Algaecide

By adjusting the Ln:Fe ratio in the rare earth ferrite and applying stress to the pulverization and sintering method, an anti-algae agent with excellent anti-algae effect and long-term sustainability is prepared, which solves the problem of the existing technology that the anti-algae effect decreases over time. question.

CN115279188BInactive Publication Date: 2024-10-18KYODO PRINTING CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202180020540.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-03-23
Publication Date
2024-10-18
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The anti-algae products in the prior art show a certain anti-algae effect when they are first manufactured, but it gradually decreases over time and cannot be sustained for a long time.

Method used

The composition formula of rare earth ferrite is Ln2xFe2(1-x)O3, where Ln is the rare earth element in lanthanum, praseodymium, neodymium and yttrium, x is a number above 0.55 and below 1.00, by adjusting the molar ratio of Ln:Fe In order to improve the anti-algae effect, the anti-algae agent is prepared by applying stress crushing and firing methods.

Benefits of technology

The anti-algae effect is improved and lasts for a long time, and from the perspective of environment and cost, lanthanum ferrite shows excellent anti-algae performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003840687990000081
    Figure BDA0003840687990000081
  • Figure BDA0003840687990000101
    Figure BDA0003840687990000101
Patent Text Reader

Abstract

An algaecide is represented by the following composition formula (1). 2x Fe 2(1‑x) O 3 (1) (In formula (1), Ln is a rare earth element selected from lanthanum, praseodymium, neodymium and yttrium, and x is a number greater than or equal to 0.55 and less than 1.00.)
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an algaecide. Background Art

[0002] In order to prevent the growth of algae, algaecides are used on ships, seawalls, building materials, fishing nets, etc.

[0003] As anti-algae agents that exhibit excellent anti-algae effects, organic tin compounds, cuprous oxide, quaternary ammonium compounds, etc. have been known in the past. However, from the viewpoint of environmental pollution, the use of these anti-algae agents has been gradually avoided.

[0004] In recent years, ferrite compounds have been proposed as algae-preventing agents with low environmental pollution and excellent safety. For example, Patent Document 1 discloses: an algae-preventing additive comprising an orthoferrite containing a rare earth element selected from La, Pr, Nd and Y, iron, and oxygen as the main component, an algae-preventing paint using the same, and an algae-preventing product obtained by applying the paint on the surface of a substrate. Patent Document 1 considers the algae-preventing effect related to the magnetism of the material, and explains that orthoferrite with a small coercive force and a magnetic force close to the inherent magnetic field of plants, and a rare earth oxide: Fe2O3 = 1:1 (molar ratio) is most preferred as an algae-preventing additive.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application Publication No. 2005-272320 Summary of the invention

[0008] Problem that the invention aims to solve

[0009] The anti-algae product obtained according to the technology of Patent Document 1 shows a certain anti-algae effect immediately after production. However, the effect is not sufficient, and the anti-algae effect gradually decreases with the passage of time, and the anti-algae effect cannot be sustained for a long time.

[0010] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide an algaecide or the like which has an excellent algaecide effect and a long-lasting algae-proofing effect.

[0011] Solutions for solving problems

[0012] The present invention is as follows.

[0013] <<Method 1>> An anti-algae agent represented by the following composition formula (1).

[0014] Ln 2x Fe 2(1-x) O3 (1)

[0015] (In formula (1), Ln is a rare earth element selected from lanthanum, praseodymium, neodymium and yttrium, and x is a number greater than or equal to 0.55 and less than 1.00.)

[0016] <<Aspect 2>> The anti-algae agent according to aspect 1, wherein x in the formula (1) is a number of 0.55 to 0.85.

[0017] <<Aspect 3>> The anti-algae agent according to aspect 2, wherein x in the formula (1) is a number of 0.55 to 0.75.

[0018] <<Aspect 4>> The anti-algae agent according to any one of aspects 1 to 3, wherein Ln in the formula (1) is lanthanum.

[0019] [Method 5] An anti-algae product comprising: a substrate, and an anti-algae layer on the substrate,

[0020] The anti-algae layer is a layer containing the anti-algae agent according to any one of aspects 1 to 4.

[0021] <<Method 6>> The anti-algae product according to Method 5, wherein the anti-algae layer further comprises a resin.

[0022] [Method 7] The anti-algae product according to method 5 or 6 is selected from ships, seawalls, building materials, fish nets, aquaculture nets, water tanks, pools, swimming lane ropes for pools, buoys and tiles.

[0023] <<Method 8>> An anti-algae paint comprising the anti-algae agent according to any one of Methods 1 to 4.

[0024] <<Method 9>> The anti-algae coating according to Method 8, which also contains a resin and a solvent.

[0025] Effects of the Invention

[0026] According to the present invention, there are provided an algae-control agent and the like which have excellent algae-control effects and which have long-lasting algae-control effects. DETAILED DESCRIPTION

[0027] 《Algaecide》

[0028] The algae control agent of the present invention is

[0029] An anti-algae agent represented by the following composition formula (1).

[0030] Ln 2x Fe 2(1-x) O3(1)

[0031] (In formula (1), Ln is a rare earth element selected from lanthanum, praseodymium, neodymium and yttrium, and x is a number greater than or equal to 0.55 and less than 1.00.)

[0032] The inventors of the present invention have conducted detailed studies on the composition of rare earth ferrite and its anti-algae effect. As a result, they have found that by setting the Ln:Fe ratio in the rare earth ferrite to a rare earth-rich region higher than 1:1 (molar ratio), the anti-algae effect is improved and the duration of the effect is prolonged, thereby completing the present invention.

[0033] In the algaecide of the present invention, x in the above composition formula (1) may be any value as long as it is greater than or equal to 0.55 and less than 1.00. For example, a solid solution having an overall uniform composition may be formed, a mixture of an LnFeO3 phase and an Ln2O3 phase may be formed, a mixture of a solid solution having a uniform composition and an LnFeO3 phase and an Ln2O3 phase may be formed, or phases other than these may be contained.

[0034] The x in the composition formula (1) may be 0.56 or more, 0.57 or more, 0.58 or more, 0.59 or more, or 0.60 or more, and may be 0.95 or less, 0.90 or less, 0.85 or less, 0.80 or less, 0.75 or less, 0.70 or less, 0.65 or less, or 0.60 or less. For example, the x in the composition formula (1) may be typically 0.55 or more and 0.75 or less.

[0035] From the viewpoint of algae prevention and cost, Ln in the composition formula (1) may be lanthanum in particular, and therefore the algae prevention agent of the present invention may be lanthanum ferrite.

[0036] The algaecide of the present invention can be produced by applying appropriate stress to a mixture containing a rare earth source and an iron source in a predetermined ratio, pulverizing and mixing, and then calcining. The stress applied here may be, for example, friction, shearing force, shear stress, impact force, etc. When such stress is applied to the mixture of the rare earth source and the iron source, for example, a method of wet pulverization in a ball mill can be used.

[0037] As the rare earth source, for example, in addition to oxides of desired rare earth elements, bastnaesite, monazite, xenotime, and the like can be used.

[0038] As the iron source, oxides such as FeO, Fe3O4, and Fe2O3; oxyhydroxides such as FeOOH, ferrihydrite, and schwertmannite; hydroxides such as Fe(OH)2 and Fe(OH)3; and the like can be used.

[0039] When the mixture of the rare earth source and the iron source is pulverized and mixed by wet pulverization, water, alcohol, or the like can be used as the liquid medium, for example.

[0040] After the mixture of the rare earth source and the iron source is crushed and mixed, the liquid medium is removed by a suitable method such as heating and drying as needed, and then sintering is performed. The sintering can be performed at a temperature of, for example, 400°C or more, 500°C or more, 600°C or more, 700°C or more, 800°C or more, 900°C or more, or 1000°C or more, and for example, 1500°C or less, 1400°C or less, 1300°C or less, 1200°C or less, 1100°C or less, or 1000°C or less, for example, 1 hour or more, 2 hours or more, 3 hours or more, 4 hours or more, 6 hours or more, 8 hours or more, 12 hours or more, or 15 hours or more, and 72 hours or less, 48 ​​hours or less, 36 hours or less, 24 hours or less, 18 hours or less, or 15 hours or less.

[0041] The surrounding atmosphere during firing may be an oxidizing atmosphere, and firing may be performed in air, for example.

[0042] After the calcination, the mixture is pulverized, classified, etc. by an appropriate method as necessary to obtain the algaecide specified in the present invention.

[0043] 《Anti-algae coating》

[0044] According to another aspect of the present invention, there is provided an anti-algae coating, which comprises the anti-algae agent described above. The anti-algae coating may further comprise a resin and a solvent in addition to the anti-algae agent of the present invention.

[0045] The resin contained in the anti-algae coating of the present invention may be, for example, acrylic resin, acrylic silicone resin, silicone resin, amino alkyd resin, epoxy resin, phenolic resin, polyurethane resin, unsaturated polyester resin, fluororesin, or the like.

[0046] The solvent contained in the anti-algae coating of the present invention can be selected from, for example, water, alcohols, ketones, aliphatic hydrocarbons, aromatic hydrocarbons, esters, and the like.

[0047] The content of the algaecide in the algaecide coating of the present invention is, in terms of the ratio of the algaecide to the total of the resin and the algaecide in the coating, from the viewpoint of exhibiting high algaecide performance, for example, 1% by mass or more, preferably 2% by mass or more, more preferably 5% by mass or more, further preferably 10% by mass or more, particularly preferably 20% by mass or more, and particularly preferably 30% by mass or more, and from the viewpoint of obtaining good coating properties, for example, 80% by mass or less, preferably 70% by mass or less, more preferably 60% by mass or less, further preferably 50% by mass or less, particularly preferably 30% by mass or less, and particularly preferably 20% by mass or less or 15% by mass or less.

[0048] The anti-algae coating of the present invention can be prepared, for example, by mixing a commercially available synthetic resin coating and the anti-algae agent of the present invention at a predetermined ratio.

[0049] The anti-algae coating of the present invention can be used not only to form the anti-algae layer in the anti-algae product described below, but also as a joint material (a filling material for gaps between tiles, cement, bricks, etc.), a sealing material, a caulking material, an adhesive, etc.

[0050] 《Anti-algae products》

[0051] According to another aspect of the present invention, there is provided an anti-algae product.

[0052] It comprises: a substrate, and an anti-algae layer on the substrate,

[0053] The anti-algae layer is a layer containing the anti-algae agent of the present invention.

[0054] The substrate in the anti-algae product of the present invention may be any article to which anti-algae properties should be imparted.

[0055] The anti-algae layer in the anti-algae product of the present invention may be a cured product of the anti-algae coating described above. Therefore, the anti-algae layer in the anti-algae product of the present invention may contain a resin derived from the anti-algae coating in addition to the anti-algae agent of the present invention.

[0056] The thickness of the anti-algae layer may be, for example, about 1 μm or more and 1 mm or less.

[0057] The coating amount of the anti-algae layer is calculated as the dry mass per unit area after the solvent is removed, for example, 5 g / m 2 Above, 10g / m 2 Above, 15g / m 2 Above, 20g / m 2 Above, or 25g / m 2 Above, for example, 200g / m 2 Below, 150g / m 2 Below, 120g / m 2 Below, 100g / m 2 Below, 80g / m 2 Below, or 70g / m 2 the following.

[0058] The anti-algae product of the present invention can be produced, for example, by applying the anti-algae coating of the present invention to an article to be given anti-algae properties. Prior to applying the anti-algae coating, an appropriate pre-treatment agent may be applied to the article in advance. In addition, the coating film formed by applying the anti-algae coating on the article may be heated as needed to remove the solvent, cure the resin, etc.

[0059] The anti-algae product of the present invention can be, for example, ships, seawalls, building materials, fish nets, aquaculture nets, water tanks, pool walls, pool bottoms, pool lane ropes, buoys, tiles, etc.

[0060] Example

[0061] 《Example 1》

[0062] (1) Synthesis of lanthanum ferrite

[0063] In a ball mill using 10 mm Φ alumina balls as a grinding medium, 0.3 mol of La2O3, 0.4 mol of FeOOH, and water were added and ground and mixed for 5 hours. The obtained ground material was dried at 300°C for 15 hours and then ground in a rotary mill. The obtained ground material was calcined at 1000°C for 15 hours and then ground in a hammer mill to obtain lanthanum ferrite (composition formula La) with La:Fe=60:40 (molar ratio). 1.2 Fe 0.8 O3).

[0064] (2) Preparation of anti-algae coating liquid

[0065] The obtained lanthanum ferrite was mixed with a commercially available synthetic resin paint (for concrete pools, containing vinyl chloride resin), and the mixture was shaken and mixed in a paint shaker to prepare an anti-algae coating liquid. The composition of the anti-algae coating liquid was adjusted so that the mixing amount of lanthanum ferrite was 10% by mass relative to 90 parts by mass of the resin contained in the synthetic resin paint.

[0066] (3) Manufacture of anti-algae products

[0067] A polyethylene terephthalate (PET) film (thickness 50 μm) was used as a substrate, and the anti-algae coating liquid was applied on one side of the substrate using a wire rod #32, and then dried at 60°C for 2 days (48 hours) to produce an anti-algae product having an anti-algae layer on one side of the PET film. The coating amount of the anti-algae layer was 36.8 g / m 2 .

[0068] (4) Evaluation of anti-algae products

[0069] The obtained anti-algae product was cut into a 5cm×5cm square evaluation sample and hung with a string in a rectangular water tank with a bottom area of ​​25cm×20cm. In the water tank, seawater collected from the sea was poured to a depth of 10cm, so that the evaluation sample was completely submerged in the seawater. The water tank in this state was left to stand in an outdoor sunlight environment, and the state of algae attached to the coating surface was visually inspected after each specified period, and evaluated according to the following criteria. The evaluation results are shown in Table 1.

[0070] There is no algae attached to the coating surface: "-"

[0071] When the algae attachment area is less than 10% of the coating surface area: "+"

[0072] When the algae adhesion area is more than 10% and less than 50% of the area of ​​the coating surface: "++"

[0073] When the algae attachment area exceeds 50% of the coating surface area: "+++"

[0074] 《Example 2》

[0075] Lanthanum ferrite (composition formula La) with a molar ratio of La:Fe=80:20 was synthesized in the same manner as in Example 1 except that the amounts of La2O3 and FeOOH were changed to 0.4 mole parts and 0.2 mole parts, respectively. 1.6 Fe 0.4 O3), and the anti-algae coating liquid was prepared using the same, and the anti-algae product was produced. The obtained anti-algae product was evaluated in the same manner as in Example 1. The evaluation results are shown in Table 1.

[0076] Comparative Example 1

[0077] The anti-algae product was evaluated in the same manner as in Example 1 except that the PET film not coated with the anti-algae coating liquid was cut into a 5 cm×5 cm square as an evaluation sample.

[0078] 《Comparative Example 2》

[0079] The evaluation samples were prepared and evaluated in the same manner as in Example 1 except that lanthanum ferrite was not blended in the coating liquid. The evaluation results are shown in Table 1.

[0080] Comparative Examples 3 to 5

[0081] Lanthanum ferrites with different La:Fe ratios were synthesized in the same manner as in Example 1 except that the input amounts of La2O3 and FeOOH were changed as described in Table 1, and anti-algae coating liquids were prepared using the same, and anti-algae products were produced. The obtained anti-algae products were evaluated in the same manner as in Example 1. The evaluation results are shown in Table 1.

[0082] [Table 1]

[0083]

[0084] The results in Table 1 show that Comparative Examples 3 to 5 and Example 1 using lanthanum ferrite exhibit anti-algae properties compared to Comparative Examples 1 and 2 not using lanthanum ferrite. However, in the anti-algae products using lanthanum ferrite with a La:Fe ratio of 50:50 (molar ratio) or a La ratio less than that, the anti-algae properties could not be maintained for a long time (Comparative Examples 3 to 5).

[0085] In contrast, it was confirmed that in the anti-algae products of Example 1 in which the La:Fe ratio was set to 60:40 (molar ratio) and Example 2 in which the La:Fe ratio was set to 80:20 (molar ratio), no algae was observed on the coated surface even after 8 weeks, showing an excellent anti-algae effect.

[0086] 《Examples 3 to 5 and Comparative Examples 6 to 12》

[0087] Lanthanum ferrites having different La:Fe ratios were synthesized in the same manner as in Example 1 except that the amounts of La2O3 and FeOOH added were changed as shown in Table 2. Using the obtained lanthanum ferrites, an anti-algae coating liquid was prepared in the same manner as in Example 1 except that the amounts of lanthanum ferrite and resin added were changed as shown in Table 2, and an anti-algae product was prepared using the liquid. The obtained anti-algae product was evaluated in the same manner as in Example 1. The evaluation results are shown in Table 2 together with the results of Examples 1 and 2 and Comparative Examples 1 to 5.

[0088] [Table 2]

[0089]

[0090] According to Table 2, the algae-proofing product of Comparative Example 6, in which the La:Fe ratio is 42:58 (molar ratio), exhibits an algae-proofing effect similar to Comparative Examples 1 and 2, in which lanthanum ferrite is not used. In addition, the algae-proofing products of Comparative Examples 3, 7, and 8, in which the La:Fe ratio is 46:54 (molar ratio), exhibit some algae-proofing effect, but the effect is low.

[0091] On the other hand, the algae-proofing products of Comparative Examples 5, 11 and 12, in which the La:Fe ratio was 50:50 (molar ratio), showed a certain algae-proofing effect. However, at this La:Fe ratio, even if the amount of lanthanum ferrite added was increased, the algae-proofing effect of the algae-proofing products could not be maintained for a long time.

[0092] In contrast, the algae-proofing products of Examples 1, 3, and 4, in which the La:Fe ratio was 60:40 (molar ratio), exhibited excellent algae-proofing effects. It was confirmed that, compared with Comparative Examples 1 and 2 in which lanthanum ferrite was not used, even in Example 2 in which the lanthanum ferrite compounding amount in the coating liquid was 2 mass %, excellent algae-proofing effects were exhibited. In addition, from the comparison between Examples 1 and 4 and Example 3, it can be seen that if the compounding amount of lanthanum ferrite is increased, the algae-proofing effect of the algae-proofing products can be maintained for a longer period of time.

[0093] Similarly, it was confirmed that the anti-algae products of Examples 2 and 5 in which the La:Fe ratio was 80:20 (molar ratio) also exhibited an excellent anti-algae effect.

[0094] The above results confirmed that the anti-algae agent formed of the lanthanum ferrite specified in the present invention can exhibit an excellent anti-algae effect by using a small amount, and that the anti-algae effect can be maintained for a longer period of time by increasing the blending amount of the lanthanum ferrite.

Claims

1. An anti-algae agent, which is represented by the following composition formula (1): <h2 style=";text-align:left;direction:ltr">Ln<h2 style=";text-align:left;direction:ltr"> 2x <h2 style=";text-align:left;direction:ltr"> Fe<h2 style=";text-align:left;direction:ltr"> 2(1-x) <h2 style=";text-align:left;direction:ltr"> O3(1) In the formula (1), Ln is lanthanum, and x is a number of 0.55 to 0.

75.

2. An anti-algae product, comprising: a substrate, and an anti-algae layer on the substrate, The anti-algae layer is a layer containing an anti-algae agent represented by the following composition formula (1): <h2 style=";text-align:left;direction:ltr">Ln<h2 style=";text-align:left;direction:ltr"> 2x <h2 style=";text-align:left;direction:ltr"> Fe<h2 style=";text-align:left;direction:ltr"> 2(1-x) <h2 style=";text-align:left;direction:ltr"> O3(1) In the formula (1), Ln is lanthanum, and x is a number of 0.55 or more and less than 1.

00.

3. The anti-algae product according to claim 2, wherein: In the above formula (1), x is a number of 0.55 or more and 0.85 or less.

4. The anti-algae product according to claim 3, wherein: In the above formula (1), x is a number of 0.55 or more and 0.75 or less.

5. The anti-algae product according to any one of claims 2 to 4, wherein The anti-algae layer further comprises resin.

6. The anti-algae product according to any one of claims 2 to 4, which is selected from ships, seawalls, building materials, fish nets, aquaculture nets, water tanks, pools, lane ropes for pools, buoys and tiles.

7. The anti-algae product according to claim 5, which is selected from the group consisting of ships, seawalls, building materials, fish nets, aquaculture nets, water tanks, pools, lane ropes for pools, buoys and tiles.

8. An anti-algae coating, comprising an anti-algae agent represented by the following composition formula (1): <h2 style=";text-align:left;direction:ltr">Ln<h2 style=";text-align:left;direction:ltr"> 2x <h2 style=";text-align:left;direction:ltr"> Fe<h2 style=";text-align:left;direction:ltr"> 2(1-x) <h2 style=";text-align:left;direction:ltr"> O3(1) In the formula (1), Ln is lanthanum, and x is a number of 0.55 to 0.

75.

9. The anti-algae coating according to claim 8, further comprising a resin and a solvent.

Citation Information

Patent Citations

  • Algaecidal additive, method for producing the same and plastic plate and coating containing the same