Aluminum-silicon alloy welding wire and preparation method and application thereof
Through the two-stage drawing treatment and ultrasonic refinement process of aluminum-silicon alloy cast rod, the problem of poor plasticity during processing of high-strength Al-Si-Cu aluminum alloy welding wire is solved, the melt fluidity and strength of the welding wire are improved, and it is suitable for Highly demanding military and aerospace fields.
Patent Information
- Application Number
- CN202211072603.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-02
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-09-02
AI Technical Summary
High-strength Al-Si-Cu aluminum alloy welding wire has poor plasticity during processing and is difficult to form, resulting in unstable welding quality, and it is difficult to overcome the problem of wire breakage with conventional methods.
A two-stage drawing process of aluminum-silicon alloy cast rod is adopted, including the first drawing and annealing treatment, combined with ultrasonic refinement and horizontal casting process, to control the grain structure and improve the plasticity and strength of the welding wire.
It improves the melt fluidity and shear strength of aluminum-silicon alloy welding wire, reduces the risk of hot cracks, simplifies the production process, improves yield and metallurgical quality, and is suitable for military and aerospace fields.
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of aluminum alloy materials, and in particular to an aluminum-silicon alloy welding wire and a preparation method and application thereof. Background Art
[0002] High-strength Al-Si-Cu aluminum alloy welding wire is widely used in welding of aerospace structural parts, fuel tanks, etc. due to its high silicon content, good melt fluidity, small solidification range, and welds that are not prone to defects such as thermal cracks. It has good welding quality and high weld shear strength. However, due to the presence of a large amount of eutectic structure and free silicon in high-strength Al-Si-Cu alloy, the alloy has high strength and poor plasticity, is easy to break during processing, and is difficult to form using conventional methods. Therefore, it is urgent to develop a new preparation method for aluminum-silicon alloy welding wire. Summary of the invention
[0003] The purpose of the present application is to provide a method for preparing an aluminum-silicon alloy welding wire, so as to improve the problem of poor plastic deformation performance of high-strength aluminum-silicon alloy in the prior art.
[0004] Another object of the present application is to provide an aluminum-silicon alloy welding wire.
[0005] Another object of the present application is to provide an application of aluminum-silicon alloy welding wire.
[0006] In a first aspect, the present application provides a method for preparing an aluminum-silicon alloy welding wire, comprising:
[0007] Provide aluminum silicon alloy casting rod;
[0008] Performing a first drawing process on the aluminum-silicon alloy cast rod to obtain a welding wire blank;
[0009] Annealing the welding wire blank at 350-400° C. for 1-3 hours;
[0010] The welding wire blank after annealing is subjected to a second drawing process to obtain an aluminum-silicon alloy welding wire.
[0011] Further, in some embodiments of the present application, the processing rate of the first drawing process is 7-12%; the diameter of the welding wire blank is 4-5 mm; and / or
[0012] The processing rate of the second drawing process is 12-15%; the diameter of the aluminum-silicon alloy welding wire is 1.6-2.0 mm.
[0013] Furthermore, in some embodiments of the present application, the size of the grains in the aluminum-silicon alloy casting rod is not greater than 50 μm.
[0014] Further, in some embodiments of the present application, the aluminum-silicon alloy casting rod includes the following components by mass fraction: Si 8-9%, Cu 2.5-3.5%, Mn 0.1-0.2%, Cr 0.1-0.2%, Zr 0.1-0.3%, Ti 0.05-0.2%, Fe≤0.15%, Sr 0.1-0.3%, Ce 0.01-0.05%, La 0.01-0.05%, and the rest are Al and unavoidable impurity elements, with a single impurity element ≤0.05% and a total of ≤0.15%.
[0015] Further, in some embodiments of the present application, the preparation of the aluminum-silicon alloy casting rod comprises the following steps:
[0016] Providing aluminum melt; the aluminum melt is obtained through a refining process;
[0017] The aluminum melt is subjected to ultrasonic refinement treatment at 18-22 kHz.
[0018] Furthermore, in some embodiments of the present application, after the ultrasonic refinement treatment and before the first drawing treatment, the method further includes: casting an aluminum-silicon alloy casting rod by a horizontal casting process;
[0019] The aluminum-silicon alloy casting rod casting comprises:
[0020] The aluminum melt after ultrasonic refinement is cast at a temperature of 720-730°C and a rod pulling speed of 700-1000 mm / min, and then cooled to obtain an aluminum-silicon alloy casting rod.
[0021] Furthermore, in some embodiments of the present application, the diameter of the aluminum-silicon alloy casting rod is 7-9 mm.
[0022] Further, in some embodiments of the present application, the refining process includes:
[0023] Provide aluminum liquid;
[0024] Adding a grain refiner to the aluminum liquid and refining it online to obtain an aluminum melt;
[0025] Wherein, the grain refiner is Al-5Ti-0.25C-8Sr; the addition amount of the grain refiner is 1.0-4.0% by mass fraction.
[0026] Furthermore, in some embodiments of the present application, the preparation of the aluminum liquid includes the following steps:
[0027] Providing raw materials according to the elemental composition of the aluminum-silicon alloy welding wire, melting and slagging to obtain a melt;
[0028] The melt is refined at 740-750° C. for 3-5 minutes, slag is removed, and the melt is allowed to stand for 30-40 minutes to obtain the aluminum liquid.
[0029] In a second aspect, the present application also provides an aluminum-silicon alloy welding wire, comprising the following components by mass fraction: Si8-9%, Cu 2.5-3.5%, Mn 0.1-0.2%, Cr 0.1-0.2%, Zr 0.1-0.3%, Ti 0.05-0.2%, Fe ≤0.15%, Sr 0.1-0.3%, Ce 0.01-0.05%, La 0.01-0.05%, and the rest are Al and unavoidable impurity elements, with a single impurity element ≤0.05% and a total of ≤0.15%;
[0030] The aluminum-silicon alloy welding wire is prepared by an aluminum-silicon alloy casting rod; the size of the grains in the aluminum-silicon alloy casting rod is not greater than 50 μm.
[0031] In a third aspect, the present application also provides the application of the aluminum-silicon alloy welding wire prepared by the preparation method of the aluminum-silicon alloy welding wire described in the first aspect or the aluminum-silicon alloy welding wire described in the second aspect in the military or aerospace fields.
[0032] The beneficial effects of the present invention are:
[0033] (1) A high-strength aluminum-silicon alloy welding wire product is provided, which has the advantages of good melt fluidity, small solidification range, low risk of thermal cracks in the weld, and high shear strength during welding.
[0034] (2) A short-process welding wire production process is provided, which has low energy consumption and high yield rate, overcomes the defects of large deformation, complex process and low yield rate existing in continuous casting and rolling and semi-continuous casting-extrusion process, and can obtain rod blanks with good metallurgical quality and surface quality;
[0035] (3) The alloy grain structure and metallurgical quality are jointly regulated by various means to improve the plasticity and toughness of the rod blank and provide good conditions for wire drawing processing. DETAILED DESCRIPTION
[0036] The technical solution of the present application will be described clearly and completely below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in the field without creative work are within the scope of protection of the present application.
[0037] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0038] In the description of the present application, it should be understood that “multiple” means two or more than two, unless otherwise clearly and specifically defined.
[0039] The disclosure below provides many different embodiments or examples to realize the different structures of the present application. In order to simplify the disclosure of the present application, the parts and settings of specific examples are described below. Of course, they are only examples, and the purpose is not to limit the present application. In addition, the present application can repeat reference numbers and / or reference letters in different examples, and this repetition is for the purpose of simplification and clarity, which itself does not indicate the relationship between the various embodiments and / or settings discussed. In addition, the examples of various specific materials provided by the present application, but those of ordinary skill in the art can be aware of the application of other processes and / or the use of other materials.
[0040] The present application provides a method for preparing an aluminum-silicon alloy welding wire, comprising:
[0041] Provide aluminum silicon alloy casting rod;
[0042] Performing a first drawing process on the aluminum-silicon alloy cast rod to obtain a welding wire blank;
[0043] Anneal the welding wire blank at 350~400℃ for 1~3h;
[0044] The annealed welding wire blank is subjected to a second drawing process to obtain an aluminum-silicon alloy welding wire.
[0045] In the present application, the aluminum-silicon alloy welding wire is obtained by a two-stage drawing process of an aluminum-silicon alloy cast rod, and the welding wire blank obtained by the first drawing process is annealed in the two-stage drawing process to eliminate the work hardening effect, improve the plasticity of the welding wire blank during the processing, reduce the breakage of the welding wire blank during the drawing process, and improve the yield; at the same time, the plasticity of the obtained aluminum-silicon alloy welding wire can also be improved.
[0046] In some embodiments, the aluminum-silicon alloy casting rod includes the following components by mass fraction: Si 8-9%, Cu 2.5-3.5%, Mn 0.1-0.2%, Cr 0.1-0.2%, Zr 0.1-0.3%, Ti 0.05-0.2%, Fe≤0.15%, Sr 0.1-0.3%, Ce 0.01-0.05%, La 0.01-0.05%, and the rest are Al and unavoidable impurity elements, with each impurity element being ≤0.05% and the total being ≤0.15%.
[0047] It should be noted that the unavoidable impurity elements are the impurity elements that are inevitably present in the raw materials used in the preparation of aluminum-silicon alloy casting rods and / or the elements that inevitably enter the aluminum alloy rod during the preparation process of the aluminum alloy rod, such as hydrogen, oxygen, nitrogen, manganese, and zinc.
[0048] In addition, the composition of the aluminum-silicon alloy cast rod used in the present application also contains Sr, Zr-based rare earth elements La and Ce, which are used to refine the grains of the aluminum-silicon alloy cast rod, so that the free silicon precipitated in the aluminum-silicon alloy cast rod is evenly distributed in the matrix in the form of fine and dispersed block phases, which greatly improves the plasticity and toughness of the rod blank, provides good conditions for subsequent welding wire drawing processing, and improves the yield and plasticity of the aluminum-silicon alloy welding wire.
[0049] In some embodiments, the first drawing process has a pass processing rate of 7-12%; the diameter of the welding wire blank is 4-5 mm; and / or
[0050] The processing rate of the second drawing process is 12~15%; the diameter of the aluminum-silicon alloy welding wire is 1.6~2.0mm.
[0051] In some embodiments, in the second drawing process, the welding wire blank is subjected to 8 consecutive drawing processes to obtain the aluminum-silicon alloy welding wire.
[0052] In some embodiments, the size of the grains in the aluminum-silicon alloy cast rod is no more than 50 μm, so that the grains in the aluminum-silicon alloy cast rod are fine particle phases, and free silicon is also dispersed in the form of fine dispersed particle phases, thereby improving the tensile strength of the aluminum-silicon alloy cast rod, facilitating the subsequent drawing process of the aluminum-silicon alloy cast rod, and improving the yield of the aluminum-silicon alloy welding wire; at the same time, the grain size in the aluminum-silicon alloy cast rod is no more than 50 μm, which can also improve the strength performance of the aluminum-silicon alloy cast rod, thereby improving the strength of the aluminum-silicon alloy welding wire and optimizing the strength performance of the aluminum-silicon alloy welding wire.
[0053] In some embodiments, the preparation of the aluminum-silicon alloy casting rod comprises the following steps:
[0054] Providing aluminum melt; the aluminum melt is obtained through a refining process;
[0055] The aluminum melt is subjected to ultrasonic refinement treatment at 18-22kHz. The aluminum melt is locally supercooled by the acoustic cavitation of ultrasound, and fine Al3Zr and Al4Ce particles are precipitated, which serve as solidification cores to refine the grains, optimize the quality of the precipitated grains in the aluminum-silicon alloy casting rod, and control the size of the precipitated grains in the aluminum-silicon alloy casting rod to be no more than 50μm.
[0056] In some embodiments, the power of the ultrasonic wave in the ultrasonic thinning process is 1-2 kW.
[0057] In some embodiments, after the ultrasonic thinning process and before the first drawing process, the method further includes: casting an aluminum-silicon alloy rod by a horizontal casting process;
[0058] Aluminum-silicon alloy rod casting includes:
[0059] The aluminum melt after ultrasonic refinement is cast at a temperature of 720-730°C and a rod pulling speed of 700-1000 mm / min, and then cooled to obtain an aluminum-silicon alloy casting rod.
[0060] The horizontal casting process has low energy consumption and high yield rate, which can overcome the defects of excessive deformation, complex procedures and low yield rate in the existing continuous casting and rolling and semi-continuous casting-extrusion processes, so that the obtained aluminum-silicon alloy cast rods have good metallurgical quality and surface quality.
[0061] In some embodiments, cooling comprises:
[0062] Use 15~30℃ cooling water to directly spray the casting rod to cool the casting rod surface.
[0063] In some embodiments, the diameter of the aluminum-silicon alloy casting rod is 7-9 mm.
[0064] In some embodiments, the refining process includes:
[0065] Provide aluminum liquid;
[0066] Adding a grain refiner to the aluminum liquid and refining it online to obtain an aluminum melt;
[0067] Among them, the grain refiner is Al-5Ti-0.25C-8Sr; the addition amount of the grain refiner is 1.0~4.0% by mass fraction.
[0068] The refiner can refine the grains by forming an Al3Ti film on the TiC particles as a crystal core, and can also form a high melting point phase SrAl2Si2, which has a metamorphic effect on the eutectic silicon during solidification, transforming it from a coarse lath shape to a fine block or dot distribution.
[0069] In some embodiments, the preparation of aluminum liquid includes the following steps:
[0070] Providing raw materials according to the elemental composition of the aluminum-silicon alloy welding wire, melting, and slagging to obtain a melt;
[0071] Refining the melt at 740-750°C for 3-5 minutes, skimming off the slag, and letting it stand for 30-40 minutes to obtain molten aluminum.
[0072] In some embodiments, the aluminum-silicon alloy welding wire further includes a peeling process, cleaning, and drying after the second drawing process.
[0073] In a second aspect, the present application also provides an aluminum-silicon alloy welding wire, comprising the following components by mass fraction: Si8-9%, Cu 2.5-3.5%, Mn 0.1-0.2%, Cr 0.1-0.2%, Zr 0.1-0.3%, Ti 0.05-0.2%, Fe ≤0.15%, Sr 0.1-0.3%, Ce 0.01-0.05%, La 0.01-0.05%, and the rest are Al and unavoidable impurity elements, with a single impurity element ≤0.05% and a total of ≤0.15%;
[0074] The aluminum-silicon alloy welding wire is prepared by an aluminum-silicon alloy casting rod; the size of the grains in the aluminum-silicon alloy casting rod is not greater than 50 μm.
[0075] In some embodiments, Ti and Sr are added in the form of grain refiners, and Ce and La are added in the form of aluminum rare earth master alloys.
[0076] In some embodiments, the online refining includes: after the casting starts, the melt is degassed online in the launder to obtain aluminum liquid.
[0077] In a third aspect, the present application also provides the application of the aluminum-silicon alloy welding wire prepared by the preparation method of the aluminum-silicon alloy welding wire described in the first aspect or the aluminum-silicon alloy welding wire described in the second aspect in the military or aerospace fields.
[0078] In order to enable the above-mentioned implementation details and operations of the present application to be clearly understood by those skilled in the art, and to significantly demonstrate the improved performance of an aluminum-silicon alloy welding wire and its preparation method and application provided in the embodiments of the present application, the above-mentioned technical scheme is illustrated by means of multiple embodiments below.
[0079] Example 1
[0080] The present embodiment provides a method for preparing an aluminum-silicon alloy welding wire, wherein the components of the aluminum-silicon alloy welding wire include, by mass fraction, Si 8.8%, Cu 3.1%, Mn 0.12%, Cr 0.15%, Zr 0.14%, Ti 0.11%, Fe0.14%, Sr0.15%, Ce0.03%, La 0.03%, and the rest are Al and unavoidable impurity elements, wherein the impurity element is ≤0.05% individually and ≤0.15% in total.
[0081] The specific preparation method comprises:
[0082] Step 1: Add a certain amount of aluminum ingots, quick-dissolving silicon, aluminum-copper alloy, aluminum-manganese alloy, aluminum-chromium alloy, aluminum-zirconium alloy, and aluminum-rare earth alloy into the smelting furnace, heat and melt them, stir the molten aluminum liquid and skim off the slag.
[0083] Step 2: Adjust the temperature of aluminum liquid to 740℃. Use argon gas to perform furnace refining for 5 minutes, then completely scrape off the slag on the surface of the aluminum melt and let it stand for 40 minutes.
[0084] Step 3: After the casting starts, Al-5Ti-0.25C-8Sr grain refiner is added online in the launder, and the amount of the refiner added is 2.0% by mass.
[0085] Step 4: The aluminum melt flowing through the launder is degassed and filtered online to further remove hydrogen and oxide inclusions in the melt and improve the purity of the melt.
[0086] Step 5: The refined aluminum melt is subjected to ultrasonic refinement treatment, with an ultrasonic power of 1.5Kw and a frequency of 20KHz. The aluminum melt after ultrasonic refinement treatment then enters the rod casting device.
[0087] Step 6: Use a multi-mode parallel horizontal casting device to prepare a 9mm diameter welding wire rod blank, with a casting temperature of 720°C and a rod pulling speed of 700mm / min. Use 20°C cooling water to spray directly on the surface of the pulled rod blank for cooling.
[0088] Step seven: Use a 6-die wire drawing machine to continuously draw the continuously cast rod, with the processing rates of 9mm-8.1mm-7.2mm-6.4mm-5.8mm-5.2mm-4.8mm respectively, and draw the rod blank to a diameter of 4.8mm.
[0089] Step 8: Anneal the welding wire blank at a temperature of 390°C and a holding time of 2 hours.
[0090] Step nine: the annealed welding wire is continuously drawn, and the processing rates of the passes are 4.8mm-4.2mm-3.7mm-3.2mm-2.8mm-2.5mm-2.3mm-2.0mm, respectively, and drawn into an aluminum alloy welding wire with a diameter of 2.0mm.
[0091] Step 10: Strip the drawn aluminum alloy welding wire, clean it online, and then dry it with hot air before winding it up.
[0092] The present embodiment provides a method for preparing an aluminum-silicon alloy welding wire, wherein the components of the aluminum-silicon alloy welding wire include, by mass fraction, Si 8.3%, Cu 2.8%, Mn 0.15%, Cr 0.13%, Zr 0.17%, Ti 0.15%, Fe0.15%, Sr0.24%, Ce0.02%, La 0.02%, and the rest are Al and unavoidable impurity elements, wherein the impurity element is ≤0.05% individually and ≤0.15% in total.
[0093] The specific preparation method comprises:
[0094] Step 1: Add a certain amount of aluminum ingots, quick-dissolving silicon, aluminum-copper alloy, aluminum-manganese alloy, aluminum-chromium alloy, aluminum-zirconium alloy, and aluminum-rare earth alloy into the smelting furnace, heat and melt them, stir the molten aluminum liquid and skim off the slag.
[0095] Step 2: Adjust the temperature of aluminum liquid to 740℃. Use argon gas to perform furnace refining for 5 minutes, then completely scrape off the slag on the surface of the aluminum melt and let it stand for 40 minutes.
[0096] Step 3: After the casting starts, Al-5Ti-0.25C-8Sr grain refiner is added online in the launder, and the amount of the refiner added is 3.0% by mass.
[0097] Step 4: The aluminum melt flowing through the launder is degassed and filtered online to further remove hydrogen and oxide inclusions in the melt and improve the purity of the melt.
[0098] Step 5: The refined aluminum melt is subjected to ultrasonic refinement treatment, with an ultrasonic power of 1.5Kw and a frequency of 20KHz. The aluminum melt after ultrasonic refinement treatment then enters the rod casting device.
[0099] Step 6: Use a multi-mode parallel horizontal casting device to prepare a 7mm diameter welding wire rod blank, with a casting temperature of 720°C and a rod pulling speed of 700mm / min. Use 20°C cooling water to spray directly on the surface of the pulled rod blank for cooling.
[0100] Step seven: Use a 6-die wire drawing machine to continuously draw the continuously cast rod, with the processing rates of 7mm-7.3mm-6.5mm-5.9mm-5.4mm-4.9mm-4.5mm respectively, and draw the rod blank to a diameter of 4.2mm.
[0101] Step 8: Anneal the welding wire blank at a temperature of 400°C and a holding time of 1.5 hours.
[0102] Step nine: The annealed welding wire is continuously drawn, and the processing rates of the passes are 4.5mm-4.0mm-3.5mm-3.1mm-2.7mm-2.4mm-2.1mm-1.8mm-1.6mm, and drawn into an aluminum alloy welding wire with a diameter of 1.6mm.
[0103] Step 10: Peel the drawn aluminum alloy welding wire, clean it online, and then dry it with hot air before winding it up.
[0104] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit it. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present application.
Claims
1. A method for preparing an aluminum-silicon alloy welding wire, characterized in that: include: Provide aluminum silicon alloy casting rod; Performing a first drawing process on the aluminum-silicon alloy cast rod to obtain a welding wire blank; Annealing the welding wire blank at 350-400° C. for 1-3 hours; Performing a second drawing process on the welding wire blank after annealing to obtain an aluminum-silicon alloy welding wire; The aluminum-silicon alloy casting rod includes the following components by mass fraction: Si 8-9%, Cu 2.5-3.5%, Mn 0.1-0.2%, Cr 0.1-0.2%, Zr 0.1-0.3%, Ti 0.05-0.2%, Fe≤0.15%, Sr 0.1-0.3%, Ce0.01-0.05%, La 0.01-0.05%, and the rest are Al and unavoidable impurity elements, with a single impurity element ≤0.05% and a total of ≤0.15%.
2. The method for preparing the aluminum-silicon alloy welding wire according to claim 1, characterized in that: The processing rate of the first drawing process is 7-12%; the diameter of the welding wire blank is 4-5 mm; and / or The processing rate of the second drawing process is 12-15%; the diameter of the aluminum-silicon alloy welding wire is 1.6-2.0 mm.
3. The method for preparing the aluminum-silicon alloy welding wire according to claim 1, characterized in that: The size of the grains in the aluminum-silicon alloy casting rod is no more than 50 μm.
4. The method for preparing the aluminum-silicon alloy welding wire according to claim 1, characterized in that: The preparation of the aluminum-silicon alloy casting rod comprises the following steps: Providing aluminum melt; the aluminum melt is obtained through a refining process; The aluminum melt is subjected to ultrasonic refinement treatment at 18 to 22 kHz.
5. The method for preparing the aluminum-silicon alloy welding wire according to claim 4, characterized in that: After the ultrasonic refinement treatment and before the first drawing treatment, the method further includes: casting an aluminum-silicon alloy casting rod by a horizontal casting process; The aluminum-silicon alloy casting rod casting comprises: The aluminum melt after ultrasonic refinement is cast at a temperature of 720-730° C. and a rod pulling speed of 700-1000 mm / min, and then cooled to obtain an aluminum-silicon alloy casting rod.
6. The method for preparing the aluminum-silicon alloy welding wire according to claim 5, characterized in that: The diameter of the aluminum-silicon alloy casting rod is 7-9 mm.
7. An aluminum-silicon alloy welding wire, characterized in that: It includes the following components by mass fraction: Si8-9%, Cu 2.5-3.5%, Mn 0.1-0.2%, Cr 0.1-0.2%, Zr 0.1-0.3%, Ti 0.05-0.2%, Fe≤0.15%, Sr 0.1-0.3%, Ce 0.01-0.05%, La 0.01-0.05%, and the rest are Al and unavoidable impurity elements, with a single impurity element ≤0.05% and a total of ≤0.15%; The aluminum-silicon alloy welding wire is prepared by an aluminum-silicon alloy casting rod; the size of the grains in the aluminum-silicon alloy casting rod is not greater than 50 μm.
8. Application of the aluminum-silicon alloy welding wire prepared by the method for preparing the aluminum-silicon alloy welding wire according to any one of claims 1 to 6 or the aluminum-silicon alloy welding wire according to claim 7 in the military or aerospace fields.
Citation Information
Patent Citations
Aluminum alloy welding wire and preparation method thereof
CN103695735A
Aluminum alloy welding wire for aerospace and preparation method of aluminum alloy welding wire for aerospace
CN105779831A
Al-Mg-Zn aluminum alloy welding wire and preparation method thereof
CN108396206A
Preparation method of aluminum-silicon wire material for additional material remanufacturing
CN110732807A
Preparation process of high-strength aluminum alloy welding wire
CN113649415A