A flexible transparent surface-enhanced Raman substrate for pesticide residue detection, its construction method and application

By using corn stalks and chloroalic acid to build a flexible transparent surface-enhanced Raman substrate, the existing pesticide residue detection methods are solved, and efficient qualitative and quantitative detection of pesticide Fumeishuang is achieved, reducing detection costs and resources waste.

CN115201178BActive Publication Date: 2024-11-05CHINA AGRI UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211023060.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-08-25
Publication Date
2024-11-05
Estimated Expiration
2042-08-25

AI Technical Summary

Technical Problem

The existing pesticide residue detection methods have complex pretreatment steps, long time and high requirements for detectors. The commonly used flexible SERS substrate preparation process is complex and costly, and has high environmental pollution.

Method used

Using corn stalks and chloroacid as raw materials, by extracting corn stalk cellulose and preparing corn stalk-based cellulose acetate, combining gold nanoparticles, building a flexible transparent surface to enhance the Raman substrate, reducing pretreatment steps, and achieving the pesticide Fumeishuang Qualitative quantitative detection.

Benefits of technology

It reduces detection costs, digests agricultural waste resources, reduces resource waste, improves detection efficiency and stability, simplifies operations, and realizes high-precision quantitative analysis of pesticide residues.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115201178B_ABST
    Figure CN115201178B_ABST
Patent Text Reader

Abstract

A flexible transparent surface-enhanced Raman substrate for pesticide residue detection, the flexible transparent surface-enhanced Raman substrate is made of corn stalks and chloroauric acid as raw materials; the Raman substrate construction method comprises the following steps: treating corn stalks with a peracetic acid / maleic acid composite acid, acetylating the obtained corn stalk-based cellulose with trifluoroacetic acid / acetic anhydride to prepare cellulose acetate, and reducing the chloroauric acid with sodium citrate to obtain gold nanoparticles; finally, a casting solution is prepared by blending, a substrate is prepared by a scraping film method, and qualitative and quantitative analysis is performed using p-aminothiophenol and thiram pesticides; the method of the invention detects pesticide residues such as thiram, and has the advantages of being non-destructive, rapid, requiring no pre-treatment, and having high sensitivity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of agricultural technology, and specifically relates to a flexible transparent surface enhanced Raman substrate for pesticide residue detection, a construction method of the flexible transparent surface enhanced Raman substrate and its application in pesticide residue detection. Background Art

[0002] Surface-enhanced Raman spectroscopy not only has the advantages of rapid, non-destructive and effective detection of aqueous samples, but also can achieve high-precision detection of biological and chemical trace molecules. The enhancement mechanism of surface-enhanced Raman technology is mainly due to the localized surface plasmon resonance phenomenon of coinage metal (gold, silver, copper) nanoparticles. When the laser irradiates the surface of the nanoparticles, there is an enhanced electric field region within the range of 2-10nm on the surface of the nanoparticles, and the Raman spectrum intensity is proportional to the fourth power of the electric field enhancement. Therefore, this phenomenon can enhance the Raman scattering signal of the molecules falling in the region, and the enhancement effect is as high as 106-1010 times.

[0003] Compared with simple nanoparticles, SERS substrates can fix "hot spots" and increase the stability and uniformity of the test. Compared with metal SERS substrates and silicon-based SERS substrates, flexible SERS substrates have flexible sampling methods, mainly using tape, cellulose materials or polymers as carriers, and using wiping sampling, filtration enrichment and adsorption sampling and other testing methods, avoiding sample pretreatment steps, greatly reducing sample pretreatment time, and improving detection efficiency. Its application potential is huge and has the opportunity to become one of the ways to commercialize products.

[0004] Commonly used pesticide residue detection methods usually include complex pre-treatment steps, the main purpose of which is to extract pesticides from samples. Mature extraction methods mainly include extraction, QuEChERS and gel chromatography, followed by quantitative detection of pesticide molecules using high-precision detection methods such as liquid or gas mass spectrometry. Based on the above detection methods, my country has implemented a series of pesticide detection standards, which stipulate detection methods for most types of pesticides on the market. However, these detection methods have many pre-treatment steps, require the destruction of the test object, take a long time for subsequent detection, and have high experimental operation requirements for the tester.

[0005] Paper was the earliest carrier material used as a flexible SERS substrate. It can achieve flexible sampling, such as for uneven sample surfaces. Later, nanocellulose was used as a substitute for paper to achieve better detection effects. Later, membrane materials were also used as flexible carriers. Nylon membranes can adsorb charged gold nanoparticles by electrostatic action, and achieve filtration enrichment tests to reduce test time and reduce the detection limit of aminothiophenol. The unique viscosity of the tape can stick silver nanoparticles to the surface, and then use the viscosity to pick up pesticide residues on the surface of the fruit for detection. The flexible and transparent PDMS film can use its unique optical transparency to realize in-situ permeability testing of pesticides on the apple surface. However, the preparation of PDMS requires complex chemical processes, which is costly and will cause certain environmental pollution.

[0006] Cellulose acetate film material, which also has good optical transparency, is a common cellulose derivative. It can be prepared by acetylation of cellulose and acetic acid, and the preparation process is very mature. Cellulose is an important biomass raw material product, and the process of purifying and separating it through straw is also very mature. The raw materials for substrate preparation can be obtained through biomass, which can not only effectively reduce costs, but also digest some agricultural waste straw resources and reduce resource waste. Summary of the invention

[0007] In view of the problems existing in the above-mentioned prior art, the present invention aims to provide a flexible transparent surface-enhanced Raman substrate for determining the residual pesticide thiram in agricultural water bodies and on the surface of fruits and vegetables, a method for constructing the substrate, and a qualitative and quantitative analysis of the pesticide. The testing method of the substrate of the present invention can greatly reduce the pre-test processing steps and can achieve qualitative and quantitative detection of thiram pesticide molecules.

[0008] To achieve the above objectives, the first aspect of the present invention is to provide a flexible transparent surface-enhanced Raman substrate for pesticide residue detection, wherein the flexible transparent surface-enhanced Raman substrate is made of corn stalks and chloroauric acid.

[0009] The second aspect of the present invention is to provide a method for constructing the above-mentioned flexible transparent surface-enhanced Raman substrate for pesticide residue detection, comprising the following steps:

[0010] The first step is the extraction and separation of corn straw cellulose:

[0011] The corn stalks are mechanically crushed into 40 mesh particles, placed in a microwave reactor, and an acid solution (peracetic acid / maleic acid) is added according to a certain solid-liquid ratio; the reaction time and temperature are adjusted to react, and then the solid residue is filtered and washed to separate the corn stalk cellulose. For details, please refer to the published patent: One-step method for separating cellulose from wood fiber raw materials (CN111101394A), which is cited in its entirety in this application.

[0012] Step 2: Preparation of corn straw-based cellulose acetate:

[0013] Take the solid dried in the first step, add trifluoroacetic acid and acetic anhydride, stir to carry out esterification reaction, pour the mixed solution after the reaction on a glass plate to completely air dry, then wash with deionized water, dry and crush for later use. For details, please refer to the published patent: A green and efficient method for preparing corn straw-based triacetyl cellulose porous membrane (CN113083039A), which is cited in the present application in its entirety.

[0014] The third step is to prepare 25mmol / L chloroauric acid aqueous solution and 0.4-1% w / v sodium citrate dihydrate aqueous solution respectively, then heat 100mL of deionized water to boiling, add 1mL of chloroauric acid aqueous solution and sodium citrate dihydrate solution in sequence, continue stirring until the solution changes from light yellow to black, and finally to brown red, continue stirring and cool to room temperature. The obtained sol is the gold nanoparticle sol, which is stored at 4°C for future use.

[0015] The fourth step is to prepare the casting solution: concentrate the sol obtained in the third step by centrifugation, then replace the solvent with N,N-dimethylacetamide, use the solid crushed in the second step as the solute, and the mixed liquid after centrifugation and concentration as the solvent to prepare the casting solution, stir it thoroughly until the solute is completely dissolved in the solvent, and let the casting solution stand for a long enough time until the bubbles are removed.

[0016] The fifth step is to prepare the substrate: use a scraper to scrape a film of a certain thickness on a flat glass plate, air-dry it in a fume hood at room temperature, use deionized water as an anti-solvent to perform solvent exchange, obtain a membrane material, and store it in deionized water for later use.

[0017] Step 6: Prepare aqueous solutions of p-aminothiophenol and thiram pesticide respectively, and immerse the substrate completely in the solution to be tested. After ultrasonic treatment for different time periods, take out the substrate, air dry it, and test the Raman signal.

[0018] Step 7. At the same time, use the aluminum foil surface to simulate the residues of p-aminothiophenol and thiram on the surface of fruits and vegetables, and immerse the substrate completely in the extraction solvent. Take out the substrate and attach it to the surface of the pesticide residues, and test the Raman signal after air drying.

[0019] Preferably, in step (3), the concentration of chloroauric acid added is 0.25 mmol / L, and the concentration of sodium citrate dihydrate is 0.004-0.01% w / v.

[0020] Preferably, in step (4), the concentration of the gold nanoparticles is 10-100 times.

[0021] Preferably, in step (4), the amount of cellulose acetate added is 7-10%.

[0022] Preferably, in step (5), the thickness of the scraped film is 0.3-0.5 mm.

[0023] Preferably, the aqueous solution of p-aminothiophenol and thiram pesticide prepared in step (6) is 10 -8 -10 - 6 g / mL.

[0024] Preferably, in step (6), the ultrasonic time in the ultrasonic test is 30-180 min.

[0025] Preferably, the amount of residue on the surface of the simulated fruits and vegetables in step (7) is 30-3000 ng / cm 2 .

[0026] Preferably, the extraction solvent in step (7) is methanol, ethanol and water.

[0027] The third aspect of the present invention is to use the flexible transparent surface-enhanced Raman substrate for pesticide residue detection of the present invention to conduct qualitative and quantitative analysis of aminothiophenol and thiram pesticides.

[0028] The present invention adopts the above technical solution to have the following advantages:

[0029] (1) The present invention uses a biomass raw material, corn stalks, as a raw material for preparing the substrate, which can not only effectively reduce costs, but also digest part of agricultural waste straw resources and reduce resource waste.

[0030] (2) The present invention encapsulates gold nanoparticles inside the corn straw-based cellulose acetate membrane material, thereby ensuring the uniformity and stability of the substrate test and improving the storage performance of the substrate.

[0031] (3) The flexible transparent substrate material of the present invention can not only detect pesticide residues in water environment through ultrasonic treatment, but also can realize in-situ permeability test on the surface of fruits and vegetables by utilizing its unique optical transparency, thereby reducing the pre-treatment steps of pesticide residue detection. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1Morphological characterization of the substrate prepared in Example 1 of the present invention.

[0033] Figure 2 UV-Visible spectrum characterization of the substrate prepared in Example 1 of the present invention.

[0034] Figure 3 The linear range of the two characteristic peaks of p-aminothiophenol in ultrasonic testing on the substrate prepared in Example 1.

[0035] Figure 4 The linear range of the characteristic peak of thiram pesticide in ultrasonic testing on the substrate prepared in Example 1.

[0036] Figure 5 The linear range of the in-situ permeability test of the two characteristic peaks of p-aminothiophenol on the substrate prepared in Example 1.

[0037] Figure 6 The linear range of the in-situ permeability test of the characteristic peak of thiram pesticide on the substrate prepared in Example 1. DETAILED DESCRIPTION

[0038] The present invention will be described in detail below with reference to embodiments.

[0039] Embodiment 1:

[0040] The construction of surface-enhanced Raman substrate for determining pesticide residues in agricultural water and on the surface of fruits and vegetables includes the following steps

[0041] The first step is the extraction and separation of corn straw cellulose:

[0042] 4 g of corn stalks crushed to 40 mesh were added to 160 mL of a mixed dilute acid solution (containing 1.5% peracetic acid and 3% maleic acid), placed in a microwave reactor, and heated at 130° C. for 1 h. The obtained solid was washed until neutral and dried for later use.

[0043] Step 2: Preparation of corn straw-based cellulose acetate:

[0044] Take 1 g of the solid dried in the first step, add 20 mL of trifluoroacetic acid and 5 mL of acetic anhydride, stir and react for 1 hour, pour the mixed solution onto a glass plate and dry it completely, then wash it with deionized water until it is neutral, dry it in an oven at 60°C, and store it at room temperature for later use.

[0045] The third step is to prepare 25mmol / L chloroauric acid aqueous solution and 1% w / v sodium citrate dihydrate aqueous solution respectively, then heat 100mL of deionized water to boiling, add 1mL of chloroauric acid aqueous solution and sodium citrate dihydrate solution in sequence, and continue stirring until the solution changes from light yellow to black and finally to brown red, and continue stirring and cooling to room temperature. The obtained sol is the gold nanoparticle sol, which is stored at 4°C for future use.

[0046] Furthermore, the sol obtained in the third step is concentrated by centrifugation 50 times, and then the solvent is replaced with N, N-dimethylacetamide. The solid crushed in the second step is used as the solute, and the mixed liquid after centrifugation and concentration is used as the solvent to prepare a casting solution with a mass fraction of 7%. The solution is stirred thoroughly until the solute is completely dissolved in the solvent, and the casting solution is allowed to stand for a sufficiently long time until the bubbles are removed.

[0047] Furthermore, a film with a thickness of 0.3 mm was scraped from a flat glass plate with a scraper, and after being completely air-dried in a fume hood at room temperature, deionized water was used as an anti-solvent for solvent exchange to obtain a membrane material, which was stored in deionized water for later use.

[0048] Step 4: Prepare different concentrations of p-aminothiophenol aqueous solutions and immerse the substrate completely in 2 mL of the solution to be tested. After ultrasonic treatment for 180 min, take out the substrate, air dry it, and test the Raman signal.

[0049] Raman spectra were measured using a confocal Raman microspectrometer (SENTERRA II, Bruker, Germany). The measurement conditions were as follows: the laser light source wavelength was 785 nm, the laser energy was 10 mW, the integration time was 1 s, the objective lens magnification was 10×, and the spectrum test range was 50-3655 cm-1. A single test spectrum had 16 items, and the average was taken as the test result for one test. The average spectrum was taken as the spectral data of the sample after three tests. The sample spectrum was intercepted from 400 to 2000 cm-1, and then baseline correction and smoothing were performed, and then the spectral intensity at the characteristic peak of the sample was qualitatively and quantitatively analyzed.

[0050] The results showed that under ultrasonic testing, the characteristic peak of p-aminothiophenol could be detected at a concentration of 10-8g / mL, and the linear range of the signal was 10 -8 -10 -7 g / mL.

[0051] Embodiment 2:

[0052] The construction of the surface-enhanced Raman substrate for the determination of pesticide residues in agricultural water and on the surface of fruits and vegetables includes the following steps:

[0053] The first step is the extraction and separation of corn straw cellulose:

[0054] 4 g of corn stalks crushed to 40 mesh were added to 160 mL of a mixed dilute acid solution (containing 1.5% peracetic acid and 3% maleic acid), placed in a microwave reactor, and heated at 130° C. for 1 h. The obtained solid was washed until neutral and dried for later use.

[0055] Step 2: Preparation of corn straw-based cellulose acetate:

[0056] Take 1 g of the solid dried in the first step, add 20 mL of trifluoroacetic acid and 5 mL of acetic anhydride, stir and react for 1 hour, pour the mixed solution onto a glass plate and dry it completely, then wash it with deionized water until it is neutral, dry it in an oven at 60°C, and store it at room temperature for later use.

[0057] The third step is to prepare 25mmol / L chloroauric acid aqueous solution and 1% w / v sodium citrate dihydrate aqueous solution respectively, then heat 100mL of deionized water to boiling, add 1mL of chloroauric acid aqueous solution and sodium citrate dihydrate solution in sequence, and continue stirring until the solution changes from light yellow to black and finally to brown red, and continue stirring and cooling to room temperature. The obtained sol is the gold nanoparticle sol, which is stored at 4°C for future use.

[0058] Furthermore, the sol obtained in the third step is concentrated by centrifugation 50 times, and then the solvent is replaced with N, N-dimethylacetamide. The solid crushed in the second step is used as the solute, and the mixed liquid after centrifugation and concentration is used as the solvent to prepare a casting solution with a mass fraction of 7%. The solution is stirred thoroughly until the solute is completely dissolved in the solvent, and the casting solution is allowed to stand for a sufficiently long time until the bubbles are removed.

[0059] Furthermore, a film with a thickness of 0.3 mm was scraped from a flat glass plate with a scraper, and after being completely air-dried in a fume hood at room temperature, deionized water was used as an anti-solvent for solvent exchange to obtain a membrane material, which was stored in deionized water for later use.

[0060] Step 4: Prepare different concentrations of thiram pesticide aqueous solutions and immerse the substrate completely in 2 mL of the solution to be tested. After ultrasonic treatment for 180 min, take out the substrate, air dry it, and test the Raman signal.

[0061] Raman spectra were measured using a confocal Raman microspectrometer (SENTERRA II, Bruker, Germany) under the following measurement conditions: laser source wavelength of 785 nm, laser energy of 10 mW, integration time of 1 s, objective lens magnification of 10×, and spectral test range of 50–3655 cm -1 . A single test spectrum has 16 pieces, and the average is taken as the test result of one test. The average spectrum is taken as the spectrum data of the sample after three tests. The sample spectrum is intercepted from 400-2000cm -1 The sample is then subjected to baseline correction and smoothing, and the spectral intensity at the characteristic peak of the sample is then subjected to qualitative and quantitative analysis.

[0062] The results showed that under ultrasonic testing, the pesticide Thiram could -7 The characteristic peak was detected at a concentration of 3 × 10 -7 -10 -6 g / mL.

[0063] Embodiment 3:

[0064] The construction of the surface-enhanced Raman substrate for the determination of pesticide residues in agricultural water and on the surface of fruits and vegetables includes the following steps:

[0065] The first step is the extraction and separation of corn straw cellulose:

[0066] 4 g of corn stalks crushed to 40 mesh were added to 160 mL of a mixed dilute acid solution (containing 1.5% peracetic acid and 3% maleic acid), placed in a microwave reactor, and heated at 130° C. for 1 h. The obtained solid was washed until neutral and dried for later use.

[0067] Step 2: Preparation of corn straw-based cellulose acetate:

[0068] Take 1 g of the solid dried in the first step, add 20 mL of trifluoroacetic acid and 5 mL of acetic anhydride, stir and react for 1 hour, pour the mixed solution onto a glass plate and dry it completely, then wash it with deionized water until it is neutral, dry it in an oven at 60°C, and store it at room temperature for later use.

[0069] The third step is to prepare 25mmol / L chloroauric acid aqueous solution and 1% w / v sodium citrate dihydrate aqueous solution respectively, then heat 100mL of deionized water to boiling, add 1mL of chloroauric acid aqueous solution and sodium citrate dihydrate solution in sequence, and continue stirring until the solution changes from light yellow to black and finally to brown red, and continue stirring and cooling to room temperature. The obtained sol is the gold nanoparticle sol, which is stored at 4°C for future use.

[0070] Furthermore, the sol obtained in the third step is concentrated by centrifugation 50 times, and then the solvent is replaced with N, N-dimethylacetamide. The solid crushed in the second step is used as the solute, and the mixed liquid after centrifugation and concentration is used as the solvent to prepare a casting solution with a mass fraction of 7%. The solution is stirred thoroughly until the solute is completely dissolved in the solvent, and the casting solution is allowed to stand for a sufficiently long time until the bubbles are removed.

[0071] Furthermore, a film with a thickness of 0.3 mm was scraped from a flat glass plate with a scraper, and after being completely air-dried in a fume hood at room temperature, deionized water was used as an anti-solvent for solvent exchange to obtain a membrane material, which was stored in deionized water for later use.

[0072] In the fourth step, aqueous solutions of p-aminothiophenol with different concentrations were prepared respectively, and 30 μL of the solution was dropped on the surface of aluminum foil to simulate the surface of fruits and vegetables. After the droplets were completely air-dried, the substrate completely immersed in the methanol solvent was taken out and attached to the air-dried pesticide droplets. After the substrate was air-dried, the Raman signal was tested.

[0073] Raman spectra were measured using a confocal Raman microspectrometer (SENTERRA II, Bruker, Germany) under the following measurement conditions: laser source wavelength of 785 nm, laser energy of 10 mW, integration time of 1 s, objective lens magnification of 10×, and spectral test range of 50–3655 cm -1 . A single test spectrum has 16 pieces, and the average is taken as the test result of one test. The average spectrum is taken as the spectrum data of the sample after three tests. The sample spectrum is intercepted from 400-2000cm -1 The sample is then subjected to baseline correction and smoothing, and the spectral intensity at the characteristic peak of the sample is then subjected to qualitative and quantitative analysis.

[0074] The results showed that under the in-situ permeability test, p-aminothiophenol could detect a characteristic peak at 30 ng / cm2, and the linear range of the signal was 30-300 ng / cm 2 .

[0075] Embodiment 4:

[0076] The construction of the surface-enhanced Raman substrate for the determination of pesticide residues in agricultural water and on the surface of fruits and vegetables includes the following steps:

[0077] The first step is the extraction and separation of corn straw cellulose:

[0078] 4 g of corn stalks crushed to 40 mesh were added to 160 mL of a mixed dilute acid solution (containing 1.5% peracetic acid and 3% maleic acid), placed in a microwave reactor, and heated at 130° C. for 1 h. The obtained solid was washed until neutral and dried for later use.

[0079] Step 2: Preparation of corn straw-based cellulose acetate:

[0080] Take 1 g of the solid dried in the first step, add 20 mL of trifluoroacetic acid and 5 mL of acetic anhydride, stir and react for 1 hour, pour the mixed solution onto a glass plate and dry it completely, then wash it with deionized water until it is neutral, dry it in an oven at 60°C, and store it at room temperature for later use.

[0081] The third step is to prepare 25mmol / L chloroauric acid aqueous solution and 1% w / v sodium citrate dihydrate aqueous solution respectively, then heat 100mL of deionized water to boiling, add 1mL of chloroauric acid aqueous solution and sodium citrate dihydrate solution in sequence, and continue stirring until the solution changes from light yellow to black and finally to brown red, and continue stirring and cooling to room temperature. The obtained sol is the gold nanoparticle sol, which is stored at 4°C for future use.

[0082] Furthermore, the sol obtained in the third step is concentrated by centrifugation 50 times, and then the solvent is replaced with N, N-dimethylacetamide. The solid crushed in the second step is used as the solute, and the mixed liquid after centrifugation and concentration is used as the solvent to prepare a casting solution with a mass fraction of 7%. The solution is stirred thoroughly until the solute is completely dissolved in the solvent, and the casting solution is allowed to stand for a sufficiently long time until the bubbles are removed.

[0083] Furthermore, a film with a thickness of 0.3 mm was scraped from a flat glass plate with a scraper, and after being completely air-dried in a fume hood at room temperature, deionized water was used as an anti-solvent for solvent exchange to obtain a membrane material, which was stored in deionized water for later use.

[0084] The fourth step is to prepare different concentrations of aqueous solutions of the pesticide thiram, and drop 30 μL of the solution on the surface of aluminum foil to simulate the surface of fruits and vegetables. After the droplets are completely air-dried, take out the substrate completely immersed in the methanol solvent and attach it to the air-dried pesticide droplets. After the substrate is air-dried, test the Raman signal.

[0085] Raman spectra were measured using a confocal Raman microspectrometer (SENTERRA II, Bruker, Germany) under the following measurement conditions: laser source wavelength of 785 nm, laser energy of 10 mW, integration time of 1 s, objective lens magnification of 10×, and spectral test range of 50–3655 cm -1 . A single test spectrum has 16 pieces, and the average is taken as the test result of one test. The average spectrum is taken as the spectrum data of the sample after three tests. The sample spectrum is intercepted from 400-2000cm -1 The sample is then subjected to baseline correction and smoothing, and the spectral intensity at the characteristic peak of the sample is then subjected to qualitative and quantitative analysis.

[0086] The results showed that under the in-situ permeability test, the pesticide thiram could penetrate the 2 The characteristic peak was detected and the signal linear range was 300-3000ng / cm 2 .

[0087] The results of this test show that:

[0088] (1) Figure 1 From the morphological characterization, it can be seen that the surface enhanced Raman substrate prepared by the present invention embeds gold nanoparticles with plasmon resonance effect inside the substrate, and the surface has a certain pore structure to ensure the diffusion of the molecules to be tested from the aqueous solution to the inside of the substrate and the adsorption of the gold nanoparticles inside it during the test process;

[0089] (2) Figure 2The UV-visible spectrum test shows that the surface enhanced Raman substrate prepared by the present invention has a plasmon resonance peak at a wavelength of 533.8nm, indicating the existence of a surface enhanced Raman effect. At an excitation wavelength of 785nm, the light transmittance of the substrate material is 15.25%, and in-situ transmittance testing can be achieved.

[0090] (3) Figure 3-4 This is an ultrasonic test of the aqueous solution of p-aminothiophenol and thiram based on the SERS substrate prepared in Example 1. The 1080 cm -1 and 1588cm -1 The two peak signals correspond to the stretching vibration of the CS bond and the stretching vibration of the CC bond respectively; the 1368cm -1 Corresponding to the asymmetric swing vibration of the CH3 group, the results showed that under ultrasonic testing, p-aminothiophenol could detect characteristic peaks at a concentration of 10-8 g / mL, and the signal linear range was 10-8-10-7 g / mL; thiram pesticide could detect characteristic peaks at a concentration of 3×10 -7 The characteristic peak was detected at a concentration of 3 × 10 -7 -10 -6 g / mL.

[0091] (4) Figure 5-6 The results show that the in-situ permeability test of p-aminothiophenol and thiram pesticide aqueous solution based on the SERS substrate prepared in Example 1 shows that p-aminothiophenol can penetrate 30 ng / cm 2 The characteristic peak was detected and the signal linear range was 30-300ng / cm 2 ; Thiram can be used at 300ng / cm 2 The characteristic peak was detected and the signal linear range was 300-3000ng / cm 2 .

[0092] In summary, the present invention constructs a flexible transparent surface-enhanced Raman substrate for pesticide residue detection based on corn straw raw materials, which belongs to the field of surface-enhanced Raman detection. First, corn straw cellulose is separated by a mature corn straw cellulose purification process; then, corn straw-based cellulose acetate is obtained by acetylation with trifluoroacetic acid / acetic anhydride.

[0093] Gold nanoparticles were prepared by the traditional citrate reduction method, then centrifuged and concentrated, and the solvent was exchanged for N, N-dimethylacetamide. Finally, corn straw-based cellulose acetate was used as the solute, and the N, N-dimethylacetamide solution of gold nanoparticles was used as the solvent to prepare casting solutions of different concentrations. The base material was scraped by the scraping method. The uniform gold nanoparticles embedded inside the base made the test have a good enhancement effect and test uniformity, and the unique light transmittance of the base made the in-situ permeability test possible. Thus, the detection limit and test linear range of p-aminothiophenol and the pesticide thiram were determined. The test method of the present invention includes ultrasonic testing for pesticide residues in water and in-situ permeability testing for pesticide residues on the surface of fruits and vegetables. The test operation is simple, the test accuracy and stability are good, the pre-treatment steps of the test are greatly reduced, and the detection of p-aminothiophenol and thiram pesticide residues in water and on the surface of fruits and vegetables can be realized.

[0094] Those skilled in the art will readily appreciate other embodiments of the present disclosure after considering the specification and practicing the disclosure disclosed herein. This application is intended to cover any variations, uses, or adaptations of the present disclosure that follow the general principles of the present disclosure and include common knowledge or customary techniques in the art that are not disclosed in the present disclosure. The specification and examples are intended to be exemplary only, and the true scope and spirit of the present disclosure are indicated by the following claims.

[0095] It should be understood that the present disclosure is not limited to the exact structures that have been described above and shown in the drawings, and that various modifications and changes may be made without departing from the scope thereof. The scope of the present disclosure is limited only by the appended claims.

Claims

1. A method for constructing a flexible transparent surface-enhanced Raman substrate for pesticide residue detection, wherein the flexible transparent surface-enhanced Raman substrate is made of corn stalks and chloroauric acid, and comprises the following steps: (1) Extraction and separation of corn straw cellulose: The crushed corn straw is added to a mixed dilute acid solution and placed in a microwave reactor for reaction to remove most of the hemicellulose and lignin. The obtained solid is separated, washed, and dried for later use; (2) Preparation of corn straw-based cellulose acetate: Take the solid dried in step (1), add trifluoroacetic acid and acetic anhydride, stir to carry out esterification reaction, pour the mixed solution after the reaction onto a glass plate to completely air dry, then wash with deionized water, and dry for later use; (3) preparing chloroauric acid aqueous solution and sodium citrate dihydrate aqueous solution respectively, then heating a certain volume of deionized water to boiling, adding chloroauric acid aqueous solution and sodium citrate dihydrate solution in sequence, and continuously stirring until the solution changes from light yellow to black and finally to brownish red, and continuing to stir and cool to room temperature. The obtained sol is the gold nanoparticle sol, which is stored at 4°C for future use; (4) centrifugally concentrating the sol obtained in step (3), then replacing the solvent with N,N-dimethylacetamide, using the solid crushed in step (2) as the solute and the mixed liquid after centrifugation and concentration as the solvent to prepare a casting solution, stirring thoroughly until the solute is completely dissolved in the solvent, and allowing the casting solution to stand for a sufficient period of time until the bubbles are removed; the amount of cellulose acetate added is 7-10%; (5) Scrape a film of a certain thickness on a flat glass plate with a scraper, air-dry in a fume hood at room temperature, use deionized water as an anti-solvent for solvent exchange, obtain a film material, and store it in deionized water for later use; the uniform gold nanoparticles embedded inside the substrate enable the test to have a good enhancement effect and test uniformity; the thickness of the scraped film is 0.3-0.5 mm; (6) preparing aqueous solutions of p-aminothiophenol and thiram pesticide respectively, immersing the substrate completely in the solution to be tested, taking out the substrate after ultrasonic treatment for different time periods, and testing the Raman signal after air drying; (7) The aluminum foil surface was used to simulate the residues of p-aminothiophenol and thiram on the surface of fruits and vegetables. The substrate was completely immersed in the extraction solvent, the substrate was taken out and attached to the residual surface, and the Raman signal was tested after air drying.

2. The construction method according to claim 1, wherein in step (1), the mixed dilute acid solution is peracetic acid and maleic acid.

3. The construction method as described in claim 1, wherein in step (3), the concentration of the added chloroauric acid is 0.25 mmol / L, and the concentration of sodium citrate dihydrate is 0.004-0.01% w / v.

4. The construction method as described in claim 1, wherein the concentration of the gold nanoparticles in step (4) is 10-100 times.

5. The method of constructing as claimed in claim 1, wherein the aqueous solution of p-aminothiophenol and thiram pesticide prepared in step (6) is 10 -8 -10 -6 g / mL.

6. The construction method as claimed in claim 1, wherein in step (6), the ultrasonic time in the ultrasonic test is 30-180 min.

7. The construction method according to claim 1, wherein in step (7), the residual amount of the simulated fruit and vegetable surface residue is 30-3000 ng / cm 2 .

8. The construction method as claimed in claim 1, wherein the extraction solvent in step (7) is methanol, ethanol and water.

9. The construction method according to any one of claims 1 to 8, for use in qualitative and quantitative analysis of aminothiophenol and thiram pesticides.