Method for manufacturing metal evaporation mask unit

During the manufacturing process of the evaporation mask unit, a combined technology of a resist film and a support frame is used to form an evaporation mask with multiple openings and fix its connection parts, thereby solving the problem of low manufacturing yield and low manufacturing yield in the prior art. The problem of high cost has been achieved, and efficient and low-cost evaporation mask unit manufacturing has been achieved.

CN115210402BActive Publication Date: 2024-10-18MAGNOLIA WHITE CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202180017957.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-02-19
Publication Date
2024-10-18
Estimated Expiration
2041-02-19

AI Technical Summary

Technical Problem

It is difficult to manufacture evaporation mask units with high efficiency and high yield with the existing technology efficiently and at low cost, resulting in low manufacturing yield and high cost.

Method used

By arranging a resist film on the first support substrate, forming a peeling layer and exposing it, a vapor deposition mask having a plurality of openings is formed, and the support frame is connected to the vapor deposition mask, and the connection portion is fixed by plating. Ensures stability and precision patterning of evaporation masks.

Benefits of technology

The evaporation mask unit is manufactured with high efficiency and high yield, which reduces the production cost, ensures the precise pattern and stability of the evaporation mask, and improves the quality of the finished product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115210402B_ABST
    Figure CN115210402B_ABST
Patent Text Reader

Abstract

The manufacturing method of the vapor deposition mask unit includes: a step of configuring a resist film on a first supporting substrate; a step of forming a stripping layer on the resist film; a step of exposing the resist film from the side of the resist film to the inside; a step of forming at least one vapor deposition mask having a plurality of openings on the stripping layer; a step of configuring a supporting frame having at least one window on the stripping layer in a manner such that at least one window overlaps with a plurality of openings of at least one vapor deposition mask; and a step of forming a connecting portion that fixes at least one vapor deposition mask and the supporting frame to each other by a plating method.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] One embodiment of the present invention relates to a method for manufacturing a vapor deposition mask unit. Background Art

[0002] As an example of a flat panel display device, a liquid crystal display device and an organic electroluminescent display device can be cited. These display devices are structures obtained by stacking thin films containing various materials such as insulators, semiconductors, and conductors on a substrate, and these thin films are appropriately patterned and connected to realize the function of a display device.

[0003] Methods for forming thin films are roughly classified into gas phase method, liquid phase method, and solid phase method. Gas phase method is classified into physical gas phase method and chemical gas phase method. As a representative example of the former, evaporation method is known. The simplest method of evaporation method is vacuum evaporation method, which generates vapor of material by heating the material under high vacuum to sublimate or evaporate the material (hereinafter, sublimation and evaporation are collectively referred to as gasification), and solidifies and deposits the vapor in the target area (hereinafter, referred to as evaporation area), thereby obtaining a thin film of the material. At this time, in order to selectively form a thin film in the evaporation area, the material is not deposited in the area outside this (hereinafter, referred to as non-evaporation area), and a mask that physically shields the non-evaporation area is used (refer to patent documents 1, 2). This mask is called an evaporation mask, etc.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2009-87840.

[0007] Patent document 2: Japanese Patent Application Publication No. 2013-209710. Summary of the invention

[0008] Problems to be solved by the invention

[0009] One object of one embodiment of the present invention is to provide a method for manufacturing a vapor deposition mask unit. For example, one object of one embodiment of the present invention is to provide a method for manufacturing a vapor deposition mask unit with high efficiency, high yield and low cost.

[0010] Technical solutions to the problem

[0011] One embodiment of the present invention is a method for manufacturing a vapor deposition mask unit. The method includes: a step of arranging a resist film on a first support substrate; a step of forming a peeling layer on the resist film; a step of exposing the resist film from the side of the resist film to the inside; a step of forming at least one vapor deposition mask having a plurality of openings on the peeling layer; a step of arranging a support frame having at least one window on the peeling layer in a manner that the at least one window overlaps with the plurality of openings of the at least one vapor deposition mask; and a step of forming a connection portion that fixes the at least one vapor deposition mask and the support frame to each other by a plating method.

[0012] One embodiment of the present invention is a support substrate including: a first metal plate; a photocurable adhesive layer on the first metal plate; and a metal layer on the adhesive layer, wherein the adhesive layer is exposed from a side surface of the first metal plate and a side surface of the metal layer and is cured. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] Figure 1A This is a schematic plan view of a vapor deposition device to which a vapor deposition mask unit manufactured by a method according to one embodiment of the present invention can be applied.

[0014] Figure 1B This is a schematic side view of a vapor deposition device to which a vapor deposition mask unit produced by a method according to one embodiment of the present invention can be applied.

[0015] Figure 2 This is a schematic top view of a vapor deposition mask unit produced by a method according to one embodiment of the present invention.

[0016] Figure 3 This is a schematic cross-sectional view of a vapor deposition mask unit produced by a method according to one embodiment of the present invention.

[0017] Figure 4A This is a schematic cross-sectional view of a vapor deposition mask unit produced by a method according to one embodiment of the present invention.

[0018] Figure 4B This is a schematic cross-sectional view of a vapor deposition mask unit produced by a method according to one embodiment of the present invention.

[0019] Figure 5A This is a schematic cross-sectional view showing a method for manufacturing a vapor deposition mask unit according to one embodiment of the present invention.

[0020] Figure 5B This is a schematic cross-sectional view showing a method for manufacturing a vapor deposition mask unit according to one embodiment of the present invention.

[0021] Figure 5C This is a schematic cross-sectional view showing a method for manufacturing a vapor deposition mask unit according to one embodiment of the present invention.

[0022] Figure 5D This is a schematic cross-sectional view showing a method for manufacturing a vapor deposition mask unit according to one embodiment of the present invention.

[0023] Fig. 6A This is a schematic cross-sectional view showing a method for manufacturing a vapor deposition mask unit according to one embodiment of the present invention.

[0024] Figure 6B This is a schematic cross-sectional view showing a method for manufacturing a vapor deposition mask unit according to one embodiment of the present invention.

[0025] Figure 6C This is a schematic cross-sectional view showing a method for manufacturing a vapor deposition mask unit according to one embodiment of the present invention.

[0026] Fig. 7A This is a schematic cross-sectional view showing a method for manufacturing a vapor deposition mask unit according to one embodiment of the present invention.

[0027] Figure 7B It is a schematic plan view showing a method of manufacturing a vapor deposition mask unit according to one embodiment of the present invention.

[0028] Figure 7C This is a schematic cross-sectional view showing a method for manufacturing a vapor deposition mask unit according to one embodiment of the present invention.

[0029] Fig. 8A This is a schematic cross-sectional view showing a method for manufacturing a vapor deposition mask unit according to one embodiment of the present invention.

[0030] Figure 8B This is a schematic cross-sectional view showing a method for manufacturing a vapor deposition mask unit according to one embodiment of the present invention.

[0031] Fig. 9A This is a schematic cross-sectional view showing a method for manufacturing a vapor deposition mask unit according to one embodiment of the present invention.

[0032] Fig. 9B This is a schematic cross-sectional view showing a method for manufacturing a vapor deposition mask unit according to one embodiment of the present invention.

[0033] Fig. 9C This is a schematic cross-sectional view showing a method for manufacturing a vapor deposition mask unit according to one embodiment of the present invention.

[0034] Fig. 10A This is a schematic cross-sectional view showing a method for manufacturing a vapor deposition mask unit according to one embodiment of the present invention.

[0035] Fig. 10B It is a schematic plan view showing a method of manufacturing a vapor deposition mask unit according to one embodiment of the present invention.

[0036] Fig.11A This is a schematic cross-sectional view showing a method for manufacturing a vapor deposition mask unit according to one embodiment of the present invention.

[0037] Fig. 11B It is a schematic plan view showing a method of manufacturing a vapor deposition mask unit according to one embodiment of the present invention.

[0038] Fig. 12A This is a schematic cross-sectional view showing a method for manufacturing a vapor deposition mask unit according to one embodiment of the present invention.

[0039] Fig. 12B This is a schematic cross-sectional view showing a method for manufacturing a vapor deposition mask unit according to one embodiment of the present invention.

[0040] Fig.13A This is a schematic cross-sectional view showing a method for manufacturing a vapor deposition mask unit according to one embodiment of the present invention.

[0041] Fig. 13B This is a schematic cross-sectional view showing a method for manufacturing a vapor deposition mask unit according to one embodiment of the present invention.

[0042] Fig.14A This is a schematic cross-sectional view showing a method for manufacturing a vapor deposition mask unit according to one embodiment of the present invention.

[0043] Fig. 14B This is a schematic cross-sectional view showing a method for manufacturing a vapor deposition mask unit according to one embodiment of the present invention.

[0044] Fig. 14C This is a schematic cross-sectional view showing a method for manufacturing a vapor deposition mask unit according to one embodiment of the present invention.

[0045] Fig.15A This is a schematic cross-sectional view showing a method for manufacturing a vapor deposition mask unit according to one embodiment of the present invention.

[0046] Fig. 15B This is a schematic cross-sectional view showing a method for manufacturing a vapor deposition mask unit according to one embodiment of the present invention.

[0047] Fig.16A This is a schematic cross-sectional view showing a method for manufacturing a vapor deposition mask unit according to one embodiment of the present invention.

[0048] Fig. 16B This is a schematic cross-sectional view showing a method for manufacturing a vapor deposition mask unit according to one embodiment of the present invention.

[0049] Fig.17A This is a schematic cross-sectional view showing a method for manufacturing a vapor deposition mask unit according to one embodiment of the present invention.

[0050] Fig. 17B This is a schematic cross-sectional view showing a method for manufacturing a vapor deposition mask unit according to one embodiment of the present invention.

[0051] Fig.18A This is a schematic cross-sectional view showing a method for manufacturing a vapor deposition mask unit according to one embodiment of the present invention.

[0052] Fig.18B This is a schematic cross-sectional view showing a method for manufacturing a vapor deposition mask unit according to one embodiment of the present invention. DETAILED DESCRIPTION

[0053] Hereinafter, various embodiments of the present invention will be described with reference to the drawings, etc. However, the present invention can be implemented in various forms without departing from the gist of the present invention, and should not be construed as being limited to the description of the embodiments illustrated below.

[0054] In order to make the description clearer, the drawings show schematically the width, thickness, shape, etc. of each part compared with the actual situation, but this is only an example and does not limit the interpretation of the present invention. In this specification and each figure, the same reference numerals are sometimes marked for the same functional elements as those described in the previous figure, and repeated descriptions are omitted.

[0055] When expressing the situation of configuring other structures on a certain structure in this specification and technical solution, when simply marked as "on...", unless otherwise specified, it includes two situations: configuring other structures directly above the certain structure in a manner of being connected to the certain structure and configuring other structures above the certain structure through other structures.

[0056] Hereinafter, the expression “a certain structure is exposed from another structure” means that a part of a certain structure is not covered by another structure, and the part not covered by the other structure includes a part further covered by another structure.

[0057] Hereinafter, a method for manufacturing the vapor deposition mask unit 100 according to one embodiment of the present invention will be described.

[0058] 1. Evaporation device

[0059] The evaporation mask unit 100 manufactured by the present manufacturing method can be used to selectively form a film in a target evaporation region when forming a film of an organic compound, an inorganic compound, or a film containing an organic compound and an inorganic compound by evaporation. Figure 1A and Figure 1BA schematic top view and side view of a typical vapor deposition apparatus used to form a film by vapor deposition are shown. The vapor deposition apparatus is composed of a plurality of chambers having various functions. A chamber is Figure 1A The evaporation chamber 160 shown is separated from the adjacent chamber by a load lock door 162, and is configured to maintain a high vacuum decompression state inside, or a state filled with an inert gas such as nitrogen or argon. Therefore, the evaporation chamber 160 is connected to a decompression device and an exhaust mechanism (not shown).

[0060] The vapor deposition chamber 160 provides a space capable of storing an object on which a film can be formed, such as a substrate. Figure 1A , Figure 1B In the example shown, a vapor deposition source 164 is arranged below the substrate 180, and the vapor deposition source 164 is filled with a material to be evaporated. In the vapor deposition source 164, the material is heated and vaporized, and the vapor of the material reaches the surface of the substrate 180 through the opening 102a (described later) of the vapor deposition mask unit 100, whereupon it is cooled and solidified, and the material is deposited on the substrate 180 (in Figure 1B A film of material is formed on the lower surface of the substrate 180. Figure 1A In the example shown, a vapor deposition source 164 (also referred to as a linear source) having a substantially rectangular shape and arranged along one side of the substrate 180 is provided, and the vapor deposition source 164 can have any shape, and may be a vapor deposition source 164 called a point source that overlaps the center of gravity of the substrate 180. In the case of a point source, the relative positions of the substrate 180 and the vapor deposition source 164 are fixed, and a mechanism for rotating the substrate 180 may be provided.

[0061] When a linear source type vapor deposition source 164 is used, the vapor deposition chamber 160 is configured to enable the substrate 180 to move relative to the vapor deposition source 164. FIG. 1 shows an example in which the vapor deposition source 164 is fixed and the substrate 180 moves thereon. Figure 1B As shown, the evaporation chamber 160 also includes a holder 170 for holding the substrate 180 and the evaporation mask unit 100, a moving mechanism 168 for moving the holder 170, a shielding member 166, etc. The holder 170 can maintain the positional relationship between the substrate 180 and the evaporation mask unit 100, and the moving mechanism 168 can move the substrate 180 and the evaporation mask unit 100 above the evaporation source 164. The shielding member 166 is arranged on the evaporation source 164 to shield the vapor of the material or allow the vapor to reach the substrate 180, and its opening and closing can be controlled by a control device not shown in the figure. Although not shown in the figure, a sensor for monitoring the evaporation speed of the material, an anti-adhesion plate for preventing contamination caused by the material, a pressure gauge for monitoring the pressure in the evaporation chamber 160, etc. are also provided in the evaporation chamber 160.

[0062] 2. Evaporation mask unit

[0063] exist Figure 2 The top surface schematic diagram of the evaporation mask unit 100 is shown in FIG. Figure 3 Indicates along Figure 2 The evaporation mask unit 100 has at least one or more evaporation masks 102. In the following description, an example in which one evaporation mask unit 100 has a plurality of evaporation masks 102 is used for description. Figure 2 , Figure 3 , a vapor deposition mask unit 100 including six vapor deposition masks 102 is shown.

[0064] Each vapor deposition mask 102 is provided with a plurality of openings 102a penetrating the vapor deposition mask 102. In each vapor deposition mask 102, the area other than the openings 102a is referred to as a non-opening portion. The non-opening portion surrounds the plurality of openings 102a. The vapor deposition mask unit 100 further includes a support frame 110 for supporting the vapor deposition mask 102, and the vapor deposition mask 102 is fixed to the support frame 110 via at least one connecting portion 120. The number of connecting portions 120 can be the same as the number of vapor deposition masks 102 (see Figure 2 Each connection portion 120 surrounds a plurality of openings 102 a of a corresponding vapor deposition mask 102 and is connected to the support frame 110 and the vapor deposition mask 102 .

[0065] During evaporation, the evaporation mask unit 100 and the substrate 180 are arranged in such a manner that the evaporation area overlaps with the opening 102a, and the non-evaporation area overlaps with the non-opening portion, and the vapor of the material passes through the opening 102a to deposit the material on the evaporation area. There is no restriction on the arrangement of the plurality of openings 102a. For example, in the case where a plurality of pixels provided in the display area of ​​the display device are formed into films respectively, the plurality of openings 102a are arranged in such a manner that they overlap with the area where the pixels are provided on the substrate 180. Therefore, in the case where a plurality of pixels are arranged in a matrix, the plurality of openings 102a are also arranged in a matrix. In the case where a plurality of display devices are manufactured using one evaporation mask unit 100, the display areas of the plurality of display devices are formed on a large substrate 180 called a mother glass. In this case, the plurality of openings 102a are arranged in such a manner that a plurality of opening groups 102b corresponding to the plurality of display areas are formed respectively. The distance between adjacent opening groups 102b is greater than the distance between adjacent openings 102a of each opening group 102b.

[0066] The support frame 110 has at least one window 110a ( Figure 3). In the case where the vapor deposition mask unit 100 has a plurality of vapor deposition masks 102, at least one window 110a includes a plurality of windows 110a. In this case, the number of windows 110a may be the same as the number of vapor deposition masks 102. Each window 110a is provided so as to overlap with a plurality of openings 102a of the vapor deposition mask 102. That is, the plurality of openings 102a are exposed from the support frame 110 through any window 110a. Each opening group 102b is also exposed from the support frame 110 through any window 110a. A portion of the support frame 110 is connected to the connecting portion 120 between adjacent opening groups 102b.

[0067] exist Figure 4A , Figure 4B The regions Ra sandwiched between the adjacent windows 110a and the regions Rb at the end of the vapor deposition mask unit 100 (see Figure 3 ) is a more detailed schematic cross-sectional view. Figure 4A As shown, the support frame 110 is not in direct contact with the vapor deposition mask 102, but is fixed to the non-opening portion of the vapor deposition mask 102 through the connecting portion 120. Although not shown, the support frame 110 may overlap a portion of the vapor deposition mask 102. The same is true for the region Rb. Figure 4B As shown, the support frame 110 is not in direct contact with the vapor deposition mask 102, but is fixed to the non-opening portion of the vapor deposition mask 102 via the connection portion 120. The support frame 110 may overlap a portion of the vapor deposition mask 102 in the region Rb.

[0068] like Figure 4A , Figure 4B As shown, it is preferred that the connection portion 120 does not contact the upper surface of the support frame 110. In other words, it is preferred that the connection portion 120 is separated from the upper surface of the support frame 110. The method for manufacturing the vapor deposition mask unit 100 will be described later. By separating the connection portion 120 from the upper surface of the support frame 110, it is possible to prevent the connection portions 120 adjacent to the support frame 110 from being deformed integrally relative to the support frame 110, thereby stabilizing the shape of the vapor deposition mask unit 100. Figure 4A , Figure 4B In the embodiment, the uppermost layer of the connection part 120 is located on the same plane as the upper surface of the support frame 110, but the uppermost layer of the connection part 120 may also be lower than the upper surface of the support frame 110. That is, the uppermost layer of the connection part 120 may also be located between the upper surface of the support frame 110 and the evaporation mask 102.

[0069] The deposition mask 102 and the connection portion 120 contain a zero-valent metal such as nickel, copper, titanium, or chromium, preferably nickel. The composition of the materials of the deposition mask 102 and the connection portion 120 may be the same. The support frame 110 also contains a zero-valent metal, and the metal is selected from nickel, iron, cobalt, chromium, manganese, and the like. For example, the support frame 110 may be an alloy containing iron and chromium, an alloy containing iron, nickel, and manganese, or may contain carbon in the alloy.

[0070] 3. Method for manufacturing evaporation mask unit

[0071] use FIG. 5A to FIG. 18B An example of a method for producing the vapor deposition mask unit 100 will be described.

[0072] 3-1. Formation of peeling layer

[0073] First, a flat surface for forming the vapor deposition mask 102 is formed. Specifically, a resist mask 132 ( Figure 5A ).

[0074] The first supporting substrate 130 is a substrate having the function of supporting a peeling layer 134 and a second supporting substrate 138 (described later) formed or arranged thereon. The first supporting substrate 130 contains glass or quartz, plastic, or a metal such as copper, aluminum, titanium, iron, nickel, cobalt, chromium, molybdenum, manganese, or an alloy thereof. In the case where the first supporting substrate 130 contains an alloy, the alloy may be, for example, an alloy containing iron and chromium, an alloy of iron, nickel and manganese, or may contain carbon in the alloy. In the case of using a substrate containing glass, quartz, or plastic, a substrate formed with a film of the above-mentioned metal or alloy may also be used. As described later, the peeling layer 134 is formed on the first supporting substrate 130. In the case where the peeling layer 134 is formed by electrolytic plating, in order to be able to function as an electrode for power supply during electroplating, it is preferred to use a metal substrate or an alloy substrate as the first supporting substrate 130.

[0075] In order to determine the shape of the stripping layer 134 formed on the first supporting substrate 130, the resist mask 132 is formed in a manner that surrounds the contour of the stripping layer 134 formed on the first supporting substrate 130. Therefore, although not shown in the figure, the resist mask 132 is set on the first supporting substrate 130 in a manner having a closed shape. There is no limitation on the method for forming the resist mask 132, and a known negative or positive resist is formed on the first supporting substrate 130, and it can be formed by exposure and development with the help of a photomask. The resist can be either liquid or solid. In the latter case, the resist is also called a resist film. In addition, in order to facilitate the stripping process described later, it is preferred that the resist mask 132 is formed in a manner that is spaced apart from its outer side 132a or the end of the first supporting substrate 130.

[0076] Then, a peeling layer 134 ( Figure 5B As described later, the peeling layer 134 is a functional layer for facilitating the peeling of the second support substrate 138 from the vapor deposition mask unit 100 formed thereon, or for growing a plating layer as the vapor deposition mask 102, and for example, a metal thin film of nickel, molybdenum, tungsten, etc. can be used. The peeling layer 134 can be formed by electroless plating, electrolytic plating (hereinafter, electroless plating and electrolytic plating are collectively referred to as plating methods), sputtering, or chemical vapor deposition (CVD) in a manner such that the thickness is, for example, not less than 20 μm and not more than 200 μm, or not less than 40 μm and not more than 150 μm.

[0077] A resist film 136 ( Figure 5C ). The second support substrate 138 is a substrate having a function of holding the evaporation mask 102 and the support frame 110 when forming the evaporation mask unit 100, and can include a material that can be used in the first support substrate 130. For example, both the first support substrate 130 and the second support substrate 138 can be an alloy of iron, nickel, and manganese. In this case, the composition of these metals can also be different between the first support substrate 130 and the second support substrate 138.

[0078] The anti-etching film 136 contains a negative photocurable resin. That is, it contains a polymer or oligomer that is cured by light. The thickness of the anti-etching film 136 can be arbitrarily selected, for example, from a range of 20 μm to 500 μm, 50 μm to 200 μm, or 50 μm to 100 μm. In order to ensure this film thickness, the anti-etching film 136 can also be stacked.

[0079] As an arbitrary structure, the resist film 136 may be exposed (one-time exposure) ( Figure 5C ). This single exposure can be performed by irradiating light through the upper surface of the resist film 136, that is, the surface opposite to the second support substrate 138. In addition, in this single exposure, the resist film 136 is exposed in a manner that does not completely cure but maintains flexibility. In other words, the resist film 136 after exposure is exposed in a manner that can still be elastically deformed. By performing the single exposure in this way, the upper surface of the resist film 136 can maintain adhesiveness, and as a result, sufficient adhesive strength can be maintained between the peeling layer 134.

[0080] Next, the first support substrate 130 and the second support substrate 138 are bonded together in such a manner that the release layer 134 and the anti-etching film 136 are in contact with each other ( Figure 5D). At this time, there is no restriction on the upper and lower relationship between the first support substrate 130 and the second support substrate 138, and the latter can be arranged on the former, or the former can be arranged on the latter. The surface of the resist film 136 is sticky before exposure, and the single exposure is also performed in a manner that maintains the stickiness. Therefore, by bonding the first support substrate 130 and the second support substrate 138, the peeling layer 134 and the resist film 136 are fixed to each other. In addition, by performing a single exposure, the flexibility of the resist film 136 is reduced compared to before exposure, so the peeling layer 134 can be stably fixed on the resist film 136, and the pattern formation accuracy in the subsequent process can be ensured.

[0081] Then, the peeling layer 134 is peeled off at the interface with the first support substrate 130, and the first support substrate 130 is removed ( Fig. 6A The peeling can be performed by fixing one of the first support substrate 130 and the second support substrate 138 and physically removing the other support substrate. The peeling layer 134 formed on the outside of the resist mask 132 is removed together with the first support substrate 130 ( Fig. 6A ). In the case where the shape of the resist film 136 is larger than the shape of the peeling layer 134, as shown in FIG. Figure 6B As shown in FIG. 1 , the end of the resist film 136 is exposed from the peeling layer 134. In this case, the end exposed from the peeling layer 134 may be removed physically or by using a developer ( Figure 6C ).

[0082] Here, the end surface of the resist film 136 is exposed. Specifically, the light source 140 is used, and the light emitted from the light source 140 is irradiated to the resist film 136 through the side surface 136a of the resist film 136 to expose the resist film 136 ( Fig. 7A For example, the exposure can be performed in a manner such that the direction of travel of the light with the maximum intensity emitted from the light source 140 is directly from the light source, or is reflected from the upper surface of the second support substrate 138 and then passes through the side surface 136a. The end surface exposure is preferably performed on all the side surfaces 136a of the resist film 136. That is, it is preferred that Figure 7B As shown, the light source 140 may be moved at a constant speed along the outer periphery of the resist film 136. At this time, the direction of the light source 140 is appropriately adjusted so that the light emitted from the light source 140 passes through the side surface 136a of the resist film 136.

[0083] The structure of the light source 140 is arbitrary, and is configured in such a way that light (e.g., ultraviolet light or visible light with a wavelength of 365 nm) effective for curing the photocurable resin contained in the resist film 136 is emitted. The light from the light source 140 may be either laser light or incoherent light. The output of the light source 140 may also be appropriately selected according to the size and thickness of the resist film 136, the photosensitivity of the photocurable resin contained in the resist film 136, the moving speed of the light source 140, etc., for example, it may be appropriately selected from the range of 1000 mW to 6000 mW, 2000 mW to 6000 mW, or 3000 mW to 5000 mW. The moving speed of the light source 140 may also be adjusted according to the size of the resist film 136 and the output of the light source 140, for example, it may be appropriately selected from the range of 0.1 cm / s to 20 cm / s, 1.0 cm / s to 10 cm / s, or 1.0 cm / s to 5.0 cm / s.

[0084] Thus, the outer peripheral portion 136b of the resist film 136 is cured, and the inner portion 136c surrounded by the outer peripheral portion 136b is maintained in an uncured state or in a semi-cured state by one exposure ( Figure 7C ). By making the inner portion 136c uncured or semi-cured, the peeling layer 134 can be stably fixed, thereby preventing the peeling layer 134 from being accidentally peeled off in the subsequent process, thereby ensuring the accuracy of pattern formation on the peeling layer 134. Furthermore, by forming the outer peripheral portion 136b, the manufacturing yield of the vapor deposition mask unit 100 can be improved, and the vapor deposition mask unit 100 can be provided efficiently and at low cost, and the details will be described later.

[0085] Through the above steps, the peeling layer 134 is formed on the second support substrate 138 via the resist film 136. The upper surface of the peeling layer 134 in this state (the surface opposite to the second support substrate 138) is the surface in contact with the first support substrate 130 before peeling. Therefore, by using the first support substrate 130 with high flatness, a flat surface can be formed on the upper surface of the peeling layer 134.

[0086] 3-2. Formation of evaporation mask

[0087] Next, a resist mask 144 is formed on the peeling layer 134. The resist mask 144 is selectively formed in an island shape in a region where a plurality of openings 102a and a dummy pattern 106 described later are formed. Specifically, a negative or positive resist 142 ( Fig. 8A ), a resist mask 144 is formed by exposure and development via a photomask ( Figure 8B). The resist 142 may be a liquid or a resist film. In addition, the resist mask 144 is preferably formed also on the outer edge of the peeling layer 134 so that the peeling layer 134 can be easily peeled off from the vapor deposition mask unit 100 in the peeling process described later.

[0088] In the development of the resist 142 after exposure, a developer is brought into contact with the resist 142, and then the first support substrate 130 and the resist mask 144 are cleaned using an aqueous cleaning solution. Droplets of the cleaning solution remaining on the second support substrate 138 immediately after cleaning are removed by blowing away the droplets by supplying compressed nitrogen or air parallel to or obliquely to the upper surface of the first support substrate 130 (see Figure 8B ).

[0089] In the development process, it is preferred to selectively remove only the uncured resist 142. However, the material contained in the resist 142 and the material contained in the resist film 136 are both photocurable resins, and their basic structures are the same or similar. Therefore, the uncured resist 142 is not necessarily more soluble in the developer than the resist film 136. Therefore, in the case where the peripheral portion 136b (refer to FIG. 1 ) that is not cured by the end face exposure is not provided, Figure 7C ), the photocurable resin from the resist film 136 is dissolved in the developer. As a result, the cleaning solution used for cleaning also contains a small amount of photocurable resin.

[0090] When the compressed nitrogen or air hits the side of the peeling layer 134 under such conditions ( Figure 8B 144). As a result, turbulence is generated, and droplets of the cleaning liquid containing the photocurable resin are scattered due to the turbulence, and sometimes adhere to the resist mask 144. When the droplets adhere to the resist mask 144 and the solvent in the droplets evaporates, the photocurable resin is precipitated on the resist mask 144. As a result, the shape of the resist mask 144 changes, and the pattern of the opening 102a of the vapor deposition mask 102 formed later cannot be controlled according to the pattern of the photomask. This causes a low manufacturing yield of the vapor deposition mask unit 100.

[0091] However, as described above, in one embodiment of the present invention, the resist film 136 is end-face exposed before the formation of the resist 142. Therefore, the peripheral portion 136b is composed of the cured resist film 136 and is not dissolved in the developer. In addition, the uncured or semi-cured inner portion 136c is surrounded by the cured peripheral portion 136b, so it does not contact the developer. Therefore, the inner portion 136c of the resist film 136 is not dissolved by the developer, and the cleaning liquid does not contain the photocurable resin from the resist film 136. For this reason, even if the droplets of the cleaning liquid adhere to the resist mask 144, the photocurable resin from the resist film 136 will not adhere to the resist mask 144. As a result, the resist mask 144 after precise patterning following the photomask pattern can be formed, and the pattern of the opening 102a of the vapor deposition mask 102 can be precisely controlled. This contributes to the efficient manufacturing and high yield of the vapor deposition mask unit 100.

[0092] Next, a metal film is grown in the region not covered by the resist mask 144 by plating to form the vapor deposition mask 102 and the dummy pattern 106 ( Fig. 9A ). The formation of the plating pattern can be performed in one step or in multiple stages. In the case of performing the process in multiple stages, the metal plating can be performed in a manner that different metals are formed in different stages. In addition, the metal plating can be performed in a manner that the upper surface of the plating pattern is lower than the upper surface of the resist mask 144, or in a manner that the upper surface of the plating pattern is higher than the upper surface of the resist mask 144. In the latter case, the upper surface of the plating pattern can also be planarized by grinding the surface. Thereafter, the resist mask 144 is removed by etching and / or ashing using a stripping solution to form a vapor deposition mask 102 having a plurality of openings 102a and a dummy pattern 106 ( Fig. 9B ).

[0093] In the area Ra between adjacent windows 110a, as shown in FIG. Fig. 10A As shown in the schematic cross-sectional view of , a dummy pattern (hereinafter, first dummy pattern) 106-1 is formed on the peeling layer 134 simultaneously with the formation of the vapor deposition mask 102. A groove (hereinafter, first groove) 104-1 is formed between the first dummy pattern 106-1 and the vapor deposition mask 102, and the first dummy pattern 106-1 and the vapor deposition mask 102 are separated by the first groove 104-1. Fig. 10B As shown in the upper surface schematic diagram of FIG. 1 , one first dummy pattern 106-1 surrounds one evaporation mask 102. Since the first dummy pattern 106-1 and the evaporation mask 102 are formed simultaneously, they can have the same composition and thickness as each other.

[0094] The same is true for the region Rb at the end of the evaporation mask unit 100. Fig.11AAs shown in FIG. 1 , a dummy pattern (hereinafter referred to as a second dummy pattern) 106-2 is formed on the peeling layer 134 simultaneously with the formation of the vapor deposition mask 102. A groove (hereinafter referred to as a second groove) 104-2 is formed between the second dummy pattern 106-2 and the vapor deposition mask 102, and the second dummy pattern 106-2 and the vapor deposition mask 102 are separated by the second groove 104-2. Fig. 11B As shown in the upper surface schematic diagram of FIG. 1 , the second dummy pattern 106 - 2 surrounds the plurality of evaporation masks 102 and Fig. 11B Since the second dummy pattern 106-2 is formed simultaneously with the evaporation mask 102, they can also have the same composition and thickness.

[0095] 3-3. Protection of openings

[0096] As described later, the support frame 110 is arranged on the vapor deposition mask 102, and the connection portion 120 is formed by a plating method, and the vapor deposition mask 102 and the support frame 110 are fixed to each other. Therefore, in order to prevent the metal from being plated on the opening 102a when the connection portion 120 is formed, a plurality of resist masks 148 are used to protect the opening 102a.

[0097] Specifically, if Fig. 9C As shown in FIG. 1 , first, a resist film 146 is arranged in a manner covering a plurality of vapor deposition masks 102. The resist film 146 is arranged in a manner covering all of the openings 102a of the plurality of vapor deposition masks 102 and the dummy pattern 106 including the first dummy pattern 106-1 and the second dummy pattern 106-2. The resist film 146 is preferably formed with a thickness that is not covered by the connecting portion 120 to be formed later. Therefore, the thickness of the resist film 146 can be selected from a range of 50 μm to 500 μm, 60 μm to 200 μm, or 100 μm to 200 μm.

[0098] Next, the resist film 146 is exposed using a photomask 150. The photomask 150 has a light shielding portion 150a and a light transmitting portion 150b. Fig. 12A As shown, the photomask 150 is constructed and arranged in a region Ra so that the portion of the resist film 146 overlapping with the opening 102a of the vapor deposition mask 102 and the portion overlapping with a portion of the non-opening portion of the vapor deposition mask 102 are exposed, and the portion overlapping with the first dummy pattern 106-1 and the portion overlapping with another portion of the non-opening portion of the vapor deposition mask 102 are not exposed. That is, the light-transmitting portion 150b is constructed and arranged so that the light-shielding portion 150a overlaps with the opening 102a of the vapor deposition mask 102 and a portion of the non-opening portion, and the light-shielding portion 150a overlaps with the first dummy pattern 106-1 and another portion of the non-opening portion.

[0099] On the other hand, in region Rb, as Fig.13AAs shown, the photomask 150 is constructed and arranged such that the light-transmitting portion 150b overlaps with the opening 102a of the vapor deposition mask 102 and a portion of the non-opening portion, and the light-shielding portion 150a overlaps with the second dummy pattern 106 - 2 and another portion of the non-opening portion of the vapor deposition mask 102 .

[0100] The resist film 146 is a negative resist containing a polymer or oligomer that is cured by light. The solubility of the exposed portion in the developer is greatly reduced, and the exposed portion remains as a mask after development. On the other hand, the unexposed portion is removed by development. Therefore, in the region Ra, the plurality of resist masks 148 generated by development cover a portion of the plurality of openings 102a and the non-opening portion, and the other portion of the non-opening portion and the first dummy pattern 106-1 are exposed from the resist mask 148 ( Fig. 12B On the other hand, in the region Rb, the resist mask 148 covers the plurality of openings 102a and a portion of the non-opening portion, and another portion of the non-opening portion and the second dummy pattern 106-2 are exposed from the resist mask 148 ( Fig. 13B As will be described later, the connection portion 120 is formed in the non-opening portion exposed from the resist mask 148 , thereby bonding the vapor deposition mask 102 to the support frame 110 .

[0101] Through the above steps, a plurality of resist masks 148 covering all the openings 102 a are formed.

[0102] 3-4. Fabrication of support frame

[0103] The support frame 110 is formed by etching a metal plate 112. Specifically, a resist 152 is formed on the metal plate 112 containing a metal or alloy such as nickel, iron, cobalt, chromium, and manganese, and exposure is performed through a photomask 156 ( Fig.14A ), and a resist mask 154 is formed by subsequent development ( Fig. 14B ). The resist 152 may be a liquid resist or a thin film resist. In addition, the resist 152 may be a negative type or a positive type. In the case of a negative type, such as Fig.14A As shown in FIG. 1 , the photomask 156 is configured and arranged so that the light-transmitting portion 156b overlaps with the region where the support frame 110 is formed, and the light-shielding portion 156a overlaps with the region removed by etching, that is, the region where the window 110a is formed. Then, the region other than the region covered by the resist mask 154 is removed by development, thereby obtaining the support frame 110 ( Fig. 14C ). The resist mask 154 is subsequently removed by a stripping solution and / or ashing.

[0104] 3-5. Arrangement of support frame and formation of joint

[0105] Next, the support frame 110 is disposed on the support substrate 138. Specifically, the vapor deposition mask 102 ( 106 - 1 ) is disposed on the second support substrate 138 via the release layer 134 so as to overlap with the first dummy pattern 106 - 1 and the second dummy pattern 106 - 2. Fig.15A , Fig.16A ). That is, the support frame 110 is configured in such a way that a window 110a overlaps with a plurality of openings 102a and a resist mask 148. At this time, an adhesive 158 may also be provided in the support frame 110, and the support frame 110 and the first dummy pattern 106-1 and the second dummy pattern 106-2 may be bonded together by the adhesive 158. As the adhesive 158, for example, it may be an acrylic adhesive or an epoxy adhesive, or a resist film similar to the resist film 146 may be used. When a resist film is used, its thickness is smaller than the thickness of the resist film 146. Specifically, the thickness of the resist film as the adhesive 158 can be selected from a range of 1 μm to 20 μm or from 1 μm to 10 μm. When a resist film is used as the adhesive 158, in order to maintain the adhesive force, the resist film may not be exposed.

[0106] In addition, as an arbitrary structure, a protective film 159 ( Fig.15A , Fig.16A ). As the protective film 159, the same resist as the resist film 146 may be used. In this case, the resist film may be exposed or not. By forming the protective film 159, when the connecting portion 120 is formed by the subsequent plating method, the connecting portion 120 can be not formed on the upper surface of the support frame 110, so as to prevent the adjacent vapor deposition masks 102 from being directly connected through the connecting portion 120.

[0107] Then, the connection portion 120 is formed by plating. The connection portion 120 grows mainly from the portion exposed from the resist mask 148 in the non-opening portion of the support frame 110 and the evaporation mask 102. As a result, Fig. 15B , Fig. 16B As shown, a connection portion 120 is formed which contacts the upper surface of the non-opening portion of the vapor deposition mask 102 and the side surface 110b constituting the window 110a of the support frame 110. Thus, the vapor deposition mask 102 and the support frame 110 are fixed.

[0108] In addition, Fig. 16B In the embodiment, the plating layer 121 is formed on the left side of the support frame 110, that is, on the outermost periphery, simultaneously with the connection portion 120. Since the plating layer 121 is located outside the substrate 180 in the vapor deposition process using the vapor deposition mask unit 100, there is no particular problem. However, if necessary, the plating layer 121 may be formed on the outer side of the support frame 110. Fig.16A In the illustrated state, the outermost periphery is covered with a resist mask 148 without forming the plating layer 121 .

[0109] At this time, the connection portion 120 is formed in a manner that does not cover the upper surface of the resist mask 148. This is because, in the case where the connection portion 120 covers the upper surface of the resist mask 148, defects may sometimes occur when the resist mask 148 is subsequently removed by a stripping solution. Specifically, when the resist mask 148 swells due to the stripping solution, the volume expands, thereby generating stress on the connection portion 120 on the resist mask 148, as a result, the connection portion 120 may sometimes be damaged. By forming the connection portion 120 in a manner that does not cover the upper surface of the resist mask 148, this problem can be effectively suppressed. By setting the resist film 146 in a manner having a thickness in the above-mentioned range, it is possible to allow the vapor deposition mask 102 to be fixed to the support frame 110 with sufficient bonding strength for the connection portion 120, and the connection portion 120 can be formed in a manner that does not cover the upper surface of the resist mask 148.

[0110] 3-6. Removal of Supporting Substrate and Release Layer

[0111] Thereafter, the resist mask 148 is removed by etching using a stripping solution ( Fig.17A , Fig.18A ). At this time, the protective film 159 is also removed. Further, the second support substrate 138 and the peeling layer 134 are peeled off in sequence. By removing the adhesive 158 simultaneously with the peeling of the peeling layer 134 or after the peeling of the peeling layer 134, the first dummy pattern 106-1 and the second dummy pattern 106-2 are removed together with the adhesive 158 ( Fig. 17B , Fig.18B ).

[0112] Through the above steps, the vapor deposition mask unit 100 can be manufactured.

[0113] As described above, in the present embodiment, during the development of the resist mask 144 for determining the shape of the opening 102a and the dummy pattern 106, the inner portion 136c of the resist film 136 for fixing the peeling layer 134 to the second support substrate 138 is prevented from contacting with the developer by the outer peripheral portion 136b solidified by the end surface exposure. Therefore, in the cleaning process after the development, the droplets containing the photocurable resin from the resist film 136 will not be scattered on the resist mask 144, and the precise pattern of the resist mask 144 can be prevented from being destroyed. As a result, the occurrence of defects in the manufacture of the vapor deposition mask unit 100 can be effectively prevented, and the vapor deposition mask unit 100 can be provided efficiently and with a high yield.

[0114] As embodiments of the present invention, the above-mentioned embodiments can be appropriately combined and implemented as long as they are not contradictory. In addition, based on the production method of each embodiment, the method obtained by adding, omitting or changing the conditions of the process appropriately by those skilled in the art is also included in the scope of the present invention as long as it has the gist of the present invention.

[0115] Even if other effects different from the effects obtained by the above-mentioned embodiments are clear from the description of this specification or can be easily predicted by a person skilled in the art, it is naturally understood that they are obtained by the present invention.

[0116] Description of Reference Numerals

[0117] 100: evaporation mask unit, 102: evaporation mask, 102a: opening, 102b: opening group, 104-1: first groove, 104-2: second groove, 106: dummy pattern, 106-1: first dummy pattern, 106-2: second dummy pattern, 110: support frame, 110a: window, 110b: side, 112: metal plate, 120: connection part, 121: plating layer, 130: first support substrate, 132: resist mask, 132a: side, 134: peeling layer, 136: resist film, 136a: side, 136b: outer periphery, 136c: inner part, 138: second support Supporting substrate, 140: light source, 142: resist, 144: resist mask, 146: resist film, 146a: exposure portion, 146b: unexposed portion, 148: resist mask, 150: photomask, 150a: light shielding portion, 150b: light transmitting portion, 152: resist, 154: resist mask, 156: photomask, 156a: light shielding portion, 156b: light transmitting portion, 158: adhesive, 159: protective film, 160: evaporation chamber, 162: load lock door, 164: evaporation source, 166: shielding member, 168: moving mechanism, 170: holding component, 180: substrate.

Claims

1. A method for manufacturing a vapor deposition mask unit, It is characterized in that include: a step of disposing a resist film on a first supporting substrate; forming a release layer on the resist film; exposing the resist film from the side surface toward the inside of the resist film to cure the outer peripheral portion of the resist film; forming at least one evaporation mask having a plurality of openings and a dummy pattern spaced apart from the evaporation mask on the release layer; A step of disposing a support frame having at least one window on the dummy pattern by an adhesive in such a manner that the at least one window overlaps with the plurality of openings of the at least one evaporation mask; and The step of forming a connection portion for fixing the at least one vapor deposition mask and the support frame to each other by a plating method.

2. The method for manufacturing the evaporation mask unit according to claim 1, Features: The exposure is performed using a light source, The exposure is performed in such a manner that the traveling direction of the light having the maximum intensity irradiated from the light source passes through the side surface.

3. The method for manufacturing the evaporation mask unit according to claim 2, Features: The light source is configured to radiate ultraviolet light.

4. The method for manufacturing the evaporation mask unit according to claim 2, Features: The exposure is performed while moving the light source along the outer periphery of the resist film.

5. The method for manufacturing the evaporation mask unit according to claim 1, Features: The peeling layer is formed as a thin film including a metal layer on the second supporting substrate, The method further comprises: a step of bonding the first support substrate and the second support substrate together in such a manner that the release layer and the resist film are in contact with each other; and A step of transferring the release layer onto the second support substrate by peeling off the first support substrate.

6. The method for manufacturing the evaporation mask unit according to claim 5, Features: Before bonding the first support substrate and the second support substrate, the method further includes exposing the resist film from the upper surface of the resist film. The exposure from the upper surface of the resist film is performed while the resist film maintains flexibility.

7. The method for manufacturing the evaporation mask unit according to claim 1, Features: Before the exposure of the resist film, the method further includes removing a portion of the resist film exposed from the release layer.

8. The method for manufacturing the evaporation mask unit according to claim 1, Features: Before the configuration of the support frame, the method further includes forming a second resist mask covering the plurality of openings on the at least one evaporation mask.

9. The method for manufacturing the evaporation mask unit according to claim 8, Features: The connecting portion is formed so as not to overlap with the second resist mask.

10. The method for manufacturing the evaporation mask unit according to claim 1, Features: The at least one evaporation mask comprises a plurality of evaporation masks, The at least one window comprises a plurality of windows, The support frame is arranged so that the plurality of windows overlap with the corresponding plurality of openings of the vapor deposition mask.

Citation Information

Patent Citations

  • Vapor deposition mask and manufacturing method of vapor deposition mask, organic el element, electronic equipment

    JP2009087840A

  • Vapor-deposition mask, method of manufacturing the same, and method of manufacturing organic el display device

    JP2013209710A

  • Forming method of submicrom photo-resist pattern

    JP1986222127A