Glass substrate

By limiting the high-temperature viscosity and optimizing the glass composition in the glass substrate, the problem of balancing heat resistance and productivity is solved, and the heat resistance and productivity of high-definition displays are improved. It is suitable for the manufacturing of LTPS TFT and oxide TFT.

CN115259660BActive Publication Date: 2024-10-29NIPPON ELECTRIC GLASS CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202210983759.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2018-04-12
Publication Date
2024-10-29
Estimated Expiration
2038-04-12

AI Technical Summary

Technical Problem

It is difficult for existing glass substrates to achieve both high productivity and clarity when improving heat resistance. On the contrary, heat resistance tends to decrease when productivity is improved, making it difficult to meet the needs of high-definition displays.

Method used

By limiting the high-temperature viscosity of the glass substrate to below 1670°C at 102.5dPa·s, and setting the estimated viscosity Logη500 at 500°C to above 26.0, combined with optimizing the glass composition and process treatment, the heat resistance of the glass substrate is improved and productivity.

Benefits of technology

It improves the heat resistance and productivity of glass substrates in high-definition display applications, ensures high-temperature stability and clarity, and is suitable for the manufacturing of LTPS TFT and oxide TFT.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003799899230000111
    Figure BDA0003799899230000111
  • Figure HDA0003799899240000011
    Figure HDA0003799899240000011
Patent Text Reader

Abstract

The glass substrate of the present invention is characterized in that the high temperature viscosity is 10 2.5 dPa·s is below 1650°C, and Logη 500 = 0.167×Ps-0.015×Ta-0.062×Ts-18.5 Estimated viscosity at 500°C Logη 500 Above 26.0.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application of the invention patent application with application number 201880023944.7, application date April 12, 2018, and invention name “Glass Substrate”. Technical Field

[0002] The present invention relates to a glass substrate, and in particular to a glass substrate suitable for use as a substrate for flat panel displays such as liquid crystal displays and organic EL displays. Background Art

[0003] Organic EL devices such as organic EL displays are thin, excellent in video display, and have low power consumption, and therefore are used for applications such as displays of mobile phones.

[0004] As a substrate for an organic EL display, a glass substrate is widely used. Glass that does not substantially contain alkali metal oxides or glass with a low content of alkali metal oxides is used as the glass substrate for this purpose. In other words, low-alkali glass is used as the glass substrate for this purpose. If low-alkali glass is used, it is possible to prevent alkali ions from diffusing into the semiconductor material produced in the heat treatment process.

[0005] In recent years, high-definition displays have been required for smartphones and mobile terminals, and LTPS (Low-temperature poly silicon) TFTs and oxide TFTs are often used as semiconductors for driving thin-film transistors (TFTs). Summary of the invention

[0006] Problems to be solved by the invention

[0007] The glass substrate for this application requires, for example, the following properties (1) and (2).

[0008] (1) Thin glass substrates have high productivity, and in particular, high meltability and clarity.

[0009] (2) In the production of LTPS TFT and oxide TFT, the heat treatment temperature is higher than that of conventional amorphous Si TFT. Therefore, in order to reduce the thermal shrinkage of the glass substrate, the heat resistance is higher than before.

[0010] However, it is not easy to achieve both the required properties (1) and (2). That is, if the heat resistance of the glass substrate is improved, the productivity (melting property, clarity) is likely to decrease, and conversely, if the productivity of the glass substrate is improved, the heat resistance is likely to decrease.

[0011] The present invention has been made in view of the above circumstances, and an object of this technology is to propose a glass substrate capable of achieving both productivity and heat resistance.

[0012] Means for solving problems

[0013] The inventors have found that the above-mentioned technical problems can be solved by limiting the viscosity characteristics of the glass substrate within a predetermined range, and thus proposed the present invention. The glass substrate of the present invention is characterized in that the high temperature viscosity is 10 2.5 The temperature at dPa·s is 1670°C or less, and the estimated viscosity Logη at 500°C is calculated by the following formula 1 500 is 26.0 or more. 2.5 The “temperature at dPa·s” can be measured by a platinum ball pulling method. The “strain point”, “annealing point” and “softening point” are values ​​measured based on the methods of ASTM C336 and ASTM C338.

[0014] [Formula 1]

[0015] Logη 500 =0.167×Ps-0.015×Ta-0.062×Ts-18.5

[0016] Ps: strain point (℃)

[0017] Ta: Annealing point (℃)

[0018] Ts: Softening point (℃)

[0019] The heat resistance of glass substrates has been evaluated by the strain point, annealing point and other temperatures that can be measured. However, these temperature ranges are about 200°C higher than the process temperature during the production of LTPS·TFT and oxide TFT, or even higher. Therefore, the strain point, annealing point and other temperatures cannot accurately evaluate the heat resistance of glass substrates.

[0020] The present inventors have repeatedly conducted various experiments and found that the heat resistance of a glass substrate can be accurately evaluated by calculating the estimated viscosity at 500° C., which is close to the process temperature when manufacturing LTPS·TFT and oxide TFT, and using it as an index of heat resistance.

[0021] Furthermore, the inventors have found that even if the strain point, which is a conventional index, is the same, the heat resistance is greatly different. Table 1 shows the estimated viscosity Logη at 500°C. 500 The glass substrate P and the glass substrate Q have the same glass composition and strain point Ps. As shown in Table 1, the estimated viscosity Logη of the glass substrate P at 500°C is 500 27.8, and the thermal shrinkage rate is 17.5 ppm. In contrast, the estimated viscosity Logη of the glass substrate Q at 500°C is 500The heat shrinkage is 29.1 and 12.8 ppm. In other words, for glass substrate P and glass substrate Q, even if the glass composition and strain point Ps are the same, the heat shrinkage is 4.7 ppm different. Considering that the heat shrinkage of glass substrates used for high-definition displays is preferably 18 ppm or less, the difference of 4.7 ppm is very large. Moreover, if the estimated viscosity Logη at 500°C is 500 As an indicator, the difference can be correctly estimated. Here, the "thermal shrinkage rate" is a value calculated as follows. First, after a linear mark is recorded at a specified position on the sample, the sample is folded vertically relative to the mark and divided into two glass sheets. Next, only one of the glass sheets is subjected to a specified heat treatment (heating from room temperature at a rate of 5°C / min, keeping at 500°C for 1 hour, and cooling at a rate of 5°C / min). Then, the glass sheets that have been heat treated and the glass sheets that have not been heat treated are arranged, and after fixing the two with adhesive tape T, the offset of the mark is measured. When the offset of the mark is ΔL and the length of the sample before heat treatment is L0, the thermal shrinkage rate is calculated using the formula ΔL / L0 (unit: ppm).

[0022] [Table 1]

[0023] P Q Ps[℃] 740 740 Thermal shrinkage [ppm] 17.5 12.8 logη[poise] at 500℃ 27.8 29.1

[0024] Here, considering the above situation, the estimated viscosity Logη of the glass substrate of the present invention at 500°C is 500 The limit is 26.0 or more. Thereby, the heat resistance of the glass substrate can be improved.

[0025] On the other hand, if a large amount of high melting point components are introduced into the glass composition, the estimated viscosity Logη at 500°C can be increased. 500 However, in this case, the melting property and the clarity are reduced, resulting in a decrease in the productivity of the glass substrate. Here, the glass substrate of the present invention is obtained by reducing the high temperature viscosity to 10 2.5 The temperature under dPa·s is limited to below 1670°C to prevent the above situation.

[0026] Moreover, it is preferable that the A value calculated by the following formula 2 of the glass substrate of this invention is 25.0 or more.

[0027] [Formula 2]

[0028] A value = Logη 500 -[β-OH value (mm -1 )]×[B2O3(mass%)]

[0029] Here, the “β-OH value” is a value calculated from the following formula 3 using FT-IR.

[0030] [Formula 3]

[0031] β-OH value = (1 / X)log(T1 / T2)

[0032] X: Plate thickness (mm)

[0033] T1: Reference wavelength 3846cm -1 Transmittance under (%)

[0034] T2: Hydroxyl absorption wavelength 3600cm -1 Minimum transmittance near (%)

[0035] Moreover, the glass substrate of the present invention preferably has a β-OH value of 0.20 / mm or less.

[0036] Moreover, the glass substrate of the present invention preferably has a β-OH value of 0.15 / mm or less.

[0037] In addition, the glass substrate of the present invention preferably has a B2O3 content of less than 2.0% by mass in the glass composition.

[0038] In addition, the glass substrate of the present invention, as a glass composition, preferably contains, by mass%, 55 to 65% SiO2, 16 to 22% Al2O3, 0 to 1% B2O3, 0 to less than 0.1% Li2O+Na2O+K2O, 1 to 6% MgO, 2 to 8% CaO, 0 to 2% SrO, 4 to 13% BaO, 0 to less than 0.010% As2O3, and 0 to less than 0.010% Sb2O3.

[0039] In addition, the glass substrate of the present invention preferably has a Fe 2 O 3 content of 0.010 mass % or less in the glass composition.

[0040] In addition, the glass substrate of the present invention preferably has a liquidus temperature of 1300° C. or less. Here, the “liquidus temperature” refers to the temperature at which devitrification (devitrified crystals) are confirmed in the glass after the glass powder remaining in the 50-mesh (300 μm) sieve is passed through a standard sieve of 30 mesh (500 μm), is placed in a platinum boat, and is kept in a temperature gradient furnace for 24 hours, and then the platinum boat is taken out.

[0041] In addition, the glass substrate of the present invention preferably has a forming confluence surface at the center of the plate thickness, in other words, is formed by an overflow down-draw method. Here, the "overflow down-draw method" is a method in which molten glass is overflowed from both sides of a heat-resistant trough-shaped structure, the overflowed molten glass is merged at the lower end of the trough-shaped structure, and is extended downward to form a glass substrate.

[0042] Furthermore, the glass substrate of the present invention is preferably used as a substrate for an organic EL device. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] Figure 1 The data show the relationship between the A value and the thermal shrinkage rate. DETAILED DESCRIPTION

[0044] In the glass substrate of the present invention, the high temperature viscosity is 10 2.5 The temperature under the water is 1670°C or lower, preferably 1650°C or lower, 1640°C or lower, 1630°C or lower, and particularly preferably 1500 to 1620°C. 2.5 When the temperature of the glass substrate increases, the melting property and the clarity decrease, and the production cost of the glass substrate increases.

[0045] In the glass substrate of the present invention, the estimated viscosity at 500°C Logη 500 It is 26.0 or more, preferably 28.0 or more, 28.5 or more, 29.0 or more, and particularly preferably 29.5 to 35. If the estimated viscosity Logη at 500°C 500 When the temperature is too low, the heat resistance of the glass substrate decreases, and the heat shrinkage rate of the glass substrate increases.

[0046] According to the investigation of the present inventors, it was found that A value = Logη 500 -[β-OH value]×(B2O3 content) shows a high correlation with the measured value of the thermal shrinkage rate. When the A value is large, the thermal shrinkage rate becomes small. Figure 1 It is data showing the relationship between the A value and the thermal shrinkage rate. In the glass substrate of the present invention, the A value is preferably 25.0 or more, 27.0 or more, 28.0 or more, 29.0 or more, and particularly preferably 30.0 to 40.0. If the A value is too small, the heat resistance of the glass substrate decreases, and the thermal shrinkage rate of the glass substrate tends to increase.

[0047] It can be seen from Formula 3 that a small amount of water in the glass affects the relaxation behavior of the glass. For relaxation, there is a rapid relaxation that is different from the slow relaxation dominated by viscosity. If the thermal shrinkage rate becomes lower, the proportion of rapid relaxation gradually increases. This rapid relaxation is easy to occur when the amount of water in the glass increases. Therefore, the less water in the glass, the more difficult it is to produce rapid relaxation. In a glass region with a low thermal shrinkage rate such as the glass substrate of the present invention, the effect of reducing the thermal shrinkage rate becomes relatively high. Therefore, the β-OH value is preferably less than 0.20 / mm, less than 0.15 / mm, less than 0.12 / mm, less than 0.11 / mm, less than 0.10 / mm, less than 0.09 / mm, less than 0.07 / mm, and particularly preferably 0.01 to 0.05 / mm.

[0048] As methods for reducing the β-OH value, there are the following methods (1) to (7), among which methods (1) to (4) are effective. (1) Selecting raw materials with low water content. (2) Adding desiccants such as Cl and SO3 to the glass batch. (3) Electrical heating by heating electrodes. (4) Using a small melting furnace. (5) Reducing the moisture content in the atmosphere in the furnace. (6) Bubbling N2 in the molten glass. (7) Increasing the flow rate of the molten glass.

[0049] It can be seen from Formula 3 that the less the content of B2O3 in the glass composition, the lower the thermal shrinkage. This is because the less the content of B2O3, the easier it is to maintain a low moisture content in the glass. Specifically, if B2O3, especially if the glass contains more tri-coordinated boron, the solubility of water becomes higher, and it is difficult to maintain a low moisture content in the glass. Therefore, in the glass substrate of the present invention, the content of B2O3 in the glass composition is preferably less than 2 mass%, less than 1.5 mass%, less than 1 mass%, less than 1.0 mass%, and particularly preferably 0.1 to 0.9 mass%.

[0050] The glass substrate of the present invention preferably contains, as a glass composition, 55-65% SiO2, 16-22% Al2O3, 0-1% B2O3, 0-less than 0.1% Li2O+Na2O+K2O, 1-6% MgO, 2-8% CaO, 0-2% SrO, 4-13% BaO, 0-less than 0.010% As2O3, and 0-less than 0.010% Sb2O3, in terms of mass%. The reasons for limiting the content of each component as described above are shown below. It should be noted that in the description of the content of each component, % represents mass%.

[0051] The suitable lower limit of SiO2 is 55% or more, 56% or more, 57% or more, 58% or more, especially 59% or more, and the suitable upper limit is preferably 65% ​​or less, 64% or less, 63% or less, especially 62% or less. If the content of SiO2 is too little, the strain point is easy to reduce while the devitrified crystal containing Al2O3 is easily produced. On the other hand, if the content of SiO2 is too much, the high temperature viscosity becomes high, the meltability is easy to reduce, and in addition, devitrified crystals such as cristobalite are precipitated, so that the liquidus temperature is easy to increase.

[0052] The suitable lower limit of Al2O3 is 16% or more, 17% or more, 18% or more, and especially 18.5% or more, and the suitable upper limit is 22% or less, 21% or less, and especially 20% or less. If the content of Al2O3 is too little, the strain point is easy to decrease, and the glass becomes easy to phase separate. On the other hand, if the content of Al2O3 is too much, devitrified crystals such as mullite and calcium feldspar are precipitated, so that the liquidus temperature is easy to become high.

[0053] Suitable contents of B2O3 are as described above.

[0054] As mentioned above, Li2O, Na2O and K2O are components that deteriorate the characteristics of the semiconductor film. Therefore, the total amount of Li2O, Na2O and K2O and their respective contents are preferably less than 1.0%, less than 0.50%, less than 0.20%, less than 0.10%, less than 0.08%, and especially less than 0.06%. On the other hand, if a small amount of Li2O, Na2O and K2O is introduced, the resistivity of the molten glass decreases, so that it becomes easy to melt the glass by heating with electricity using the heating electrode. Therefore, the total amount of Li2O, Na2O and K2O and their respective contents are preferably more than 0.01%, more than 0.02%, more than 0.03%, more than 0.04%, and especially more than 0.05%. It should be noted that, if the influence on the semiconductor film and the reduction of resistivity are comprehensively considered, it is preferred to preferentially introduce Na2O among Li2O, Na2O and K2O.

[0055] MgO is a component that reduces high temperature viscosity and improves solubility. The content of MgO is preferably 1-6%, 2-5.5%, 2.5-5.5%, and particularly 3-5%. If the content of MgO is too low, it is difficult to obtain the above effects. On the other hand, if the content of MgO is too high, the strain point tends to decrease.

[0056] CaO is a component that reduces high temperature viscosity and improves solubility without lowering the strain point. In addition, CaO is a component that reduces the cost of raw materials by introducing relatively low-priced raw materials among alkaline earth metal oxides. The content of CaO is preferably 2-8%, 3-8%, 4-9%, 4.5-8%, and particularly 5-7%. If the content of CaO is too little, it is difficult to obtain the above-mentioned effect. On the other hand, if the content of CaO is too much, the thermal expansion coefficient becomes too high and the glass is prone to devitrification.

[0057] SrO is a component that improves the resistance to devitrification, and is also a component that reduces high-temperature viscosity and improves solubility without lowering the strain point. The content of SrO is preferably 0-2%, 0-1.5%, 0.1-1.5%, 0.2-1%, and particularly 0.3 to less than 1.0%. If the content of SrO is too little, it becomes difficult to obtain the effect of suppressing phase separation and improving the resistance to devitrification. On the other hand, if the content of SrO is too much, the component balance of the glass composition is destroyed, and strontium silicate-type devitrification crystals are easily precipitated.

[0058] BaO is a component that significantly improves the resistance to devitrification among alkaline earth metal oxides. The content of BaO is preferably 4-13%, 5-12%, 6-11%, and particularly 7-10%. If the content of BaO is too little, the liquidus temperature becomes high and the resistance to devitrification is easily reduced. On the other hand, if the content of BaO is too much, the component balance of the glass composition is destroyed, and devitrification crystals containing BaO are easily precipitated.

[0059] RO (the total amount of MgO, CaO, SrO and BaO) is preferably 10-22%, 13-21%, 14-20%, and particularly 15-20%. If the RO content is too low, the meltability is likely to decrease. On the other hand, if the RO content is too high, the component balance of the glass composition is destroyed, and the devitrification resistance is likely to decrease.

[0060] When the glass is melted by energizing a heating electrode instead of heating by a combustion flame of a burner, As2O3 and Sb2O3 are components that color the glass, and their contents are preferably less than 0.010%, particularly preferably less than 0.0050%.

[0061] In addition to the above components, for example, the following components may be added to the glass composition. In order to reliably obtain the effects of the present invention, the total content of the components other than the above components is preferably 5% or less, particularly preferably 3% or less.

[0062] ZnO is a component that improves melting properties, but if a large amount of ZnO is contained, the glass is likely to lose clarity and the strain point is likely to decrease. The ZnO content is preferably 0 to 5%, 0 to 3%, 0 to 0.5%, and particularly 0 to 0.2%.

[0063] P2O5 is a component that increases the strain point, but if a large amount of P2O5 is contained, the glass is prone to phase separation. The content of P2O5 is preferably 0 to 1.5%, 0 to 1.2%, and particularly 0 to 1%.

[0064] TiO2 is a component that reduces high temperature viscosity and improves melting properties, and is also a component that suppresses solarization. However, if a large amount of TiO2 is contained, the glass will be colored, and the transmittance will be easily reduced. Therefore, the content of TiO2 is preferably 0 to 3%, 0 to 1%, 0 to 0.1%, and particularly 0 to 0.02%.

[0065] Fe2O3 is a component that is inevitably mixed in as an impurity from glass raw materials. In addition, Fe2O3 is also expected to act as a clarifier and to reduce the resistivity of molten glass and is actively added (for example, more than 0.003%, especially more than 0.005%). On the other hand, from the viewpoint of improving the transmittance in the ultraviolet region, it is preferred to reduce the content of Fe2O3 as much as possible. It should be noted that if the transmittance in the ultraviolet region is improved, the irradiation efficiency when using the laser in the ultraviolet region in the process related to the display can be improved. Therefore, the content of Fe2O3 is preferably less than 0.020%, less than 0.015%, less than 0.010%, especially less than 0.010%.

[0066] Y2O3, Nb2O5, and La2O3 have the effects of increasing the strain point and Young's modulus. However, if the content of these components is too much, it is easy to increase the density and raw material cost. Therefore, the content of Y2O3, Nb2O5, and La2O3 is preferably 0-3%, 0-1%, and 0-less than 0.10%, respectively, and particularly preferably 0-less than 0.05%.

[0067] Cl is a component that acts as a desiccant and reduces the β-OH value. Therefore, when Cl is introduced, the suitable lower limit content is 0.001% or more, 0.003% or more, and especially 0.005% or more. However, if the Cl content is too much, the strain point is easily reduced. Therefore, the suitable upper limit content of C1 is 0.5% or less, 0.2% or less, and especially 0.08% or less. It should be noted that as the introduction raw material of Cl, chlorides of alkaline earth metal oxides such as strontium chloride, or aluminum chloride, etc. can be used.

[0068] SO3 is a component that acts as a desiccant and reduces the β-OH value. Therefore, when SO3 is introduced, the suitable lower limit content is 0.0001% or more, and particularly preferably 0.0005% or more. However, if the content of SO3 is too much, reboil bubbles are easily generated. Therefore, the suitable upper limit content of SO3 is 0.05% or less, 0.01% or less, 0.005% or less, and particularly 0.001% or less.

[0069] SnO2 is a component that has a good clarification effect in the high temperature region, is a component that increases the strain point, and is also a component that reduces the high temperature viscosity. The content of SnO2 is preferably 0-1%, 0.001-1%, 0.05-0.5%, and is particularly preferably 0.1-0.3%. If the content of SnO2 is too much, devitrified crystals of SnO2 are easily precipitated. It should be noted that if the content of SnO2 is less than 0.001%, it is difficult to obtain the above effect.

[0070] As long as the glass properties are not significantly impaired, clarifiers other than SnO2 may be used. Specifically, CeO2, F, and C may be added to, for example, 1% in total, and metal powders such as Al and Si may be added to, for example, 1% in total.

[0071] The glass substrate of the present invention preferably has the following properties.

[0072] The strain point is preferably 700° C. or higher, 720° C. or higher, 730° C. or higher, 740° C. or higher, 750° C. or higher, and particularly 760 to 840° C. This makes it easy to suppress thermal shrinkage of the glass substrate in the manufacturing process of LTPS·TFT or oxide TFT.

[0073] The liquidus temperature is preferably below 1300°C, below 1280°C, below 1260°C, below 1250°C, and particularly 900 to 1230°C. In this way, it is easy to prevent the occurrence of devitrified crystals during forming. In addition, since the glass substrate is easily formed by the overflow down-draw method, the surface quality of the glass substrate can be improved. It should be noted that the liquidus temperature is an indicator of devitrification resistance, and the lower the liquidus temperature, the better the devitrification resistance.

[0074] The viscosity at liquidus temperature is preferably 10 4.8 More than berth, 10 5.0 More than berth, 10 5.3 Above 10 5.5 ~10 7.0 In this way, it is easy to prevent the occurrence of devitrified crystals during forming. In addition, since the glass substrate is easily formed by the overflow down-draw method, the surface quality of the glass substrate can be improved. It should be noted that the "viscosity at liquidus temperature" can be measured by the platinum ball pulling method.

[0075] The heat shrinkage rate when the temperature is raised from room temperature at a rate of 5°C / min, maintained at 500°C for 1 hour, and then cooled at a rate of 5°C / min is preferably 21 ppm or less, 18 ppm or less, 15 ppm or less, 12 ppm or less, and particularly 1 to 10 ppm. If the heat shrinkage rate is large, the manufacturing yield of the high-definition panel is likely to decrease.

[0076] In the glass substrate of the present invention, the thickness is preferably 0.05 to 0.7 mm, 0.1 to 0.5 mm, and particularly 0.2 to 0.4 mm. The smaller the thickness, the easier it is to achieve lightweight and thin display. It should be noted that if the thickness is small, the necessity of increasing the forming speed (plate stretching speed) becomes high. In this case, the thermal shrinkage rate of the glass substrate is likely to increase. However, in the present invention, due to the high heat resistance, even if the forming speed (plate stretching speed) is high, the above situation can be effectively suppressed.

[0077] The glass substrate of the present invention preferably has a forming confluence surface at the central portion of the plate thickness, in other words, is formed by the overflow down-draw method. In the overflow down-draw method, the surface that should become the surface of the glass substrate does not contact the trough-shaped refractory material, but is formed in the state of a free surface. Therefore, a glass substrate that is not ground and has good surface quality can be manufactured at a low price. In addition, the overflow down-draw method also has this advantage of being easy to form a thin glass substrate.

[0078] The manufacturing process of a glass substrate generally includes: a blending process, a melting process, a clarification process, a supply process, a stirring process, and a forming process. The blending process is a process of blending glass raw materials to make a glass batch. The melting process is a process of melting a glass batch to obtain molten glass. The clarification process is a process of clarifying the molten glass obtained by the melting process by the action of a clarifier, etc. The supply process is a process of transferring the molten glass between each process. The stirring process is a process of stirring the molten glass and homogenizing it. The forming process is a process of forming the molten glass into a plate shape. It should be noted that, as needed, processes other than the above, such as a state adjustment process for adjusting the molten glass to a state suitable for forming, may also be introduced after the stirring process.

[0079] Low-alkali glass is usually melted by heating with a burner. The burner is usually arranged above the melting furnace, and uses fossil fuels, specifically liquid fuels such as heavy oil, gaseous fuels such as LPG, etc. as fuel. The combustion flame can be obtained by burning a mixed gas of fossil fuel and oxygen.

[0080] However, in the combustion heating of the burner, a large amount of water is mixed into the molten glass, so the β-OH value of the glass substrate is easy to rise. For this reason, as a method for industrially manufacturing the glass substrate of the present invention, it is preferred to perform energized heating using a heating electrode on a glass batch. In this way, by energizing the heating electrode provided on the wall of the melting furnace, the temperature of the molten glass decreases from the bottom surface of the melting furnace toward the upper surface of the melting furnace, so that on the liquid surface of the molten glass in the melting furnace, there are a large number of solid-state glass batches. As a result, the water attached to the solid-state glass batch evaporates, which can suppress the increase in the amount of water caused by the raw materials. In addition, if energized heating is performed using a heating electrode, while the energy per unit mass used to obtain the molten glass is reduced, the molten volatiles decrease, thereby reducing the environmental load.

[0081] As a method for industrially manufacturing the glass substrate of the present invention, it is more preferred to use a heating electrode for energizing heating without using a burner for heating. If a burner is used for heating, the moisture generated when the fossil fuel is burned is easily mixed into the molten glass. Therefore, when a burner is not used for heating, it is easy to reduce the β-OH value of the molten glass. It should be noted that "using a heating electrode for energizing heating without using a burner for heating" means that the glass batch is continuously melted by only using a heating electrode for energizing heating, but the following situations are excluded: for example, when a burner is used for heating when the melting furnace is started, the burner is used for local and auxiliary heating of a specific part of the melting furnace.

[0082] The energized heating by the heating electrode is preferably performed by applying an AC voltage to the heating electrode disposed at the bottom or side of the melting furnace in a manner that the heating electrode contacts the molten glass in the melting furnace. The material used for the heating electrode preferably has heat resistance and corrosion resistance to the molten glass, and for example, tin oxide, molybdenum, platinum, rhodium, etc. can be used. In particular, molybdenum has high heat resistance and a high degree of freedom in being disposed in the melting furnace, so it is preferred.

[0083] Low-alkali glass has a high resistivity due to the low content of alkali metal oxides. Therefore, when the electric heating performed by the heating electrode is applied to the low-alkali glass, the current not only flows through the molten glass but also flows through the refractory material constituting the melting furnace, so that the refractory material may be damaged faster. In order to prevent the above situation, as the refractory material in the furnace, it is preferred to use a zirconia refractory material with high resistivity, and zirconia electrocasting bricks are particularly preferred. In addition, as mentioned above, it is also preferred to introduce a small amount of components (Li2O, Na2O, K2O, Fe2O3, etc.) that reduce the resistivity into the molten glass. It should be noted that the content of ZrO2 in the zirconia refractory material is preferably 85% by mass or more, especially 90% by mass or more.

[0084] Example

[0085] Hereinafter, the present invention will be described based on examples. However, the following examples are only illustrative. The present invention is not limited to the following examples in any way.

[0086] Table 2 shows Examples (Sample Nos. 1 to 6) and Comparative Examples (Sample Nos. 7 to 9) of the present invention.

[0087] [Table 2]

[0088]

[0089] First, in order to obtain molten glass according to the glass composition and β-OH value in the table, the prepared glass batch was put into a small test melting furnace constructed of zirconium oxide electrocasting bricks, and then heated by electric heating using molybdenum electrodes instead of the combustion flame of the burner, so as to melt at 1600-1650°C. It should be noted that for samples No. 1 to 6, the burner was used only when the melting furnace started to operate, and the burner was stopped after the molten glass was generated. For samples No. 7 to 9, the melting was performed by heating by the combustion flame of the oxygen burner and electric heating by the heating electrode at the same time. Next, the molten glass was clarified and stirred using a Pt-Rh container, and then supplied to a zircon formed body, and formed into a flat plate shape with a thickness of 0.5 mm using an overflow down-draw method. The obtained glass substrate was evaluated for its β-OH value, thermal shrinkage, and estimated viscosity Logη at 500°C. 500 , strain point Ps, annealing point Ta, softening point Ts, 10 4.0 Temperature at a viscosity of 10 3.0 Temperature at a viscosity of 10 2.5 The temperature at which the viscosity is poise, the liquidus temperature TL, the viscosity at the liquidus temperature logηTL and the A value.

[0090] Estimated viscosity at 500°C Logη 500 It is the value calculated by the above-mentioned formula 1.

[0091] The A value is a value calculated from the above-mentioned formula 2.

[0092] The thermal shrinkage rate is a value calculated as follows. First, after a linear mark is made at a specified position on the sample, the sample is folded vertically relative to the mark and divided into two glass sheets. Next, only one of the glass sheets is subjected to a specified heat treatment (heating from room temperature at a rate of 5°C / min, holding at 500°C for 1 hour, and cooling at a rate of 5°C / min). Then, the glass sheets that have been heat-treated and the glass sheets that have not been heat-treated are arranged, and after fixing the two with adhesive tape T, the offset of the mark is measured. When the offset of the mark is ΔL and the length of the sample before heat treatment is L0, the thermal shrinkage rate is calculated using the formula ΔL / L0 (unit: ppm).

[0093] The β-OH value is a value calculated from the above-mentioned formula 3 using FT-IR.

[0094] The strain point Ps, annealing point Ta, and softening point Ts are values ​​measured according to the methods of ASTM C336 and ASTM C338.

[0095] High temperature viscosity 10 4.0 mooring, 10 3.0 mooring, 10 2.5The temperature under the water was measured by the platinum ball pulling method.

[0096] The liquidus temperature TL is the value obtained by measuring the temperature at which crystals are precipitated after the glass powder remaining in the 50-mesh (300-μm) standard sieve is passed through a 30-mesh (500-μm) standard sieve in a platinum boat and then kept in a temperature gradient furnace for 24 hours. The viscosity at the liquidus temperature log η TL is the value measured by the platinum ball pulling method.

[0097] As shown in Table 2, the estimated viscosity Logη of samples No. 1 to 6 at 500°C is 500 High, high temperature viscosity 10 2.5 The temperature under the sway is low, so the heat shrinkage is small and the productivity is high. On the other hand, sample No. 7 has a high temperature viscosity of 10 2.5 The temperature under the water is high, so the productivity is low. Sample No. 8 and 9 have an estimated viscosity Logη at 500°C. 500 Low, so the thermal shrinkage is large.

[0098] Industrial Applicability

[0099] The glass substrate of the present invention is suitable for use as a substrate for flat panel displays such as liquid crystal displays and organic EL displays, as well as cover glass for image sensors such as charge coupled devices (CCDs) and equal magnification contact solid-state imaging elements (CISs), substrates and cover glass for solar cells, and substrates for organic EL lighting.

Claims

1. A glass substrate, characterized in that: The content of Al2O3 in the glass composition is 18% to 22% by mass, the content of Li2O+Na2O+K2O is 0 to less than 1%, and the high temperature viscosity is 10 2.5 The temperature under the water is 1670°C or less, and the estimated viscosity Logη at 500°C is calculated by the following formula 500 is 26.0 or above, Logη 500 =0.167×Ps-0.015×Ta-0.062×Ts-18.5 Ps: strain point (℃) Ta: Annealing point (℃) Ts: softening point (°C).

2. The glass substrate according to claim 1, wherein: The A value calculated by the following formula is 25.0 or more, A value = Logη 500 -[β-OH value (mm -1 )]×[B2O3(mass %)].

3. The glass substrate according to claim 1 or 2, characterized in that: The β-OH value is 0.20 / mm or less.

4. The glass substrate according to claim 1 or 2, characterized in that: The β-OH value is 0.15 / mm or less.

5. The glass substrate according to claim 1 or 2, characterized in that: The content of B2O3 is less than 2.0 mass %.

6. The glass substrate according to claim 1 or 2, characterized in that: As for the glass composition, in terms of mass%, it contains 55-65% SiO2, 18-22% Al2O3, 0-1% B2O3, 0 to less than 0.1% Li2O+Na2O+K2O, 1 to 6% MgO, 2 to 8% CaO, 0 to 2% SrO, 4 to 13% BaO, 0 to less than 0.010% As2O3, and 0 to less than 0.010% Sb2O3.

7. The glass substrate according to claim 1 or 2, characterized in that: The content of Fe2O3 in the glass composition is 0.003 mass % to 0.010 mass %.

8. The glass substrate according to claim 1 or 2, characterized in that: The liquidus temperature is below 1300°C.

9. The glass substrate according to claim 1 or 2, characterized in that: A formed confluence surface is provided at the center of the plate thickness.

10. The glass substrate according to claim 1 or 2, characterized in that: The glass substrate is used for a substrate of an organic EL device.

11. The glass substrate according to claim 1 or 2, characterized in that: The content of RO in the glass composition is 14 mass % to 20 mass %, wherein the content of RO is the total amount of MgO, CaO, SrO, and BaO.

12. The glass substrate according to claim 2, wherein: The A value calculated by the above formula is 30.0 to 40.

0.

13. The glass substrate according to claim 1 or 2, characterized in that: The content of B2O3 in the glass composition is 1.5% by mass to 2% by mass.

14. The glass substrate according to claim 1 or 2, characterized in that: The content of SiO2 in the glass composition is 55 mass % to 65 mass %, the content of B2O3 is 1.5 mass % to 2 mass %, and the content of CaO is 2 mass % to 6.3 mass %.

15. The glass substrate according to claim 1 or 2, characterized in that: The content of Al2O3 in the glass composition is 18.1 mass % to 22 mass %.

16. The glass substrate according to claim 1 or 2, characterized in that: High temperature viscosity 10 2.5 The temperature under the suspension is below 1650°C.

17. The glass substrate according to claim 1 or 2, characterized in that: High temperature viscosity 10 2.5 The temperature under the water is below 1640°C.

18. The glass substrate according to claim 1 or 2, characterized in that: High temperature viscosity 10 2.5 The temperature under the water is below 1630°C.

19. The glass substrate according to claim 1 or 2, characterized in that: The strain point is 700°C or higher.

20. The glass substrate according to claim 1 or 2, characterized in that: The strain point is 720°C or higher.

21. The glass substrate according to claim 1 or 2, characterized in that: The strain point is 730°C or higher.

22. The glass substrate according to claim 1 or 2, characterized in that: The strain point is 740°C or higher.

23. The glass substrate according to claim 1 or 2, characterized in that: The strain point is 750°C or higher.

Citation Information

Patent Citations

  • Non-alkali glass

    CN105452182A

  • Alkali-free glass

    JP2016113361A