A method for manufacturing high-efficiency LED beads

By combining a secondary dispensing process with a nano-protective film, the luminous efficacy and heat dissipation performance of LED beads are improved, solving the problem of low luminous efficacy in existing technologies and achieving higher luminous flux and color rendering index.

CN115172562BActive Publication Date: 2026-11-10NINGBO KLITE ELECTRIC MFG
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202210579243.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-05-25
Publication Date
2026-11-10
Estimated Expiration
2042-05-25

AI Technical Summary

Technical Problem

The luminous efficacy of existing LED chips is low, making it difficult to meet the requirements for high energy efficiency.

Method used

A two-stage dispensing process is adopted, first dispensing a first encapsulating adhesive containing fluoride red powder, then dispensing a second encapsulating adhesive containing nitride yellow-green powder, and coating the surface of the LED bead with a nano-protective film. Flip-chip and a bracket made of specific materials are used to improve luminous efficiency.

Benefits of technology

The light efficiency is improved by 10%-15%, the light flux is increased by 3%-5%, the heat dissipation performance and reliability are improved, and the problems of light decay and shading are avoided.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115172562B_ABST
    Figure CN115172562B_ABST
Patent Text Reader

Abstract

This invention discloses a method for manufacturing high-efficiency LED beads, comprising the following steps: S1: Baking and cooling the bracket, applying conductive silver paste to the middle part of the bracket cup pad, and placing the LED chip on the silver paste-applied position of the bracket; S2: Inspecting and baking the bracket; S3: Applying a first encapsulating adhesive to the bracket cup according to technical specifications and baking, then applying a second encapsulating adhesive to the bracket cup; S4: Debubbling, baking, and cooling the LED beads; S5: Coating the surface of the LED bead encapsulant and the bracket with a nano-protective film, completing the manufacturing process. In this high-efficiency LED bead manufacturing method, the phosphor adhesive application part employs a two-stage dispensing process. The two-stage dispensing first applies a first encapsulating adhesive containing fluoride red powder, and then applies a second encapsulating adhesive containing nitride yellow-green powder, thereby improving the luminous efficiency of the manufactured LED beads.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of LED lamp bead technology, and in particular to a method for manufacturing high-efficiency LED lamp beads. Background Technology

[0002] As the European market demands increasingly higher energy efficiency ratings for lighting products, higher requirements are being placed on the luminous efficacy of LED light sources to meet the Class A energy efficiency requirements. Currently, the best LED chips on the market can only achieve a luminous efficacy of 215 lm / W for warm white 3000K under a 60mA current, and 225 lm / W for cool white 4000K, which are relatively low.

[0003] Currently, most existing LED chip manufacturing processes employ centrifugal sedimentation. For example, a method for centrifugally manufacturing LED chips, disclosed in Chinese patent literature (CN108447960A), includes an LED chip and a cup-shaped support, with the following steps: A. Fixing the LED chip onto the cup-shaped support using a die-bonding process, and connecting the positive and negative terminals of the LED chip with gold wire; B. Filling the cup-shaped support with encapsulating adhesive, wherein phosphor is pre-mixed in the encapsulating adhesive; C. After fixing the cup-shaped support filled with encapsulating adhesive with a material box, placing it in a centrifuge for centrifugation, thereby settling the phosphor in the encapsulating adhesive onto the upper surface of the LED chip; D. After centrifugation, baking the cup-shaped support filled with encapsulating adhesive, and then separating the material box to form the LED chip. This invention, by stirring phosphor in the encapsulating adhesive and then using high-speed centrifugation to set the phosphor onto the upper surface of the LED chip, can improve the light concentration emitted by the LED chip and increase the brightness of the finished product, but the effect is not significant enough, and the resulting LED chips still suffer from low luminous efficacy. Summary of the Invention

[0004] The present invention aims to overcome the problem of low luminous efficacy of LED beads manufactured in the prior art, and to provide a method for manufacturing high-efficiency LED beads.

[0005] To achieve the above objectives, the present invention adopts the following technical solution:

[0006] A method for manufacturing high-efficiency LED chips includes the following steps: S1: Baking and cooling the bracket, applying conductive silver paste to the center of the bracket cup pads, and placing the LED chip on the silver paste-applied area of ​​the bracket; S2: Inspecting and baking the bracket; the inspection mainly includes: the amount of adhesive applied, the height of the adhesive application, the location of the adhesive application, the location of die bonding, and the inspection of the chip push force after die bonding; S3: According to the technical specifications, applying the first encapsulating adhesive into the bracket cup and baking it, then applying the second encapsulating adhesive into the bracket cup; S4: Debubbling, baking, and cooling the LED chip; S5: Coating the surface of the LED chip adhesive and the bracket with a nano-protective film, completing the manufacturing process. This invention discloses a method for manufacturing high-efficiency LED beads. The phosphor application process employs a two-stage dispensing process. The two-stage dispensing first applies a first encapsulating adhesive containing fluoride red phosphor, followed by a second encapsulating adhesive containing nitride yellow-green phosphor, thereby increasing the luminous flux. The use of fluoride phosphor results in a 10%-15% higher color rendering index (Ra90 and above) compared to the nitride red phosphor + aluminate green phosphor scheme. Compared to the Ra80 color rendering index scheme, the luminous efficacy is also improved by 3-5%. Due to the different proportions of red phosphor, the luminous efficacy is further improved for color temperatures such as 2700K and 3000K, where a higher proportion of red phosphor is required.

[0007] As a preferred embodiment of the present invention, step S1 specifically involves: baking the bracket at a temperature of 120-150°C for 5-10 minutes, then cooling the bracket to 50-70°C, applying conductive silver paste to the center of the bracket's cup pads, with the amount of conductive silver paste controlled between 1 / 3 and 2 / 3 of the LED chip height, and using a bakelite nozzle to pick up the LED chip and place it on the bracket at the silver paste application point. The chip is fixed in the center of the bracket, ensuring that the distance between the chip and the bracket is consistent in all four directions (up, down, left, and right). When placing the chip on the bracket at the silver paste application point, the chip pushing force should be greater than 120gf to ensure stable contact between the chip and the bracket and good heat dissipation.

[0008] As a preferred embodiment of the present invention, step S2 specifically involves: inspecting and baking the substrate at a temperature of 150-170°C for 1-2 hours. The purpose of step S2 is to cure the silver paste, thus fixing the chip onto the substrate. During the baking process, the dedicated baking oven should not be opened arbitrarily, and care should be taken to prevent contamination from other harmful substances.

[0009] As a preferred embodiment of the present invention, S3 specifically involves: according to the technical requirements of color temperature, color rendering index and R9 value, applying the prepared first encapsulating adhesive containing fluoride red powder into the support cup and baking it at a temperature of 60-80°C for 10-20 minutes, and then applying the prepared second encapsulating adhesive containing nitride yellow-green powder into the support cup. This invention discloses a method for manufacturing high-efficiency LED beads. The phosphor application process employs a two-stage dispensing process. The two-stage dispensing first applies a first encapsulating adhesive containing fluoride red phosphor, followed by a second encapsulating adhesive containing nitride yellow-green phosphor, thereby increasing the luminous flux. The use of fluoride phosphor results in a 10%-15% higher color rendering index (Ra90 and above) compared to the nitride red phosphor + aluminate green phosphor scheme. Compared to the Ra80 color rendering index scheme, the luminous efficacy is also improved by 3-5%. Due to the different proportions of red phosphor, the luminous efficacy is further improved for color temperatures such as 2700K and 3000K, where a higher proportion of red phosphor is required.

[0010] As a preferred embodiment of the present invention, step S4 specifically involves: placing the LED beads, after being coated in step S3, into a heated vacuum chamber to degas the encapsulating adhesive. The temperature of the heated vacuum chamber is 60-80°C. After degassing until no bubbles remain, the beads are baked at 135-150°C for 3-4 hours, followed by cooling. The purpose of step S4 is to allow the adhesive to fully cure and to thermally age the LED beads.

[0011] As a preferred embodiment of the present invention, the thickness of the nano-protective film in S5 is 30-50 μm. To solve the problems of fluoride phosphors being susceptible to moisture and light decay in high temperature and humidity environments, a nano-film is coated on the fluorescent adhesive coating and the entire surface of the scaffold to protect it, preventing sulfur- or halogen-containing elements and oxygen ions from invading the functional areas of the scaffold and reacting with silver.

[0012] As a preferred embodiment of the present invention, the LED chip is a square flip chip with a package size of 40mil*40mil. The heat generated at the PN junction of a conventional chip needs to pass through a sapphire substrate to be conducted to the heat sink. The poor thermal conductivity of the sapphire substrate results in poor thermal conductivity of the structure, thus reducing the chip's luminous efficiency and reliability. In contrast, the heat generated at the PN junction of the flip chip can be directly conducted to the heat sink without passing through the substrate, resulting in excellent heat dissipation and high luminous efficiency and reliability. In the flip structure, both the p-electrode and n-electrode are located on the bottom surface, avoiding obstruction of emitted light and resulting in high chip light extraction efficiency. Furthermore, the greater distance between the electrodes of the flip chip reduces the risk of short circuits caused by electrode metal migration. Using a large-size square 4040 flip chip effectively avoids the impact of multiple chips on light output.

[0013] As a preferred embodiment of the present invention, the bracket is made of SMC material, and the package size of the bracket is 3.0mm*3.0mm. SMC material is chosen for the bracket because its whiteness is comparable to PCT material and higher than PPA and EMC materials, with a reflectance greater than 90%. Furthermore, SMC has higher hardness and heat resistance, allowing for seamless fusion with the encapsulating adhesive during encapsulation, resulting in better anti-sulfurization performance. Tests also show that the bracket does not change color after three reflow soldering cycles, demonstrating high resistance to yellowing. Additionally, the bracket of the present invention uses a 3030 package, combined with a 4040 square chip, to ensure more balanced light emission from all directions of the LED's emitting surface, achieving optimal performance.

[0014] Therefore, the present invention has the following beneficial effects: In the method for manufacturing high-efficiency LED beads of the present invention, the phosphor dispensing part adopts a two-stage dispensing process. The two-stage dispensing first dispenses a first encapsulating adhesive containing fluoride red phosphor, and then dispenses a second encapsulating adhesive containing nitride yellow-green phosphor, thereby improving the luminous flux. The use of fluoride phosphor, since the luminous efficacy of fluoride red phosphor + aluminate green phosphor is 10%-15% higher than that of the nitride red phosphor + aluminate green phosphor scheme, and the luminous efficacy is also 3-5% higher than that of Ra80 phosphor. Due to the different proportions of red phosphor, the luminous efficacy of color temperatures such as 2700K and 3000K with a higher proportion of red phosphor is improved even more. Attached Figure Description

[0015] Figure 1 This is a flowchart of the method of the present invention. Detailed Implementation

[0016] The present invention will now be further described with reference to the accompanying drawings and specific embodiments.

[0017] like Figure 1As shown, a method for manufacturing high-efficiency LED chips includes the following steps: S1: Baking and cooling the bracket; applying conductive silver paste to the center of the bracket's cup pads; and placing the LED chip on the silver paste-applied position on the bracket. Specifically, the bracket is baked at a temperature between 120-150℃ for 5-10 minutes, then cooled to 50-70℃. Conductive silver paste is applied to the center of the bracket's cup pads, with the amount of paste controlled between 1 / 3 and 2 / 3 of the LED chip height. The LED chip is then picked up using a bakelite nozzle and placed on the silver paste-applied position on the bracket. S2: Inspecting and baking the bracket; specifically, the bracket is inspected and baked at a temperature between 150-170℃ for 1-2 hours. S3: According to the technical specifications, apply the first encapsulating adhesive to the bracket cup and bake it. Then apply the second encapsulating adhesive to the bracket cup. Specifically, according to the technical specifications for color temperature, color rendering index, and R9 value, apply the prepared first encapsulating adhesive containing fluoride red powder to the bracket cup and bake it at a temperature of 60-80℃ for 10-20 minutes. Then apply the prepared second encapsulating adhesive containing nitride yellow-green powder to the bracket cup. S4: De-bubbling, baking, and cooling the LED beads. S5: Coat the surface of the LED bead adhesive and the bracket with a nano-protective film to complete the process. Specifically, place the LED beads after S3 adhesive application in a heated vacuum chamber to de-bubble the encapsulating adhesive at a temperature of 60-80℃ until no bubbles are present. Then bake at a temperature of 135-150℃ for 3-4 hours. Finally, cool the LED beads. The thickness of the nano-protective film is 30-50μm. In this invention, the LED chip is a square flip chip with a package size of 40mil*40mil; the bracket is made of SMC material and the package size of the bracket is 3.0mm*3.0mm.

[0018] In this embodiment, a method for manufacturing a high-efficiency LED chip is as follows: Step 1: Applying silver paste and die bonding: After baking the bracket (baking temperature: 120-150℃, baking time: 5-10 minutes), cool it to 50-70℃. Apply conductive silver paste to the center of the bracket's cup pad (the amount of paste should be controlled at 1 / 3 to 1 / 2 of the chip height to ensure adhesion on more than three sides of the chip). Then, use a bakelite nozzle to pick up the LED chip and place it on the silver paste-applied position on the bracket. The chip is fixed in the center of the bracket, ensuring that the distance between the chip and the bracket in the four directions (up, down, left, and right) is basically the same. The chip pushing force should be greater than 120gf to ensure stable contact between the chip and the bracket and good heat dissipation. Step 2: Inspection and baking: Baking temperature 150-170℃, baking time 1-2 hours. The purpose is to cure the silver paste and fix the chip on the bracket. During the baking process, do not open the dedicated baking oven at will, and take care to prevent contamination by other harmful substances. Step 3: Applying Encapsulating Adhesive: Based on the required technical specifications such as color temperature, color rendering index, and R9 value, apply the prepared encapsulating adhesive containing fluoride red powder to the die-bonded support cup in the specified amount. This is the first application. After the first application, perform a short bake (baking temperature: 60-80℃, baking time: 10-20 minutes). Then, perform a second application, applying the prepared nitride yellow-green powder encapsulating adhesive to the support cup. The encapsulating adhesive must be thoroughly stirred and vacuum-sealed until air bubbles are removed before use. The encapsulating adhesive after the first application and short bake should not be completely cured; it should be just solidified and not move. The second application should not fuse with the first application and should not show obvious layering. The second application should be performed immediately after the first application and short bake to prevent contamination and moisture absorption from the air. Control the amount of adhesive applied; the adhesive surface should not be significantly concave or convex above the cup rim, ideally flush with the rim (0-0.2mm horizontally). Step 4: Baking: After dispensing the adhesive, the LED beads are degassed in a vacuum chamber at 60-80℃. Once no bubbles remain, they are baked at 135-150℃ for 3-4 hours. This is to allow the adhesive to fully cure and to thermally age the LED beads. Step 5: After baking and cooling, a nano-film is coated onto the surface of the LED bead adhesive and the support structure for protection. The coating thickness is between 30-50μm. Finally, after spectral inspection, the beads are packaged.

[0019] The LED chip of this invention uses a flip-chip design: Because heat generated at the PN junction of a conventional chip needs to pass through a sapphire substrate to be conducted to the heat sink, the poor thermal conductivity of the sapphire substrate results in poor thermal conductivity of the structure, thus reducing the chip's luminous efficiency and reliability. In contrast, heat generated at the PN junction of a flip-chip can be directly conducted to the heat sink without passing through the substrate, resulting in excellent heat dissipation and higher luminous efficiency and reliability. In the flip-chip structure, both the p-electrode and n-electrode are located on the bottom surface, avoiding obstruction of emitted light and resulting in higher light extraction efficiency. Furthermore, the greater distance between the electrodes in a flip-chip reduces the risk of short circuits caused by electrode metal migration.

[0020] Currently, packaging manufacturers commonly use two large-sized upright LED chips connected in parallel to increase luminous flux while keeping the LED voltage (power P) constant, thus attempting to improve luminous efficacy. However, in practice, insufficient spacing between the two or more chips leads to mutual blocking and diffraction of the light output, which to some extent affects the improvement in luminous efficacy. This invention uses large-sized square 4040 flip-chip LEDs, thereby avoiding the impact of multiple chips on light output.

[0021] In terms of package size, after continuous market screening and product replacement, the industry generally agrees that the 2835 and 3030 package sizes have the highest luminous efficiency for SMD LEDs. In combination with the characteristics of the chips used in this process, the bracket adopts a 3030 package and is matched with a 4040 square LED chip to ensure that the light output of the LEDs is more balanced in all directions and achieves the best effect.

[0022] For the support structure material, SMC was selected. SMC's whiteness is comparable to PCT and higher than PPA and EMC, with light reflectance exceeding 90%. Furthermore, SMC exhibits higher hardness and heat resistance. During encapsulation, it can seamlessly fuse with the encapsulating adhesive, resulting in better resistance to sulfurization. Tests also show that the support structure does not exhibit discoloration after three reflow soldering cycles, demonstrating high resistance to yellowing. Table 1 compares the Reflow test results of SMC, PCT, and EMC support structures.

[0023] Table 1. Comparison of Reflow tests for SMC stents, PCT stents, and EMC stents.

[0024]

[0025]

[0026] After two reflow soldering cycles, the PCT stent showed significant yellowing, the EMC stent showed slight yellowing, and the SMC stent showed no change. It can be concluded that the SMC stent has higher heat resistance and stronger resistance to yellowing.

[0027] In this invention, the fluorescent adhesive adopts a two-stage dispensing process. Compared with conventional dispensing and centrifugal sedimentation processes, the two-stage dispensing first dispenses yellow-green powder and then dispenses fluoride red powder, which can increase the light flux by 1-2%.

[0028] Table 2 Comparison of data between centrifugal sedimentation dispensing process and secondary dispensing process

[0029]

[0030] Where IF is the current, VF is the voltage, P is the power, Φ is the luminous flux, x and y are the chromaticity coordinates, and Ra is the color rendering index. Table 2 shows that the luminous flux of the LEDs manufactured using the secondary dispensing process is 1.54% higher than that manufactured using the centrifugal sedimentation dispensing process.

[0031] This invention uses fluoride phosphors. The luminous efficacy of fluoride red phosphor + aluminate green phosphor is 10%-15% higher than that of nitride red phosphor + aluminate green phosphor (Ra90 and above), and also shows a 3-5% improvement compared to the Ra80 phosphor. Due to the different proportions of red phosphor, the luminous efficacy improvement is even greater at color temperatures such as 2700K and 3000K where a higher proportion of red phosphor is required. Table 3 shows the comparison data between fluoride red phosphor and nitride red phosphor with a CRI of 80.

[0032] Table 3. Comparison data between fluoride red pigment and nitride red pigment with 80 CRI.

[0033]

[0034] As can be seen from Table 3, the luminous flux of the lamp beads made using fluoride red powder and secondary dispensing process is increased by 4.46%.

[0035] To address the issues of fluoride phosphors being susceptible to moisture and light decay in high-temperature and high-humidity environments, this invention coats the fluorescent adhesive coating and the entire support surface with a nanofilm. The nanofilm is an organic or inorganic compound material that can protect the LED beads and prevent sulfur- or halogen-containing elements and oxygen ions from invading the functional areas of the support and reacting with silver.

[0036] The above description is merely a specific embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any changes or substitutions conceived without creative effort should be included within the scope of protection of the present invention.

Claims

1. A method for manufacturing high-efficiency LED beads, characterized in that, Includes the following steps: S1: Bake and cool the bracket, apply conductive silver paste to the middle part of the bracket cup pad, and place the LED chip on the bracket where the silver paste is applied. S2: Inspect and bake the support frame; S3: According to the technical specifications, the first encapsulant is applied to the bracket cup and baked, and then the second encapsulant is applied to the bracket cup. The fluorescent adhesive application process adopts a two-stage dispensing process. The first encapsulant containing fluoride red powder is applied first, and then the second encapsulant containing nitride yellow-green powder is applied. S4: De-bubbling, baking, and cooling of the LED beads; S5: A nano-protective film is coated on the surface of the LED bead colloid and the bracket, and the manufacturing process is complete.

2. The method for manufacturing a high-efficiency LED bead according to claim 1, characterized in that, S1 specifically involves: baking the bracket at a temperature of 120-150℃ for 5-10 minutes, then cooling the bracket to 50-70℃, applying conductive silver paste to the center of the bracket's cup pads, with the amount of conductive silver paste controlled between 1 / 3 and 2 / 3 of the LED chip height, and using a bakelite nozzle to pick up the LED chip and place it on the bracket where the silver paste is applied; when placing the chip on the bracket where the silver paste is applied, the chip pushing force should be greater than 120gf.

3. The method for manufacturing high-efficiency LED beads according to claim 1, characterized in that, S2 specifically involves inspecting and baking the substrate. The inspection includes checking the amount of adhesive applied, the height of the adhesive application, the location of the adhesive application, the location of the die bonding, and the push force on the wafer after die bonding. The baking temperature is 150-170℃, and the baking time is 1-2 hours.

4. The method for manufacturing a high-efficiency LED bead according to claim 1, characterized in that, S3 specifically involves: according to the technical requirements of color temperature, color rendering index, and R9 value, applying the prepared first encapsulating adhesive containing fluoride red powder into the support cup and baking it at a temperature of 60-80℃ for 10-20 minutes; then applying the prepared second encapsulating adhesive containing nitride yellow-green powder into the support cup; the encapsulating adhesive after the first application and short baking should not be completely cured, and should be just solidified on the surface without moving.

5. The method for manufacturing a high-efficiency LED bead according to claim 1, characterized in that, S4 specifically involves placing the LED beads, after being coated in S3, into a heated vacuum chamber to degas the encapsulating adhesive. The temperature of the heated vacuum chamber is 60-80℃. After degassing until no bubbles remain, the LED beads are baked at a temperature of 135-150℃ for 3-4 hours, followed by cooling.

6. The method for manufacturing a high-efficiency LED bead according to claim 1, characterized in that, The thickness of the nano-protective film in S5 is 30-50 μm.

7. A method for manufacturing high-efficiency LED beads according to any one of claims 1-6, characterized in that, The LED chip is a square flip chip with a package size of 40*40mil.

8. The method for manufacturing a high-efficiency LED lamp bead according to claim 7, characterized in that, The bracket is made of SMC material, and the package size of the bracket is 3.0*3.0mm.

Citation Information

Patent Citations

  • Centrifugal manufacturing method of LED lamp bead and LED lamp bead

    CN108447960A

  • LED lamp bead and manufacturing method

    CN110444652A

  • LED lamp bead and dispensing method thereof

    CN111710772A

  • LED lamp bead and backlight module

    CN209926055U