 100g to 60cm 3 / 100g; The void volume of 100GM is 45cm 3 / 100g to 55cm 3 / 100g; Moisture content of 2.5 wt% to 4.5 wt%; The volatile matter content is 4.5 wt% to 6.5 wt%; An oxygen content of 2.5 wt % to 5.5 wt %; or Any combination of them.
15. The tire composition according to claim 1 or 2, wherein the separator comprises the carbon black filler, the elastomer latex and the wax.
16. The tire composition of claim 1 or 2, wherein the weight ratio of the separator to the nanocellulose is in the range of 0.1:1 to 25:1, 0.1:1 to 10:1, 0.1:1 to 5:1, 0.1:1 to 1:1, 0.25:1 to 15:1, 0.3:1 to 10:1, 0.5:1 to 25:1, 0.75:1 to 15:1 or 1:1 to 10:
1.
17. The tire composition according to claim 1 or 2, wherein the nanocellulose dispersion composition (NDC) is produced by a process comprising the steps of: (a) combining the aqueous dispersion of nanocellulose with the separator to form a mixture; and (b) drying the mixture to form the nanocellulose dispersion composition (NDC).
18. The tire composition according to claim 1 or 2, wherein the nanocellulose dispersion composition (NDC) is produced by a process comprising the steps of: (A) combining the aqueous dispersion of nanocellulose with the separator to form a mixture; and (B) drying the mixture to form the nanocellulose dispersion composition (NDC); The separator is stable in the NDC and is spaced between the nanocellulose particles to reduce or prevent aggregation of the nanocellulose particles in the NDC.
19. The tire composition according to claim 1 or 2, wherein the tire composition comprises: 20 to 150 phr of carbon black, 1 to 15 phr of nanocellulose and 1 to 15 phr of hydrocarbon oil; or 30 to 100 phr of carbon black, 2 to 10 phr of nanocellulose and 2 to 10 phr of hydrocarbon oil; or 40 to 80 phr of carbon black, 2 to 7.5 phr of nanocellulose and 3 to 9 phr of hydrocarbon oil.
20. The tire composition of claim 1 or 2, wherein the tire composition is characterized by a dispersion index of at least 92%, at least 93%, at least 94%, at least 95%, at least 96%, at least 97% or at least 98% as measured by interferometric microscopy (IFM).
21. The tire composition of claim 1 or 2, wherein the tire composition is characterized by an area fraction of undispersed material as measured by interferometry microscopy (IFM) of less than or equal to 8%, less than or equal to 6%, less than or equal to 4%, less than or equal to 3%, or less than or equal to 2%.
22. The tire composition of claim 1 or 2, wherein the tire composition is characterized by a fatigue life at 100% tensile strain of at least 325,000 cycles, at least 350,000 cycles, at least 375,000 cycles, or at least 400,000 cycles.
23. A manufactured article comprising the tire composition of any one of claims 1-22.
24. The article of claim 23, wherein the article is a pneumatic tire, a passenger vehicle tire, or a truck and bus radial tire.
25. The article of claim 23, wherein the article is a tire tread.