Antipathogen structure, method for producing an antipathogen structure, device for producing an antipathogen structure and liquid composition

By using an anti-pathogen structure with a porous resin structure, the problem of reduced activity of conventional anti-pathogen structures is solved, and anti-microbial and anti-viral effects of high durability and low allergic response are achieved.

CN115243731BActive Publication Date: 2024-10-11RICOH CO LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
CN202180020259.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-11-24
Filing Date
2021-02-10
Publication Date
2024-10-11
Estimated Expiration
2041-02-10

AI Technical Summary

Technical Problem

Conventional anti-pathogen structures can easily lead to a reduction in antimicrobial or antiviral activity during use, and there is a risk of potential allergic reactions to the human body.

Method used

A resin structure with multiple openings is used as the anti-pathogen structure, and its surface forms a porous structure through the polymerization of polymeric compounds, which is combined with a light or thermal initiator to solidify the liquid composition to form an anti-pathogen active resin structure, avoiding the need for antimicrobial agents or Antiviral dependence.

Benefits of technology

Improved durability and antimicrobial or antiviral activity of the antipathogenic structure, reduced risk of allergic reactions caused by antimicrobial or antiviral agents, and prolonged retention of activity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115243731B_ABST
    Figure CN115243731B_ABST
Patent Text Reader

Abstract

An anti-pathogen structure includes a resin structure having a plurality of openings in a surface of the resin structure, wherein the resin structure has antimicrobial activity or antiviral activity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to antipathogenic structures, methods for producing antipathogenic structures, apparatuses for producing antipathogenic structures, and liquid compositions. Background Art

[0002] In recent years, many products that exhibit antimicrobial or antiviral activity are commercially available. Antimicrobial activity refers to, for example, a property of reducing the number of microorganisms. Antiviral activity refers to a property of reducing the number of viruses or reducing overall viral activity (e.g., the ability to infect a host and the efficacy of proliferation in a host). As methods for achieving antimicrobial or antiviral activity, for example, methods of introducing agents that are known to cause certain damage to or kill microorganisms or viruses into structures, and methods of using structures with special surface structures to cause certain damage to or kill microorganisms or viruses in contact with the surface structure.

[0003] Non-patent document 1 discloses that there is a fine protrusion structure on the surface of cicada wings, and the protrusion structure exhibits antimicrobial activity. More specifically, it discloses that a column (nanopillar) with a fine protrusion structure destroys the outer shell part (e.g., cell membrane and cell wall) of a microorganism to exhibit antimicrobial activity.

[0004] Non-patent document 2, Patent document 1, and Patent document 2 disclose that antimicrobial activity can be exhibited even when a structure simulating the aforementioned pillars with fine protrusion structures (nanopillars) is artificially produced.

[0005] Citations

[0006] Patent Literature

[0007] PTL1: Japanese Unexamined Patent Application Publication No. 2019-72475

[0008] PTL2: Japanese Patent No. 6454710

[0009] Non-patent literature

[0010] NPL1: Elena P. Ivanova et al., “Natural Bactericidal Surfaces: Mechanical Rupture of Pseudomonas aeruginosa Cells by Cicada Wings”, small, 2012, Vol. 8, No. 16, pp. 2489-2494

[0011] NPL2: Elena P.Ivanova et al., "Bactericidal activity of black silicon", Nature Communications, November 26, 2013 Summary of the invention

[0012] Technical issues

[0013] However, conventional antipathogenic structures have a problem in that the antimicrobial activity or antiviral activity is easily reduced.

[0014] Problem Solution

[0015] According to one aspect of the present disclosure, an antipathogen structure includes a resin structure having a plurality of openings in a surface thereof, and having antimicrobial activity or antiviral activity.

[0016] Advantageous Effects of the Invention

[0017] The present disclosure achieves a superior effect of preventing reduction in antimicrobial activity or antiviral activity. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] [ Figure 1 ] Figure 1 is a schematic diagram presenting one example of an apparatus for producing an antipathogen structure to implement a method for producing an antipathogen structure of an embodiment of the present disclosure.

[0019] [ Figure 2 ] Figure 2 This is a view obtained when observing the surface of a resin structure (antipathogen structure) using a scanning electron microscope (SEM), the resin structure including: a skeleton having a shape in which a plurality of particles are connected to each other; and openings shaped by the skeleton.

[0020] [ Figure 3 ] Figure 3 This is a view obtained when observing the surface of a resin structure (antipathogenic structure) using a scanning electron microscope (SEM), the resin structure including a skeleton having a substantially flat shape; and openings shaped by the skeleton.

[0021] [ Figure 4 ] Figure 4 This is a view obtained when the surface of the antipathogen structure of Example 1 was observed using a scanning electron microscope (SEM).

[0022] [ Figure 5 ] Figure 5 This is a view obtained when the surface of the structure of Comparative Example 1 was observed with a scanning electron microscope (SEM).

[0023] [ Figure 6] Figure 6 This is a view obtained when the surface of the structure of Example 4 was observed using a scanning electron microscope (SEM). DETAILED DESCRIPTION

[0024] Hereinafter, one embodiment of the present disclosure will be described.

[0025] <<Anti-pathogen structure>>

[0026] The antipathogen structure of the present embodiment includes a resin structure having a plurality of openings in a surface of the resin structure, and may further include other substances as required. The antipathogen structure may not include other substances, and may include only the resin structure.

[0027] The antipathogen structure represents the concept of including an antimicrobial structure that exhibits antimicrobial activity and an antiviral structure that exhibits antiviral activity. The antipathogen structure is a structure that exhibits antimicrobial activity or antiviral activity as a whole, because the resin structure that constitutes the antipathogen structure has antimicrobial activity or antiviral activity. In other words, the resin structure itself is a structure that can exhibit antimicrobial activity or antiviral activity. Note that when only the resin structure is included to exhibit antimicrobial activity or antiviral activity, an agent with antimicrobial activity (hereinafter referred to as an antimicrobial agent) or an agent with antiviral activity (hereinafter referred to as an antiviral agent) as other substances may be additionally included in the structure or may be carried on the surface of the structure. In the following description, when antimicrobial activity and antiviral activity are mentioned together, these activities are referred to as "antipathogen activity". Note that pathogens generally represent one of the properties of causing disease in an organism as a host. However, in the present disclosure, pathogens represent the concept of collectively referring to microorganisms and viruses, regardless of whether they have the property of causing disease.

[0028] Antimicrobial activity refers to the property of reducing the number of microorganisms by contacting the resin structure with the microorganisms to have a certain influence (for example, damage and kill microorganisms) on the microorganisms. That is, it cannot be said that the resin structure has antimicrobial activity when it is difficult to contact the resin structure with the microorganisms because the resin structure is sealed or tightly sealed by other components. Here, the phrase "reducing the number of microorganisms" means that the number of microorganisms applied to the test piece (test piece C) including the antipathogen structure is reduced over time compared with the number of microorganisms applied to the test piece (test piece B), wherein the test piece (test piece B) is formed by the same material as the material constituting the antipathogen structure, but has a flat surface structure and does not have a plurality of openings. There is no specific restriction on the method for confirming this property. The example of the method includes: a method for directly observing the movement of microorganisms using, for example, a method for observing the dead body of microorganisms using SEM, and a confirmation method using, for example, an antimicrobial test. Specifically, the antimicrobial test is preferably a test carried out according to the method described in, for example, JIS Z 2801 (2012), JIS Z 2901 (2018) and ISO 22196 (2011).

[0029] When tested according to the method of JIS Z 2801 (2012), the antimicrobial activity value evaluated in this test is preferably 0.3 or more, and is preferably judged to have antimicrobial activity. The antimicrobial activity value is preferably 0.5 or more, more preferably 1.0 or more, even more preferably 1.5 or more, and particularly preferably 2.0 or more. Here, the antimicrobial activity value obtained according to the method of JIS Z 2801 (2012) is represented by the following numerical formula. Specifically, the same bacterial culture is inoculated into an unprocessed test piece (test piece A) as a glass substrate, a test piece B formed on the test piece A, and a test piece C formed on the test piece A. Then, the viable cell count obtained after 24 hours is measured, and the antimicrobial activity value is calculated based on the following numerical formula. The situation where the antimicrobial activity value is more than 2 can be defined as an antimicrobial material. However, in the present embodiment, the situation where the antimicrobial activity value is more than 0.3 is judged to have antimicrobial activity in preventing microbial proliferation.

[0030] Antimicrobial activity value = (log B-log A)*(log C-log A).

[0031] A: Average value of viable cell counts on test piece A obtained after 24 hours.

[0032] B: Average value of viable cell counts on test piece B obtained after 24 hours.

[0033] C: Mean value of the viable cell count on test piece C obtained after 24 hours.

[0034] When tested according to the method of ISO 22196 (2011), the case where the antibacterial activity value evaluated in this test is 0.3 or more is preferably judged to have antimicrobial activity. The antibacterial activity value is preferably 0.5 or more, more preferably 1.0 or more, even more preferably 1.5 or more, and particularly preferably 2.0 or more. Here, the antibacterial activity value obtained according to the method of ISO 22196 (2011) is expressed by the following numerical formula. Specifically, the same bacterial culture is inoculated into test piece B and test piece C, respectively, and the viable cell count obtained after 24 hours is measured to calculate the antibacterial activity value based on the following numerical formula. Note that JIS Z2801 (2012) and ISO 22196 (2011) are standards that basically correspond to each other.

[0035] Antibacterial activity value = Ut-At.

[0036] Ut: average value of the common logarithm value of the live cell count on the test piece B obtained after 24 hours.

[0037] At: average value of the common logarithm value of the live cell count on the test piece C obtained after 24 hours.

[0038] Antiviral activity refers to the property of reducing the number of viruses or reducing the activity (for example, the infectivity of the host and the propagation efficacy in the host) by contacting the resin structure with the virus to have a certain effect on the virus (for example, damage and kill the virus). That is, it cannot be said that the resin structure has antiviral activity when it is difficult to contact the resin structure with the virus because the resin structure is sealed or tightly sealed by other components. Here, the phrase "reduce the number of viruses" or "reduce the overall viral activity" means that the number of viruses applied to the test piece (test piece X) including the antipathogen structure or the activity obtained in the overall virus is reduced over time compared with the number of viruses applied to the test piece (test piece Y) or the activity obtained in the overall virus, wherein the test piece (test piece Y) is formed by the same material as the material constituting the antipathogen structure, but has a flat surface structure and does not have a plurality of openings. There is no specific limitation on the method for confirming the above-mentioned properties. For example, the following method is adopted: specifically, viruses with the same concentration are each applied to test piece X and test piece Y, and left to stand for a certain time. Then, the viruses that have been left to stand are each exposed to the host to infect the host with the virus. Then, it is observed whether the host is infected with the virus and whether the host survives or dies. When the onset is not observed or when the host is not dead, a portion of the host's tissue obtained after a period of time has passed since the virus exposure is removed, crushed, and suspended to prepare a suspension. Then, a dilution series of the suspension is prepared, and the dilution series is used to infect cultured cells with the virus. Determine the TCID 50Value (50% tissue culture infection dose) to quantify the virus. Specifically, the antiviral test is preferably a test performed according to the method described in, for example, ISO 21702 (2019). Note that ISO 21702 (2019) is a virus test obtained by improvement of the above-mentioned antimicrobial test (ISO 22196 and JIS Z2801).

[0039] When tested according to the method of ISO 21702 (2019), the case where the antiviral activity value evaluated in this test is 0.2 or more is preferably judged to have antiviral activity. The antiviral activity value is preferably 0.5 or more, more preferably 1.0 or more, even more preferably 1.5 or more, and particularly preferably 2.0 or more. Here, the antiviral activity value obtained according to the method of ISO 21702 (2019) is expressed by the following numerical formula. Specifically, the same virus culture is inoculated into test piece X and test piece Y, respectively, and the virus infectivity titer (PFU / cm 2 ), to calculate the antiviral activity value based on the following numerical formula. The case where the antiviral activity value is 2 or more can be defined as an antiviral material. However, in this embodiment, the case where the antiviral activity value is 0.2 or more is judged to have antiviral activity in preventing antiviral proliferation.

[0040] Antiviral activity value = Ut-At.

[0041] Ut: average value of the common logarithm of the virus infectivity titer on test piece Y obtained after 24 hours.

[0042] At: the average of the common logarithm values ​​of the virus infectivity titers on the test pieces X obtained after 24 hours.

[0043] The antipathogen structure preferably has water resistance. Specifically, the antipathogen structure more preferably has antipathogen activity even when immersed in water (specifically, such as purified water and ion exchange water) at 25 degrees Celsius for 24 hours. This is because it is assumed that the antipathogen structure is used in an environment where water adheres when the antipathogen structure is used.

[0044] Microorganisms refer to small prokaryotes and eukaryotes. Examples of microorganisms include: Gram-negative and Gram-positive bacteria, Staphylococcus aureus, Escherichia coli, Yersinia pestis, Vibrio cholerae, Mycobacterium tuberculosis, Pseudomonas aeruginosa, aeruginosa), spirochetes that cause syphilis or Lyme disease, Rickettsia that causes epidemic louse-borne typhus or scrub typhus (tsutsugamushi), chlamydia, mycoplasmas, and cyanobacteria, which are classified as prokaryotes; methanogens and hyperthermophiles, which are classified as prokaryotes; and molds, fungi, yeasts, Candida, Trichophyton, and Plasmodium, which causes malaria, which are classified as eukaryotes.

[0045] The microorganisms in the present application are not limited to the currently identified microorganisms, and also include microorganisms to be identified in the future. Examples of microorganisms to be identified in the future include drug-resistant bacteria, such as MRSA (methicillin-resistant Staphylococcus aureus) and microorganisms to be newly identified or named.

[0046] Viruses are tiny infectious structures that replicate themselves by exploiting the cells of other organisms. Examples of viruses include DNA viruses, including, for example, herpes viruses, pox viruses, and hepadnaviruses; and RNA viruses, including, for example, flaviviruses, togaviruses, coronaviruses, hepatitis delta virus, orthomyxoviruses, paramyxoviruses, rhabdoviruses, bunyaviruses, filoviruses, and retroviruses.

[0047] Examples of orthomyxoviruses include influenza virus A, influenza virus B, influenza virus C, infectious salmon anemia virus (isavirus), thogoto virus, and quaranjavirus.

[0048] Examples of coronaviruses include alphacoronavirus, betacoronavirus, gammacoronavirus, and deltacoronavirus.

[0049] Examples of paramyxoviruses include paramyxovirus, rubulavirus, morbillivirus, and pneumovirus.

[0050] The viruses in this application are not limited to the currently identified viruses, and also include viruses to be identified in the future. Examples of viruses to be identified in the future include mutant new viruses and viruses to be newly identified or named.

[0051] The shape of the antipathogen structure can be appropriately selected according to the intended purpose. Examples of shapes include shapes such as layer shapes (film shapes) and particle shapes. When using an antipathogen structure with a layer shape (film shape), the layer shape (film shape) can be a flat shape or a curved shape. A composite material formed by aggregating multiple antipathogen structures or a coating formed on the surface of another member can be used.

[0052] When in use, the shape of the antipathogen structure is preferably a shape in which the surface structure is easily affected by, for example, wear. The reason is as follows. Specifically, even when having such a shape, the antipathogen structure of the present disclosure has high durability, and can further significantly achieve the effect of preventing the reduction of antimicrobial activity or antiviral activity. When used in this way, the shape that makes the surface structure easily affected by, for example, wear can be, for example, a layer shape (film shape). At the same time, in the case of a particle shape, the surface structure has a shape in which the surface structure is hardly affected by, for example, wear during use. Therefore, the shape of the antipathogen structure may not be a particle shape.

[0053] <Resin structure>

[0054] The resin structure is a structure formed using a resin as a material. The resin structure refers to: a structure including a synthetic resin produced by artificially polymerizing a polymerizable compound as a material; or a structure including a resin of natural origin produced by artificially processing or treating a natural resin derived from a plant or animal as a material. The resin structure does not include a structure including only an unprocessed or untreated material such as a natural resin. The resin structure according to the present embodiment itself exhibits antipathogenic activity, as described above.

[0055] On the surface of the resin structure, a surface structure including multiple openings is formed. When a microorganism or virus contacts the surface structure, the surface adsorption force originating from the opening destroys the shell portion of the microorganism or virus, and exhibits antipathogenic activity. In this behavior, even the antipathogenic structure that does not substantially contain an antimicrobial or antiviral agent as a medicament can also exhibit antipathogenic activity. This makes it possible to prevent the effects on the human body (such as allergic reactions) that may be caused by an antimicrobial or antiviral agent. Unlike an antimicrobial or antiviral agent, it is consumed without passing time, thereby improving the persistence of the effect (antipathogenic activity). In addition, the appearance of microorganisms or viruses that are tolerant to an antimicrobial or antiviral agent can be prevented.

[0056] The surface structure includes a plurality of openings and a skeleton that shapes the plurality of openings. The opening is the portion of the surface structure other than the skeleton, and at least represents a space open to the outside world. The skeleton is the portion of the surface structure other than the plurality of openings, and represents a structural portion formed by a resin. The skeleton is a continuous structure on the surface of the resin structure, and the continuous structure shapes the plurality of openings. Therefore, a conventional structure having a column (nanopillar) with a fine protrusion structure but having a discontinuous surface structure has low durability. At the same time, the surface structure of the present embodiment is not susceptible to fine structure degradation caused by wear. Therefore, the durability of the antipathogen structure is improved. That is, the surface structure according to the present embodiment easily maintains the shape of the plurality of openings, which helps to achieve antipathogen activity to prevent the antipathogen activity from being reduced.

[0057] The shape of the opening is not specifically limited. Examples of the shape include various shapes, such as a substantially circular shape, a substantially elliptical shape, and a substantially polygonal shape. The aperture of the opening is not specifically limited. The aperture of the opening refers to the length of the longest straight line drawn when observing the opening (in other words, when viewing the opening in a plane). Specifically, the aperture of the opening can be determined using a photograph taken, for example, by a scanning electron microscope (SEM).

[0058] In order to achieve antimicrobial activity, the aperture of the opening is preferably less than 10 microns, more preferably less than 5 microns, still more preferably less than 1 micron, particularly preferably less than 0.5 micron. When the aperture of the opening is less than 10 microns, the surface adsorption force from the opening destroys the shell part (for example, the cell membrane and cell wall of the microorganism), and the antimicrobial activity is appropriately expressed. Preferably, the aperture of the opening is appropriately changed according to the type or size of the microorganism that will present antimicrobial activity. In general, the aperture of the opening is preferably less than the maximum diameter of the microorganism. For example, the aperture of the opening is preferably less than 10 microns in the case of fungi, the aperture of the opening is preferably less than 1 micron in the case of Staphylococcus aureus, and the aperture of the opening is preferably less than 4 microns in the case of Escherichia coli. The surface adsorption force is inversely proportional to the aperture of the opening. Therefore, the smaller the aperture, the greater the surface adsorption force, and therefore a higher antimicrobial activity can be expected. The aperture of the opening can be appropriately adjusted by, for example, the polymerization conditions (for example, the irradiation intensity and irradiation time of the emission active energy ray) that allow the polymerization of the polymerizable compound. To distinguish the opening pore size for achieving the following antiviral activity purpose, the opening pore size for achieving the antibacterial activity purpose may be larger than 0.1 micron.

[0059] In order to achieve antiviral activity, the aperture of the opening is preferably less than 0.1 micron, more preferably less than 0.05 micron. When the aperture of the opening is less than 0.1 micron, the surface adsorption force from the opening destroys the outer shell part (e.g., envelope) of the virus and appropriately expresses antiviral activity. Preferably, the aperture of the opening is appropriately changed according to the type or size of the virus that will present antiviral activity. In general, the aperture of the opening is preferably less than the maximum diameter of the virus. The surface adsorption force is inversely proportional to the aperture of the opening. Therefore, the smaller the aperture, the greater the surface adsorption force, and therefore the higher antiviral activity can be expected. The aperture of the opening can be appropriately adjusted by, for example, the polymerization conditions (e.g., the irradiation intensity and irradiation time of the emission active energy ray) that allow the polymerization of the polymerizable compound. Specifically, the aperture of the opening can be reduced by, for example, increasing the amount of the polymerizable compound or enhancing the irradiation intensity of the emission active energy ray. The lower limit of the aperture of the opening in the case where the antiviral activity will be presented is not specifically limited, but is preferably, for example, more than 0.001 micron.

[0060] The shape of the skeleton is not particularly limited as long as it can shape the opening. Examples of the shape include various shapes such as a shape obtained by coupling a plurality of particles to each other and a substantially planar shape. Figure 2 is a view obtained by observing the surface of a resin structure (antipathogenic structure) with SEM, the resin structure including: a skeleton having a shape obtained by coupling a plurality of particles to each other; and openings shaped by the skeleton. Figure 3 It is a view obtained by observing the surface of a resin structure (antipathogen structure) with SEM, the resin structure comprising: a skeleton having a substantially planar shape; and an opening shaped by the skeleton. As the shape of the skeleton, a substantially planar shape is more preferred than a shape obtained by connecting a plurality of particles to each other. The reasons are as follows. Specifically, in the case of a substantially planar shape, the surface of the surface structure forming the resin structure has a high hardness, which can reduce the impact caused by the wear degradation of the fine structure, and improve the durability of the antipathogen structure. Therefore, the antipathogen activity can be prevented from decreasing. Regarding the hardness of the surface of the surface structure forming the resin structure, it is preferred to use a pencil hardness evaluated according to the method described in, for example, ISO 15184. At this time, when the skeleton has a shape obtained by connecting a plurality of particles to each other, the pencil hardness is 6B to 2B. At the same time, when the shape of the skeleton is a substantially planar shape, the pencil hardness can be B or more, and further can be F or more. This evaluation can be performed by applying a load (750g) using, for example, a pencil hardness tester (available from Toyo Seiki Seisaku-sho, Ltd.). Furthermore, in order to improve the durability of the antipathogen structure and prevent the antipathogen activity from being reduced, the pencil hardness is preferably high.

[0061] The resin structure preferably has a porous structure having a co-continuous structure in which a plurality of pores are continuously coupled to each other. More preferably, the plurality of openings are each independently coupled to some of the pores constituting the co-continuous structure.

[0062] As mentioned above, the resin structure includes a plurality of holes, and preferably a structure in which these holes are connected to each other (in other words, the plurality of holes are continuously connected to each other). This structure is also referred to as a co-continuous structure or a monolithic structure. Since the resin structure includes a plurality of holes and a hole is connected to another hole around the hole, it has a connected property, and the continuous hole is three-dimensionally expanded. When the plurality of openings are independently connected to some of the holes constituting the co-continuous structure, the continuous capillary action (capillarity) from the opening on the surface to the internal co-continuous structure is performed, further improving the antipathogen activity. In addition, the dead body of microorganisms or viruses is discharged from the opening on the surface to the internal co-continuous structure, and prevented from remaining on the surface. Therefore, it is possible to prevent the antipathogen activity from decreasing over time. In addition, even when the surface of the resin structure is shaved, the inner hole is exposed as a new opening to present the antipathogen activity. Therefore, compared with the conventional structure with a column (nanopillar) with a fine protrusion structure, the expected effect of the antipathogen structure lasts for a long time.

[0063] Examples of methods for confirming that holes are connected to each other include a method in which a cross-sectional image of a resin structure is observed using, for example, a scanning electron microscope (SEM) to confirm that the holes connected to each other are continuous. An example of a physical property obtained when the holes are connected to each other is, for example, air permeability resistance. The air permeability resistance of the resin structure is measured according to, for example, JIS P8117. The air permeability resistance of the resin structure is preferably less than 1,000 seconds / 100ml, more preferably less than 500 seconds / 100ml, and even more preferably less than 300 seconds / 100ml. At this time, the air permeability resistance is measured using, for example, a gurley-type densitometer (available from Toyo Seiki Seisaku-sho, Ltd.). As an example, when the air permeability resistance is less than 1,000 seconds / 100ml, it can be judged that the holes are connected to each other.

[0064] The porosity of the resin structure is preferably 10% or more, more preferably 15% or more, still more preferably 30% or more, particularly preferably 50% or more. In addition, the porosity of the resin structure is preferably 90% or less. When the porosity is 30% or more, the continuous capillary action from the opening of the surface to the internal co-continuous structure is further manifested, and the antipathogen activity is further improved. When the porosity is 90% or less, the strength of the resin structure is improved. The method for measuring the porosity of the resin structure is not specifically limited. An example of the method is as follows. Specifically, the resin structure is loaded with unsaturated fatty acids (commercially available butter) and osmium staining is performed. Then, the internal cross-sectional structure is cut by FIB, and the porosity of the antipathogen structure is measured using SEM.

[0065] The shape of the cross section of the hole in the resin structure is not specifically limited. Examples of the shape include various shapes, such as a substantially circular shape, a substantially elliptical shape, and a substantially polygonal shape. The pore size of the hole is also not specifically limited. Here, the pore size of the hole refers to the length of the longest straight line drawn in the cross-sectional shape. Specifically, the pore size of the hole can be determined by a photograph of the cross section taken, for example, by a scanning electron microscope (SEM).

[0066] In order to realize antimicrobial activity, the pore size of the pore of resin structure is preferably below 10 microns, more preferably below 5 microns, still more preferably below 1 micron, particularly preferably below 0.5 micron.When the pore size of the pore is below 10 microns, the shell part (for example, cell membrane and cell wall) of microorganism is more easily destroyed in the opening connected to each other by the capillary action derived from the pore, and antimicrobial activity is suitably shown.Here, capillary action is inversely proportional to the pore size of the pore.Therefore, the smaller the pore size, the larger the capillary action, and therefore higher antimicrobial activity can be expected.The pore size of opening can be suitably adjusted by, for example, the polymerization conditions (for example, the irradiation intensity and the irradiation time of the emission active energy ray) that allow the polymerization of polymerizable compounds.

[0067] -Materials that make up the resin structure-

[0068] The resin as a material constituting the resin structure will be described.

[0069] An example of an available resin is not specifically limited. Examples thereof include: resins (e.g., acrylate resins, methacrylate resins, urethane acrylate resins, vinyl ester resins, unsaturated polyester resins, epoxy resins, oxetane resins, and vinyl ether resins) that can be formed by irradiating active energy rays such as ionizing irradiation, ultraviolet rays, and infrared rays (heat); and resins that utilize ene-thiol reactions. Among them, acrylate resins, methacrylate resins, urethane acrylate resins, and vinyl ester resins that can be formed by highly reactive free radical polymerization are preferred, and acrylate resins and (meth) acrylic resins such as methacrylate resins are more preferred.

[0070] Another example of available resin is not specifically limited. Examples thereof include biodegradable resins and thermoplastic resins. Preferred examples of biodegradable resins include aliphatic polyester resins. Examples of aliphatic polyester resins include polylactic acid / glycolic acid copolymers (PLGA), polylactic acid (PLA), poly-ε-caprolactone, succinate polymers and polyhydroxyalkanoates. Examples of thermoplastic resins include polyvinylidene fluoride (PVDF), polyethylene, polypropylene, polystyrene, acrylic resins, polyvinyl chloride, polyvinyl acetate, ABS resins, polyamides, polyesters, polycarbonates, Teflon (registered trademark), polyimides and polysulfones.

[0071] There is no specific limitation on the method of producing a resin structure including a plurality of openings in the surface using the aforementioned materials. Examples of the method include methods such as: using heat or light to cause phase separation, using laser tracking etching, using gas foaming, film stretching, and the application of good solvents and poor solvents for resins. Among them, the method using heat or light to cause phase separation and the method using good solvents and poor solvents for resins are preferred. Therefore, these methods will be described below.

[0072] -Liquid composition that forms a resin structure by curing-

[0073] The liquid composition (also referred to as curing type composition) of the resin that is cured to form a resin structure by polymerization preferably includes a polymerizable compound, a solvent, a polymerization initiator and an organic polymer compound. In the resin structure formed by the liquid composition, it is preferably formed to include a surface structure including a plurality of openings when solidified. More preferably, in the resin structure formed by the liquid composition, a surface structure including the plurality of openings is formed when solidified, and a co-continuous structure obtained by connecting the openings to each other is formed simultaneously. This method is more advantageous because the antipathogenic structure can be produced in a short process time, compared with the structure including the column (nanopillar) with a fine protrusion structure, which requires a long process time for production (for example, transfer method, such as nanoimprinting and patterning). In addition, this method is more advantageous for the following reasons. That is, since the liquid composition can be discharged on the object (substrate) to be realized for antipathogenic activity by, for example, inkjet method and spray method, compared with the transfer method such as nanoimprinting, the antipathogenic structure can be generated on the object (substrate) in a non-contact manner. More specifically, the generation of antipathogenic structures in a non-contact manner is advantageous in the following cases: cases where the transfer method cannot be applied due to the fragile structure of the object (substrate); cases where the object (substrate) has a complex three-dimensional shape such as a curved structure; and cases where it is necessary to handle the object (substrate) in a non-contact manner from, for example, a public health perspective. Whether the liquid composition forms a resin structure having a predetermined shape and characteristics is determined based on the structure formed in the following manner. First, the liquid composition (20 μl / cm 2 ) was applied to the glass plate to form a solid image. Immediately thereafter, ultraviolet light (UV) (light source: UV-LED (available from Phoseon, product name: FJ800), wavelength: 365 nm, irradiation intensity: 30 mW / cm 2 , irradiation time: 20 s) irradiates the applied area of ​​the liquid composition to cure the applied area of ​​the liquid composition. Thus, a structure is obtained.

[0074] --Polymerizable compounds--

[0075] The polymerizable compound forms a resin by polymerization, and forms a porous resin with openings and holes when polymerized in a liquid composition. The polymerizable compound preferably forms a resin by irradiation with active energy rays. The resin formed by the polymerizable compound preferably has a cross-linked structure in its molecule--by utilizing a difunctional or higher polymerizable compound. This makes it possible to increase the glass transition temperature or melting point of the resin, which leads to increased strength. In addition, the cross-linked structure also improves water resistance.

[0076] There is no specific limitation on the active energy ray, as long as the active energy ray can supply the necessary energy to allow the polymerization reaction of the polymerizable compound in the liquid composition to proceed. Examples of active energy rays include ultraviolet rays, electron beams, α rays, β rays, γ rays and X-rays. Among them, ultraviolet rays are preferred. When a light source with particularly high energy is utilized, the polymerization reaction can be carried out without using a polymerization initiator.

[0077] The polymerizable compound preferably includes at least one free radical polymerizable functional group. Examples thereof include monofunctional free radical polymerizable compounds, difunctional free radical polymerizable compounds, trifunctional or higher free radical polymerizable compounds, functional monomers, and free radical polymerizable oligomers. Among them, difunctional or higher free radical polymerizable compounds are preferred.

[0078] Preferred examples of the polymerizable compound include polymerizable compounds having a (meth)acryloyl group or a vinyl group.

[0079] Examples of the monofunctional free radical polymerizable compound include 2-(2-ethoxyethoxy)ethyl acrylate, methoxypolyethylene glycol monoacrylate, methoxypolyethylene glycol monomethacrylate, phenoxypolyethylene glycol acrylate, 2-acryloyloxyethyl succinate, 2-ethylhexyl acrylate, 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, tetrahydrofurfuryl acrylate, 2-ethylhexyl carbitol acrylate, 3-methoxybutyl acrylate, benzyl acrylate, cyclohexyl acrylate, isoamyl acrylate, isobutyl acrylate, methoxytriethylene glycol acrylate, phenoxytetraethylene glycol acrylate, cetyl acrylate, isostearyl acrylate, stearyl acrylate, and styrene monomers. These may be used alone or in combination.

[0080] Examples of the bifunctional free radical polymerizable compound include 1,3-butanediol diacrylate, 1,4-butanediol diacrylate, 1,4-butanediol dimethacrylate, 1,6-hexanediol diacrylate, 1,6-hexanediol dimethacrylate, diethylene glycol diacrylate, polyethylene glycol diacrylate, neopentyl glycol diacrylate, EO-modified bisphenol A diacrylate, EO-modified bisphenol F diacrylate, neopentyl glycol diacrylate, and tricyclodecane dimethanol diacrylate. These may be used alone or in combination.

[0081] Examples of the trifunctional or higher radical polymerizable compound include trimethylolpropane triacrylate (TMPTA), trimethylolpropane trimethacrylate, EO-modified trimethylolpropane triacrylate, PO-modified trimethylolpropane triacrylate, caprolactone-modified trimethylolpropane triacrylate, HPA-modified trimethylolpropane trimethacrylate, pentaerythritol triacrylate, pentaerythritol tetraacrylate (PETA), glycerol triacrylate, ECH-modified glycerol triacrylate, EO-modified glycerol triacrylate, PO-modified trimethylolpropane triacrylate, caprolactone-modified trimethylolpropane triacrylate, HPA-modified trimethylolpropane trimethacrylate, pentaerythritol triacrylate, pentaerythritol tetraacrylate (PETA), glycerol triacrylate, ECH-modified glycerol triacrylate, EO-modified glycerol triacrylate, PO-modified -modified glycerol triacrylate, tri(acryloyloxyethyl) isocyanurate, dipentaerythritol hexaacrylate (DPHA), caprolactone-modified dipentaerythritol hexaacrylate, dipentaerythritol hydroxypentaacrylate, alkyl-modified dipentaerythritol pentaacrylate, alkyl-modified dipentaerythritol tetraacrylate, alkyl-modified dipentaerythritol triacrylate, dimethylolpropane tetraacrylate (DTMPTA), pentaerythritol ethoxy tetraacrylate, EO-modified phosphoric acid triacrylate, and 2,2,5,5-tetrahydroxymethylcyclopentanone tetraacrylate. These may be used alone or in combination.

[0082] The amount of the polymerizable compound in the liquid composition is preferably 5.0% by mass or more but 70.0% by mass or less, more preferably 10.0% by mass or more but 50.0% by mass or less, and still more preferably 20.0% by mass or more but 50.0% by mass or less, relative to the total amount of the liquid composition. It is preferred that the amount of the polymerizable compound satisfies 70.0% by mass or less because the size of the opening or pore of the resin structure to be obtained can fall within an appropriate range. It is preferred that the amount of the polymerizable compound satisfies 5.0% by mass or more because the strength of the resin structure is improved.

[0083] --Solvents--

[0084] The solvent (hereinafter also referred to as porogen) is a liquid that is compatible with the polymerizable compound.

[0085] The solvent (hereinafter also referred to as a porogen) is a liquid compatible with the polymerizable compound. The solvent is a liquid that becomes incompatible (phase separation occurs) with the polymer (resin) in the process of allowing the polymerizable compound to polymerize in the liquid composition. That is, the meaning of "solvent" in the present disclosure is different from the meaning of the common term "solvent". The inclusion of a solvent in the liquid composition makes it possible to form a porous resin having the aforementioned openings and pores when the polymerizable compound is polymerized in the liquid composition. In addition, the solvent can preferably dissolve a compound that generates free radicals or acids by applying light or heat (i.e., a polymerization initiator to be described below). The solvent can be used alone, or two or more solvents can be used in combination. Note that the solvent does not have the ability to polymerize.

[0086] The boiling point of the porogen used alone or the boiling points of two porogens used in combination is preferably 50 degrees Celsius or more but 250 degrees Celsius or less, more preferably 70 degrees Celsius or more but 200 degrees Celsius or less at normal pressure. When the boiling point is 50 degrees Celsius or more, the porogen can be prevented from evaporating at nearly room temperature, the liquid composition is easy to handle, and the porogen content in the liquid composition can be easily controlled. When the boiling point is 250 degrees Celsius or less, the time required in the step of drying the porogen after polymerization is shortened to improve the productivity of the resin structure.

[0087] Examples of the porogen include glycols such as diethylene glycol monomethyl ether, ethylene glycol monobutyl ether, ethylene glycol monoisopropyl ether, triethylene glycol monobutyl ether, and dipropylene glycol monomethyl ether; esters such as γ-butyrolactone and propylene carbonate; and amides such as NN dimethylacetamide.

[0088] Examples of the porogen include liquids having a relatively large molecular weight (eg, methyl myristate, methyl decanoate, methyl myristate, and tetradecane). In addition, liquids such as acetone, 2-ethylhexanol, and 1-bromonaphthalene can also be used.

[0089] Note that the aforementioned exemplary liquids do not always correspond to porogens. As described above, a porogen is a liquid that is compatible with a polymerizable compound and becomes incompatible (phase-separated) with a polymer (resin) in a process of allowing the polymerizable compound to polymerize in a liquid composition. In other words, whether a liquid corresponds to a porogen can be determined by the relationship between the polymerizable compound and the polymer (resin formed by allowing the polymerizable compound to polymerize).

[0090] Note that the liquid composition may include at least one porogen that satisfies the above-mentioned specific relationship between the above-mentioned polymerizable compound and the polymer as described above. Therefore, a liquid that does not satisfy the above-mentioned specific relationship between the polymerizable compound and the polymer (i.e., a liquid that is not a porogen) may be additionally included. The amount of the liquid that does not satisfy the above-mentioned specific relationship between the polymerizable compound and the polymer (i.e., a liquid that is not a porogen) relative to the total amount of the liquid composition is preferably 10.0% by mass or less, more preferably 5.0% by mass or less, and even more preferably 1.0% by mass or less. It is particularly preferred that a liquid that does not satisfy the above-mentioned specific relationship between the polymerizable compound and the polymer (i.e., a liquid that is not a porogen) is not included.

[0091] The amount of the porogen in the liquid composition is preferably 30.0% by mass or more but 95.0% by mass or less, more preferably 50.0% by mass or more but 90.0% by mass or less, and still more preferably 50.0% by mass or more but 80.0% by mass or less, relative to the total amount of the liquid composition. It is preferred that the amount of the porogen satisfies 30.0% by mass or more because the size of the openings or pores of the obtained resin structure can fall within an appropriate range. It is preferred that the amount of the porogen satisfies 95.0% by mass or less because the strength of the resin structure can be improved.

[0092] The mass ratio between the amount of the polymerizable compound and the amount of the porogen in the liquid composition (polymerizable compound:porogen) is preferably 1.0:0.4 to 1.0:19.0, more preferably 1.0:1.0 to 1.0:9.0, still more preferably 1.0:1.0 to 1.0:4.0.

[0093] --Polymerization Initiator--

[0094] A polymerization initiator is a material that can generate active substances such as free radicals or cations to initiate polymerization of polymerizable compounds by applying energy such as light or heat. As a polymerization initiator, free radical polymerization initiators, cationic polymerization initiators and base generators known in the art can be used alone or in combination. Among them, a light free radical polymerization initiator is preferably used.

[0095] As the photoradical polymerization initiator, a photoradical generator can be used. Examples thereof include photoradical polymerization initiators such as Michler's ketone and benzophenone, which are known by product names: IRGACURE and DAROCUR. As more specific compounds, for example, benzophenone, acetophenone derivatives (e.g., α-hydroxyacetophenone and α-aminoacetophenone), 4-aroyl-1,3-dioxolane, benzyl ketal, 2,2-diethoxyacetophenone, p-dimethylaminoacetophenone, p-dimethylaminopropiophenone, benzophenone, 2-chlorobenzophenone, pp'-dichlorobenzophenone, pp'-bisdiethylaminobenzophenone, Michler's ketone, benzyl, benzoin, benzyl dimethyl ketal, tetramethylthiuram monosulfide, thioxanthone, 2-chlorothioxanthone, 2-methylthioxanthone, azobisisobutyronitrile, benzoin peroxide, di-tert-butyl peroxide, 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenyl-1-one, 1-(4-isopropylphenyl)- 2-Hydroxy-2-methylpropan-1-one, methyl benzoylformate, benzoin isopropyl ether, benzoin methyl ether, benzoin ethyl ether, benzoin ether, benzoin isobutyl ether, benzoin n-butyl ether, benzoin n-propyl, 1-hydroxycyclohexyl phenyl ketone, 2-benzyl 2-dimethylamino 1-(4-morpholinophenyl)-butanone-1,1-hydroxycyclohexyl-phenyl-ketone, 2,2-dimethoxy-1, 2-Diphenylethan-1-one, bis(η5-2,4-cyclopentadien-1-yl)-bis(2,6-difluoro-3-(1H-pyrrol-1-yl)-phenyl)titanium, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, 2-methyl-1[4-(methylthio)phenyl]-2-morpholinopropan-1-one, 2-hydroxy-2-methyl-1-phenyl-propan-1-one (DAROCUR 1173), bis(2,6-dimethoxybenzoyl)-2,4,4-trimethyl-pentylphosphine oxide, 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propan-1-one monoacylphosphine oxide, bisacylphosphine oxide or cyclopentadienyl titanium (titanocene), fluorescein, anthraquinone, thioxanthone or xanthone, lorphenamine dimer, trihalomethyl compound or dihalomethyl compound, active ester compound and organic boron compound.

[0096] A photo-crosslinkable free radical generator, such as a bisazide compound, may also be included. Alternatively, when the polymerization is carried out by applying heat, a thermal polymerization initiator may be utilized, such as azobisisobutyronitrile (AIBN), which is a general free radical generator.

[0097] When the total mass of the polymerizable compound is 100.0 mass%, the amount of the polymerization initiator is preferably 0.05 mass% or more but 10.0 mass% or less, more preferably 0.5 mass% or more but 5.0 mass% or less, in order to obtain a sufficient curing rate.

[0098] --Organic polymer compounds--

[0099] The organic polymer compound is an organic compound that is a polymer and will be added to the liquid composition. Examples of organic polymer compounds include resins (hereinafter also referred to as "addition resins") and organic polymer compounds derived from natural products. Note that the addition resin is distinguished from a resin formed by polymerization of a polymerizable compound (which may be referred to as a "polymerizable resin"). The organic polymer compound is preferably added to the liquid composition, but may not be added to the liquid composition. The organic polymer compound preferably does not include a polymerizable functional group.

[0100] Adding the organic polymer compound to the liquid composition can improve the hardness of the resin structure formed by curing the liquid composition. The reason why the organic polymer compound can improve the hardness of the resin structure will be described below.

[0101] The following can be assumed. In general, in the process of curing a liquid composition containing no organic polymer compound, the resin formed by the polymerization of the polymerizable compound becomes insoluble in the liquid composition as the polymerization proceeds to form a particle core. The core is aggregated and combined by intermolecular forces. Therefore, a resin structure can be formed, which includes a skeleton having a shape obtained by connecting a plurality of particles to each other. At the same time, in the process of curing a liquid composition containing an organic polymer compound, there is a bonding strength between the organic polymer compound and the polymerizable compound that can achieve reversible bonding and dissociation, so as to allow the polymerization of the polymerizable compound to proceed along the long chain of the organic polymer compound (in other words, even between the polymer of the polymerizable compound and the organic polymer compound, there is a bonding strength that can achieve reversible bonding and dissociation). Therefore, as the polymerization proceeds, the resin formed by the polymerization of the polymerizable compound becomes insoluble in the liquid composition. Then, the particle core is prevented from forming to form a resin structure including a skeleton having a substantially planar shape. As described above, the hardness of the resin structure including a skeleton having a substantially planar shape is higher than the hardness of the resin structure including a skeleton having a shape obtained by connecting a plurality of particles to each other. Therefore, it can be said that the organic polymer compound can improve the hardness of the resin structure.

[0102] Note that the bonding strength capable of achieving reversible bonding and dissociation is preferably a hydrogen bond (2 kJ / mol to 40 kJ / mol) That is, the organic polymer compound preferably includes a functional group that can bond the polymerizable compound and the polymer of the polymerizable compound by hydrogen bonding.

[0103] The organic polymer compound is preferably dissolved in a solvent. This is because when the organic polymer compound can be dissolved in a solvent, polymerization of the polymerizable compound proceeds appropriately along the long chain of the organic polymer compound. Here, the phrase "the organic polymer compound is dissolved in a solvent" means that when 20 g of the organic polymer compound is added to 100 g of a solvent (25 degrees Celsius) and then mixed and stirred, 90% by mass or more of the organic polymer compound is dissolved.

[0104] There is no specific limitation on the addition of resin, as long as there is a bonding strength between the polymerizable compound and the polymer of the polymerizable compound that can achieve reversible bonding and dissociation. Examples of the addition of resin include resins containing hydroxyl groups in their molecules, because they preferably include functional groups that can form hydrogen bonds. Specific examples thereof include polyacrylic acid polyols, polyester polyols, polybutadiene polyols, polyvinyl butyral, polyvinyl acetal, ethyl cellulose and nitrocellulose. Among them, polyvinyl butyral, for example, is preferred. These can be used alone or in combination. In addition, appropriately synthesized products or commercially available products can be used.

[0105] The organic polymer compound derived from natural products is not specifically limited, as long as there is a binding strength between the polymerizable compound and the polymerizable compound that can achieve reversible binding and dissociation. The organic polymer compound derived from natural products preferably includes a functional group that can form a hydrogen bond. Specifically, its preferred example includes a lignin derivative derived from natural lignin.

[0106] Examples of natural lignin include lignin contained in natural wood and lignin contained in herbaceous plants such as rice straw and wheat straw.

[0107] The lignin derivative can be obtained by subjecting natural lignin to, for example, the following predetermined treatment.

[0108] As an example of a predetermined treatment, a treatment method for removing lignin from natural wood to obtain pulp is a representative treatment method. An example thereof is pulp treatment using the Kraft process. This is a method using an aqueous sodium hydroxide solution and an aqueous sodium sulfide solution as a cooking liquid. When a molecular weight reduction treatment is performed to separate lignin from natural wood, a lignin derivative can be obtained. The lignin derivative obtained in this treatment is called "kraft lignin".

[0109] An example of another treatment is as follows. Specifically, a material such as wood is saccharified using sulfuric acid to obtain residual lignin. Then, the residual lignin is hydrothermally treated in an alkaline aqueous solution to be water-soluble to obtain a lignin derivative. The lignin derivative obtained by this treatment is referred to as "hydrothermally treated sulfated lignin".

[0110] As an example of another treatment, herbaceous plant materials such as rice straw or wheat straw are treated in an alkaline aqueous solution for water dissolution to obtain a lignin derivative. The lignin derivative obtained in this treatment is called "alkaline lignin".

[0111] In addition, enzymatically saccharified lignin can also be utilized.

[0112] The lignin derivatives in the present disclosure are not limited to those obtained after the aforementioned predetermined treatment. Lignin that has been subjected to additional treatment (eg, hydroxymethylation treatment and phosphorylation treatment) after the aforementioned predetermined treatment may be used.

[0113] When the total mass of the liquid composition is 100.0 mass%, the amount of the organic polymer compound is preferably 1.0 mass% or more but 15.0 mass% or less, more preferably 1.3 mass% or more but 10.0 mass% or less, in order to obtain sufficient hardness of the resin structure.

[0114] --Physical Properties of Liquid Compositions--

[0115] In terms of operability when applying the liquid composition, the viscosity of the liquid composition at 25 degrees Celsius is preferably 1.0 mPa·s or more but 200.0 mPa·s or less, more preferably 1.0 mPa·s or more but 150.0 mPa·s or less, still more preferably 1.0 mPa·s or more but 100.0 mPa·s or less, still more preferably 1.0 mPa·s or more but 30.0 mPa·s or less, particularly preferably 1.0 mPa·s or more but 25.0 mPa·s or less. The viscosity of the liquid composition satisfies 1.0 mPa·s or more but 200.0 mPa·s or less so that good discharge properties can be obtained when the liquid composition is applied to a discharge method (preferably, an inkjet method). Here, the viscosity can be measured using, for example, a viscometer (device name: RE-550L, available from Toki Sangyo Co., Ltd).

[0116] -Liquid composition that forms a resin structure by drying-

[0117] The liquid composition (also referred to as a precipitation type composition) - which is dried to precipitate or aggregate the dissolved or dispersed resin (hereinafter "precipitation or aggregation" will be simply referred to as "precipitation") to form a resin structure - preferably includes, for example, a resin (hereinafter also referred to as "precipitation resin"), a good solvent for the precipitation resin, and a poor solvent for the precipitation resin. In the resin structure formed by the liquid composition, a surface structure including a plurality of openings is preferably formed when drying. More preferably, in the resin structure formed by the liquid composition, a surface structure including the plurality of openings and a co-continuous structure obtained by connecting the openings to each other are formed simultaneously when drying. The present method is more advantageous because the antipathogenic structure can be produced in a short process time, compared to the production of a structure including a column (nanopillar) with a fine protrusion structure that requires a long process time (for example, transfer methods such as nanoimprinting and patterning). In addition, the present method is more advantageous for the following reasons. That is, compared to transfer methods such as nanoimprinting, since the liquid composition can be discharged on an object (substrate) that will achieve antipathogenic activity by, for example, an inkjet method and a spray method, the antipathogenic structure can be formed on the object (substrate) in a non-contact manner. More specifically, producing anti-pathogen structures in a non-contact manner is advantageous in the following situations: when the transfer method cannot be applied due to the fragile structure of the object (substrate); when the object (substrate) has a complex three-dimensional shape such as a curved structure; and when it is necessary to handle the object (substrate) in a non-contact manner from, for example, a public health perspective.

[0118] First, the reason why a liquid composition containing, for example, a precipitation resin, a good solvent, and a poor solvent is dried to form a resin structure will be described.

[0119] When the precipitation resin is dissolved or dispersed in a liquid containing a good solvent and a poor solvent to form a liquid composition, the precipitation resin is mainly dissolved or dispersed in the good solvent, and the precipitation resin is substantially not present in the poor solvent. That is, a state in which the precipitation resin is unevenly distributed can be achieved in the liquid composition. When the liquid composition in this state is dried to precipitate the precipitation resin, the precipitation resin remains in the portion where the good solvent exists, and voids are formed in the portion where the poor solvent exists. Therefore, the resin structure of the produced precipitation resin becomes a porous structure including a plurality of openings in its surface.

[0120] --Resin (precipitation resin)--

[0121] The liquid composition is dried to precipitate the precipitation resin and form a porous resin including the openings and the pores. As described above, the precipitation resin is dissolved or dispersed in a good solvent and is substantially not dissolved or dispersed in a poor solvent.

[0122] The resin that can be used as the precipitation resin is not particularly limited as long as the resin is soluble or dispersed in a good solvent and is substantially insoluble or dispersed in a poor solvent. Examples of the resin include the above-mentioned biodegradable resins and thermoplastic resins.

[0123] When the total mass of the liquid composition is 100.0 mass%, the amount of the precipitated resin is preferably 0.1 mass% or more but 20.0 mass% or less, more preferably 5.0 mass% or more but 15.0 mass% or less.

[0124] --Good solvent--

[0125] A good solvent is a liquid that can dissolve or disperse the precipitation resin. In the present disclosure, a good solvent preferably means a liquid that can dissolve or disperse the precipitation resin when the precipitation resin (0.1 g) is added to a liquid (100 g) at 25 degrees Celsius.

[0126] The good solvent is not particularly limited as long as it is a liquid that can dissolve or disperse the precipitated resin. Examples of the good solvent include alcohols, ketones, ethers, acetonitrile, and tetrahydrofuran.

[0127] Examples of the alcohol include alcohols having 1 or more but 4 or less carbon atoms. Examples of the alcohols having 1 or more but 4 or less carbon atoms include methanol, ethanol, propanol, and butanol.

[0128] Examples of ketones include ketones having 3 or more but 6 or less carbon atoms. Examples of ketones having 3 or more but 6 or less carbon atoms include acetone, methyl ethyl ketone, and cyclohexanone.

[0129] Examples of the ether include ethers having 2 or more but 6 or less carbon atoms. Examples of the ethers having 2 or more but 6 or less carbon atoms include dimethyl ether, methyl ethyl ether, and diethyl ether.

[0130] These may be used alone or in combination. When two or more good solvents are used, alcohol and ketone are preferably used in combination, and ethanol and acetone are more preferably used in combination.

[0131] The amount of the good solvent is not particularly limited as long as it is an amount capable of dissolving or dispersing the precipitated resin. For example, when the total mass of the liquid composition is 100.0 mass%, the amount of the good solvent is preferably 30.0 mass% or more but 90.0 mass% or less, more preferably 40.0 mass% or more but 80.0 mass% or less.

[0132] --Poor solvents--

[0133] A poor solvent is a liquid that does not substantially dissolve or disperse the precipitation resin. In the present disclosure, the poor solvent is preferably a liquid that, when the precipitation resin is added to a liquid (100 g) at 25 degrees Celsius, can dissolve or disperse the mass of the precipitation resin, relative to the mass of the precipitation resin that can be dissolved or dispersed by a good solvent (100 g) at 25 degrees Celsius when the precipitation resin is added to a good solvent, is less than half.

[0134] A poor solvent is a liquid that is compatible with a certain amount of a good solvent and does not separate from the good solvent.

[0135] The poor solvent is not specifically limited as long as it is a liquid that does not substantially dissolve or disperse the precipitated resin and is compatible with a certain amount of the good solvent without separating from the good solvent. Examples of the poor solvent include methanol, ethanol and water. These can be used alone or in combination.

[0136] The amount of the poor solvent is not particularly limited as long as it is an amount in which the poor solvent can be dispersed in the good solvent. For example, when the total mass of the liquid composition is 100.0 mass%, the amount of the poor solvent is preferably 10.0 mass% or more but 60.0 mass% or less, more preferably 20.0 mass% or more but 50.0 mass% or less.

[0137] --Physical Properties of Liquid Compositions--

[0138] In terms of operability when applying the liquid composition, the viscosity of the liquid composition at 25 degrees Celsius is preferably 1.0 mPa·s or more but 200.0 mPa·s or less, more preferably 1.0 mPa·s or more but 150.0 mPa·s or less, still more preferably 1.0 mPa·s or more but 100.0 mPa·s or less, still more preferably 1.0 mPa·s or more but 30.0 mPa·s or less, particularly preferably 1.0 mPa·s or more but 25.0 mPa·s or less. The viscosity of the liquid composition satisfies 1.0 mPa·s or more but 200.0 mPa·s or less so that good discharge properties can be obtained when the liquid composition is applied to a discharge method (preferably, an inkjet method). Here, the viscosity can be measured using, for example, a viscometer (device name: RE-550L, available from Toki Sangyo Co., Ltd).

[0139] <Other substances>

[0140] In addition to the resin structure, the antipathogen structure may include other substances if necessary. Examples of other substances include antimicrobial agents and antiviral agents. Specific examples of antimicrobial agents and antiviral agents include: organic substances (e.g., medicaments) in which the substance itself has antimicrobial activity or antiviral activity; substances that exhibit antimicrobial activity or antiviral activity over time (e.g., hypochlorous acid); inorganic substances (e.g., silver and copper) having antimicrobial activity or antiviral activity; and inorganic substances (e.g., titanium oxide and tungsten oxide) having the function of decomposing organic substances by photocatalytic reactions. Note that the starting material (e.g., polymerizable compound) of the resin structure retained after production should not be included in the antimicrobial or antiviral agent in the present disclosure.

[0141] Preferably, the antipathogen structure of the present embodiment does not substantially include an antimicrobial or antiviral agent. More preferably, the antipathogen structure of the present embodiment does not contain an antimicrobial and an antiviral agent. The reasons are as follows. Specifically, when the antipathogen structure does not contain an antimicrobial and an antiviral agent, the effects on the human body caused by the antimicrobial or antiviral agent (e.g., allergic reactions) can be prevented, and the emergence of microorganisms or viruses tolerant to the antimicrobial or antiviral agent can be prevented. The phrase "substantially does not include an antimicrobial agent" means any of the following situations: the situation where the amount of the antimicrobial agent is less than 1.0 mass % relative to the mass of the antipathogen structure; the situation where the amount of the antimicrobial agent is less than 0.5 mass % relative to the mass of the antipathogen structure; the situation where the amount of the antimicrobial agent is less than 0.1 mass % relative to the mass of the antipathogen structure; the situation where the antimicrobial activity achieved by the antimicrobial agent cannot be observed; and the situation where the amount of the antimicrobial agent is undetectable. The phrase "substantially does not include an antiviral agent" means any of the following cases: a case where the amount of the antiviral agent relative to the mass of the antipathogen structure is 1.0 mass % or less; a case where the amount of the antiviral agent relative to the mass of the antipathogen structure is 0.5 mass % or less; a case where the amount of the antiviral agent relative to the mass of the antipathogen structure is 0.1 mass %; a case where the antiviral activity achieved by the antiviral agent cannot be observed; and a case where the amount of the antiviral agent is undetectable. Note that the observation of the antimicrobial activity achieved by the antimicrobial agent, the detection of the amount of the antimicrobial agent, the observation of the antiviral activity achieved by the antiviral agent, and the detection of the amount of the antiviral agent are all performed by known means commonly used in the art.

[0142] <<Apparatus for producing an antipathogen structure and method for producing an antipathogen structure>>

[0143] Figure 1 is a schematic diagram showing an example of an apparatus for producing an antipathogen structure to implement a method for producing an antipathogen structure of an embodiment of the present disclosure. Figure 1The production equipment of shows an example of an equipment in the case where a liquid composition (curing type composition) is used that forms a resin constituting a resin structure by polymerization and curing. Even when a liquid composition (precipitation type composition) is used that forms a resin structure by drying the liquid composition to precipitate the dissolved or dispersed resin, Figure 1 Production equipment can also be added, deleted and changed Figure 1 Therefore, the following will describe Figure 1 production equipment.

[0144] <Equipment for producing pathogen-resistant structures>

[0145] The apparatus 100 for producing an antipathogen structure is an apparatus for producing an antipathogen structure using the above-mentioned liquid composition. The apparatus 100 for producing an antipathogen structure comprises: an application step section 10; a polymerization step section 20; and a heating step section 30. The application step section 10 is configured to apply the liquid composition to a substrate 4. The polymerization step section 20 is configured to allow a polymerizable compound to polymerize, thereby obtaining a precursor 6 of an antipathogen structure, which is contained in a liquid composition layer obtained by applying the liquid composition to the substrate 4. The heating step section 30 is configured to heat the precursor 6 of the antipathogen structure to obtain an antipathogen structure. The apparatus 100 for producing an antipathogen structure comprises a conveying section 5 configured to convey a substrate 4. The conveying section 5 is configured to convey the substrate 4 at a previously set rate in the order of the application step section 10, the polymerization step section 20, and the heating step section 30.

[0146] When a precipitation type composition is used as the liquid composition, the polymerization step part 20 may be omitted.

[0147] - Application Steps Section -

[0148] The application step section 10 includes an application device 1a, a storage container 1b, and a supply pipe 1c. The application device 1a is an example of an application unit that implements the step of applying the liquid composition to the substrate 4. The storage container 1b is configured to store the liquid composition. The supply pipe 1c is configured to supply the liquid composition stored in the storage container 1b to the application device 1a.

[0149] The storage container 1b is configured to store the liquid composition 7. In the application step section 10, the liquid composition 7 is discharged from the application device 1a in the direction of the substrate 4 to apply the liquid composition 7. Then, a liquid composition layer is formed in the form of a thin film.

[0150] Note that the storage container 1b may be integrated with the apparatus for producing the antipathogen structure 100, but may be detachable from the apparatus for producing the antipathogen structure 100. The storage container 1b may be a container for being added to a storage container integrated with the apparatus for producing the antipathogen structure 100 or a storage container detachable from the apparatus for producing the antipathogen structure 100.

[0151] The application device 1a is not particularly limited as long as it can apply the liquid composition 7. For example, any application device can be applied as follows: for example, spin coating, casting, micro-gravure coating, gravure coating, rod coating, roller coating, wire rod coating, dip coating, slit coating, capillary coating, spray coating, nozzle coating, and various printing methods such as gravure printing, screen printing, flexographic printing, offset printing, reverse printing, and inkjet printing. Among them, inkjet printing is preferred because the liquid composition 7 can be applied to the target position of the substrate. In addition, the inkjet printing method is preferred because a uniform film thickness of the antipathogenic structure can be achieved.

[0152] The storage container 1b or the supply pipe 1c can be optionally selected as long as the liquid composition 7 can be stably stored and supplied. The material constituting the storage container 1b or the supply pipe 1c preferably has a light-proof property in the relatively short wavelength region of ultraviolet light and visible light. This makes it possible to prevent the liquid composition 7 from starting to polymerize due to natural light.

[0153] -Polymerization Step Section-

[0154] like Figure 1 As shown, the polymerization step part 20 includes a light emitting device 2a and a polymerization inert gas circulation device 2b. The light emitting device 2a is an example of a curing unit, which is configured to irradiate the liquid composition with active energy rays such as heat and light to cure the liquid composition. The polymerization inert gas circulation device 2b is configured to circulate the polymerization inert gas. The light emitting device 2a is configured to emit light to the liquid composition layer formed by the application step part 10 in the presence of the polymerization inert gas to allow it to be photopolymerized. Thus, the precursor 6 of the antipathogenic structure is obtained.

[0155] The light emitting device 2a is appropriately selected according to the absorption wavelength of the photopolymerization initiator contained in the liquid composition layer. The light emitting device 2a is not specifically limited as long as the polymerization of the compound in the liquid composition layer can be started and carried out. Examples thereof include high pressure mercury lamps, metal halide lamps, hot cathode tubes, cold cathode tubes, and ultraviolet light sources such as LEDs. Note that since light with a shorter wavelength tends to reach a deep portion in general, it is preferred to select a light source according to the thickness of the antipathogen structure to be formed.

[0156] The irradiation intensity of the light source of the light emitting device 2a will be described. When the irradiation intensity is too strong, polymerization proceeds rapidly before phase separation occurs sufficiently. Therefore, it is difficult to obtain an antipathogen structure with a sufficient number of openings and holes. At the same time, when the irradiation intensity is too weak, phase separation proceeds above the microscale. Therefore, the size of the openings and holes tends to become uneven and increase. In addition, the irradiation time is prolonged and productivity tends to decrease. Therefore, the irradiation intensity is preferably 10mW / cm 2 Above but 1W / cm 2 Below, more preferably 30mW / cm 2 Above 300mW / cm 2 the following.

[0157] The polymerization inert gas circulation device 2b reduces the concentration of polymerization-active oxygen contained in the air to promote the polymerization reaction of the polymerizable compound near the surface of the liquid composition layer without interference. Therefore, the polymerization inert gas used is not specifically limited as long as it satisfies the above-mentioned function. Examples of the polymerization inert gas include nitrogen, carbon dioxide and argon.

[0158] Considering that its flow rate can effectively achieve the suppression reduction effect, the concentration of O2 is preferably less than 20% (an environment in which the oxygen concentration is lower than that in the air), more preferably 0% or more but 15% or less, and still more preferably 0% or more but 5% or less. The polymerization inert gas circulation device 2b is preferably provided with a temperature adjustment unit configured to adjust the temperature to achieve stable polymerization promoting conditions.

[0159] -Heating Step Section-

[0160] like Figure 1 As shown, the heating step section 30 includes a heating device 3a, which is an example of a heating unit that implements the heating step. The heating step section 30 includes a step (solvent removal step) of heating and drying the solvent remaining on the precursor 6 of the antipathogenic structure formed by the polymerization step section 20 with the heating device 3a to remove the solvent. This allows the antipathogenic structure to be formed. In the heating step section 30, the solvent removal step may be performed under reduced pressure.

[0161] The heating step section 30 also includes a polymerization promoting step and an initiator removing step. The polymerization promoting step is a step of heating the precursor 6 of the antipathogen structure using the heating device 3a to further promote the polymerization reaction performed in the polymerization step section 20. The initiator removing step is a step of heating and drying the photopolymerization initiator remaining in the precursor 6 of the antipathogen structure using the heating device 3a to remove the initiator. Note that the polymerization promoting step and the initiator removing step may not be performed simultaneously with the solvent removing step, and may be performed before or after the solvent removing step.

[0162] The heating step section 30 also includes a step of heating the antipathogen structure under reduced pressure after the solvent removal step (polymerization completion step). The heating device 3a is not particularly limited as long as it satisfies the aforementioned functions. Examples of the heating device 3a include an IR heater and a warm air heater.

[0163] The heating temperature or the time thereof may be appropriately selected according to the boiling point of the solvent contained in the precursor 6 of the antipathogenic structure or the film thickness to be formed.

[0164] When a precipitation type composition is used as a liquid composition, the heating step part 30 uses a heating unit to heat and dry the good solvent and the poor solvent to precipitate the dissolved or dispersed precipitation resin to form an antipathogen structure. At this time, the drying unit, as a unit for drying the good solvent and the poor solvent (drying step), is not limited to the heating unit. For example, an air blowing unit can be used as the drying unit.

[0165] -Base Material-

[0166] As the material of the substrate 4, any material can be used regardless of whether the material is transparent or opaque. Examples of transparent substrates include: glass substrates; resin film substrates such as various plastic films; and composite substrates of these substrates. Examples of opaque substrates include: metal substrates such as stainless steel; and substrates obtained by stacking the foregoing.

[0167] Regarding the shape of the substrate, any shape may be adopted without particular limitation as long as the substrate may be a substrate suitable for the applying step section 10 and the polymerizing step section 20. For example, a substrate having a curved surface shape or an uneven shape may be adopted.

[0168] <<Use of Antipathogen Structure>>

[0169] The use of the antipathogen structure of the present embodiment is not specifically limited, as long as the antipathogen structure can be presented. Examples of uses include uses in which the antipathogen structure is formed on the surface of various substrates (e.g., resins, paper, metals, and fabrics), thereby imparting antipathogen activity to these substrates. More specifically, the use is preferably applied to food uses and medical uses. Examples include food trays, food containers, food packaging films, medical trays, medical containers, medical fabrics, medical gloves, medical covers (caps), medical masks, medical belts, antibacterial films, and antibacterial tissues.

[0170] Here, in the present application, a product including a substrate and an antipathogenic structure formed on the surface of the substrate and having the antipathogenic activity added to the substrate is referred to as an "antipathogenic active adduct".

[0171] Example

[0172] Embodiments of the present disclosure will be described below. However, the present disclosure should not be construed as being limited to these embodiments.

[0173] <Preparation Example of Liquid Composition>

[0174] (Preparation Example 1)

[0175] Materials were mixed in the following ratios to prepare a liquid composition 1.

[0176] Polymerizable compound: tricyclodecane dimethanol diacrylate (obtained from DAICEL-ALLNEX LTD.): 29.0 parts by mass

[0177] Porogen: dipropylene glycol monomethyl ether (obtained from Kanto Chemical Industry Co., Ltd.): 70.0 parts by mass

[0178] Polymerization initiator: IRGACURE 184 (available from BASF): 1.0 part by mass

[0179] When the viscosity of the liquid composition 1 at 25 degrees Celsius was measured using a viscometer (device name: RE-550L, available from Toki Sangyo Co., Ltd), it was found to be 30.0 mPa·s or less.

[0180] (Preparation Example 2)

[0181] The materials were mixed in the following ratio to prepare a liquid composition 2.

[0182] Polymerizable compound: tris(2-hydroxyethyl)isocyanurate triacrylate (obtained from ARKEMA (SARTOMER)): 29.0 parts by mass

[0183] Porogen: dipropylene glycol monomethyl ether (obtained from Kanto Chemical Industry Co., Ltd.): 70.0 parts by mass

[0184] Polymerization initiator: IRGACURE 184 (available from BASF): 1.0 part by mass

[0185] When the viscosity of the liquid composition 2 at 25 degrees Celsius was measured using a viscometer (device name: RE-550L, available from Toki Sangyo Co., Ltd), it was found to be 30.0 mPa·s or less.

[0186] (Comparative Preparation Example 1)

[0187] The materials were mixed in the following ratios to prepare a comparative liquid composition 1.

[0188] Polymerizable compound: tricyclodecane dimethanol diacrylate (obtained from DAICEL-ALLNEX LTD.): 29.0 parts by mass

[0189] Porogen: Cyclohexanone (obtained from Kanto Chemical Industry Co., Ltd.): 70.0 parts by mass.

[0190] Polymerization initiator: IRGACURE 184 (available from BASF): 1.0 part by mass

[0191] When the viscosity of Comparative Liquid Composition 1 at 25 degrees Celsius was measured using a viscometer (device name: RE-550L, available from Toki Sangyo Co., Ltd), it was found to be 30.0 mPa·s or less.

[0192] <Preparation Example of Antipathogen Structure>

[0193] (Example 1)

[0194] Liquid composition 1 was loaded into an inkjet discharge device equipped with a GEN5 head (obtained from Ricoh Printing Systems, Ltd.) and discharged onto a glass plate to form an application area of ​​a solid image. Immediately thereafter, ultraviolet light (UV) (light source: UV-LED (obtained from Phoseon, product name: FJ800), wavelength: 365 nm, irradiation intensity: 30 mW / cm 2 , irradiation time: 20 seconds) irradiated the application area of ​​the liquid composition 1 to cure the application area of ​​the liquid composition 1, and then, the cured product was heated at 120 degrees Celsius for 1 minute using a hot plate to remove the porogen. Thus, the antipathogen structure of Example 1 was obtained. When the liquid composition 1 was discharged by the inkjet method, discharge failures such as nozzle clogging and discharge bending were not found. Therefore, it was found that the liquid composition 1 had high discharge stability.

[0195] Figure 4 Result obtained by observing the surface of the antipathogenic structure of Example 1 with a scanning electron microscope (SEM) are shown in FIG.

[0196] (Example 2)

[0197] The antipathogen structure of Example 2 was obtained in the same manner as in Example 1, except that the liquid composition 1 was changed to the liquid composition 2. When the liquid composition 2 was discharged by the inkjet method, discharge failures such as nozzle clogging and discharge bending were not found. Therefore, it was found that the liquid composition 2 had high discharge stability.

[0198] (Comparative Example 1)

[0199] The structure of Comparative Example 1 was obtained in the same manner as in Example 1, except that Liquid Composition 1 was changed to Comparative Liquid Composition 1. When Comparative Liquid Composition 1 was discharged by the inkjet method, discharge failures such as nozzle clogging and discharge bending were not found. Therefore, it was found that Comparative Liquid Composition 1 had high discharge stability.

[0200] Figure 5 Result obtained by observing the surface of the structure of Comparative Example 1 with a scanning electron microscope (SEM) are shown in FIG.

[0201] The obtained antipathogen structures of Examples 1 and 2 and the structure of Comparative Example 1 were evaluated for the pore size of the surface openings, the pore size of the inner pores, and the porosity.

[0202] <Evaluation of Surface Opening Diameter>

[0203] The surface of the antipathogen structure was observed with a scanning electron microscope (SEM). As a result, openings with a pore size of about 1.0 μm were found on the entire surface of the antipathogen structure in Examples 1 and 2, while no openings were found in Comparative Example 1.

[0204] <Evaluation of Inner Hole Diameter>

[0205] A cross section of the antipathogen structure was prepared and the cross section was observed with a scanning electron microscope (SEM). As a result, pores with a pore size of about 1.0 micrometer were found throughout the cross section of the antipathogen structure in Examples 1 and 2. While no pores were found in Comparative Example 1, it was found that the pores in Examples 1 and 2 were connected to each other and further connected to the openings of the surface.

[0206] <Evaluation of Porosity>

[0207] The antipathogen structure was loaded with unsaturated fatty acid (commercially available butter) and osmium stained. Then, the internal cross-sectional structure was cut by FIB, and the porosity of the antipathogen structure was measured by SEM. The result was that the porosity of Examples 1 and 2 was more than 30%. Meanwhile, the porosity of the comparative example was less than 30%.

[0208] Next, the antipathogenic activities (antibacterial activities) of the obtained antipathogenic structures of Examples 1 and 2 and the structure of Comparative Example 1 were evaluated.

[0209] <Evaluation of antipathogen activity (antibacterial activity)>

[0210] According to the method of JIS Z 2801 (2012), the antipathogenic activity was evaluated. Specifically, the same bacterial culture was inoculated into an unprocessed test piece (glass plate) and a sample (the antipathogenic structure of Examples 1 and 2 and the structure of Comparative Example 1), and the viable cell count obtained after 24 hours was measured. The results are shown in Table 1 below.

[0211] [Table 1]

[0212]

[0213] The obtained antipathogen structures of Examples 1 and 2 and the structure of Comparative Example 1 were evaluated for durability and water resistance.

[0214] <Durability Evaluation>

[0215] First, according to the method of JIS Z 2801 (2012), the antibacterial activity values ​​of the antipathogen structures of Examples 1 and 2 obtained and the structure of Comparative Example 1 were evaluated. Specifically, the same bacterial culture was inoculated into an unprocessed test piece (test piece A) as a glass substrate, a test piece B formed on the test piece A, and a test piece C formed on the test piece A. Then, the viable cell count obtained after 24 hours was measured, and the antibacterial activity value was calculated based on the following numerical formula. The antibacterial activity value of 0.3 or more was considered to be "a", and the antibacterial activity value of less than 0.3 was considered to be "b". The results are shown in Table 2 below.

[0216] Here, the test piece C is the antipathogenic structures of Examples 1 and 2 and the structure of Comparative Example 1.

[0217] Test piece B is a test piece prepared by using the following liquid composition. Specifically, the above-mentioned liquid composition is obtained in the same manner as Preparation Examples 1 and 2 and Comparative Preparation Example 1, except that the porogen is not included. More specifically, Test piece B is obtained in the following manner. First, the liquid composition is applied to a glass plate to form a coating area of ​​a solid image. Immediately thereafter, under N2 atmosphere, ultraviolet light (UV) (light source: UV-LED (obtained from Phoseon, product name: FJ800), wavelength: 365nm, irradiation intensity: 30mW / cm 2 , irradiation time: 20s) irradiating the coating area of ​​the liquid composition to cure the coating area of ​​the liquid composition. All the test pieces B prepared using the liquid composition have a planar surface structure and do not include a plurality of openings.

[0218] Antimicrobial activity value = (log B-log A)-(log C-log A).

[0219] A: The average value of the live cell count on the test piece A obtained after 24 hours.

[0220] B: The average value of the live cell count on the test piece B obtained after 24 hours.

[0221] C: The average value of the live cell count on the test piece C obtained after 24 hours.

[0222] The surface of the test piece C (the antipathogenic structures of Examples 1 and 2 and the structure of Comparative Example 1) was wiped 10 times with a dry cotton cloth (canequim No. 3) by applying a load (400 g). After wiping, the antibacterial activity values ​​of the antipathogenic structures of Examples 1 and 2 and the structure of Comparative Example 1 were determined in the above manner. The results are shown in Table 2 below.

[0223] <Evaluation of water resistance>

[0224] First, according to the method of JIS Z 2801 (2012), the antibacterial activity values ​​of the antipathogen structures of Examples 1 and 2 obtained and the structure of Comparative Example 1 were evaluated. Specifically, the same bacterial culture was inoculated into an unprocessed test piece (test piece A) as a glass substrate, a test piece B formed on the test piece A, and a test piece C formed on the test piece A. Then, the viable cell count obtained after 24 hours was measured, and the antibacterial activity value was calculated based on the following numerical formula. The antibacterial activity value of 0.3 or more was considered to be "a", and the antibacterial activity value of less than 0.3 was considered to be "b". The results are shown in Table 2 below.

[0225] Here, the test piece C is the antipathogenic structures of Examples 1 and 2 and the structure of Comparative Example 1.

[0226] Test piece B is a test piece prepared by using the following liquid composition. Specifically, the above-mentioned liquid composition is obtained in the same manner as Preparation Examples 1 and 2 and Comparative Preparation Example 1, except that the porogen is not included. More specifically, Test piece B is obtained in the following manner. First, the liquid composition is applied to a glass plate to form a coating area of ​​a solid image. Immediately thereafter, under N2 atmosphere, ultraviolet light (UV) (light source: UV-LED (obtained from Phoseon, product name: FJ800), wavelength: 365nm, irradiation intensity: 30mW / cm 2 , irradiation time: 20s) irradiating the coating area of ​​the liquid composition to cure the coating area of ​​the liquid composition. All the test pieces B prepared using the liquid composition have a planar surface structure and do not include a plurality of openings.

[0227] Antimicrobial activity value = (log B-log A)-(log C-log A).

[0228] A: The average value of the live cell count on the test piece A obtained after 24 hours.

[0229] B: The average value of the live cell count on the test piece B obtained after 24 hours.

[0230] C: The average value of the live cell count on the test piece C obtained after 24 hours.

[0231] Test piece C (antipathogenic structures of Examples 1 and 2 and the structure of Comparative Example 1) was immersed in distilled water, the temperature of which was maintained at 25 degrees Celsius, and left to stand for 24 hours. Then, the resultant was further air-dried for one day. The antimicrobial activity values ​​of the antipathogenic structures of Examples 1 and 2 and the structure of Comparative Example 1 obtained after drying were determined in the above manner. The results are shown in Table 2 below.

[0232] [Table 2]

[0233]

[0234] <Preparation Example of Liquid Composition>

[0235] (Preparation Example 3)

[0236] The materials were mixed in the following ratios to prepare Comparative Liquid Composition 3.

[0237] Polymerizable compound: tricyclodecane dimethanol diacrylate (obtained from DAICEL-ALLNEX LTD.): 28.0 parts by mass

[0238] Porogenic agent: Ethylene glycol monobutyl ether: 70.0 parts by mass

[0239] Polymerization initiator: IRGACURE 819 (available from BASF): 1.0 part by mass

[0240] When the viscosity of Liquid Composition 3 at 25 degrees Celsius was measured using a viscometer (device name: RE-550L, available from Toki Sangyo Co., Ltd), it was found to be 30.0 mPa·s or less.

[0241] <Preparation Example of Antipathogen Structure>

[0242] (Example 3)

[0243] The antipathogen structure of Example 3 was obtained in the same manner as in Example 1, except that the liquid composition 1 was changed to the liquid composition 3. When the liquid composition 3 was discharged by the inkjet method, discharge failures such as nozzle clogging and discharge bending were not found. Therefore, it was found that the liquid composition 3 had high discharge stability.

[0244] The surface opening pore size, inner pore size and porosity of the obtained antipathogen structure of Example 3 were evaluated in the same manner as in Example 1. As a result, openings with a pore size of about 0.1 μm to 0.5 μm were found on the entire surface of the antipathogen structure. Pores with a pore size of about 0.1 μm to 0.5 μm were found on the entire cross section of the antipathogen structure. Its porosity was 30% or more.

[0245] The antipathogenic activity (antibacterial activity) of the obtained antipathogenic structure of Example 3 was evaluated.

[0246] <Evaluation of antipathogen activity (antibacterial activity)>

[0247] First, according to the method of ISO 22196 (2011), the antibacterial activity value of the antipathogen structure of Example 3 was determined. Specifically, the same bacterial culture was inoculated into the test piece B formed on the glass substrate and the test piece C formed on the glass substrate, respectively. Then, the viable cell count obtained after 24 hours was measured, and the antibacterial activity value was calculated based on the following numerical formula. The results are shown in Table 3.

[0248] Here, test piece C is the antipathogen structure of Example 3.

[0249] Test piece B is a test piece prepared by using the following liquid composition. Specifically, the above liquid composition is obtained in the same manner as in Preparation Example 3, except that the porogen is not included. More specifically, test piece B is obtained in the following manner. First, the liquid composition is applied to a glass plate to form a coating area of ​​a solid image. Immediately thereafter, under N2 atmosphere, ultraviolet light (UV) (light source: UV-LED (obtained from Phoseon, product name: FJ800), wavelength: 365nm, irradiation intensity: 30mW / cm 2 , irradiation time: 20s) irradiating the coating area of ​​the liquid composition to cure the coating area of ​​the liquid composition. The test piece B prepared using the liquid composition is a test piece having a planar surface structure and not including a plurality of openings.

[0250] Antibacterial activity value = Ut-At.

[0251] Ut: The average value of the common logarithm value of the live cell count on the test piece B obtained after 24 hours.

[0252] At: The average value of the common logarithm value of the live cell count on the test piece C obtained after 24 hours.

[0253] [Table 3]

[0254]

[0255] The obtained antipathogen structure of Example 3 was evaluated for durability and water resistance.

[0256] <Durability Evaluation>

[0257] The surface of the test piece C (the antipathogenic structure of Example 3) was wiped 10 times with a dry cotton cloth (fine white cloth No. 3) by applying a load (400 g). After wiping, the antibacterial activity value of the antipathogenic structure of Example 3 was determined by the method according to ISO 22196 (2011) as described above. The antibacterial activity value of 0.3 or more was considered to be "a", and the antibacterial activity value of less than 0.3 was considered to be "b". The results are shown in Table 4 below.

[0258] <Evaluation of water resistance>

[0259] Test piece C (antipathogen structure of Example 3) was immersed in distilled water, the temperature of which was maintained at 25 degrees Celsius, and left to stand for 24 hours. Then, the resultant was further air-dried for one day. The antimicrobial activity value of the antipathogen structure of Example 3 obtained after drying was determined as described above by the method according to ISO 22196 (2011). Antimicrobial activity values ​​above 0.3 were considered to be "a", and antimicrobial activity values ​​less than 0.3 were considered to be "b". The results are shown in Table 4 below.

[0260] [Table 4]

[0261]

[0262] <Preparation Example of Liquid Composition>

[0263] (Preparation Example 4)

[0264] The materials were mixed in the following ratio to prepare a liquid composition 4.

[0265] Polymerizable compound: tricyclodecane dimethanol diacrylate (obtained from DAICEL-ALLNEX LTD.): 48.0 parts by mass

[0266] Porogenic agent: Ethylene glycol monoisopropyl ether: 50.0 parts by mass

[0267] Polymerization initiator: IRGACURE 819 (available from BASF): 1.0 part by mass

[0268] When the viscosity of Liquid Composition 4 at 25 degrees Celsius was measured using a viscometer (device name: RE-550L, available from Toki Sangyo Co., Ltd), it was found to be 30.0 mPa·s or less.

[0269] <Preparation Example of Antipathogen Structure>

[0270] (Example 4)

[0271] Liquid composition 4 was loaded into an inkjet discharge device equipped with a GEN5 head (obtained from Ricoh Printing Systems, Ltd.) and discharged onto a glass plate to form an application area of ​​a solid image. Immediately thereafter, ultraviolet rays (UV) (light source: UV-LED (obtained from Phoseon, product name: FJ800), wavelength: 365 nm, irradiation intensity: 400 mW / cm 2 , irradiation time: 20s) irradiated the application area of ​​liquid composition 4 to cure the application area of ​​liquid composition 4. Then, the cured product was heated at 120 degrees Celsius for 1 minute using a hot plate to remove the porogen. Thus, the antipathogen structure of Example 4 was obtained. When liquid composition 4 was discharged by the inkjet method, discharge failures such as nozzle clogging and discharge bending were not found. Therefore, it was found that liquid composition 4 had high discharge stability.

[0272] The results obtained by observing the surface of the antipathogenic structure of Example 4 with a scanning electron microscope (SEM) are shown in Figure 6 middle.

[0273] The obtained antipathogen structure of Example 4 was evaluated in the same manner as in Example 1 for the surface opening pore size, inner pore size, and porosity.

[0274] As a result, openings with a pore size of about 0.05 micrometers were found on the entire surface of the antipathogen structure. Pores with a pore size of about 0.05 micrometers were found on the entire cross-section of the antipathogen structure. Its porosity was more than 30%.

[0275] The antipathogenic activities (antiviral activities) of the antipathogenic structures obtained in Examples 1 and 4 were evaluated.

[0276] <Evaluation of antipathogen activity (antiviral activity)>

[0277] According to the method of ISO 21702 (2019), the antiviral activity values ​​of the antipathogen structures of Example 1 and Example 4 were determined. Specifically, the same virus culture was inoculated into a test piece Y formed on a glass plate and a test piece X formed on a glass plate, respectively. The virus infectivity titer (PFU / cm2) obtained after 24 hours was measured. 2 ), to calculate the antiviral activity value based on the following numerical formula. The results are shown in Table 5 below.

[0278] Here, the test piece X is the antipathogen structure of Example 1 or Example 4.

[0279] Test piece Y is a test piece prepared by using the following liquid composition. Specifically, the above-mentioned liquid composition is obtained in the same manner as Preparation Example 1 or Preparation Example 4, except that the porogen is not included. More specifically, test piece Y is obtained in the following manner. First, the liquid composition is applied to a glass plate to form a coating area of ​​a solid image. Immediately thereafter, under N2 atmosphere, ultraviolet light (UV) (light source: UV-LED (obtained from Phoseon, product name: FJ800), wavelength: 365nm, irradiation intensity: 30mW / cm 2 , irradiation time: 20s) irradiating the coating area of ​​the liquid composition to cure the coating area of ​​the liquid composition. The test piece Y prepared using the liquid composition is a test piece having a planar surface structure and not including a plurality of openings.

[0280] Antiviral activity value = Ut-At.

[0281] Ut: average value of the common logarithm of the virus infectivity titer on the test piece Y obtained after 24 hours.

[0282] At: the average value of the common logarithm of the virus infectivity titer on the test piece X obtained after 24 hours.

[0283] [Table 5]

[0284]

[0285] The obtained antipathogen structures of Example 1 and Example 4 were evaluated for durability and water resistance.

[0286] <Durability Evaluation>

[0287] The surface of the test piece X (the antipathogen structure of Example 1 and Example 4) was wiped 10 times by applying a load (400 g) using a dry cotton cloth (fine white cloth No. 3). After wiping, the antiviral activity values ​​of the antipathogen structures of Example 1 and Example 4 were determined by the method according to ISO 21702 (2019) as described above. An antiviral activity value of 0.2 or more was considered to be "a", and an antiviral activity value of less than 0.2 was considered to be "b". The results are shown in Table 6 below.

[0288] <Evaluation of water resistance>

[0289] The test piece X (the antipathogen structure of Example 1 and Example 4) was immersed in distilled water, the temperature of which was maintained at 25 degrees Celsius, and left to stand for 24 hours. Then, the resultant was further air-dried for one day. The antiviral activity values ​​of the antipathogen structures of Example 1 and Example 4 obtained after drying were determined as described above by the method according to ISO 21702 (2019). Antiviral activity values ​​above 0.2 were considered to be "a", and antiviral activity values ​​less than 0.2 were considered to be "b". The results are shown in Table 6 below.

[0290] [Table 6]

[0291]

[0292] <Preparation Example of Liquid Composition>

[0293] (Preparation Example 5)

[0294] The materials were mixed in the following ratio to prepare a liquid composition 5.

[0295] Polymerizable compound: tricyclodecane dimethanol diacrylate (obtained from DAICEL-ALLNEX LTD.): 29.0 parts by mass

[0296] Porogen: dipropylene glycol monomethyl ether (obtained from Kanto Chemical Industry Co., Ltd.): 65.0 parts by mass

[0297] Polymerization initiator: IRGACURE 184 (available from BASF): 1.0 part by mass

[0298] Polyvinyl butyral resin (available from Kuraray Co., Ltd., Mowital B20H): 5.0 parts by mass

[0299] When the viscosity of the liquid composition 5 at 25 degrees Celsius was measured using a viscometer (device name: RE-550L, available from Toki Sangyo Co., Ltd), it was found to be 100.0 mPa·s or less.

[0300] <Preparation Example of Antipathogen Structure>

[0301] (Example 5)

[0302] Liquid composition 5 was applied to a glass plate to form an application area of ​​a solid image. Immediately thereafter, ultraviolet rays (UV) (light source: UV-LED (obtained from Phoseon, product name: FJ800), wavelength: 365 nm, irradiation intensity: 30 mW / cm 2, irradiation time: 20s) irradiated the application area of ​​the liquid composition 5 to cure the application area of ​​the liquid composition 5. Then, the cured product was heated at 120 degrees Celsius for 1 minute using a hot plate to remove the porogen. Thus, the antipathogen structure of Example 5 was obtained.

[0303] The results obtained by observing the surface of the antipathogenic structure of Example 5 with a scanning electron microscope (SEM) are shown in Figure 3 middle.

[0304] The obtained antipathogen structure of Example 5 was evaluated in the same manner as in Example 1 for the surface opening pore size, inner pore size, and porosity.

[0305] As a result, openings with a pore size of about 0.5 micrometers were found on the entire surface of the antipathogen structure. Pores with a pore size of about 0.5 micrometers were found on the entire cross-section of the antipathogen structure. Its porosity was more than 15%.

[0306] The obtained antipathogen structure of Example 5 was evaluated for pencil hardness.

[0307] <Evaluation of Pencil Hardness>

[0308] The surface hardness of the surface structure on which the antipathogen structure (resin structure) of Example 5 was formed was determined according to the method of ISO 15184. The measurement was performed using a pencil hardness tester (available from Toyo Seiki Seisaku-sho, Ltd.) by applying a load (750 g).

[0309] As a result, the pencil hardness of the antipathogen structure of Example 5 was F.

[0310] Similar to Example 3, the antipathogenic activity (antibacterial activity) of the antipathogenic structure obtained in Example 5 was evaluated according to the method of ISO 22196 (2011).

[0311] As a result, the antimicrobial activity value of the antipathogen structure of Example 5 was 0.3 or more.

[0312] The obtained antipathogen structure of Example 5 was evaluated for durability in the same manner as in Example 3.

[0313] As a result, the antimicrobial activity value of the antipathogen structure of Example 5 obtained after wiping was 0.3 or more.

[0314] The obtained antipathogen structure of Example 5 was evaluated for water resistance in the same manner as in Example 3.

[0315] The antimicrobial activity value obtained after the antipathogen structure of Example 5 was immersed in distilled water and then dried was 0.3 or more.

[0316] <Preparation Example of Liquid Composition>

[0317] (Preparation Example 6)

[0318] The materials were mixed in the following ratios to prepare a liquid composition 6.

[0319] Precipitation resin: polylactic acid-glycolic acid copolymer (PLGA7520, obtained from FUJIFILM Wako Pure Chemical Corporation): 10.0 parts by mass

[0320] Good solvent: Acetone: 67.5 parts by mass (obtained from FUJIFILM Wako Pure Chemical Corporation)

[0321] Poor solvent: Ethanol: 22.5 parts by mass (obtained from FUJIFILM Wako Pure Chemical Corporation)

[0322] When the viscosity of Liquid Composition 6 at 25 degrees Celsius was measured using a viscometer (device name: RE-550L, available from Toki Sangyo Co., Ltd), it was found to be 30.0 mPa·s or less.

[0323] <Preparation Example of Liquid Composition>

[0324] (Preparation Example 7)

[0325] The materials were mixed in the following ratio to prepare a liquid composition 7.

[0326] Precipitation resin: polylactic acid (RESOMER R 203H, obtained from Sigma-Aldrich): 15.0 parts by mass

[0327] Good solvent: methyl ethyl ketone: 45.0 parts by mass (obtained from FUJIFILM Wako Pure Chemical Corporation)

[0328] Poor solvent: Methanol: 45.0 parts by mass (obtained from FUJIFILM Wako Pure Chemical Corporation)

[0329] When the viscosity of Liquid Composition 7 at 25 degrees Celsius was measured using a viscometer (device name: RE-550L, available from Toki Sangyo Co., Ltd), it was found to be 30.0 mPa·s or less.

[0330] <Preparation Example of Antipathogen Structure>

[0331] (Example 1)

[0332] Liquid compositions 6 and 7 are each loaded into an inkjet discharge device equipped with a GEN5 head (derived from Ricoh Printing Systems, Ltd.) and discharged onto a glass plate to form an application area of ​​a solid image. Immediately thereafter, the glass plate is placed in a vacuum dryer with a temperature setting of 25 degrees Celsius and dried for 6 hours to remove good solvents and poor solvents. Therefore, the antipathogenic structures of embodiments 6 and 7 are obtained. When liquid compositions 6 and 7 are discharged by an inkjet method, discharge failures such as nozzle clogging and discharge bending are not found. Therefore, it is found that liquid compositions 6 and 7 have high discharge stability.

[0333] The obtained antipathogen structures of Examples 6 and 7 were evaluated in the same manner as in Example 1 for the surface opening pore size, inner pore size, and porosity.

[0334] As a result, openings with a pore size of about 0.5 micrometers were found on the entire surface of the antipathogen structure. Pores with a pore size of about 0.5 micrometers were found on the entire cross-section of the antipathogen structure. Its porosity was more than 15%.

[0335] Similar to Example 3, the antipathogenic activity (antibacterial activity) of the antipathogenic structures obtained in Examples 6 and 7 was evaluated according to the method of ISO 22196 (2011).

[0336] As a result, the antimicrobial activity values ​​of the antipathogen structures of Examples 6 and 7 were 0.3 or more.

[0337] The obtained antipathogen structures of Examples 6 and 7 were evaluated for durability in the same manner as in Example 3.

[0338] As a result, the antimicrobial activity values ​​of the antipathogen structures of Examples 6 and 7 obtained after wiping were 0.3 or more.

[0339] The obtained antipathogen structures of Examples 6 and 7 were evaluated for water resistance in the same manner as in Example 3.

[0340] The antimicrobial activity values ​​obtained after the antipathogen structures of Examples 6 and 7 were immersed in distilled water and then dried were 0.3 or more.

[0341] Reference Mark List

[0342] 1a: Application device

[0343] 1b: Container

[0344] 1c: Supply pipe

[0345] 2a: Light-emitting device

[0346] 2b: Polymerization inert gas circulation device

[0347] 3a: Heating device

[0348] 4: Base material

[0349] 5: Conveying part

[0350] 6: Precursors of antipathogen structures

[0351] 7: Liquid composition

[0352] 10: Application Steps

[0353] 20: Polymerization step section

[0354] 30: Heating step section

[0355] 100: Production equipment

Claims

1. Anti-pathogen structures, including: a resin structure having a plurality of openings in a surface of the resin structure such that the resin structure has antimicrobial activity, and The resin structure has an air permeation resistance of less than 1,000 seconds / 100 ml, the air permeation resistance being determined in accordance with JIS P8117.

2. The antipathogen structure according to claim 1, The resin structure has antiviral activity.

3. The antipathogen structure according to claim 1, wherein the resin structure has a porous structure, the porous structure has a co-continuous structure in which a plurality of pores are continuously connected to each other, and The plurality of openings are each independently coupled to some of the plurality of holes constituting the co-continuous structure.

4. The antipathogen structure according to any one of claims 1 to 3, wherein the resin structure has the antimicrobial activity even after the antipathogen structure is immersed in water at 25 degrees Celsius for 24 hours.

5. The antipathogen structure according to claim 1, The aperture of the opening is less than 10 micrometers.

6. The antipathogen structure according to claim 2, The aperture of the opening is less than 0.1 micrometer.

7. The antipathogen structure according to any one of claims 1 to 3, The term “having the antimicrobial activity” means that the antimicrobial activity value of the antipathogen structure is 0.3 or more, and the antimicrobial activity value is evaluated according to the method described in JIS Z 2801-2012 or ISO 22196-2011.

8. The antipathogen structure according to claim 2, Wherein having the antiviral activity means that the antiviral activity value of the antipathogen structure is greater than 0.2, and the antiviral activity value is evaluated according to the method described in ISO 21702-2019.

9. The antipathogen structure according to any one of claims 1 to 3, The porosity of the resin structure is greater than 10%.

10. The antipathogen structure according to any one of claims 1 to 3, wherein the antipathogenic structure is free of antimicrobial agents.

11. The antipathogen structure according to any one of claims 1 to 3, wherein the anti-pathogen structure does not contain an anti-viral agent.

12. The antipathogen structure according to any one of claims 1 to 3, wherein the resin structure comprises a skeleton, the skeleton shapes the plurality of openings, and The skeleton has a shape in which a plurality of particles are coupled to each other.

13. The antipathogenic structure according to any one of claims 1 to 3, wherein the resin structure comprises a framework for shaping the plurality of openings, and The skeleton has a planar shape.

14. The antipathogen structure according to any one of claims 1 to 3, The pencil hardness of the surface of the resin structure is B or higher, and the pencil hardness is evaluated according to the method described in ISO 15184.

15. A method for producing an antipathogen structure having a resin structure having a plurality of openings in a surface of the resin structure such that the resin structure has antimicrobial activity, the method comprising: applying a liquid composition comprising a polymerizable compound and a solvent; as well as polymerizing the polymerizable compound to form the resin structure, The resin structure has an air permeation resistance of less than 1,000 seconds / 100 ml, the air permeation resistance being determined in accordance with JIS P8117.

16. The method for producing an antipathogen structure according to claim 15, wherein said applying is expelling said liquid composition.

17. A method for producing an antipathogen structure according to claim 15 or 16, The viscosity of the liquid composition at 25 degrees Celsius is 1 mPa·s or more but 200 mPa·s or less.

18. A method for producing an antipathogen structure according to claim 15 or 16, The resin structure has antiviral activity.

19. An apparatus for producing an antipathogen structure having a resin structure having a plurality of openings in a surface of the resin structure such that the resin structure has antimicrobial activity, the apparatus comprising: an application unit configured to apply a liquid composition comprising a polymerizable compound and a solvent; as well as a polymerization unit configured to polymerize the polymerizable compound to form the resin structure, The resin structure has an air permeation resistance of less than 1,000 seconds / 100 ml, the air permeation resistance being determined in accordance with JIS P8117.

20. The apparatus for producing an anti-pathogen structure according to claim 19, The applying unit is a unit configured to discharge the liquid composition.

21. The apparatus for producing an antipathogen structure according to claim 19 or 20, The viscosity of the liquid composition at 25 degrees Celsius is 1 mPa·s or more but 200 mPa·s or less.

22. The apparatus for producing an antipathogen structure according to claim 19 or 20, The resin structure has antiviral activity.

23. A method for producing an antipathogen structure having a resin structure having a plurality of openings in a surface of the resin structure such that the resin structure has antimicrobial activity, the method comprising: applying a liquid composition comprising a resin, a good solvent, and a poor solvent; as well as drying the good solvent and the poor solvent to form the resin structure, The resin structure has an air permeation resistance of less than 1,000 seconds / 100 ml, the air permeation resistance being determined in accordance with JIS P8117.

24. The method for producing an antipathogen structure according to claim 23, wherein said applying is expelling said liquid composition.

25. A method for producing an antipathogen structure according to claim 23 or 24, The viscosity of the liquid composition at 25 degrees Celsius is 1 mPa·s or more but 200 mPa·s or less.

26. A method for producing an antipathogen structure according to claim 23 or 24, The resin structure has antiviral activity.

27. An apparatus for producing an antipathogen structure having a resin structure having a plurality of openings in a surface of the resin structure such that the resin structure has antimicrobial activity, the apparatus comprising: an application unit configured to apply a liquid composition including a resin, a good solvent, and a poor solvent; as well as a drying unit configured to dry the good solvent and the poor solvent to form the resin structure, The resin structure has an air permeation resistance of less than 1,000 seconds / 100 ml, the air permeation resistance being determined in accordance with JIS P8117.

28. The apparatus for producing an anti-pathogen structure according to claim 27, The applying unit is a unit configured to discharge the liquid composition.

29. Apparatus for producing an antipathogen structure according to claim 27 or 28, The viscosity of the liquid composition at 25 degrees Celsius is 1 mPa·s or more but 200 mPa·s or less.

30. The apparatus for producing an antipathogen structure according to claim 27 or 28, The resin structure has antiviral activity.

31. A liquid composition comprising: polymerizable compounds; organic polymer compounds; and Solvents, wherein the liquid composition is cured to form a resin structure, The resin structure has a plurality of openings in a surface of the resin structure such that the resin structure has antimicrobial activity, and The resin structure has an air permeation resistance of less than 1,000 seconds / 100 ml, the air permeation resistance being determined in accordance with JIS P8117.

32. The liquid composition according to claim 31, wherein the organic polymer compound is dissolved in the solvent.

33. The liquid composition according to claim 31 or 32, The organic polymer compound includes a functional group that can form a hydrogen bond with the polymerizable compound and a polymer of the polymerizable compound.

34. The liquid composition according to claim 31 or 32, The resin structure has antiviral activity.

Citation Information

Patent Citations

  • High-breathability sub-nanometer filter filtration membrane mask capable of preventing PM2.5, haze, viruses and germs

    CN104055247A

  • Synthetic polymer film having surface provided with bactericidal activity

    CN106133033A

  • Synthetic polymer film provided with surface having sterilizing activity

    CN107709419A

  • Plastic product which includes synthetic polymer film whose surface has microbicidal activity

    CN109503875A

  • Method for producing recycled product, recycled resin pellet, and recycled film

    CN110337350A