Method for recovering active metals from lithium secondary batteries
Through two-step hydrogen reduction process and water washing, the side reactions and pollution problems caused by reaction heat in the recovery of active metals in lithium secondary batteries are solved, high-purity and high-efficiency lithium precursor recovery is achieved, and the recovery rate and The eco-friendliness of the craft.
Patent Information
- Application Number
- CN202180017025.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-02-27
- Filing Date
- 2021-02-23
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2041-02-23
AI Technical Summary
When recycling active metals from lithium secondary batteries in the existing technology, the reaction heat in the dry method causes side reactions and particle agglomeration, which reduces the recovery rate. In addition, the wet method has problems of environmental pollution and low selectivity.
A two-step hydrogen reduction process is adopted. In the first step, hydrogen with a low hydrogen concentration is used for preliminary reduction, and in the second step, hydrogen with a high hydrogen concentration is used for further reduction. The cathode active material of the lithium secondary battery is converted into The primary precursor mixture is recovered through water washing and acid solution treatment to recover high-purity lithium precursors.
The recovery rate and purity of lithium precursors are improved, side reactions and particle aggregation are suppressed, environmental pollution and by-products are reduced, and an efficient and eco-friendly recycling process is achieved.
Smart Images

Figure CN115175876B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for recovering active metals from lithium secondary batteries. More specifically, the present invention relates to a method for recovering active metals from waste positive electrodes of lithium secondary batteries. Background Art
[0002] Recently, secondary batteries have been widely used as power sources for mobile electronic devices such as camcorders, mobile phones, laptop computers, etc., and vehicles such as electric vehicles, hybrid vehicles, etc. Lithium secondary batteries have been actively developed and used in secondary batteries due to their advantages such as high operating voltage, high energy density per unit weight, high charging rate, and compact size.
[0003] Lithium metal oxide can be used as an active material for a positive electrode of a lithium secondary battery. Lithium metal oxide may further contain a transition metal such as nickel, cobalt, manganese, and the like.
[0004] Since the above-mentioned high-cost valuable metals are used for the positive electrode active material, the production cost of manufacturing the positive electrode material is more than 20%. In addition, due to the increasing prominence of environmental protection issues, people are studying the recycling method of the positive electrode active material.
[0005] Conventionally, a method of sequentially recovering valuable metals by leaching spent positive electrode active materials in strong acids such as sulfuric acid has been used, but wet methods may be disadvantageous in terms of regeneration selectivity and regeneration time, and may cause environmental pollution. Therefore, a method of recovering valuable metals using dry reactions is being studied.
[0006] However, due to the reaction heat generated in the dry reaction process, side reactions and particle agglomeration may occur, thereby reducing the recovery rate of active materials.
[0007] For example, Korean Registered Patent Publication No. 10-0709268 discloses an apparatus and method for recycling waste manganese batteries and alkaline batteries, but does not provide a dry method for regenerating valuable metals with high selectivity and high yield. Summary of the invention
[0008] [Technical goals]
[0009] According to one aspect of the present invention, there is provided a method for recovering active metals of a lithium secondary battery with high recovery efficiency and high yield.
[0010] [Technical means]
[0011] In a method for recovering active metals of a lithium secondary battery according to an embodiment of the present invention, a positive electrode active material mixture is prepared from a positive electrode of a lithium secondary battery. A first reduction process using a first reduction reaction gas and a second reduction process using a second reduction reaction gas having a higher reaction source concentration than the first reduction reaction gas are sequentially and continuously performed to convert the positive electrode active material mixture into a primary precursor mixture. A lithium precursor is recovered from the primary precursor mixture.
[0012] In some embodiments, the first reduction reaction gas and the second reduction reaction gas may include hydrogen, and the hydrogen concentration of the first reduction reaction gas may be less than the hydrogen concentration of the second reduction reaction gas.
[0013] In some embodiments, the hydrogen concentration of the first reduction reaction gas may be in a range of 5 vol % to 15 vol %, and the hydrogen concentration of the second reduction reaction gas may be 20 vol % or more.
[0014] In some embodiments, the hydrogen concentration of the first reduction reaction gas may be in a range of 5 vol% to 10 vol%, and the hydrogen concentration of the second reduction reaction gas may be in a range of 20 vol% to 40 vol%.
[0015] In some embodiments, the reaction temperature of the second reduction process may be higher than the reaction temperature of the first reduction process.
[0016] In some embodiments, the reaction temperature of the first reduction process may be in the range of 300°C to 450°C, and the reaction temperature of the second reduction process may be in the range of 460°C to 800°C.
[0017] In some embodiments, the first reduction process and the second reduction process may include supplying a first reduction reaction gas and a second reduction reaction gas into a fluidized bed reactor, respectively.
[0018] In some embodiments, the primary precursor mixture may include primary lithium precursor particles and transition metal-containing particles.
[0019] In some embodiments, the primary lithium precursor particles may include at least one of lithium hydroxide, lithium oxide, and / or lithium carbonate.
[0020] In some embodiments, in recovering the lithium precursor, the primary lithium precursor particles may be washed with water.
[0021] In some embodiments, the transition metal-containing particles may include nickel, cobalt, manganese, or oxides thereof.
[0022] In some embodiments, the transition metal-containing particles can be selectively treated with an acid solution to recover the transition metal precursor in the form of an acid salt.
[0023] [Effects of the Invention]
[0024] According to the exemplary embodiment described above, the lithium precursor can be recovered from the spent positive electrode active material by a dry method using a hydrogen reduction process. Therefore, the lithium precursor can be recovered with high purity without performing an additional process caused by a wet method.
[0025] In an exemplary embodiment, the hydrogen reduction process may include a first hydrogen reduction process performed under conditions where the hydrogen concentration is reduced and a second hydrogen reduction process performed under conditions where the hydrogen concentration is increased. The initial hydrogen concentration may be reduced to prevent sudden heating during hydrogen reduction, thereby inhibiting side reactions and particle aggregation. Therefore, the recovery rate of the desired lithium precursor may be increased. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 is a schematic flow chart for describing a method of recovering active metals of a lithium secondary battery according to an exemplary embodiment. DETAILED DESCRIPTION
[0027] Embodiments of the present invention provide a high-purity, high-yield method for recovering active metals from lithium secondary batteries using a dry reduction reaction.
[0028] Hereinafter, embodiments of the present invention will be described in detail with reference to the accompanying drawings. However, these embodiments are provided as examples, and the present invention is not limited to the specific embodiments described herein.
[0029] As used herein, the term "precursor" is used to generally refer to a compound containing a specific metal to provide the specific metal contained in an electrode active material.
[0030] Figure 1 Schematic flow chart for describing a method for recovering active metals of a lithium secondary battery according to an exemplary embodiment. For convenience of description, Figure 1 The schematic structure of the reactor and the process flow are also shown.
[0031] Reference Figure 1 , a positive electrode active material mixture (waste positive electrode active material mixture) can be prepared from waste positive electrodes of lithium secondary batteries (for example, in the process of S10 ).
[0032] A lithium secondary battery may include an electrode assembly including a positive electrode, a negative electrode, and a separator layer interposed between the positive electrode and the negative electrode. The positive electrode and the negative electrode may include a positive electrode active material layer coated on a positive electrode current collector and a negative electrode active material layer coated on a negative electrode current collector, respectively.
[0033] For example, the positive electrode active material included in the positive electrode active material layer may include an oxide containing lithium and a transition metal.
[0034] In some embodiments, the positive electrode active material may include a compound represented by the following Chemical Formula 1.
[0035] [Chemical Formula 1]
[0036] Li x M1 a M2 b M3 c O y
[0037] In Chemical Formula 1, M1, M2, and M3 may each independently include at least one element selected from Ni, Co, Mn, Na, Mg, Ca, Ti, V, Cr, Cu, Zn, Ge, Sr, Ag, Ba, Zr, Nb, Mo, Al, Ga, or B. In Chemical Formula 1, 0 < x ≤ 1.1, 2 ≤ y ≤ 2.02, 0 < a < 1, 0 < b < 1, 0 < c < 1, and 0 < a + b + c ≤ 1.
[0038] In some embodiments, the positive electrode active material may be an NCM-based lithium oxide including nickel, cobalt, and manganese.
[0039] The waste positive electrode can be recovered by separating the positive electrode from the waste lithium secondary battery. The waste positive electrode may include a positive electrode current collector (e.g., aluminum (Al)) and the positive electrode active material layer as described above, and the positive electrode active material layer may include a conductive material, a binder, and the positive electrode active material as described above.
[0040] The conductive material may include, for example, a carbon-based material such as graphite, carbon black, graphene, carbon nanotubes, etc. The binder may include a resin material such as polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinylidene fluoride (PVDF), polyacrylonitrile, polymethyl methacrylate, etc.
[0041] In an exemplary embodiment, the recovered waste positive electrode may be pulverized to produce a positive electrode active material mixture. Accordingly, the positive electrode active material mixture may be prepared in a powder form. As described above, the positive electrode active material mixture may include a powder of a lithium-transition metal oxide, for example, a powder of an NCM-based lithium oxide (e.g., Li(NCM)O2).
[0042] The term "positive electrode active material mixture" used in the present application may refer to the raw materials put into the reduction reaction treatment to be described below after the positive electrode current collector is substantially removed from the waste positive electrode. In one embodiment, the positive electrode active material mixture may include positive electrode active material particles, such as NCM-based lithium oxide. In one embodiment, the positive electrode active material mixture may include a portion of a component derived from a binder or a conductive material. In one embodiment, the positive electrode active material mixture may be substantially composed of positive electrode active material particles.
[0043] In some embodiments, the average particle size (D50) of the positive active material mixture (e.g., a particle size based on volume cumulative particle size distribution) may be 5 μm to 100 μm. Within the above range, the lithium-transition metal oxide to be recycled, such as Li(NCM)O2, can be easily separated from the positive current collector, the conductive material contained in the positive active material mixture, and the binder.
[0044] In some embodiments, the positive electrode active material mixture may be heat treated before being put into the reduction reactor to be described below. Impurities such as conductive materials and binders contained in the positive electrode active material mixture may be removed or reduced by heat treatment, so that the lithium-transition metal oxide may be introduced into the reduction reactor with high purity.
[0045] The temperature of the heat treatment may be, for example, about 100° C. to 500° C., preferably about 350° C. to 450° C. Within the above range, impurities may be substantially removed while preventing the lithium-transition metal oxide from being decomposed and damaged.
[0046] For example, in the process of S20 , the positive electrode active material mixture may react in the reduction reactor 100 to form the primary precursor mixture 80 .
[0047] like Figure 1 As shown, the reduction reactor 100 may be divided into a reactor body 130, a lower reactor portion 110, and an upper reactor portion 150. The reactor body 130 may include a heating means such as a heater or may be integrated with a heating means such as a heater.
[0048] The positive active material mixture may be supplied to the reactor body 130 through the supply flow path 106a and the supply flow path 106b. The positive active material mixture may be dripped through the first supply flow path 106a connected to the upper reactor portion 150, or may be introduced through the second supply flow path 106b connected to the bottom of the reactor body 130. In one embodiment, the first supply flow path 106a and the second supply flow path 106b may be used together to supply the positive active material mixture.
[0049] For example, the support unit 120 may be disposed between the reactor body 130 and the lower reactor portion 110 so that the spent positive active material mixture powder may be placed thereon. The support unit 120 may include holes or injection holes through which the reduction reaction gas and / or carrier gas described below may pass.
[0050] Reduction reaction gas for converting the cathode active material mixture into a primary precursor may be supplied into the reactor body 130 through a reaction gas flow path 102 connected to the lower reactor portion 110. In an exemplary embodiment, the reduction reaction gas may include hydrogen (H2) as a reaction source.
[0051] The reduction reaction gas may be supplied from the lower portion of the reduction reactor 100 to contact the cathode active material mixture so that the cathode active material mixture may react with the reduction reaction gas to be converted into a primary precursor while moving to the upper reactor portion 150 or residing in the reactor body 130 .
[0052] In some embodiments, the reduction reaction gas may be injected to form a fluidized bed in the reactor body 130. Therefore, the reduction reactor 100 may be a fluidized bed reactor. The positive electrode active material mixture may contact the reduction reaction gas while repeatedly rising, staying, and falling in the fluidized bed, thereby increasing the reaction contact time and improving particle dispersion. Therefore, a primary precursor mixture 80 having a substantially uniform size distribution may be obtained.
[0053] However, the concept of the present invention is not necessarily limited to a fluidized bed reaction. For example, a fixed reaction in which a reduction reaction gas is supplied after pre-loading a cathode active material mixture in a batch reactor may be performed.
[0054] In an exemplary embodiment, a first reduction process using a first reduction reaction gas having a relatively low reduction concentration (reaction source concentration) and a second reduction process using a second reduction reaction gas having a relatively high reduction concentration may be sequentially and continuously performed in the reduction reactor 100 .
[0055] For example, a first reduction reaction gas having a relatively low hydrogen concentration is used in the first reduction process, and a second reduction reaction gas having a relatively high hydrogen concentration may be used in the second reduction process.
[0056] In some embodiments, the hydrogen concentration of the first reduction reaction gas may be in the range of about 5 vol% to 15 vol%. The hydrogen concentration of the second reduction reaction gas may be in the range of about 20 vol% or more.
[0057] For example, the reducing reaction gas may further include a carrier gas, such as nitrogen (N2) or argon (Ar). The reducing concentration or hydrogen concentration may be the volume % of the reducing component (eg, hydrogen) in the total volume of the reaction gas including the carrier gas.
[0058] The hydrogen reduction process of metal components such as lithium and transition metals is an exothermic process, so the heat generation increases rapidly as the concentration of hydrogen used increases. In this case, the temperature in the reduction reactor 100 may also increase, and the positive active material mixture may melt or aggregate with each other. Therefore, the final recovery rate of the lithium precursor may also be reduced.
[0059] When the reaction temperature in the reduction reactor 100 is lowered to reduce the amount of heat generated, sufficient reaction rate and yield may not be achieved.
[0060] However, according to an exemplary embodiment, a first reduction process with a low hydrogen concentration may be performed before a second reduction process with an increased hydrogen concentration. The positive electrode active material mixture may be subjected to a primary reduction treatment by the first reduction process. Therefore, even if the hydrogen concentration increases in the subsequent second reduction process, a reduction reaction for sufficiently generating a lithium precursor may be performed while suppressing rapid heat generation.
[0061] In a preferred embodiment, the hydrogen concentration of the first reduction reaction gas may be in the range of about 5 vol% to 10 vol%. The hydrogen concentration of the second reduction reaction gas may be adjusted in the range of about 20 vol% to 40 vol% to suppress excessive heat generation.
[0062] In some embodiments, the reaction temperature of the first reduction process may be in the range of about 300° C. to 450° C. The reaction temperature of the second reduction process may be higher than the reaction temperature of the first reduction process.
[0063] The first reduction process using the first reduction reaction gas with low hydrogen concentration can suppress the heating amount, so the reaction temperature can be relatively increased in the second reduction process using the second reduction reaction gas with high hydrogen concentration. Therefore, a sufficient reduction reaction and recovery rate of the lithium precursor can be achieved through the second reduction process.
[0064] For example, the reaction temperature of the second reduction process may be in the range of about 460°C to 800°C.
[0065] In some embodiments, if the first reduction reaction gas and the second reduction reaction gas are supplied at the same flow rate, the reaction time of the second reduction process can be increased compared to the reaction time of the first reduction process. As described above, the heat generation can be suppressed by the first reduction process, so that the reaction time of the second reduction process can be increased to obtain a sufficient reduction reaction and a recovery rate of the lithium precursor.
[0066] The reduction reaction gas may be supplied from the bottom of the reduction reactor 100 to contact the positive active material mixture, so that the positive active material mixture may move to the upper reactor portion 150 to expand the reaction area and may be converted into a primary precursor.
[0067] In some embodiments, the lithium-transition metal oxide can be reduced by a reducing reaction gas to produce a primary lithium precursor including, for example, lithium hydroxide (LiOH), lithium oxide (e.g., Li2O) and a transition metal or transition metal oxide. For example, Ni, Co, NiO, CoO and MnO can be produced together with the primary lithium precursor by a reduction reaction.
[0068] Thus, a primary precursor mixture 80 including primary lithium precursor particles 60 and transition metal-containing particles 70 (eg, transition metal or transition metal oxide) may be formed in the reactor body 130. The primary lithium precursor particles 60 may include, for example, lithium hydroxide, lithium oxide, and / or lithium carbonate.
[0069] The transition metal-containing particles 70 including nickel, cobalt, or manganese may be relatively heavier than the primary lithium precursor particles 60 , and thus the primary lithium precursor particles 60 may be pre-collected through the outlet 160 a and the outlet 160 b .
[0070] In one embodiment, the primary lithium precursor particles 60 may be discharged through the first outlet 160a connected to the upper reactor portion 150. In this case, selective recovery of the primary lithium precursor particles 60 based on a weight gradient may be facilitated.
[0071] In one embodiment, the primary precursor mixture 80 including the primary lithium precursor particles 60 and the transition metal-containing particles 70 may be collected through the second outlet 160b connected to the reactor body 130. In this case, the primary precursor mixture 80 may be directly recovered from the fluidized bed forming area to increase productivity.
[0072] In one embodiment, the primary precursor mixture 80 may be collected together through the first outlet 160a and the second outlet 160b.
[0073] The primary lithium precursor particles 60 collected through the outlet 160 a and the outlet 160 b may be recovered as a lithium precursor (eg, in the process of S30 ).
[0074] In some embodiments, the primary lithium precursor particles 60 may be washed with water. The primary lithium precursor particles in the form of lithium hydroxide (LiOH) may be substantially dissolved in water by the washing process, separated from the transition metal precursor, and recovered in advance. The lithium precursor substantially consisting of lithium hydroxide may be obtained by subjecting lithium hydroxide dissolved in water to a crystallization process, etc.
[0075] In one embodiment, the primary lithium precursor particles in the form of lithium oxide and lithium carbonate may be substantially removed by the washing process. In one embodiment, the primary lithium precursor particles in the form of lithium oxide and lithium carbonate may be at least partially converted into lithium hydroxide by the washing process.
[0076] In some embodiments, the primary lithium precursor particles 60 can react with a carbon-containing gas such as carbon monoxide (CO), carbon dioxide (CO2), etc. to obtain lithium carbonate (e.g., Li2CO3) as a lithium precursor. A crystalline lithium precursor can be obtained by reacting with a carbon-containing gas. For example, lithium carbonate can be collected by injecting a carbon-containing gas together during a washing process.
[0077] The crystallization reaction temperature by the carbon-containing gas may be in the range of, for example, about 60° C. to 150° C. Within the above temperature range, lithium carbonate with high reliability may be produced without destroying the crystal structure.
[0078] As described above, according to exemplary embodiments, a lithium precursor may be recovered from a spent positive electrode through a continuous dry method.
[0079] In the comparative example, a wet method such as a leaching method with a strong acid can be used to recover lithium or transition metals from waste secondary batteries. However, the selective separation of lithium in the wet method may be limited. In addition, a washing process is required to remove solution residues, and the formation of byproducts such as hydrates may be increased due to solution contact.
[0080] However, according to an embodiment of the present invention, the lithium precursor can be collected by a dry reduction reaction, in which the use solution can be excluded. Therefore, the yield can be increased and the by-products can be reduced, and wastewater treatment may not be required, so that an eco-friendly process design can be implemented.
[0081] In addition, the reduction process can be performed in a stepwise manner by changing the reducing concentration to suppress excessive heat generation, so that the lithium precursor can be recovered with high purity and high yield.
[0082] In some embodiments, a transition metal precursor may be obtained from the collected transition metal-containing particles 70 (eg, in the process of S40 ).
[0083] For example, primary lithium precursor particles 60 may be collected through outlet 160a and outlet 160b, and then transition metal-containing particles 70 may be recovered. Thereafter, transition metal-containing particles 70 may be treated with an acid solution to form a precursor in the form of an acid salt of each transition metal.
[0084] In one embodiment, the primary lithium precursor particles 60 and the transition metal-containing particles 70 may be collected together and may be subjected to a washing process. In this case, the primary lithium precursor particles 60 may be converted and dissolved into a lithium precursor such as lithium hydroxide, and the transition metal-containing particles 70 may be precipitated. The precipitated transition metal-containing particles 70 may be collected again and treated with an acid solution.
[0085] In one embodiment, sulfuric acid can be used as the acid solution. In this case, NiSO4, MnSO4 and CoSO4 can each be recovered as a transition metal precursor.
[0086] As described above, the lithium precursor can be collected by a dry method, and then the transition metal precursor can be selectively extracted using an acid solution. Therefore, the purity and selectivity of each metal precursor can be improved, and the load of the wet method can be reduced, thereby also reducing the amount of wastewater and by-products.
[0087] Hereinafter, preferred embodiments are proposed to more specifically describe the present invention. However, the following examples are only used to illustrate the present invention, and those skilled in the relevant art will clearly understand that various changes and modifications can be made within the scope and spirit of the present invention. Such changes and modifications are appropriately included in the appended claims.
[0088] Example 1
[0089] 1kg of positive electrode material separated from waste lithium secondary batteries was heat treated at 450°C for 1 hour. The heat-treated positive electrode material was cut into small pieces and ground to obtain a Li-Ni-Co-Mn oxide positive electrode active material sample. 20g of the positive electrode active material sample was placed in a fluidized bed reactor, and a 10 volume % hydrogen / 90 volume % nitrogen mixed gas was injected from the bottom of the reactor at a flow rate of 400mL / min for 1 hour, while the temperature inside the reactor was maintained at 460°C (first reduction process).
[0090] After this, 20 volume % hydrogen / 80 volume % nitrogen mixed gas was injected at a flow rate of 400 mL / minute for 2 hours (the second reduction reaction process). After the reduction reaction, the sample was recovered, 19 times of water (based on weight) was added, and the lithium concentration dissolved in the water was analyzed to measure the final lithium recovery rate. In addition, the rising of the reaction temperature in the reduction process was also measured.
[0091] Example 2
[0092] Lithium was recovered by the same method as in Example 1, except that a mixed gas of 5 vol % hydrogen / 90 vol % nitrogen was used in the first reduction process, and a mixed gas of 20 vol % hydrogen / 80 vol % nitrogen was used in the second reduction process.
[0093] Example 3
[0094] Lithium was recovered by the same method as in Example 1, except that the reaction temperature of the first reduction process was adjusted to 400°C, and the reaction temperature of the second reduction process was adjusted to 500°C.
[0095] Example 4
[0096] Lithium was recovered by the same method as in Example 1, except that a mixed gas of 15 vol % hydrogen / 85 vol % nitrogen was used in the first reduction process.
[0097] Comparative Example
[0098] Lithium was recovered by the same method as in Example 1, except that the reduction process was performed by injecting a mixed gas of 20 vol % hydrogen / 80 vol % nitrogen from the bottom of the reactor at a flow rate of 10 mL / min for 3 hours.
[0099] The evaluation results are shown in Table 1 below.
[0100] [Table 1]
[0101] Reaction temperature rise (℃) Lithium recovery rate (%) Example 1 16 74 Example 2 8 81 Example 3 15 80 Example 4 18 71 Comparative Example 58 60
[0102] Referring to Table 1, in the example of performing the two-step reduction process, compared with the comparative example, the lithium recovery rate was improved while the increase of the reaction temperature was significantly suppressed.
Claims
1. A method for recovering active metals from a lithium secondary battery, comprising: Preparing a positive electrode active material mixture from a positive electrode of a lithium secondary battery; sequentially and continuously performing a first reduction process using a first reduction reaction gas and a second reduction process using a second reduction reaction gas having a higher reaction source concentration than that of the first reduction reaction gas to convert the positive electrode active material mixture into a primary precursor mixture; and recovering a lithium precursor from the primary precursor mixture, wherein the first reduction reaction gas and the second reduction reaction gas include hydrogen, and The hydrogen concentration of the first reduction reaction gas is in the range of 5 volume % to 15 volume %, and the hydrogen concentration of the second reduction reaction gas is greater than 20 volume %.
2. The method for recovering active metals from lithium secondary batteries according to claim 1, wherein: The hydrogen concentration of the first reduction reaction gas is in a range of 5 volume % to 10 volume %, and the hydrogen concentration of the second reduction reaction gas is in a range of 20 volume % to 40 volume %.
3. The method for recovering active metals from lithium secondary batteries according to claim 1, wherein: A reaction temperature of the second reduction process is higher than a reaction temperature of the first reduction process.
4. The method for recovering active metals from lithium secondary batteries according to claim 3, wherein: A reaction temperature of the first reduction process is in a range of 300°C to 450°C, and a reaction temperature of the second reduction process is in a range of 460°C to 800°C.
5. The method for recovering active metals from lithium secondary batteries according to claim 1, wherein: The first reduction process and the second reduction process include supplying the first reduction reaction gas and the second reduction reaction gas into a fluidized bed reactor, respectively.
6. The method for recovering active metals from lithium secondary batteries according to claim 1, wherein: The primary precursor mixture includes primary lithium precursor particles and transition metal-containing particles.
7. The method for recovering active metals from lithium secondary batteries according to claim 6, wherein: The primary lithium precursor particles include at least one of lithium hydroxide, lithium oxide and lithium carbonate.
8. The method for recovering active metals from lithium secondary batteries according to claim 6, wherein: The recovering of the lithium precursor includes washing the primary lithium precursor particles with water.
9. The method for recovering active metals from lithium secondary batteries according to claim 6, wherein: The transition metal-containing particles include nickel, cobalt, manganese or oxides thereof. 10 . The method for recovering active metals of lithium secondary batteries according to claim 9 , further comprising selectively treating the transition metal-containing particles with an acid solution to recover the transition metal precursor in the form of an acid salt.
Citation Information
Patent Citations
A recycling apparatus for used zinc-carbon and alkaline batteries and its method
KR100709268B1
Recovery method of positive active material in lithium ion battery waste material
CN103794832A
Method for comprehensively recycling valuable metals from spent lithium ion battery
CN107017443A
Method for recovering lithium from lithium-containing electrode waste material
CN108220607A
Method for efficiently and selectively extracting lithium from waste lithium battery through flash reduction
CN110408796A