Polyester film and its use

By using a polyester film with a bending direction retention angle of 155° or more and adding a hard coating, the problem of image distortion in foldable displays after repeated folding is solved, achieving high durability and excellent mobility and functionality.

CN115210304BActive Publication Date: 2024-10-25TOYOBO CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202180018802.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-03-09
Filing Date
2021-03-02
Publication Date
2024-10-25
Estimated Expiration
2041-03-02

Smart Images

  • Figure CN115210304B_ABST
    Figure CN115210304B_ABST
Patent Text Reader

Abstract

[Subject] In order to provide a foldable display with excellent mass productivity and no worries about distortion of the image displayed on the folded portion after bending, and a portable terminal device equipped with such a foldable display, a polyester film for a foldable display without creases or cracks in the folded portion is provided. [Solution] A polyester film for a foldable display, wherein the holding angle in the bending direction is greater than 155° and the maximum thermal shrinkage at 150°C is less than 1.5%. (Here, the holding angle refers to the angle of the bending mark formed after fixing at room temperature for 72 hours in a manner that applies a strain of 1.7% to each surface of the bent portion. In addition, the bending direction refers to the direction orthogonal to the folded portion).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a polyester film for a foldable display, a hard-coated film for a foldable display, a foldable display, and a portable terminal device, a foldable display and a portable terminal device that are not prone to image distortion due to film deformation even when repeatedly folded, and the aforementioned polyester film and hard-coated film for a foldable display. Background Art

[0002] As the lightweight of portable terminal devices is promoted, portable terminal devices represented by smartphones have become widely popular. Portable terminal devices are required to have various functions, but also convenience. Therefore, in the popular portable terminal devices, it is assumed that they can be easily operated with one hand and can be stored in the pocket of clothes, so a small screen size of about 6 inches is sometimes required.

[0003] On the other hand, tablet terminals with a screen size of 7 to 10 inches are expected to be used not only for video content and music but also for business purposes, drawing purposes, reading, etc., and have high functionality. However, they cannot be operated with one hand and have poor mobility, which poses a problem in terms of convenience.

[0004] In order to achieve these problems, a method of connecting a plurality of displays to make them compact has been proposed. However, since the remaining frame portion interrupts the image, a reduction in visibility is a problem and has not yet been widely used.

[0005] Therefore, in recent years, a portable terminal equipped with a flexible display or a foldable display has been proposed. In this way, the image is not interrupted, and the convenience of carrying the portable terminal device equipped with a large-screen display is good.

[0006] Here, for existing displays and portable terminal devices that do not have a folding structure, the surface of the display can be protected by non-flexible raw materials such as glass, but in a folding display, in the case of a display that forms one side with a folding portion, a hard-coated film that is flexible and can protect the surface must be used. However, in a folding display, the part that contacts the constant folding part is repeatedly bent, so the film in this part will deform over time, causing problems such as distortion of the image displayed in the display. In addition, not only can a film be used as a surface protection film, but also in a folding display, a polarizing plate, a phase difference plate, a touch panel substrate, a substrate of a display unit such as an organic EL, a protective component on the back, and various other parts can also use a film, and these films are also required to be durable against repeated folding.

[0007] Therefore, a method of partially changing the film thickness has been proposed (see, for example, Patent Document 1), but there is a problem of lack of mass productivity.

[0008] In addition, a method of adjusting the refractive index of the polyester film in the bending direction has been proposed, but there is a problem that the pencil hardness during hard coating is reduced as the refractive index in the bending direction is reduced, and the surface protection function of the display is reduced. In addition, if the refractive index in one direction is gradually reduced, the deformation during folding is gradually improved, but the uniaxial orientation in the folding direction is improved, and there is a problem of cracks or breaks in the folded part. In biaxially stretched films, no breakage occurs and productivity is also good, but deformation during folding is easily caused, and the resistance to bending is deteriorated.

[0009] Prior art literature

[0010] Patent Literature

[0011] Patent Document 1: Japanese Patent Application Publication No. 2016-155124 Summary of the invention

[0012] Problem that the invention aims to solve

[0013] The present invention intends to solve the above-mentioned problems of the components of the previous displays. In order to provide a foldable display with excellent mass producibility and no worries about distortion in the image displayed in the folded portion after bending, and a portable terminal device equipped with such a foldable display, the present invention intends to provide a polyester film for a foldable display that does not produce creases or cracks in the folded portion.

[0014] Solutions for solving problems

[0015] That is, the present invention includes the following configurations.

[0016] 1. A polyester film for a foldable display, wherein the holding angle in the bending direction is 155° or more and the maximum heat shrinkage at 150° C. is 1.5% or less.

[0017] (Here, the holding angle refers to the angle of the bend mark formed after fixing at room temperature for 72 hours in a manner that a strain of 1.7% is applied to both surfaces of the bent portion. In addition, the bending direction refers to the direction perpendicular to the folded portion.)

[0018] 2. The polyester film for foldable displays according to item 1 above, wherein the total light transmittance is 85% or more and the haze is 3% or less.

[0019] 3. The polyester film for foldable displays according to the first or second aspect, wherein an easy-adhesion layer is provided on at least one surface of the polyester film.

[0020] 4. A hard coat film for a foldable display, comprising a hard coat layer having a thickness of 1 to 50 μm on at least one surface of the polyester film for a foldable display according to any one of the first to third items.

[0021] 5. A foldable display, which is a foldable display configured with the hard coating film for foldable display described in the above-mentioned 4 as a surface protection film in a manner so that the hard coating layer is located on the surface, and is configured with a single hard coating film continuous through the folding portion of the foldable display.

[0022] 6. A portable terminal device having the foldable display as described in item 5 above.

[0023] Effects of the Invention

[0024] The polyester film for foldable displays and the foldable displays using the hard coating film of the present invention maintain mass productivity while not generating cracks in the folded portion of the polyester film, not causing deformation after folding, and not generating distortion of the image at the folded portion of the display. Portable terminal devices equipped with the polyester film and the foldable displays using the hard coating film provide beautiful images, are rich in functionality, and have excellent convenience such as portability. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 It is a schematic diagram for illustrating the bending radius when the foldable display of the present invention is folded.

[0026] Figure 2 This is a schematic diagram for illustrating the bending direction of the polyester film for a foldable display of the present invention.

[0027] Figure 3 It is a schematic diagram for illustrating the method of measuring the holding angle in the bending direction of the present invention.

[0028] Figure 4 This is a schematic diagram of a bent portion of a sample film for explaining a method of calculating the thickness of a spacer used in measuring a holding angle in a bending direction of the present invention. DETAILED DESCRIPTION

[0029] (monitor)

[0030] The display referred to in the present invention refers to all display devices. The types of displays include LCD, organic EL display, inorganic EL display, LED, FED, etc., but LCD, organic EL, and inorganic EL having a bendable structure are preferred. In particular, organic EL and inorganic EL that can reduce the layer structure are particularly preferred, and organic EL with a wide color gamut is further preferred.

[0031] (Foldable Display)

[0032] For a foldable display, a continuous single display can be folded in half or the like when moving. By folding, the size is reduced by half, and mobility can be improved. The bending radius of the foldable display is preferably 5 mm or less, and more preferably 3 mm or less. When the bending radius is 5 mm or less, thinning in the folded state becomes possible. It can be said that the smaller the bending radius, the better, but the smaller the bending radius, the easier it is to produce creases. The bending radius is preferably 0.1 mm or more, can be 0.5 mm or more, and can be 1 mm or more. Even if the bending radius is 1 mm, it is possible to achieve a thinness that is practical enough when moving. The bending radius when folded refers to the measurement of Figure 1 The radius of the inner side of the folded portion when folded is obtained from the position of the symbol 11 in the schematic diagram. It should be noted that the surface protection film described later may be located on the outer side or the inner side of the folded foldable display.

[0033] In addition, the foldable display may be folded in three or four ways, or may be a so-called rollable display, all of which fall within the scope of the foldable display in the present invention.

[0034] The polyester film for foldable display of the present invention can be used in any part as long as it is a constituent member of the foldable display. Hereinafter, the representative structure of the foldable display and the part where the polyester film of the present invention can be used are described by taking an organic EL display as an example. It should be noted that, hereinafter, the polyester film for foldable display of the present invention is sometimes referred to as the polyester film of the present invention.

[0035] (Foldable organic EL display)

[0036] The essential components of a foldable organic EL display are an organic EL module, and a circular polarizing plate, a touch panel module, a surface protection film, a back protection film, etc. may be further provided as necessary.

[0037] (Organic EL components)

[0038] The general structure of an organic EL component is formed by an electrode / electron transport layer / luminescent layer / hole transport layer / transparent electrode. As a substrate for providing an electrode, an electron transport layer, a luminescent layer, and a hole transport layer, the polyester film of the present invention can be used. It can be particularly preferably used as a substrate for a transparent electrode. In this case, the substrate film requires high barrier properties for water vapor and oxygen, and therefore, it is preferred to provide a barrier layer such as a metal oxide layer on the polyester film of the present invention. In order to improve the barrier properties, multiple barrier layers can be provided, and multiple polyester films provided with barrier layers can be used.

[0039] (Touch Panel Assembly)

[0040] Preferably, the portable terminal device has a touch panel. When an organic EL display is used, the touch panel assembly is preferably arranged on the upper part of the organic EL display or between the organic EL assembly / circular polarizer. The touch panel assembly has a transparent substrate such as a film and a transparent electrode arranged thereon. The polyester film of the present invention can be used as the transparent substrate. When used as a transparent substrate of a touch panel, a hard coating layer and a refractive index adjustment layer are preferably provided on the polyester film.

[0041] (Circular polarizing plate)

[0042] The circular polarizer reflects external light from the components inside the display to suppress the reduction of image quality. The circular polarizer has a linear polarizer and a phase difference plate. The linear polarizer has a protective film on at least the visible side of the polarizer. It is also possible to have a protective film on the surface of the polarizer opposite to the visible side, and it is also possible to directly laminate the phase difference plate on the polarizer. The phase difference plate uses a resin film with a phase difference such as polycarbonate, cyclic olefin, etc., and a phase difference layer formed by a liquid crystal compound is provided on the resin film. The polyester film of the present invention can be used as a polarizer protective film and a resin film of a phase difference plate. In these cases, the polyester film of the present invention preferably has a slow axis direction of the polyester film parallel or orthogonal to the absorption axis direction of the polarizer. It should be noted that a deviation of 10 degrees, preferably within 5 degrees, is allowed relative to the parallel or orthogonal.

[0043] (Surface protection film)

[0044] When an impact is applied to the display from above, there is a concern that the circuit of the organic EL component and the touch panel component may be broken, so in most cases, a surface protection film is provided. The polyester film of the present invention is used as the surface protection film. The surface protection film includes: the one that is loaded into the outermost surface of the display is called a cover window, and the one that is attached by the user himself, can be peeled off, and can be exchanged is called a back film, but the polyester film of the present invention can be used for all of them. When the polyester film of the present invention is used as a surface protection film, it is preferred that a hard coating layer is laminated on at least the surface side of the polyester film. The hard coating layer is made to be the visible side and is provided on the surface of the foldable display. It should be noted that the hard coating layer can also be provided on both sides.

[0045] (Back protection film)

[0046] It is also preferable to provide a protective film on the back side of the display. The polyester film of the present invention can be used as the protective film on the back side.

[0047] The polyester film of the present invention may be any other than the above-mentioned one as long as it is used in a folding portion of a constituent member of a foldable display.

[0048] Among these, the polyester film of the present invention is preferably used for covering a window surface protection film, a back film surface protection film, a base film of a touch panel module, and a back protection film. Furthermore, it is preferably used for covering a window surface protection film and a back film surface protection film.

[0049] In addition, as a foldable display, the polyester film of the present invention does not need to be used for all of the above. In addition to the polyester film of the present invention, a polyimide film, a polyamide film, a polyamideimide film, a polyester film other than the polyester film of the present invention, a polycarbonate film, an acrylic film, a triacetyl cellulose film, a cycloolefin polymer film, a polyphenylene sulfide film, a polymethylpentene film, etc. can be appropriately used in the foldable display according to suitability.

[0050] The polyester film of the present invention may be a single-layer film composed of one or more polyester resins, or, when two or more polyesters are used, may be a multilayer film or a super-multilayer laminated film having a repeated structure.

[0051] Examples of the polyester resin used in the polyester film include polyethylene terephthalate, polybutylene terephthalate, polyethylene 2,6-naphthalate, or a polyester film formed of a copolymer having the constituent components of these resins as the main component. Among them, a stretched polyethylene terephthalate film is particularly preferred from the perspectives of mechanical properties, heat resistance, transparency, price, etc.

[0052] When a polyester copolymer is used in a polyester film, as the dicarboxylic acid component of the polyester, for example, aliphatic dicarboxylic acids such as adipic acid and sebacic acid; aromatic dicarboxylic acids such as terephthalic acid, isophthalic acid, phthalic acid, and 2,6-naphthalene dicarboxylic acid; polyfunctional carboxylic acids such as trimellitic acid and pyromellitic acid. In addition, as the glycol component, for example, aliphatic glycols such as ethylene glycol, diethylene glycol, 1,4-butanediol, propylene glycol, and neopentyl glycol, aromatic glycols such as terephthalic alcohol, alicyclic glycols such as 1,4-cyclohexanedimethanol, and polyethylene glycols with an average molecular weight of 150 to 20,000 can be cited. The mass ratio of the copolymer components of the preferred copolymer is less than 20% by mass. When it is less than 20% by mass, the film strength, transparency, and heat resistance can be maintained, which is preferred.

[0053] In addition, in the manufacture of polyester film, the intrinsic viscosity of at least one or more resin pellets is preferably in the range of 0.50 to 1.0 dl / g. When the intrinsic viscosity is 0.50 dl / g or more, the impact resistance of the obtained film is improved, and it is not easy to cause the internal circuit of the display to break due to external impact, which is preferred. On the other hand, when the intrinsic viscosity is 1.00 dl / g or less, the filter pressure of the molten fluid will not increase excessively, and it is easy to operate the film production stably, which is preferred.

[0054] The thickness of the polyester film is preferably 10 to 80 μm, more preferably 25 to 75 μm. When the thickness is 10 μm or more, pencil hardness and impact resistance can be improved, and when the thickness is 80 μm or less, it is advantageous for weight reduction and has excellent flexibility, processability, and operability.

[0055] The surface of the polyester film of the present invention may be smooth or may have concavoconvexities, but since it is used for surface covering of a display, it is not preferred that the optical properties be reduced due to the concavoconvexities. As for the haze, it is preferably 3% or less, more preferably 2% or less, and most preferably 1% or less. When the haze is 3% or less, the visibility of the image can be improved. The lower limit of the haze is as small as possible, but from the perspective of stable production, it is preferably 0.1% or more, and can be 0.3% or more.

[0056] As mentioned above, in order to reduce the haze, it is preferred that the surface roughness of the film is not too large. However, from the perspective of operability, as a method of forming roughness in order to impart a certain degree of slippage, particles can be blended into the polyester resin layer of the surface layer, or a coating layer containing particles can be applied in the middle of film formation, thereby forming roughness.

[0057] As a method for blending particles in the polyester resin layer, a known method can be used. For example, the particles can be added at any stage of the polyester production, preferably in the stage of esterification or after the end of the transesterification reaction and before the start of the polycondensation reaction, in the form of a slurry dispersed in ethylene glycol or the like, to promote the polycondensation reaction. In addition, the particles can be blended by the following methods: a method of blending a slurry of particles dispersed in ethylene glycol or water or the like with a polyester raw material using a kneading extruder with a vent; or a method of blending dried particles with a polyester raw material using a kneading extruder.

[0058] Among them, the following method is preferred: adding the inorganic particles in the form of aggregates uniformly dispersed in a monomer solution that is a part of the polyester raw material and then filtered to the remaining portion of the polyester raw material before, during or after the esterification reaction. According to this method, since the monomer solution has a low viscosity, it is easy to uniformly disperse the particles and filter the slurry with high precision, and when adding to the remaining portion of the raw material, the particles have good dispersibility and are less likely to form new aggregates. From the above viewpoints, it is particularly preferred to add to the remaining portion of the raw material in a low temperature state before the esterification reaction.

[0059] Alternatively, the number of protrusions on the film surface can be further reduced by obtaining a polyester containing particles in advance and then kneading and extruding the pellets with a pellet not containing particles (masterbatch method).

[0060] The polyester film may contain various additives within a range in which the total light transmittance is maintained within a preferred range. Examples of the additives include antistatic agents, UV absorbers, and stabilizers.

[0061] The total light transmittance of the polyester film is preferably 85% or more, and more preferably 87% or more. If the light transmittance is 85% or more, visibility can be fully ensured. The higher the total light transmittance of the polyester film, the better, but from the perspective of stable production, it is preferably 99% or less, and can also be 97% or less.

[0062] The surface of the polyester film of the present invention may be subjected to a treatment for improving adhesion with a resin forming a hard coat layer or the like.

[0063] Examples of surface treatment methods include sandblasting, roughening treatment by solvent treatment, corona discharge treatment, electron beam irradiation treatment, plasma treatment, ozone / ultraviolet irradiation treatment, flame treatment, chromic acid treatment, and oxidation treatment such as hot air treatment, and any of the above methods can be used without particular limitation.

[0064] In addition, adhesion can be improved by an adhesion improving layer such as an easy-adhesion layer. As the easy-adhesion layer, acrylic resin, polyester resin, polyurethane resin, polyether resin, etc. can be used without particular limitation, and can be formed by a general coating technique, preferably a so-called in-line coating recipe.

[0065] The above-mentioned polyester film can be manufactured, for example, through the following steps: a polymerization step of uniformly dispersing inorganic particles in a monomer liquid that becomes a part of the polyester raw material and filtering, and then adding it to the remaining amount of the polyester raw material to polymerize the polyester; and a film forming step of melt-extruded the polyester into a sheet through a filter, cooling it, and then stretching it to form a substrate film.

[0066] Next, regarding the method for producing a biaxially stretched polyester film, an example of using pellets of polyethylene terephthalate (hereinafter, sometimes referred to as PET) as a raw material for a substrate film is described in detail, but the invention is not limited thereto. In addition, the number of layers such as a single-layer structure and a multi-layer structure is not limited.

[0067] After the pellets of PET are mixed and dried in a prescribed ratio, they are supplied to a known melt lamination extruder, extruded from a slit-shaped die into a sheet, cooled and solidified on a casting roll to form an unstretched film. In the case of a single layer, one extruder may be used, and in the case of a multi-layer film, two or more extruders, a multi-manifold or a confluence block (e.g., a confluence block with a square confluence portion) may be used to laminate a plurality of film layers constituting each outermost layer, extrude a sheet of two or more layers from a nozzle, and cool it on a casting roll to form an unstretched film.

[0068] In the above case, during melt extrusion, it is preferred to perform high-precision filtration at any position while the molten resin is maintained at about 280° C. to remove foreign matter contained in the resin. The filter material used in the high-precision filtration of the molten resin is not particularly limited, but a filter material made of sintered stainless steel is preferred because it excels in removing aggregates having Si, Ti, Sb, Ge, and Cu as main components and high-melting-point organic matter.

[0069] Furthermore, the filter particle size (initial filtration efficiency 95%) of the filter material is preferably less than 20 μm, particularly preferably less than 15 μm. When the filter particle size (initial filtration efficiency 95%) of the filter material exceeds 20 μm, foreign matter larger than 20 μm cannot be fully removed. Although high-precision filtration of molten resin using a filter material having a filter particle size (initial filtration efficiency 95%) of less than 20 μm sometimes reduces productivity, it is preferred in terms of obtaining a film with fewer protrusions caused by coarse particles.

[0070] (About maximum thermal shrinkage)

[0071] In the present invention, the maximum heat shrinkage of the polyester film after heat treatment at 150°C for 30 minutes is preferably 1.5% or less, more preferably 1.3% or less, further preferably 1.0% or less, and particularly preferably 0.5% or less. If the maximum heat shrinkage is 1.5% or less, it is possible to suppress planar defects such as curling and bending during hard coating processing. It can be said that the lower the heat shrinkage, the better, but it is preferably -1.0% or more, and more preferably 0% or more. A negative value of the heat shrinkage means that expansion occurs after heating, and even if it is less than -1.0%, it sometimes becomes planar defects. The maximum heat shrinkage can be effectively adjusted by adjusting the stretching ratio, using an offline annealing treatment or an aging treatment.

[0072] (About holding angle)

[0073] In the present invention, the holding angle in the bending direction is preferably 155° or more, more preferably 158° or more, and even more preferably 160° or more. The holding angle here refers to the angle of the bending trace formed after fixing at room temperature for 72 hours in a manner that a strain of 1.7% is applied to both surfaces of the bent portion according to the calculation described below. In addition, in the present invention, the bending direction refers to, Figure 2As shown by symbol 22 on the polyester film (symbol 2), it is in a direction orthogonal to the folding portion (symbol 21) envisioned in the use of the foldable display. If the holding angle is less than 155°, there is a possibility of causing deformation of the film and reducing the visibility of the display when the display is opened after folding for use, which may have an adverse effect on the function of the display. If the holding angle is more than 155°, there is less deformation and visibility can be well maintained. The holding angle can be effectively adjusted by controlling the refractive index by adjusting the stretching ratio and the stretching temperature. In addition, in order to increase the holding angle, a relaxation process in the stretching direction, an annealing treatment in the offline process, and an aging treatment can also be used. The holding angle in the bending direction is preferably 180°, but can be less than 175°, or less than 170°.

[0074] (About offline annealing treatment)

[0075] In the present invention, in order to increase the holding angle and reduce the maximum heat shrinkage, the manufactured film may be temporarily rolled up into a roll and then annealed offline. The temperature of the annealing treatment is 150°C to 200°C, more preferably 170°C to 190°C. The time for applying the above temperature is preferably 3 seconds to 90 seconds, more preferably 5 seconds to 60 seconds. By setting it within the above temperature range and time range, a good film that can achieve the target annealing treatment and maintain transparency can be obtained.

[0076] (About offline aging treatment)

[0077] In the present invention, in order to increase the holding angle and to reduce the maximum heat shrinkage, the manufactured film can be temporarily rolled up into a roll and then subjected to offline aging treatment. The temperature of the aging treatment is preferably above 50°C and below 70°C, and more preferably above 55°C and below 65°C. The treatment time is preferably above 72 hours, and more preferably above 120 hours. In the offline aging treatment, crystallization does not advance, causing conformational changes in the amorphous part, and it is believed that densification has occurred. It is believed that the elongation of the amorphous part occurs in the fatigue caused by the tensile stress applied to the outside during folding, so it is believed that densification has occurred, thereby reducing tensile fatigue. There is no upper limit for the aging time. If it is too long, it is sometimes difficult to produce. Therefore, it is preferably less than 1 month, can be less than 480 hours, and can also be less than 360 hours.

[0078] In the present invention, the stretching ratio of the unstretched polyester sheet is not particularly limited, but is preferably 1.2 to 6.0 times.

[0079] The stretching ratio in at least one of the longitudinal direction (mechanical flow direction) and the width direction, or the direction forming the bending direction, is preferably set to 1.2 to 2.0 times, and more preferably 1.7 to 2.0 times. By reducing the stretching ratio in the bending direction, the stress applied to the folded portion during folding can be reduced, and compression and tensile fatigue can be suppressed, thereby increasing the holding angle in the bending direction.

[0080] The stretching ratio in the direction perpendicular to the bending direction is preferably 4.2 times or less, and more preferably 4.0 times or less. By reducing the stretching ratio in the direction perpendicular to the bending direction, a maximum heat shrinkage of 1.5% or less can be achieved.

[0081] When the stretching is performed at 1.2 to 2.0 times in the bending direction, the stretching temperature is preferably 75 to 120° C., and more preferably 75 to 105° C. It should be noted that the heating method during stretching can be a conventionally known method such as a hot air heating method, a roller heating method, and an infrared heating method. By setting the stretching temperature to 75 to 120° C., large thickness unevenness caused by stretching at the above stretching ratio can be prevented.

[0082] The preheating temperature for stretching in the direction perpendicular to the bending direction is preferably 70 to 110° C. When multiple stretching is performed in the direction perpendicular to the bending direction, the stretching ratio in the second and subsequent stages is preferably higher than that in the first stage. Film relaxation can be performed by 1 to 10% in both the mechanical flow direction (length direction) and the perpendicular direction (width direction).

[0083] (About the density of polyester film)

[0084] The density of the polyester film is preferably 1.380 g / cm 3 More preferably 1.383 g / cm 3 By setting it to 1.380g / cm 3 The density is preferably higher, and although it depends on the presence or absence of particles in the film, 1.40 g / cm is preferred. 3 By setting the heat setting temperature during film formation to 180 to 240° C., crystallization can be advanced and the density can be effectively increased.

[0085] The intrinsic viscosity of the polyester film is preferably in the range of 0.50 to 1.0 dl / g. If the intrinsic viscosity is 0.50 dl / g or more, the impact resistance is improved, and the circuit breakage of the display internal circuit due to external impact is less likely to occur, which is preferred. On the other hand, if the intrinsic viscosity is 1.00 dl / g or less, the filter pressure of the molten fluid will not increase excessively, and the film production is stable, which is preferred.

[0086] (Easy Adhesion Layer)

[0087] In the present invention, in order to improve the adhesion between the polyester film and the hard coating layer, etc., it is also preferred to laminate an easy-adhesion layer on the polyester film. The easy-adhesion layer can be obtained as follows: After applying the coating liquid for forming the easy-adhesion layer to one or both sides of an unstretched or longitudinally uniaxially stretched film, heat treatment and drying are performed as required, and further stretching is performed in at least one direction of the unstretched film to obtain it. Heat treatment can also be performed after biaxial stretching. The final coating amount of the easy-adhesion layer is preferably managed to be 0.005 to 0.20 g / m 2 If the coating amount is 0.005g / m 2 On the other hand, if the coating amount is 0.20 g / m 2 Below, blocking resistance can be obtained and is therefore preferred.

[0088] As the resin contained in the coating liquid used in the lamination of the easy-adhesive layer, for example, polyester resin, polyether polyurethane resin, polyester polyurethane resin, polycarbonate polyurethane resin, acrylic resin, etc. can be used without particular limitation. As the cross-linking agent contained in the coating liquid for forming the easy-adhesive layer, melamine compounds, isocyanate compounds, oxazoline compounds, epoxy compounds, carbodiimide compounds, etc. can be cited. It is also possible to mix two or more and use them respectively. They are preferably coated with water-based coating liquids on the properties of the above-mentioned online coating, and the aforementioned resins and cross-linking agents are preferably water-soluble or water-dispersible resins and compounds.

[0089] In order to impart slipperiness to the easy-adhesive layer, it is preferred to add particles. The average particle size of the fine particles is preferably less than 2 μm. If the average particle size of the particles exceeds 2 μm, the particles become easy to fall off from the easy-adhesive layer. As the particles contained in the easy-adhesive layer, for example, inorganic particles such as titanium oxide, barium sulfate, calcium carbonate, calcium sulfate, silicon dioxide, aluminum oxide, talc, kaolin, clay, calcium phosphate, mica, hectorite, zirconium oxide, tungsten oxide, lithium fluoride, calcium fluoride, styrene-based, acrylic, melamine-based, benzoguanamine-based, silicone-based, etc. can be cited. Organic polymer particles, etc., can be added to the easy-adhesive layer alone, or two or more can be combined and added.

[0090] In addition, as a method for applying the coating liquid, a known method can be used in the same manner as the above-mentioned coating layer. For example, reverse roll / coating method, gravure / coating method, lip mouth / coating method, roller brush method, spray method, air knife coating method, wire rod coating method, tubular doctor blade method, etc. can be mentioned, and these methods can be carried out alone or in combination.

[0091] (Hard Coating)

[0092] When the polyester film of the present invention is located on the surface of a foldable display and used as a surface protection film to protect the display, it is preferred that at least one surface thereof has a hard coating layer. The hard coating layer is preferably located on the display surface side of the polyester film and used for the display. As the resin forming the hard coating layer, acrylic, siloxane, inorganic mixture, urethane acrylate, polyester acrylate, epoxy, etc. can be used without particular limitation. In addition, two or more materials can be mixed and used, and particles such as inorganic fillers and organic fillers can also be added.

[0093] (Film thickness of hard coat layer)

[0094] The film thickness of the hard coating layer is preferably 1 to 50 μm. If it is 1 μm or more, it is fully cured and the pencil hardness becomes high, which is preferred. In addition, by making the thickness less than 50 μm, curling caused by curing shrinkage of the hard coating layer can be suppressed, and the operability of the film can be improved.

[0095] (Coating method)

[0096] As the coating method of the hard coat layer, a Meyer bar, a gravure coater, a die coater, a knife coater, etc. can be used without particular limitation, and it can be appropriately selected according to the viscosity and the film thickness.

[0097] (Curing conditions)

[0098] As a method for curing the hard coat layer, a curing method using energy rays such as ultraviolet rays, electron beams, or heat can be used. In order to reduce damage to the film, a curing method using ultraviolet rays, electron beams, or the like is preferred.

[0099] (Pencil hardness)

[0100] The pencil hardness of the hard coat layer is preferably 3H or more, and more preferably 4H or more. If the pencil hardness is 3H or more, scratches are not easily caused, and visibility is not reduced. Generally, the pencil hardness of the hard coat layer is preferably high, but it can be 9H or less, 8H or less, or 6H or less, and it can be used without problems in practice.

[0101] (Characteristics of hard coating)

[0102] The hard coating layer in the present invention can be used for the purpose of improving the pencil hardness of the above-mentioned surface and protecting the display, and preferably has a high transmittance. As the transmittance of the hard coating film, it is preferably 87% or more, and more preferably 88% or more. If the transmittance is 87% or more, sufficient visibility is obtained. The total transmittance of the hard coating film is generally higher, the more preferred, but from the perspective of stable production, it is preferably 99% or less, and it can also be 97% or less. In addition, the haze of the hard coating film is generally preferably low, preferably 3% or less. The haze of the hard coating film is more preferably 2% or less, and most preferably 1% or less. If the haze is 3% or less, the visibility of the image can be improved. The lower the haze, the better, but from the perspective of stable production, it is preferably 0.1% or more, and it can also be 0.3% or more.

[0103] The hard coat layer may be further provided with other functions. For example, a hard coat layer provided with functions such as an antiglare layer, an antiglare antireflection layer, an antireflection layer, a low reflection layer, and an antistatic layer having a constant pencil hardness as described above may also be preferably applied to the present invention.

[0104] Moreover, in the case of a substrate film used as a touch panel component, a hard coating layer may also be provided. When an ITO layer is used as a transparent electrode layer of a touch panel component, for example, a refractive index adjustment layer is preferably provided between the substrate film and the transparent electrode layer in order to make the electrode pattern less visible. In this case, the hard coating layer itself may also serve as a refractive index adjustment layer, or a refractive index adjustment layer may be further laminated separately.

[0105] Example

[0106] Next, the present invention will be described using Examples and Comparative Examples. First, the evaluation method of the characteristic values ​​implemented in the present invention is shown below.

[0107] (1) Intrinsic viscosity

[0108] The film or polyester resin was crushed and dried, and then dissolved in a mixed solvent of phenol / tetrachloroethane = 60 / 40 (mass ratio). The solution was centrifuged to remove inorganic particles, and then the flow time of the solution with a concentration of 0.4 (g / dl) at 30°C and the flow time of the solvent alone were measured using an Ubbelohde viscometer. From the ratio of these time, the intrinsic viscosity was calculated using the Huggins formula, assuming that the Huggins constant was 0.38.

[0109] (2) Refractive index

[0110] The refractive index in the longitudinal direction, the refractive index in the width direction, and the refractive index in the thickness direction were determined using an Abbe refractometer (NAR-4T manufactured by ATAGO CO., LTD., measuring wavelength 589 nm) in accordance with JIS K7142:2008 “Method for determination of refractive index of plastics (Method A)”.

[0111] (3) Pencil hardness

[0112] The hard coating film was used as a sample and the pencil hardness was measured at a load of 750 g and a speed of 1.0 mm / s in accordance with JIS K 5600-5-4: 1999. In the present invention, a pencil hardness of 3H or more was regarded as acceptable.

[0113] (4) Total light transmittance, haze

[0114] The measurement was conducted using a haze meter (NDH5000, manufactured by Nippon Denshoku Industries, Ltd.).

[0115] (5) Density

[0116] The density was measured by the method according to JIS K 7112:1999 (density gradient tube method). (Unit: g / cm 3 ).

[0117] (6) Maximum thermal shrinkage

[0118] The sample film was cut into 10 mm in length and 250 mm in width, and marked at intervals of 200 mm along the direction of the long side to be measured. The marked interval A was measured under a constant tension of 5 g. Next, the sample film was placed in an oven at 150°C for 30 minutes without load, then taken out of the oven and cooled to room temperature. Then, the marked interval B was calculated under a constant tension of 5 g, and the heat shrinkage rate (%) was calculated using the following formula. It should be noted that the above heat shrinkage rate was measured at three equal positions along the width direction of the sample film, and the average value of the three points was taken as the heat shrinkage rate (%).

[0119] Thermal shrinkage (%) = [(AB) × 100] / A

[0120] The sample film was cut and measured in both the bending direction and the folding direction so that the longitudinal and transverse directions were different, and the data in the direction with the larger measured value was taken as the maximum heat shrinkage (%).

[0121] (7) Maintaining angle

[0122] The strength of the fold marks formed when the bent portion was fixed so as to apply a strain of 1.7% to each of the two surfaces was evaluated.

[0123] Figure 3This is a schematic diagram for illustrating the method of measuring the holding angle in the bending direction. The sample film (symbol 3) is cut into 10 mm in the width direction and 50 mm in the flow direction. Two PTFE plates (symbol 31) are overlapped. In the case of a 50 μm sample film, a 3 mm thick PTFE plate (symbol 32) is sandwiched between them as a spacer to form a gap. Double-sided tape is pasted on both ends of the sample, and the 3 mm gap of the PTFE plate is inserted in a bent state, and the two ends are fixed with double-sided tape. After being placed in an environment of 20°C and 65% RH for 72 hours, it is taken out from between the two PTFE plates (symbol 32), and the angle of the crease formed on the film is measured after 5 minutes (symbol 33). This angle is used as the holding angle.

[0124] In order to make the strain constant, the thickness of the PTFE plate used as a spacer was changed according to the thickness of the film. Figure 4 : An enlarged schematic diagram of a sample film (symbol 4) sandwiched between two PTFE plates (symbol 32) is shown in FIG. The neutral plane to which neither the compressive stress nor the tensile stress is applied is determined as the center in the thickness direction, and the difference between the neutral plane and the two surfaces is taken as strain. That is, the strain applied to the two surfaces can be expressed by the following formula.

[0125] Strain (1.7%)

[0126] =(|outermost or inner semicircle - neutral semicircle| / neutral semicircle) × 100

[0127] Here, when the thickness of the sample film is t (mm) and the bending diameter (outermost diameter), that is, the thickness of the spacer used, is d (mm) for the semicircle, they can be respectively calculated by the following formulas.

[0128] Outermost semicircle = d × π / 2

[0129] The semicircle of the neutral plane = (dt) × π / 2

[0130] The innermost semicircle = (d-2t) × π / 2

[0131] Based on the above, when the strain is set to 1.7%, the thickness is t (mm), and the bending diameter, i.e., the thickness of the spacer used is d (mm), the thickness of the PTFE sheet used for the spacer is determined by the following formula. The spacer thickness relative to the typical film thickness is shown in Table 1.

[0132] Spacer thickness d (mm) = film thickness (mm) × 60

[0133] Incidentally, in the case of the sample film having a thickness of 50 μm, the outermost diameter (symbol 41) is 3 mm, which is the same as the thickness d of the spacer, the innermost diameter (symbol 43) is 2.9 mm, and the diameter of the neutral plane (symbol 42) is 2.95 mm.

[0134] [Table 1]

[0135]

[0136] (Preparation of polyethylene terephthalate pellets (a))

[0137] As the esterification reaction apparatus, a continuous esterification reaction apparatus consisting of a stirring device, a partial condenser, and a three-stage complete mixing tank with a raw material input port and a product output port was used. TPA was set to 2 tons / hour, EG was set to 2 mol relative to 1 mol of TPA, and antimony trioxide was set to an amount in which Sb atoms were 160 ppm relative to the generated PET. These slurries were continuously supplied to the first esterification reactor of the esterification reaction apparatus, and the reaction was carried out at 255° C. under normal pressure with an average residence time of 4 hours.

[0138] Next, the reaction product in the first esterification reactor was continuously taken out of the system and supplied to the second esterification reactor, and EG distilled from the first esterification reactor was supplied to the second esterification reactor in an amount of 8% by mass relative to the produced polymer (produced PET), and further, an EG solution containing magnesium acetate in an amount of 65 ppm of Mg atoms relative to the produced PET and an EG solution containing TMPA in an amount of 20 ppm of P atoms relative to the produced PET were added, and the mixture was reacted at 260° C. at an average residence time of 1.5 hours under normal pressure. Next, the reaction product in the second esterification reactor was continuously taken out of the system and supplied to the third esterification reactor, and an EG solution containing TMPA in an amount of 20 ppm of P atoms relative to the produced PET was further added, and the mixture was reacted at 260° C. at an average residence time of 0.5 hours under normal pressure. The esterification reaction product generated in the third esterification reactor is continuously supplied to a three-stage continuous polycondensation reaction device for polycondensation, and then filtered using a stainless steel sintered filter material (nominal filtration accuracy 5 μm particles 90% cutoff) to obtain polyethylene terephthalate pellets (a) with an intrinsic viscosity of 0.62 dl / g.

[0139] (Preparation of polyethylene terephthalate pellets (b))

[0140] In the production process of the polyethylene terephthalate pellets (a), except that the residence time of the third esterification reaction was adjusted, the intrinsic viscosity was adjusted to 0.580 dl / g in the same manner to obtain polyethylene terephthalate pellets (b).

[0141] (Preparation of polyethylene terephthalate pellets (c))

[0142] The polyethylene terephthalate pellets (a) were subjected to solid phase polymerization using a rotary vacuum polymerization apparatus at a reduced pressure of 0.5 mmHg and 220° C. for varying periods of time to prepare polyethylene terephthalate pellets (c) having an intrinsic viscosity of 0.75 dl / g.

[0143] (Polymerization of polyurethane resin)

[0144] In a four-necked flask equipped with a stirrer, a serpentine condenser, a nitrogen inlet tube, a silicone gel drying tube and a thermometer, 72.96 parts by mass of 1,3-bis(isocyanatomethyl)cyclohexane, 12.60 parts by mass of dimethylolpropionic acid, 11.74 parts by mass of neopentyl glycol, 112.70 parts by mass of polycarbonate diol with a number average molecular weight of 2000, and 85.00 parts by mass of acetonitrile and 5.00 parts by mass of N-methylpyrrolidone as solvents were added, and stirred at 75°C for 3 hours under a nitrogen atmosphere to confirm that the reaction liquid reached the specified amine equivalent. Then, after cooling the reaction liquid to 40°C, 9.03 parts by mass of triethylamine was added to obtain a polyurethane prepolymer D solution. Next, 450 g of water was added to a reaction container equipped with a homogenizer capable of high-speed stirring, and the temperature was adjusted to 25°C while stirring for 2000 minutes. -1 The isocyanate group-terminated prepolymer was added and dispersed in water while stirring and mixing. Thereafter, acetonitrile and part of the water were removed under reduced pressure to prepare a water-soluble polyurethane resin (A) having a solid content of 35% by mass.

[0145] (Polymerization of water-soluble carbodiimide compounds)

[0146] In a flask equipped with a thermometer, a nitrogen inlet tube, a reflux condenser, a dropping funnel and a stirrer, 200 parts by mass of isophorone diisocyanate and 4 parts by mass of 3-methyl-1-phenyl-2-phosphorus-1-oxide as a carbodiimidization catalyst were added, and stirred at 180° C. for 10 hours under a nitrogen atmosphere to obtain isocyanate-terminated isophorone carbodiimide (polymerization degree = 5). Next, 111.2 g of the obtained carbodiimide and 80 g of polyethylene glycol monomethyl ether (molecular weight 400) were reacted at 100° C. for 24 hours. Water was slowly added thereto at 50° C. to obtain a yellow transparent water-soluble carbodiimide compound (B) having a solid content of 40% by mass.

[0147] (Preparation of coating liquid for forming an easily adhesive layer)

[0148] The following coating agents were mixed to prepare a coating liquid.

[0149]

[0150] 0.1 parts by weight of a leveling agent (BYK307, manufactured by BYK Japan, Ltd., concentration 100%) was added to 100 parts by weight of a hard coating material (Opstar (registered trademark) Z7503, manufactured by JSR Corporation, concentration 75%), and the mixture was diluted with methyl ethyl ketone to prepare a hard coating liquid a having a solid content concentration of 40% by weight.

[0151] (Example 1)

[0152] The pellets (a) of polyethylene terephthalate are supplied to the extruder and melted at 285°C. The polymer is filtered with a filter material of a stainless steel sintered body (nominal filtration accuracy 10μm particles 95% cutoff), extruded from a nozzle into a sheet, and then, by an electrostatic application casting method, contacted with a casting drum with a surface temperature of 30°C to cool and solidify, to prepare an unstretched film. The unstretched film is uniformly heated to 75°C with a heating roller, heated to 85°C with a non-contact heater, and 1.4 times roller stretching (longitudinal stretching) is performed. On the obtained uniaxially stretched film, the above-mentioned coating liquid for forming the easy-adhesion layer is applied on both sides by a roller coating method, and then dried at 80°C for 20 seconds. It should be noted that the final (after biaxial stretching) dried coating amount is 0.06g / m 2 Then, the film was introduced into a tenter and preheated at 105°C, stretched to 4.4 times in the transverse direction at 95°C, fixed in width, heat-set at 220°C for 5 seconds, and then relaxed by 4% in the width direction at 180°C to obtain a polyethylene terephthalate film roll with a thickness of 50 μm. The obtained polyethylene terephthalate film roll was subjected to an offline annealing treatment at 180°C for 30 seconds to obtain a polyester film. The evaluation results are shown in Table 2.

[0153] (Example 2)

[0154] The film roll obtained in the same manner as in Example 1 was subjected to an aging treatment at 60° C. for one week instead of an off-line annealing treatment, thereby obtaining a polyester film.

[0155] (Example 3)

[0156] A polyester film was obtained in the same manner as in Example 1 except that the stretching ratio in the longitudinal direction was changed to 2.7 times and the stretching ratio in the width direction was changed to 4.0 times.

[0157] (Example 4)

[0158] A polyester film was obtained in the same manner as in Example 2 except that the stretching ratio in the longitudinal direction was changed to 2.7 times and the stretching ratio in the width direction was changed to 4.0 times.

[0159] (Example 5)

[0160] A polyester film was obtained in the same manner as in Example 1 except that the stretching ratio in the longitudinal direction was changed to 3.4 times, the stretching ratio in the width direction was changed to 4.0 times, the heat setting temperature was changed to 230° C., and the annealing time was changed to 10 seconds.

[0161] (Example 6)

[0162] A polyester film was obtained in the same manner as in Example 1 except that the stretching ratio in the longitudinal direction was changed to 3.4 times, the stretching ratio in the width direction was changed to 4.0 times, and the heat setting temperature was changed to 230°C.

[0163] (Example 7)

[0164] A polyester film was obtained in the same manner as in Example 2 except that the stretching ratio in the longitudinal direction was changed to 3.4 times, the stretching ratio in the width direction was changed to 4.0 times, the heat setting temperature was changed to 230° C., and the aging time was changed to 5 days.

[0165] (Example 8)

[0166] A polyester film was obtained in the same manner as in Example 2 except that the stretching ratio in the longitudinal direction was changed to 3.4 times, the stretching ratio in the width direction was changed to 4.0 times, and the heat setting temperature was changed to 230°C.

[0167] (Example 9)

[0168] A polyester film was obtained in the same manner as in Example 2 except that the stretching ratio in the longitudinal direction was changed to 3.4 times, the stretching ratio in the width direction was changed to 4.0 times, the heat setting temperature was changed to 230° C., and the aging time was changed to 10 days.

[0169] (Example 10)

[0170] A polyester film was obtained in the same manner as in Example 1 except that the thickness was changed to 38 μm and the heat setting temperature was changed to 190° C.

[0171] (Example 11)

[0172] A polyester film was obtained in the same manner as in Example 2 except that the thickness was changed to 38 μm and the heat setting temperature was changed to 190° C.

[0173] (Example 12)

[0174] A polyester film was obtained in the same manner as in Example 1 except that the thickness was changed to 75 μm and the heat setting temperature was changed to 190° C.

[0175] (Example 13)

[0176] A polyester film was obtained in the same manner as in Example 2 except that the thickness was changed to 75 μm and the heat setting temperature was changed to 190° C.

[0177] (Comparative Example 1)

[0178] The film roll obtained in the same manner as in Example 1 was not subjected to annealing or aging treatment, thereby obtaining an untreated polyester film.

[0179] (Comparative Example 2)

[0180] The film roll obtained in the same manner as in Examples 3 to 4 was not subjected to annealing or aging treatment, thereby obtaining an untreated polyester film.

[0181] (Comparative Example 3)

[0182] The film rolls obtained in the same manner as in Examples 5 to 9 were not subjected to annealing or aging treatment to obtain untreated polyester films.

[0183] The hard coating solution a was applied to one side of the film prepared above using a Meyer bar so that the film thickness after drying was 5 μm, and then dried at 80° C. for 1 minute and irradiated with ultraviolet light (accumulated light intensity 200 mJ / cm 2 ) to obtain a hard coating film.

[0184] [Table 2A]

[0185]

[0186] [Table 2B]

[0187]

[0188] The hard coating film was bonded to the organic EL element via a 25 μm thick adhesive layer to form a Figure 1 A foldable display of the smartphone type in which the radius equivalent to the bending radius is 3 mm and can be folded in the center of the whole. The hard coating film is arranged on the surface of a continuous display with the folding portion sandwiched therebetween, and the hard coating layer is arranged on the surface of the display. When the hard coating film of each embodiment is used, the movement and visibility of a smartphone that can be folded and moved in the center are satisfied. In addition, the surface will not be dented due to external force. On the other hand, the foldable display using the hard coating film of each comparative example feels that the image is distorted at the folding portion of the display as the frequency of use increases, which is not preferred. In addition, dents and scratches are confirmed on the surface.

[0189] Industrial Applicability

[0190] The foldable display using the polyester film or hard coating film for foldable display of the present invention maintains mass productivity while not causing deformation after repeated folding of the polyester film or hard coating film on the surface of the foldable display, so that the image at the folded portion of the display is not distorted. In particular, a portable terminal device or image display device equipped with a foldable display using the polyester film or hard coating film of the present invention as a surface protection film provides beautiful images, is rich in functionality, and has excellent convenience such as mobility.

[0191] Description of Reference Numerals

[0192] 1: Foldable display

[0193] 11: Bending radius

[0194] 2: Polyester film for surface protection film of foldable display

[0195] 21: Folding part

[0196] 22: Bending direction (direction perpendicular to the folded portion)

[0197] 3: Sample film

[0198] 31: PTFE sheet

[0199] 32: Spacer (PTFE sheet)

[0200] 33: Keep Angle

[0201] 4: Sample film

[0202] 41: Outermost diameter

[0203] 42: Diameter of the neutral plane

[0204] 43: Innermost diameter

Claims

1. A polyethylene terephthalate film for a foldable display, having a bending angle of 164° or more, a maximum heat shrinkage of 1.5% or less at 150°C, an intrinsic viscosity of 0.50 to 1.0 dl / g, and a density of 1.380 g / cm 3 The polyethylene terephthalate film has a thickness of 10 to 80 μm. The polyethylene terephthalate film has an easy-adhesion layer on at least one side thereof. Here, the retention angle refers to the angle of the bending mark formed after fixing at room temperature for 72 hours in such a way that a strain of 1.7% is applied to both surfaces of the bent portion, and the bending direction refers to the direction orthogonal to the folded portion.

2. The polyethylene terephthalate film for a foldable display according to claim 1, wherein the total light transmittance is 85% or more and the haze is 3% or less.

3. A hard coating film for a foldable display, comprising a hard coating layer having a thickness of 1 to 50 μm on at least one surface of the polyethylene terephthalate film for a foldable display according to claim 1 or 2.

4. A foldable display, which is a foldable display configured with the hard coating film for a foldable display according to claim 3 as a surface protection film in a manner such that the hard coating layer is located on the surface, and is configured with a single hard coating film that is continuous through a folded portion of the foldable display.

5. A portable terminal device comprising the foldable display according to claim 4.