Negative electrode sheet baking process, negative electrode sheet and lithium battery

By uniformly baking the single-layer negative electrode strip, the problem of uneven heating during the baking of the negative electrode roll is solved, the thickness consistency and internal stress release of the negative electrode sheet are improved, the cycle performance of the lithium battery is enhanced, and the production cost is reduced. cost.

CN115275112BActive Publication Date: 2024-10-18EVE POWER CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202210912181.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-07-29
Publication Date
2024-10-18
Estimated Expiration
2042-07-29

AI Technical Summary

Technical Problem

In the existing baking process of negative electrode sheets of lithium batteries, the inner and outer layers of the negative electrode roll are heated unevenly, resulting in poor baking effect and poor consistency in thickness and internal stress of the negative electrode sheets, which affects the cycle performance of lithium batteries.

Method used

The process of baking a single-layer negative electrode belt is adopted. By unwinding on the coating machine, balancing the roller, setting the ear pad height ring, and adjusting the oven temperature and belt conveying speed, it is ensured that the negative electrode belt is heated evenly during the baking process. , to achieve thickness consistency of the negative electrode sheet and uniform release of internal stress.

Benefits of technology

It improves the consistency of thickness rebound and internal stress release of the negative electrode sheet, reduces the rate of tab misalignment, enhances the cycle stability performance of lithium batteries, and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115275112B_ABST
    Figure CN115275112B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of lithium battery preparation, and discloses a negative electrode sheet baking process, a negative electrode sheet and a lithium battery, wherein the negative electrode sheet baking process comprises the following steps: S1: providing a rolled negative electrode coil, and loading the negative electrode coil in a coating machine; S2: unwinding the negative electrode coil, so that the negative electrode tape enters an oven; S3: adjusting the oven temperature and the tape speed, and baking the negative electrode tape; S4: unloading, die-cutting and slitting the baked negative electrode tape to obtain the negative electrode sheet. Through the negative electrode sheet baking process of the present invention, the negative electrode sheet is evenly heated and stressed at each position during the baking operation, so that the internal stress of the negative electrode sheet is evenly released and the thickness rebounds fully, the thickness consistency of the baked negative electrode sheet is high, and the misalignment rate of the tabs caused by uneven thickness is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium battery preparation, and in particular to a negative electrode sheet baking process, a negative electrode sheet and a lithium battery. Background Art

[0002] In the production process of lithium-ion batteries, pole piece manufacturing belongs to the front-end process and occupies an important position in the whole process. The quality of pole pieces is related to the progress of the middle-stage assembly process of lithium batteries, and also affects the back-end and the electrochemical performance of lithium batteries.

[0003] A baking process is added to the negative electrode sheet of the lithium-ion battery after rolling (rolling → electrode sheet baking → die-cutting). On the one hand, the baking process maximizes the thickness rebound rate of the negative electrode sheet before winding after rolling, thereby completely releasing the physical internal stress between the negative electrode material particles after rolling, eliminating the rebound of the thickness of the negative electrode sheet caused by the physical internal stress when the battery is charging, ensuring a closer contact between the positive and negative electrode sheets, shortening the lithium ion migration path, and thus improving the battery's cycle performance. On the other hand, the full rebound of the thickness of the negative electrode sheet after rolling can effectively increase the porosity of the negative electrode sheet, thereby improving the electrolyte infiltration effect, and effectively solving the reaction heat caused by insufficient electrolyte infiltration during the charge and discharge process, thereby improving the battery's cycle performance.

[0004] At present, the baking process in the industry mainly winds the negative electrode sheets into negative electrode coils. However, when the required electrode sheets are long and have more core layers, the inner and outer electrode sheets of the negative electrode coil are prone to uneven heating during the baking process, which directly leads to large differences in the baking effect, resulting in different degrees of stress release and thickness rebound of the negative electrode sheets, and poor consistency of electrode sheet thickness and internal stress. In addition, the electrode coil baking process requires the construction of a new high-temperature baking room, which increases production costs. Summary of the invention

[0005] The primary purpose of the present invention is to overcome the deficiencies in the prior art and provide a negative electrode sheet baking process, which adopts a method of baking a single-layer negative electrode strip to improve the consistency of the thickness rebound and internal stress release of the negative electrode sheet after baking.

[0006] Another object of the present invention is to provide a negative electrode sheet prepared by the above-mentioned negative electrode sheet baking process.

[0007] Another object of the present invention is to provide a lithium battery comprising the negative electrode sheet.

[0008] The objective of the present invention is achieved through the following technical solutions:

[0009] A negative electrode sheet baking process, characterized in that it comprises the following steps:

[0010] S1: providing a rolled negative electrode coil, and loading the negative electrode coil into a coating machine;

[0011] S2: unwinding the negative electrode coil to allow the negative electrode tape to enter the oven;

[0012] S3: Adjust the oven temperature and the belt speed to perform baking operation;

[0013] S3: adjusting the oven temperature and the belt speed to bake the negative electrode belt;

[0014] S4: performing blanking, die-cutting and slitting operations on the baked negative electrode tape to obtain the negative electrode sheet.

[0015] Furthermore, the oven is provided with a roller, the negative electrode belt is in contact with the roller, and the balance of the roller is adjusted before the baking operation.

[0016] Furthermore, the negative electrode belt includes a coating area and a pole lug area located at one end of the coating area, and a pole lug raising ring is provided at a contact position of the roller with the pole lug area.

[0017] Furthermore, the thickness of the tab raising ring is 5 to 10 μm smaller than the thickness of the coating on one side of the negative electrode belt.

[0018] Furthermore, the tab raising ring is arranged at a position 0.5 to 2.0 mm away from the coating area.

[0019] Furthermore, the tab raising ring is obtained by winding a smooth soft tape around the roller.

[0020] Furthermore, the oven temperature is 90-110°C.

[0021] Furthermore, the length of the oven is 35 to 150 m, and the belt speed is 5 to 25 m / min.

[0022] The present invention also provides a negative electrode sheet, which is prepared by the negative electrode sheet baking process and has good thickness consistency.

[0023] Finally, the present invention also provides a lithium battery using the negative electrode sheet, and the lithium battery has good cycle stability performance.

[0024] Compared with the prior art, the present invention has at least the following advantages:

[0025] 1. The negative electrode sheet baking process provided by the present invention is different from the traditional method of directly using the negative electrode coil for baking. Instead, the negative electrode coil is unwound by equipment and then the negative electrode tape is transferred to an oven for baking. Through the baking process of the present invention, each position of the negative electrode sheet is heated and stressed uniformly, so that the internal stress of the negative electrode sheet is evenly released and the electrode sheet rebounds fully. The thickness consistency of the negative electrode sheet after baking is high, and the tab misalignment rate caused by uneven thickness is reduced.

[0026] 2. The negative electrode sheet baking process provided by the present invention can be directly carried out using existing coating equipment, without the need to purchase new equipment or build a high-temperature baking room. The cost is low and it is suitable for industrial promotion and application. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is a process flow chart of baking the negative electrode sheet of Example 1 of the present invention. DETAILED DESCRIPTION

[0028] In order to facilitate the understanding of the present invention, the present invention will be described more fully below with reference to the relevant drawings. The preferred embodiments of the present invention are given in the drawings. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present invention more thoroughly understood.

[0029] Traditionally, the entire negative electrode roll is sent into an oven for drying. As mentioned above, the negative electrode sheets in the inner and outer layers of the negative electrode roll are not heated evenly, which easily leads to poor consistency in thickness of the negative electrode sheets after final baking. The problem of uneven thickness has a greater impact on wound lithium batteries. The preparation of wound lithium batteries requires a winding process, in which the thickness of the core package increases by one unit (2 layers of diaphragm, one layer of positive electrode, and one layer of negative electrode) for each additional layer. The thickness of the positive electrode sheet and the diaphragm is basically a fixed value, while the negative electrode sheet is prone to not fully release the internal stress. The thickness of the negative electrode sheet wound in different time periods fluctuates greatly, resulting in different thickness of the core package for each additional layer during winding, resulting in poor thickness consistency. At the same time, the position of the pole ear is fixed after the pole sheet is die-cut. When the thickness is thick, the pole ear will shift against the winding direction. When the thickness is thin, the pole ear will shift along the winding direction, causing the pole ear to be misaligned. Only when the thickness of the negative electrode sheet is stable can the consistency of the thickness of the winding core package be improved and the misalignment of the pole ear be reduced.

[0030] Therefore, the thickness consistency of the negative electrode sheet is a key factor affecting the performance of the lithium battery. In order to improve the thickness consistency of the negative electrode sheet, the present invention provides a negative electrode sheet baking process, which abandons the traditional process of baking the entire negative electrode coil, and adopts the method of uniformly baking the single-layer negative electrode tape after unwinding the negative electrode coil. High temperature acceleration is used to ensure that the negative electrode sheet has reached the maximum rebound value during winding, so that the internal stress of the negative electrode sheet is evenly released and the electrode sheet rebounds fully, thereby improving the thickness consistency of the negative electrode sheet, thereby improving the thickness consistency of the winding core package and reducing the misalignment of the pole ear.

[0031] See also Figure 1 The negative electrode sheet baking process provided by the present invention comprises the following steps:

[0032] S1: providing a rolled negative electrode coil, and performing a feeding operation on the negative electrode coil on a coating machine.

[0033] It should be noted that the existing coating machine generally includes an unwinding mechanism, a guiding / tension adjusting mechanism, a coating mechanism, a drying mechanism, and a winding mechanism. Multiple mechanisms work together to achieve the coating and drying of the electrode sheet. In this application, the existing coating machine is used to realize the negative electrode sheet baking process. Compared with the existing negative electrode coil baking, which requires the purchase of new equipment and the construction of a high-temperature baking room, it has the characteristics of low cost and is conducive to promotion. In the process of using a coating machine to bake the rolled negative electrode coil, the unwinding mechanism and the winding mechanism are located at both ends of the drying mechanism. Under the driving action of the unwinding mechanism and the winding mechanism, the transmission of the negative electrode tape in the drying mechanism is realized; the guiding mechanism is generally composed of a number of rollers, and the rollers are related to the running direction, balance and electrode tension of the negative electrode tape; the drying mechanism and the oven need to have a heating function and a heating channel of a certain length.

[0034] In step S1, the loading operation includes transporting the rolled negative electrode coil to the unwinding mechanism and then threading the negative electrode tape.

[0035] S2: unwinding the negative electrode coil to allow the negative electrode tape to enter an oven.

[0036] Furthermore, the oven is provided with a roller, the negative electrode belt is in contact with the roller, and the balance of the roller is adjusted before the baking operation.

[0037] It should be noted that generally, the oven is equipped with several rollers. The negative electrode tape is stably transmitted under the guidance of the rollers. Before the baking operation, the balance of the rollers is adjusted to prevent uneven tension in different areas of the negative electrode tape during the tape feeding process due to the tilt of the rollers, and to avoid deformation of the negative electrode tape due to uneven tension, thereby affecting the final yield of the negative electrode sheet.

[0038] The balance adjustment includes the following steps: parallelism adjustment is performed by adjusting the horizontal adjustment screw on the left side of the roller, and the bubble of the level is adjusted to the center position, that is, parallel. If the bubble is centered, no adjustment is required; if the bubble is offset to the left, the adjustment screw is adjusted to adjust the left side of the roller downward until the bubble is centered.

[0039] Furthermore, the negative electrode belt includes a coating area and a pole lug area located at one end of the coating area, and a pole lug raising ring is provided at a contact position of the roller with the pole lug area.

[0040] It should be noted that before the die-cutting and slitting processes are carried out on the negative electrode tape, the lug area is continuous and uninterrupted. Since the thickness of the coating area is thicker than that of the lug area, it is difficult for the cylindrical roller to adjust the tension of the coating area and the lug area at the same time. As a result, the lug area is easily folded and wrinkled during the baking process. Therefore, a lug heightening ring is provided at the position of the roller in contact with the lug area to reduce the height difference between the coating area and the lug area during the conveying of the negative electrode tape, thereby ensuring that the lug area is flat and free of wrinkles.

[0041] Furthermore, the thickness of the tab raising ring is 5 to 10 μm smaller than the thickness of the coating on one side of the negative electrode sheet.

[0042] It should be noted that, generally, the negative electrode sheet is coated on both sides of the current collector, and the tab is arranged between the two coatings. Therefore, during the rolling process, the height difference between the coating area and the tab area is actually the thickness of the coating on one side of the negative electrode sheet. The thickness of the tab raising ring is set to be 5 to 10 μm less than the thickness of the coating on one side of the negative electrode sheet. This can ensure that the tab is fully stretched during the rolling process to prevent wrinkling. At the same time, the thickness difference is reserved for tension release to prevent the tab from breaking due to excessive tension during the rolling process.

[0043] Furthermore, the tab raising ring is arranged at a position 0.5 to 2.0 mm away from the coating area.

[0044] It should be noted that such a setting can make the tab raising ring as close to the coating area as possible, ensuring that the root of the tab area is fully stretched, and dissolution can prevent the tab raising ring from scratching the coating area and causing the coating to fall off.

[0045] Furthermore, the tab raising ring is obtained by winding a smooth soft tape around the roller.

[0046] It should be noted that the use of a smooth soft tape to wrap the roller to prepare the tab raising pad can flexibly adjust the thickness of the tab raising ring according to the different thicknesses of the negative electrode sheets. At the same time, the use of a smooth soft tape can reduce the friction between the tab raising ring and the tab area, preventing deformation of the tab area due to the tab raising ring material being too hard and rough.

[0047] Furthermore, the smooth soft tape can be Teflon tape.

[0048] It should be noted that Teflon tape has the advantages of high strength, high temperature resistance, smooth surface, good anti-stickiness, and electrical insulation performance. Using Teflon tape to wrap around the roller to form the tab pad ring is a good choice.

[0049] Furthermore, the air outlet direction of the oven air nozzle is adjusted so that the air outlet direction is toward the coating area.

[0050] It should be noted that, in order to improve the heating uniformity inside the oven, the existing coating machine oven is generally provided with a blower mechanism. In the technical solution of the present invention, the air outlet direction of the air nozzle is adjusted, that is, the angle of the air nozzle is adjusted to tilt 30 to 60 degrees toward the coating area to avoid the air outlet blowing directly to the pole ear area, causing the pole ear to be folded and wrinkled.

[0051] S3: adjusting the oven temperature and the belt speed to bake the negative electrode belt.

[0052] Furthermore, the oven temperature is 90-110°C.

[0053] It should be noted that the oven temperature needs to be adjusted within the range of 90-110°C to prevent the temperature from being too low, which will cause the electrode to expand and contract too much and fail to fully rebound and release the internal stress. At the same time, it should also avoid the decomposition and failure of the coating auxiliary materials (CMC and SBR) due to excessive temperature, which will reduce the adhesion of the coating.

[0054] Furthermore, the length of the oven is 35 to 150 m, and the belt speed is 5 to 25 m / min.

[0055] It should be noted that the belt speed is adjusted according to the different lengths of the oven so that the time for the negative electrode belt to pass through the oven is more appropriately controlled within 1 to 5 minutes, that is, the baking time is controlled within 1 to 5 minutes.

[0056] S4: performing blanking, die-cutting and slitting operations on the baked negative electrode tape to obtain the negative electrode sheet.

[0057] It should be noted that in order to facilitate the transportation of the negative electrode tape, the baked negative electrode tape is rolled up by a winding mechanism and then unrolled, wherein die-cutting and slitting are to cut the continuous negative electrode tape into single negative electrode sheets with negative electrode tabs using specific tools and equipment.

[0058] Example 1

[0059] S1: providing a rolled negative electrode coil, and loading the negative electrode coil into a coating machine, wherein the thickness of the negative electrode sheet is 110 μm, and the thickness of the single-side coating is 50 μm;

[0060] S2: Unwinding the negative electrode coil, so that the negative electrode tape enters the oven, wherein the oven is provided with a roller, wherein a lug heightening ring is provided at the contact position of the roller with the lug area, and the lug heightening ring is obtained by winding a Teflon tape around the roller, and the height of the lug heightening ring is 40 μm and the distance from the coating area is 1 mm. Before the unwinding operation, the balance of the roller is adjusted, and the air outlet direction of the oven nozzle is adjusted to avoid the air outlet blowing directly on the lug area;

[0061] S3: The oven length is 40m, the oven temperature is adjusted to 100°C, the tape speed is controlled to 10m / min, and the negative electrode tape is baked.

[0062] S4: Cutting, die-cutting and slitting the baked negative electrode strip to obtain a number of single negative electrode sheets.

[0063] Example 2

[0064] S1: providing a rolled negative electrode coil, and loading the negative electrode coil into a coating machine, wherein the thickness of the negative electrode sheet is 110 μm, and the thickness of the coating on one side is 50 μm;

[0065] S2: Unwinding the negative electrode coil, so that the negative electrode tape enters the oven, wherein the oven is provided with a roller, wherein a lug heightening ring is provided at the contact position of the roller with the lug area, and the lug heightening ring is obtained by winding a Teflon tape around the roller, and the height of the lug heightening ring is 45 μm and the distance from the coating area is 0.5 mm. Before the unwinding operation, the balance of the roller is adjusted, and the air outlet direction of the oven nozzle is adjusted to avoid the air outlet blowing directly on the lug area;

[0066] S3: The oven length is 40m, the oven temperature is adjusted to 110°C, the tape speed is controlled to 20m / min, and the negative electrode tape is baked.

[0067] S4: Cutting, die-cutting and slitting the baked negative electrode strip to obtain a number of single negative electrode sheets.

[0068] Example 3

[0069] S1: providing a rolled negative electrode coil, and loading the negative electrode coil into a coating machine, wherein the thickness of the negative electrode sheet is 110 μm, and the thickness of the coating on one side is 50 μm;

[0070] S2: Unwinding the negative electrode coil, so that the negative electrode tape enters the oven, wherein the oven is provided with a roller, wherein a lug heightening ring is provided at the contact position of the roller with the lug area, and the lug heightening ring is obtained by winding a Teflon tape around the roller, and the height of the lug heightening ring is 48 μm and the distance from the coating area is 2 mm. Before the unwinding operation, the balance of the roller is adjusted, and the air outlet direction of the oven nozzle is adjusted to avoid the air outlet blowing directly on the lug area;

[0071] S3: The oven length is 40m, the oven temperature is adjusted to 90°C, the tape speed is controlled to 8m / min, and the negative electrode tape is baked.

[0072] S4: Cutting, die-cutting and slitting the baked negative electrode strip to obtain a number of single negative electrode sheets.

[0073] Comparative Example 1

[0074] A rolled negative electrode coil with the same number of windings as in Example 1 is provided, wherein the thickness of the negative electrode sheet is 110 μm and the thickness of the coating on one side is 50 μm. The negative electrode coil is transported to a high-temperature baking room for baking, wherein the baking temperature is 100° C. and the baking time is 4 min. After baking, die-cutting and slitting operations are performed to obtain a number of single negative electrode sheets.

[0075] Comparative Example 2

[0076] The difference between Comparative Example 2 and Example 1 is that in step S2, no tab raising ring is provided on the roller.

[0077] Comparative Example 3

[0078] The difference between Comparative Example 3 and Example 1 is that the height of the tab raising ring in step S2 is 50 μm.

[0079] Comparative Example 4

[0080] The difference between Comparative Example 4 and Example 1 is that in step S3, the oven temperature is 80° C. and the tape speed is 50 m / min.

[0081] 200 single negative electrode sheets were randomly selected from Examples 1 to 3 and Comparative Examples 1 to 4 for lug appearance inspection and thickness measurement. The specific results are shown in Table 1.

[0082] Tab appearance inspection: Observe the tabs of the negative electrode with the naked eye to see if there are any wrinkles, folds, damages or deformations. If so, it is considered defective.

[0083] Thickness measurement: Use a thickness detection device to test the thickness of the coating area of ​​the negative electrode sheet, and calculate the average thickness and standard deviation of 200 negative electrode sheets.

[0084] Table 1 Thickness of negative electrode sheets and number of bad tabs of examples and comparative examples (n=200)

[0085]

[0086]

[0087] Negative electrode sheet rebound rate = (negative electrode sheet thickness after baking - unbaked negative electrode sheet thickness - collector thickness) / unbaked negative electrode sheet thickness. In the embodiment, the collector thickness is 10 μm.

[0088] It can be seen from the data in Table 1 that after the negative electrode sheet baking process of the present invention, the rebound rate of the negative electrode sheets of Examples 1 to 3 can reach more than 14%, and the thickness consistency of the negative electrode sheets can be controlled within ±2.5μm. At the same time, by adjusting the structure of the roller during the baking process, the number of defective tabs can be kept within a certain range.

[0089] Comparative Example 1 adopts the traditional negative electrode coil baking process. It can be seen from the data that the average thickness of the negative electrode sheet of Comparative Example 1 is significantly lower than that of Example 1, the thickness rebound rate is 8.9%, and the thickness standard deviation is ±8.8μm. Obviously, after adopting the baking process provided by the present invention, the thickness consistency of the negative electrode sheet is significantly improved, and the present invention bakes the single-layer negative electrode strip, and the heat is more sufficient and uniform. Under the same baking conditions, the thickness rebound rate of the negative electrode sheet finally prepared by the present invention is improved; further, it can be seen from the number of defective tabs that after the present invention has undergone process adjustments such as roller balance adjustment, setting of tab heightening rings, and changing the wind direction of the nozzle, the number of defective tabs is not significantly improved compared with the traditional baking process.

[0090] The roller of Comparative Example 2 is not equipped with a tab raising ring, and the number of defective tabs increases significantly, indicating that the tab raising ring can reduce the height difference between the coating area and the tab area during the conveying of the negative electrode strip, and can ensure that the tab area is flat and free of wrinkles, thus significantly reducing the number of defective tabs; at the same time, it can be seen from the data of Comparative Example 3 that when the thickness of the tab raising ring is equivalent to the thickness of the coating on one side of the negative electrode sheet, and no thickness difference is reserved, it may cause excessive tension in the tab area when passing the roller, resulting in the tab breaking, which increases the final number of defective tabs.

[0091] The oven of Comparative Example 4 sets a lower baking temperature and a higher belt speed, resulting in a poor thickness rebound rate of the negative electrode sheet finally prepared. This indicates that during the baking process of the negative electrode sheet, it is necessary to adjust the parameters of the oven according to the negative electrode sheet so that the negative electrode sheet can be fully baked and the thickness rebound rate can reach the best.

[0092] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A negative electrode sheet baking process, characterized in that: The negative electrode sheet baking process comprises the following steps: S1: providing a rolled negative electrode coil and loading the negative electrode coil onto a coating machine; S2: unwinding the negative electrode coil to allow the negative electrode tape to enter the oven; S3: adjusting the oven temperature and the belt speed to bake the negative electrode belt; S4: performing blanking, die-cutting, and slitting operations on the baked negative electrode strip to obtain the negative electrode sheet; The oven is provided with a roller, the negative electrode strip contacts the roller, and the roller is balanced before the baking operation. The negative electrode strip includes a coating area and a tab area located at one end of the coating area. A tab raising ring is provided on the roller at a contact position with the tab area. The oven temperature is 90-100°C, and the belt speed is 5-25m / min; The thickness of the tab raising ring is 10 μm smaller than the thickness of the coating on one side of the negative electrode belt, and the tab raising ring is obtained by winding a smooth soft tape around the roller.

2. The negative electrode sheet baking process according to claim 1, characterized in that: The tab raising ring is arranged at a position 0.5 to 2.0 mm away from the coating area.

3. The negative electrode sheet baking process according to claim 1, characterized in that: The length of the oven is 35 to 150 m.

4. A negative electrode sheet, characterized in that: The negative electrode sheet is prepared by the negative electrode sheet baking process according to any one of claims 1 to 3.

5. A lithium battery, characterized in that: Including the negative electrode sheet according to claim 4.

Citation Information

Patent Citations

  • Pole piece drying and forming machine

    CN206619646U

  • Pole piece rolling device of lithium battery

    CN211247949U