Drag reducer

By using a combination of a bis-biphenylphenoxy catalyst and an activated co-catalyst to prepare C6-C14 α-olefin polymers, the problems of low efficiency and wide molecular weight distribution of Ziegler-Natta catalysts were solved, achieving efficient reduction of turbulent friction loss and improvement of fluid transport efficiency.

CN115279803BActive Publication Date: 2024-11-05DOW GLOBAL TECHNOLOGIES LLC
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202180021021.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-03-31
Filing Date
2021-03-26
Publication Date
2024-11-05
Estimated Expiration
2041-03-26

AI Technical Summary

Technical Problem

Existing Ziegler-Natta catalysts are inefficient for producing ultra-high molecular weight polymers, have a wide molecular weight distribution, and are difficult to control in terms of properties. This results in large turbulent friction losses in hydrocarbon liquid pipelines, increasing equipment and operating costs.

Method used

A polymer composed of C6-C14 α-olefin monomers was prepared by combining a bis-phenylphenoxy catalyst with an activated co-catalyst. The polymer had an absolute weight-average molecular weight greater than 1,300,000 g/mol and a narrow molecular weight distribution. The polymer was dispersed or dissolved in a liquid carrier to form a drag-reducing agent.

Benefits of technology

It significantly reduces frictional losses caused by turbulence, improves fluid transport efficiency, and reduces pressure drop, making it superior to drag reducers prepared from traditional Ziegler-Natta catalysts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003844384400000041
    Figure BDA0003844384400000041
  • Figure BDA0003844384400000051
    Figure BDA0003844384400000051
  • Figure BDA0003844384400000052
    Figure BDA0003844384400000052
Patent Text Reader

Abstract

The present disclosure provides a drag reducer. In one embodiment, the drag reducer comprises a polymer and a liquid carrier. The polymer is composed of one or more C 6 ‑C 14 The polymer comprises an α-olefin monomer. The polymer comprises a residual amount of zirconium. The polymer has an absolute weight average molecular weight (Mw) greater than 1,300,000 g / mol (Abs) ) and Mw of 1.3 to 3.0 (Abs) / Mn (Abs) .
Need to check novelty before this filing date? Find Prior Art

Description

Background Art

[0001] In the case of long distance transport of fluids, such as in oil pipelines and other hydrocarbon liquid pipelines, significant turbulence and wall friction are generated. These friction losses lead to inefficiencies, thereby increasing equipment and operating costs. Drag reducing agents (DRAs) are known, which reduce turbulence-mediated friction and eddies, thereby reducing friction losses and pressure drops in hydrocarbon liquid pipelines. Drag reducing agents are typically ultra-high molecular weight polymers (greater than 5,000,000 g / mol) that have the ability to dissolve in hydrocarbons under turbulent flow.

[0002] Ziegler-Natta catalyst systems are used to produce conventional DRAs. However, there are several disadvantages to producing ultra-high molecular weight polymers by Ziegler-Natta catalysis. Ziegler-Natta catalysis for ultra-high molecular weight polymers is inefficient because polymerization temperatures are typically low and reaction times are long in order to produce the high molecular weight polymers required for the application. In addition, the polymers typically have a broad molecular weight distribution, and the final polymer properties are typically difficult to control.

[0003] The art recognizes the need for drag reducers produced by means other than Ziegler-Natta catalysis. It is also recognized that there is a need for high molecular weight polymers having a narrow molecular weight distribution for effective drag reduction. Summary of the invention

[0004] The present disclosure provides a drag reducer. In one embodiment, the drag reducer comprises a polymer and a liquid carrier. The polymer is composed of one or more C6-C 14 The polymer comprises a residual amount of zirconium. The polymer has an absolute weight average molecular weight (Mw) greater than 1,300,000 g / mol. (Abs) ) and Mw of 1.3 to 3.0 (Abs) / Mn (Abs) . BRIEF DESCRIPTION OF THE DRAWINGS

[0005] Figure 1 is a schematic diagram of an experimental device for evaluating drag reduction according to an embodiment of the present disclosure.

[0006] Figure 2 is a schematic diagram of a pressure measurement assembly for determining the effectiveness of a drag reducer according to an embodiment of the present disclosure.

[0007] Figure 3 is a graph showing a quantitative comparison of the drag reducing performance of each drag reducer expressed as percent drag reduction (%DR).

[0008] Figure 4 is a graph showing a comparison of the percent drag reduction between a broad molecular weight distribution (MWD) octene homopolymer and a narrow MWD octene homopolymer at high molecular weight.

[0009] definition

[0010] Any reference to the Periodic Table of the Elements is to the Periodic Table as published by CRC Press, Inc., 1990-1991. A group of elements in this table is referred to by a new notation for numbering the groups.

[0011] For purposes of U.S. patent practice, the contents of any referenced patent, patent application, or publication are incorporated by reference in their entirety (or their equivalent U.S. versions are so incorporated by reference), especially with respect to definitions (to the extent not inconsistent with any definitions specifically provided in this disclosure) and common general knowledge in the art.

[0012] Numerical ranges disclosed herein include all values ​​from the lower limit to the upper limit, and include the lower limit and the upper limit. For ranges containing explicit values ​​(e.g., 1 or 2 or 3 to 5 or 6 or 7), any subrange between any two explicit values ​​is included (e.g., above range 1-7 includes subranges 1 to 2; 2 to 6; 5 to 7; 3 to 7; 5 to 6; etc.).

[0013] Unless stated to the contrary, implicit from the context, or customary in the art, all parts and percentages are based on weight and all test methods are current as of the filing date of this disclosure.

[0014] As used herein, the term "blend" or "polymer blend" is a blend of two or more polymers. The blend may or may not be miscible (not phase separated at the molecular level). The blend may or may not be phase separated. The blend may or may not contain one or more domain configurations, as determined by transmission electron spectroscopy, light scattering, x-ray scattering, and other methods known in the art.

[0015] The term "composition" refers to a mixture of materials comprising the composition, as well as reaction products and decomposition products formed from the materials of the composition.

[0016] The terms "comprising", "including", "having" and their derivatives are not intended to exclude the presence of any additional components, steps or procedures, whether or not the components, steps or procedures are specifically disclosed. For the avoidance of any doubt, unless stated to the contrary, all compositions claimed by using the term "comprising" may include any additional additives, adjuvants or compounds, whether in polymeric form or otherwise. In contrast, the term "consisting essentially of excludes any other components, steps or procedures (except those that are not essential to operability) from the scope of any subsequent statements. The term "consisting of" excludes any components, steps or procedures that are not specifically described or listed. Unless otherwise stated, the term "or" refers to the listed members individually and in any combination. The use of the singular includes the use of the plural, and vice versa.

[0017] As used herein, the term "1-hexene" is a molecule having the molecular formula C6H 12 The unsaturated hydrocarbon α-olefin whose unsaturation is at the α position. 1-Hexene has a molecular structure (A) shown below.

[0018] Structure (A)

[0019]

[0020] A "hexene polymer" is a polymer containing more than 50 weight percent (wt%) of polymerized hexene monomer (based on the total amount of polymerizable monomers) and optionally may contain at least one comonomer other than hexene (such as selected from C 2-7 α-olefins and / or C 9-12 Hexene polymers include hexene homopolymers and hexene copolymers (meaning units derived from hexene and one or more comonomers). The terms "hexene polymer" and "polyhexene" are used interchangeably.

[0021] As used herein, the term "1-octene" is a 1-octene having the molecular formula C8H 16 The unsaturated hydrocarbon α-olefin whose unsaturation is at the α position. 1-octene has a molecular structure (B) shown below.

[0022] Structure (B)

[0023]

[0024] As used herein, the term "isomers of octene" refers to isomers of the molecular formula C8H 16And the unsaturated hydrocarbon that the unsaturation (double bond) is not in the alpha position. In other words, the term "isomer of octene" is any octene except 1-octene. Non-limiting examples of octene isomers include cis-2-octene, trans-2-octene, cis-3-octene, trans-3-octene and combinations thereof, as well as cis-4-octene, trans-4-octene, branched octene isomers and combinations thereof.

[0025] An "octene polymer" is a polymer containing more than 50 weight percent (wt%) polymerized octene monomer (based on the total amount of polymerizable monomers) and optionally may contain at least one comonomer other than octene (such as selected from C 2-7 α-olefins and / or C 9-12 Octene polymers include octene homopolymers and octene copolymers (meaning units derived from octene and one or more comonomers). The terms "octene polymers" and "polyoctene" are used interchangeably.

[0026] "Polymer" is a compound prepared by polymerizing monomers of the same or different types, which provide multiple and / or repeated "units" or "monomer units" constituting the polymer in a polymerized form. Therefore, the general term polymer covers the term homopolymer, which is usually used to refer to polymers prepared from only one type of monomer, and the term copolymer, which is usually used to refer to polymers prepared from at least two types of monomers. It also covers all forms of copolymers, such as random copolymers, block copolymers, etc. The terms "ethylene / α-olefin polymer" and "octene / α-olefin polymer" represent copolymers prepared by polymerizing ethylene or octene and one or more other polymerizable α-olefin monomers, respectively, as described above. It should be noted that although polymers are usually referred to as "made of" one or more specified monomers, "based on" a specified monomer or monomer type, "containing" a specified monomer content, etc., in this context, the term "monomer" should be understood to refer to the polymerized residue of the specified monomer rather than the unpolymerized substance. Generally, the polymers herein are referred to as "units" based on the polymerized form of the corresponding monomers.

[0027] Test Method

[0028] Gel Permeation Chromatography (GPC)

[0029] The chromatographic system consists of a PolymerChar GPC-IR (Valencia, Spain) high temperature GPC chromatograph equipped with an internal IR5 infrared detector (IR5). The column oven chamber of the autosampler is set to 160 degrees Celsius, and the column chamber is set to 150 degrees Celsius. The columns used are 4 Agilent "Mixed A" 30cm 20 micron linear mixed bed columns and a 20μm pre-column. The chromatographic solvent used is 1,2,4 trichlorobenzene and contains 200ppm of butylated hydroxytoluene (BHT). The solvent source is nitrogen sparged. The injection volume used is 200 microliters, and the flow rate is 1.0 ml / min.

[0030] The GPC column set was calibrated with 21 narrow molecular weight distribution polystyrene standards ranging from 580 to 8,400,000 molecular weights and arranged in 6 "cocktail" mixtures with at least ten times intervals between individual molecular weights. Standards were purchased from Agilent Technologies. For molecular weights equal to or greater than 1,000,000, 0.025 g of polystyrene standards were prepared in 50 ml of solvent, and for molecular weights less than 1,000,000, 0.05 g of polystyrene standards were prepared in 50 ml of solvent. The polystyrene standards were dissolved at 80 degrees Celsius and gently stirred for 30 minutes. A third-order polytopic was used to fit the corresponding polystyrene equivalent calibration points.

[0031] Plate counts for the GPC column set were performed using decane (prepared as 0.04 g in 50 mL TCB and dissolved for 20 minutes under slow stirring). Plate counts (Equation 2) and symmetry (Equation 3) were measured at 200 μL injection according to the following equations:

[0032]

[0033] Where RV is the retention volume in milliliters, peak width is in milliliters, peak maximum is the maximum height of the peak, and 1 / 2 height is 1 / 2 the height of the peak maximum.

[0034]

[0035] Where RV is the retention volume in milliliters, and peak width is in milliliters, peak maximum is the maximum position of the peak, tenth height is 1 / 10 of the height of the peak maximum, and where post-peak refers to the tail of the peak with a retention volume later than the peak maximum, and where pre-peak refers to the front of the peak with a retention volume earlier than the peak maximum. The plate count of the chromatographic system should be greater than 18,000, and the symmetry should be between 0.98 and 1.22.

[0036] The samples were prepared semi-automatically using the PolymerChar "Instrument Control" software, where the target weight of the sample was set to 2 mg / ml, and the solvent (containing 200 ppm BHT) was added to a septum-covered vial previously sparged with nitrogen by the PolymerChar high temperature autosampler. The samples were dissolved at 160 degrees Celsius for 2 hours under "slow" shaking.

[0037] Based on the GPC results, the internal IR5 detector (measurement channel) of the PolymerChar GPC-IR spectrometer was used, according to Equations 4-6, using the PolymerChar GPCOne TM The software was used to calculate the Mn value of the baseline-subtracted IR chromatogram at each equidistant data collection point (i) and the polystyrene equivalent molecular weight obtained from the narrow standard calibration curve at point (i) according to Equation 1. (GPC) 、Mw (GPC) and Mz (GPC) Calculation.

[0038]

[0039]

[0040]

[0041] To monitor deviations over time, a flow rate marker (decane) was introduced into each sample via a micropump controlled by the PolymerChar GPC-IR system. This flow rate marker (FM) was used to linearly correct the pump flow rate (flow rate (nominal)) for each sample by comparing the RV of the corresponding decane peak in the sample (RV (FM sample)) with the retention volume of the decane peak in the narrow standard calibration (RV (FM calibration)). It was then assumed that any changes in the decane marker peak time were related to linear changes in the flow rate (flow rate (effective)) throughout the run. In order to facilitate the highest accuracy measured for the RV of the flow marker peak, a least squares fitting procedure was used to fit the peak of the flow marker concentration chromatogram to a quadratic equation. The first derivative of the quadratic equation was then used to solve for the true peak position. After calibrating the system based on the flow marker peak, the effective flow rate (relative to the narrow standard calibration) was calculated as Equation 7. By PolymerCharGPCOne TM The software completes the processing of the flow marker peaks. An acceptable flow rate correction is such that the effective flow rate should be within + / - 1% of the nominal flow rate.

[0042] Flow rate (effective) = flow rate (nominal) * (RV (FM calibration) / RV (FM sample)) (Equation 7)

[0043] Triple Detector GPC (TDGPC)

[0044] The chromatography system, running conditions, column setup, column calibration and calculation of conventional molecular weight moments and distributions were performed according to the methods described in Gel Permeation Chromatography (GPC).

[0045] To determine the offset of the viscometer and light scattering detectors relative to the IR5 detector, a systematic method for determining the multiple detector offset was performed in a manner consistent with that published by Balke, Mourey et al. (Mourey and Balke, Chromatography Polym. Chapter 12, (1992)) (Balke, Thitiratsakul, Lew, Cheung, Mourey, Chromatography Polym. Chapter 13, (1992)) using the PolymerChar GPCOne TM The software optimizes the triple detector log (MW and IV) results from broad homopolymer polyethylene standards (Mw / Mn>3) with the narrow standards column calibration results from the narrow standards calibration curve.

[0046] Absolute molecular weight data using PolymerChar GPCOne TM The software is obtained in a manner consistent with that published by Zimm (Zimm, BH, J. Chem. Phys., 16, 1099 (1948)) and Kratochvil (Kratochvil, P., Classical Light Scattering from Polymer Solutions, Elsevier, Oxford, NY (1987)). The total injected concentration used to determine the molecular weight is obtained based on the mass detector area and the mass detector constant, which is derived from a suitable linear polyethylene homopolymer or one of the polyethylene standards of known weight average molecular weight. The calculated molecular weight (using GPCOne TM ) is obtained using the light scattering constants from one or more of the polyethylene standards mentioned below and a refractive index concentration coefficient dn / dc of 0.104. Typically, the mass detector response (IR5) and the light scattering constant (using GPCOne TM The viscosity should be determined by a linear polyethylene standard with a molecular weight of approximately 120,000 g / mole. Viscometer calibration (using GPCOne TMDetermination) can be achieved using methods described by the manufacturer, or alternatively, by using published values ​​for appropriate linear standards. Calculation of viscometer constants (using GPCOne TM The specific viscosity area (DV) and injected mass of the calibration standard are related to its intrinsic viscosity. The chromatographic concentration is assumed to be low enough to eliminate the effect of resolving the second viral coefficient (the effect of concentration on molecular weight).

[0047] Absolute weight average molecular weight (Mw (Abs) )Yes (Using GPCOne TM ) is obtained by dividing the area of ​​the light scattering (LS) integrated chromatogram (calculated from the light scattering constant) by the mass recovered from the mass constant and the mass detector (IR5) area. Molecular weight and intrinsic viscosity responses are at the end of the chromatogram where the signal-to-noise ratio becomes low (using GPCOne TM ) linear extrapolation. Other corresponding moments Mn (Abs) and Mz (Abs) The calculations based on equations 8 to 9 are as follows:

[0048]

[0049]

[0050] Residual amount of catalyst metal. The "residual amount" of catalyst metal (Ti, Hf, Zr and Ge) is 0 ppm or more to less than 300 ppm and is determined by a mass balance based on the amount of catalyst added and the amount of polymer formed during the reaction. The results are reported in parts per million (ppm).

[0051] Viscosity. The viscosity was measured at a shear rate of 0.01-100 l / sec using the viscosity steady state method using an Anton Paar MCR102 equipped with a CC27 cylinder measuring system and a C-ETD300 heating system. About 20 ml of sample was added to a measuring cup and then heated to 100 ° C. The measuring system was then lowered into the sample until it reached 0.0 mm. This was done over a period of time so that the force did not reach more than 15 Newtons (N). Once the measuring system reached 0.0 mm, the sample was kept at 100 ° C together with the measuring system for 10 minutes to allow the temperature to equilibrate. The results are reported in milliPascal seconds (m-Pas). DETAILED DESCRIPTION

[0052] The present disclosure provides a drag reducer. In one embodiment, the drag reducer comprises one or more C6-C 14 The polymer is composed of α-olefin monomers. The polymer contains a residual amount of zirconium and has an absolute weight average molecular weight (Mw) greater than 1,300,000 g / mol. (Abs)) and Mw of 1.3 to 3.0 (Abs) / Mn (Abs) The drag reducer also includes a liquid carrier.

[0053] As used herein, a "drag reducer" (or "DRA") is a composition that reduces friction losses caused by turbulence of a fluid. 14 A polymer, copolymer or terpolymer composed of α-olefin monomers; the polymer is dispersed in a liquid carrier or otherwise dissolved in a liquid carrier. Suitable C6-C 14 Non-limiting examples of α-olefin monomers include 1-hexene, 1-heptene, 1-octene, 1-nonene, 1-decene, 1-dodecene, 1-tetradecene, and combinations thereof.

[0054] 1. Composed of one or more C6-C 14 Polymers composed of α-olefin monomers

[0055] Make the one or more C6-C 14 The α-olefin monomers are polymerized in the presence of a bis-biphenyl phenoxy catalyst under polymerization conditions to form homopolymers, copolymers or terpolymers. As used herein, "polymerization conditions" are temperature, pressure, reactant concentrations, liquid carrier selection, chain transfer agent (CTA), reactant mixing / addition parameters, and other conditions in the polymerization reactor that promote the reaction between the reactants and the formation of the resulting polymer product, i.e., a polymer having a carbonyl group selected from C6-C 14 A homopolymer of a monomer of α-olefin, having a monomer selected from C6-C 14 A copolymer of two monomers of α-olefin or a monomer selected from C6-C 14 Terpolymers of three monomers of alpha-olefins. The polymerization can be carried out in a batch process or a continuous process in a tubular reactor, a stirred autoclave reactor, a continuous stirred tank reactor, a gas phase polymerization reactor, a slurry phase polymerization reactor, a loop reactor, an isothermal reactor, a fluidized bed gas phase reactor and combinations thereof.

[0056] Make the one or more C6-C 14 The α-olefin monomer is contacted with a bis-biphenylphenoxy catalyst (or interchangeably referred to as "BBP") under polymerization conditions. The bis-biphenylphenoxy catalyst is a metal-ligand complex having a structure as shown in Formula (I):

[0057] Formula (I):

[0058]

[0059] in

[0060] M is a metal selected from zirconium or hafnium, said metal being in a formal oxidation state of +2, +3 or +4;

[0061] n is an integer from 0 to 3, and wherein when n is 0, X is absent; and

[0062] Each X is independently a neutral, monoanionic or dianionic monodentate ligand; or two X taken together form a neutral, monoanionic or dianionic bidentate ligand; and X and n are selected in such a way that the metal-ligand complex of formula (I) is neutral overall; and

[0063] Each Z is independently O, S, N (C1-C 40 ) alkyl or P(C1-C 40 ) a hydrocarbon group; and

[0064] O is O (oxygen atom);

[0065] L is (C1-C 40 )alkylene or (C1-C 40 ) heteroalkylene, wherein the (C1-C 40 )alkylene has a moiety comprising a 1-carbon atom to a 10-carbon atom main chain connecting two Z groups in formula (I) (L is bonded to the two Z groups), or the (C1-C 40 ) heteroalkylene has a moiety comprising a 1-atom to 10-atom connecting backbone connecting two Z groups in formula (I), wherein the (C1-C 40 ) wherein each of the 1 to 10 atoms of the 1-atom to 10-atom connected main chain of the heteroalkylene group is independently a carbon atom or a heteroatom, wherein each heteroatom is independently O, S, S(O), S(O)2, Si(R C )2、Ge(R C )2. P(R C ) or N(R C ), where each R C Independently (C1-C 30 )alkyl or (C1-C 30 ) heteroalkyl; and

[0066] Each R 1-16 Selected from (C1-C 40 ) hydrocarbon group, (C1-C 40 ) heteroalkyl, Si(R C )3、Ge(R C )3. P(R C )2、N(R C )2.OR C , SR C 、NO2、CN、CF3、R C S(O),R C S(O)2、(R C )2C=N、RC C(O)O、R C OC(O),R C C(O)N(R),(R C )2NC(O), halogen atoms, hydrogen atoms and combinations thereof.

[0067] The bis-biphenylphenoxy catalyst having the structure of formula (I) can be rendered catalytically active by contacting the metal-ligand complex with an activating co-catalyst, or by combining the metal-ligand complex with an activating co-catalyst.

[0068] Non-limiting examples of suitable activating cocatalysts for use herein include alkylaluminums; polymeric or oligomeric aluminoxanes (also referred to as alumoxanes); neutral Lewis acids; and non-polymeric, non-coordinating, ion-forming compounds (including the use of such compounds under oxidizing conditions). Combinations of one or more of the foregoing activating cocatalysts and techniques are also contemplated. The term "alkylaluminum" means a monoalkylaluminum dihydride or dihalide, a dialkylaluminum hydride or halide, or a trialkylaluminum. Examples of polymeric or oligomeric aluminoxanes include methylaluminoxane, triisobutylaluminum-modified methylaluminoxane, and isobutylaluminoxane.

[0069] Non-limiting examples of suitable Lewis acid activators (cocatalysts) include those containing 1 to 3 (C1-C 20 In one embodiment, the Group 13 metal compound is tri((C1-C 20 ) alkyl) substituted aluminum, tri((C1-C 20 )alkyl)-boron compounds, tri((C1-C 10 )alkyl)aluminum, tri((C6-C 18 ) aryl) boron compounds and their halogenated (including perhalogenated) derivatives. In other embodiments, the Group 13 metal compound is tri(fluoro-substituted phenyl) borane, tri(pentafluorophenyl) borane. In some embodiments, the activating cocatalyst is tetra((C1-C 20 ) alkyl) borate or tetra((C1-C 20 )alkyl)boric acid tri((C1-C 20 As used herein, the term "ammonium" means a (C1-C 20 )alkyl)N(H)3 + or N(H)4 + The nitrogen cation, each of which (C1-C 20 ) The hydrocarbon groups, when present in two or more, may be the same or different.

[0070] Non-limiting examples of combinations of neutral Lewis acid activators (cocatalysts) include those comprising tri((C1C4)alkyl)aluminum and tri((C6C 18 In some embodiments, the present invention relates to a mixture of a neutral Lewis acid mixture and a combination of a (pentafluorophenyl) borane and a (pentafluorophenyl) borane. Other embodiments are combinations of such neutral Lewis acid mixtures with polymeric or oligomeric aluminoxanes and combinations of a single neutral Lewis acid (especially tris(pentafluorophenyl) borane) with polymeric or oligomeric aluminoxanes. The ratio of the number of moles of (metal-ligand complex):(tris(pentafluorophenyl) borane):(aluminoxane) [e.g., (Group 4 metal-ligand complex):(tris(pentafluorophenyl) borane):(aluminoxane)] is 1:1:1 to 1:10:100, and in other embodiments is 1:1:1.5 to 1:5:30.

[0071] The bis-biphenyl phenoxy catalyst having the structure of formula (I) can be activated by combining with one or more cocatalysts (e.g., a cation-forming cocatalyst, a strong Lewis acid, or a combination thereof) to form an active catalyst composition. Suitable activating cocatalysts include polymeric or oligomeric aluminoxanes (especially methylaluminoxane) and inert, compatible, non-coordinating, ion-forming compounds. Exemplary suitable cocatalysts include, but are not limited to, modified methylaluminoxane (MMAO), bis(hydrogenated tallow alkyl) methyltetrakis(pentafluorophenyl)borate (1<->)amine (i.e., [HNMe(C 18 H 37 )2][B(C6F5)4]) and a combination of the two.

[0072] One or more of the aforementioned activating co-catalysts are used in combination with each other. In one embodiment, the co-catalyst is a mixture of tri((C1-C4)hydrocarbyl)aluminum, tri((C1-C4)hydrocarbyl)borane or ammonium borate and an oligomeric or polymeric aluminoxane compound. The ratio of the total number of moles of one or more metal-ligand complexes of formula (I) to the total number of moles of one or more activating co-catalysts in the activating co-catalyst is 1:10,000 to 100:1. In some embodiments, the ratio is at least 1:5000, in some other embodiments, at least 1:1000; and 10:1 or less, and in some other embodiments, 1:1 or less. When aluminoxane is used alone as an activating co-catalyst, preferably, the number of moles of aluminoxane employed is at least 100 times the number of moles of the metal-ligand complex of formula (I). In some other embodiments, when tri(pentafluorophenyl)borane is used alone as an activating co-catalyst, the ratio of the number of moles of tri(pentafluorophenyl)borane employed to the total number of moles of the one or more metal-ligand complexes of formula (I) is 0.5: 1 to 10: 1, 1: 1 to 6: 1, or 1: 1 to 5: 1. The remaining activating co-catalyst is typically employed in a molar amount approximately equal to the total molar amount of the one or more metal-ligand complexes of formula (I).

[0073] In one embodiment, the bis-biphenylphenoxy catalyst having the structure of formula (I) includes a metal M that is zirconium.

[0074] The polymerization comprises reacting one or more C6-C 14 The α-olefin monomer is contacted with a bis-biphenyl phenoxy catalyst of formula (I) under polymerization conditions to form a C6-C 14 The polymer may be a polymer composed of α-olefin monomers. 14 A homopolymer of a monomer of an α-olefin (hereinafter referred to as "C6-C 14 α-olefin homopolymer”), having a 14 Copolymers of two monomers of α-olefins (hereinafter referred to as "C6-C 14 α-olefin copolymers") or having a copolymer selected from C6-C 14 The terpolymer of three monomers of α-olefin (hereinafter referred to as "C6-C 14 α-olefin terpolymer"). The polymer (i.e. C6-C 14 α-olefin homopolymer, C6-C 14 α-olefin copolymer or C6-C 14 The α-olefin terpolymer contains a residual amount of zirconium or hafnium and has an absolute weight average molecular weight (Mw) greater than 1,300,000 g / mol. (Abs) ) and Mw of 1.3 to 3.0 (Abs) / Mn (Abs) .

[0075] The polymer (i.e., C6-C 14 α-olefin homopolymer, C6-C 14 α-olefin copolymer or C6-C 14 The α-olefin terpolymer) contains a residual amount of hafnium or zirconium, or from greater than 0 ppm to 300 ppm of hafnium or zirconium.

[0076] In one embodiment, the bis-biphenylphenoxy catalyst is a metal-ligand complex having the following structural formula (V):

[0077] Formula (V)

[0078]

[0079] wherein Ge is germanium, Me is a methyl group, tBu is a tert-butyl group, and iPr is an isopropyl group. The polymerization conditions include making one or more C6-C 14 The α-olefin is contacted with a bis-biphenyl phenoxy catalyst of formula (V) under polymerization conditions and a polymer (i.e., C6-C 14 α-olefin homopolymer, C6-C 14 α-olefin copolymer or C6-C 14 α-olefin terpolymer). The polymer (i.e., C6-C 14 α-olefin homopolymer, C6-C 14 α-olefin copolymer or C6-C 14 α-olefin terpolymer) has one, some or all of the following properties:

[0080] (i) Mw greater than 1,300,000 g / mol to 12,000,000 g / mol, or 1,400,000 g / mol to 10,000,000 g / mol, or 1,400,000 g / mol to 9,000,000 g / mol, or 1,500,000 g / mol to 8,000,000 g / mol (Abs) ; and / or

[0081] (ii) Mw of 1.3 to 3.0, or 1.4 to 2.9, or 1.5 to 2.8, or 2.1 to 2.7, or 2.2 to 2.6 (Abs) / Mn (Abs) ; and / or

[0082] (iii) residual amounts of zirconium, or greater than 0 ppm, or from 1 ppm to less than 300 ppm, or from 10 ppm to 200 ppm, or from 15 ppm to 180 ppm, or from 20 ppm to 170 ppm, or from 30 ppm to 160 ppm of zirconium; and / or

[0083] (iv) residual amounts of germanium, or greater than 0 ppm, or 1 ppm to less than 300 ppm, or 10 ppm to 200 ppm, or 12 ppm to 150 ppm, or 14 ppm to 130 ppm, or 14 ppm to 125 ppm of germanium.

[0084] In one embodiment, the bis-biphenylphenoxy catalyst is a metal-ligand complex having the following structural formula (VI):

[0085] Formula (VI)

[0086]

[0087] Wherein Me is a methyl group and tBu is a tert-butyl group. The polymerization conditions include making one or more C6-C 14 The α-olefin is contacted with a bis-biphenyl phenoxy catalyst of formula (VI) under polymerization conditions and a polymer (i.e., C6-C 14 α-olefin homopolymer, C6-C 14 α-olefin copolymer or C6-C 14 α-olefin terpolymer). The polymer (i.e., C6-C 14 α-olefin homopolymer, C6-C 14 α-olefin copolymer or C6-C 14 α-olefin terpolymer) has one, some or all of the following properties:

[0088] (i) Mw greater than 1,300,000 g / mol to 12,000,000 g / mol, or 1,400,000 g / mol to 10,000,000 g / mol, or 1,400,000 g / mol to 9,000,000 g / mol, or 1,500,000 g / mol to 8,000,000 g / mol (Abs) ; and / or

[0089] (ii) Mw of 1.3 to 3.0, or 1.4 to 2.9, or 1.5 to 2.8, or 2.1 to 2.7, or 2.2 to 2.6 (Abs) / Mn (Abs) ; and / or

[0090] (iii) residual amounts of zirconium, or greater than 0 ppm, or 1 ppm to less than 300 ppm, or 10 ppm to 200 ppm, or 15 ppm to 180 ppm, or 20 ppm to 170 ppm, or 30 ppm to 160 ppm of zirconium (hereinafter referred to as Polymer 1).

[0091] In one embodiment, zirconium is present in a mixture of one or more C6-C 14 In the polymer composed of C6-C 14 The polymer composed of α-olefin (Polymer 1) contains 0 ppm to less than 10 ppm of titanium.

[0092] In one embodiment, the one or more C6-C 14 The α-olefin is one or more C6-C8 α-olefins, and the polymer obtained by polymerization of one or more C6-C8 α-olefins is a hexene homopolymer, a heptene homopolymer, an octene homopolymer, a hexene / heptene copolymer, a hexene / octene copolymer, a heptene / octene copolymer or a hexene / heptene / octene terpolymer. The polymer composed of one or more C6-C8 α-olefin monomers contains a residual amount of zirconium and has one, some or all of the following properties:

[0093] (i) Mw greater than 1,300,000 g / mol to 12,000,000 g / mol, or 1,400,000 g / mol to 10,000,000 g / mol, or 1,400,000 g / mol to 9,000,000 g / mol, or 1,500,000 g / mol to 8,000,000 g / mol (Abs) ; and / or

[0094] (ii) Mw of 1.3 to 3.0, or 1.4 to 2.9, or 1.5 to 2.8, or 2.1 to 2.7, or 2.2 to 2.6 (Abs) / Mn (Abs) ; and / or

[0095] (iii) residual amounts of zirconium, or greater than 0 ppm, or 1 ppm to less than 300 ppm, or 10 ppm to 200 ppm, or 15 ppm to 180 ppm, or 20 ppm to 170 ppm, or 30 ppm to 160 ppm of zirconium (hereinafter referred to as Polymer 2).

[0096] In one embodiment, zirconium is present in the polymer composed of one or more C6-C8 alpha-olefins (Polymer 2), in addition to titanium. In another embodiment, the polymer composed of one or more C6-C8 alpha-olefins (Polymer 2) contains 0 ppm to less than 10 ppm of titanium.

[0097] In one embodiment, C6-C 14 The α-olefin is an octene monomer, and the polymer obtained by polymerizing the octene monomer with the catalyst of formula (V) is an octene homopolymer. The octene homopolymer has one, some or all of the following properties:

[0098] (i) Mw greater than 1,300,000 g / mol to 12,000,000 g / mol, or 1,400,000 g / mol to 10,000,000 g / mol, or 1,400,000 g / mol to 9,000,000 g / mol, or 1,500,000 g / mol to 8,000,000 g / mol (Abs) ; and / or

[0099] (ii) Mw of 1.3 to 3.0, or 1.4 to 2.9, or 1.5 to 2.8, or 2.1 to 2.7, or 2.2 to 2.6 (Abs) / Mn (Abs) ; and / or

[0100] (iii) residual amounts of zirconium, or greater than 0 ppm, or from 1 ppm to less than 300 ppm, or from 10 ppm to 200 ppm, or from 15 ppm to 180 ppm, or from 20 ppm to 170 ppm, or from 30 ppm to 160 ppm of zirconium; and / or

[0101] (iv) a residual amount of germanium, or greater than 0 ppm, or 1 ppm to less than 300 ppm, or 10 ppm to 200 ppm, or 12 ppm to 150 ppm, or 14 ppm to 130 ppm, or 14 ppm to 125 ppm of germanium (hereinafter referred to as Polymer 3).

[0102] In one embodiment, germanium and / or zirconium are present in the octene homopolymer (Polymer 3) in addition to titanium. In other embodiments, the octene homopolymer (Polymer 3) contains 0 ppm to less than 10 ppm titanium.

[0103] In one embodiment, C6-C 14 The α-olefin is a hexene monomer, and the polymer obtained by polymerizing the hexene monomer with the catalyst of formula (V) is a hexene homopolymer. The hexene homopolymer has one, some or all of the following properties:

[0104] (i) Mw greater than 1,300,000 g / mol to 12,000,000 g / mol, or 1,400,000 g / mol to 10,000,000 g / mol, or 1,400,000 g / mol to 9,000,000 g / mol, or 1,500,000 g / mol to 8,000,000 g / mol (Abs) ; and / or

[0105] (ii) Mw of 1.3 to 3.0, or 1.4 to 2.9, or 1.5 to 2.8, or 2.1 to 2.7, or 2.2 to 2.6 (Abs) / Mn (Abs) ; and / or

[0106] (iii) residual amounts of zirconium, or from greater than 1 ppm to less than 300 ppm, or from 10 ppm to 200 ppm, or from 15 ppm to 180 ppm, or from 20 ppm to 170 ppm, or from 30 ppm to 160 ppm of zirconium; and / or

[0107] (iv) residual amounts of germanium, or greater than 0 ppm, or 1 ppm to less than 300 ppm, or 10 ppm to 200 ppm, or 12 ppm to 150 ppm, or 14 ppm to 130 ppm, or 14 ppm to 125 ppm of germanium (Polymer 4).

[0108] In one embodiment, germanium and / or zirconium are present in the hexene homopolymer (Polymer 4) in addition to titanium. In other embodiments, the hexene homopolymer (Polymer 4) contains 0 ppm to less than 10 ppm titanium.

[0109] 2. Liquid carrier

[0110] In addition to one or more C6-C 14 Polymers composed of α-olefin monomers (the polymer has a Mw greater than 1,300,000 g / mol (Abs) , Mw of 1.3 to 3.0 (Abs) / Mn (Abs) The drag reducer comprises, in addition to the polymer (e.g., 1, 2, 3, 4, 5, 6, 7, 8, 9, 11, 12, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, 31, 32, 33, 34, 35, 36, 37, 38, 39, 40, 41, 42, 43, 44, 45, 46, 47, 48, 49, 51, 52, 53, 54, 55, 56, 57, 58, 59, 61, 62, 63, 64, 65, 67, 68, 70, 71, 72, 73, 74, 75

[0111] The liquid carrier is selected to (i) disperse the polymer as a gel, suspension or slurry or (ii) dissolve the polymer.

[0112] In one embodiment, the liquid carrier is a hydrocarbon. Non-limiting examples of suitable hydrocarbons include aromatic hydrocarbons and aliphatic hydrocarbons and combinations thereof. A non-limiting example of a suitable aromatic hydrocarbon is toluene.

[0113] In one embodiment, the liquid carrier is an aliphatic hydrocarbon. An aliphatic hydrocarbon is a straight chain, branched chain or cyclic C4-C 16 or C6-C 12 Aliphatic Hydrocarbons. Non-limiting examples of suitable aliphatic hydrocarbon solvents include butane, pentane, hexane, heptane, octane, nonane, decane, undecane, dodecane, tridecane, tetradecane, pentadecane, hexadecane, and combinations thereof.

[0114] In one embodiment, the liquid carrier is a paraffin solvent, such as Isopar sold by Exxon-Mobil. TM Solvents. Non-limiting examples of suitable paraffin solvents include Isopar TM E and Isopar TM L.

[0115] 3. Drag reducer

[0116] In one embodiment, the drag reducer comprises:

[0117] (A) 10 to 80% by weight of one or more C6-C 14 Polymers composed of α-olefin monomers (the polymer has a Mw greater than 1,300,000 g / mol (Abs) , Mw of 1.3 to 3.0 (Abs) / Mn (Abs) and residual amounts of zirconium (polymer 1)); and

[0118] (B) 20 to 90 wt % of a liquid carrier.

[0119] In one embodiment, the drag reducer comprises (A) 10 wt % to 80 wt %, or 25 wt % to 45 wt % of an octene homopolymer,

[0120] The octene homopolymer has one, some or all of the following properties:

[0121] (i) Mw greater than 1,300,000 g / mol to 12,000,000 g / mol, or 1,400,000 g / mol to 10,000,000 g / mol, or 1,400,000 g / mol to 9,000,000 g / mol, or 1,500,000 g / mol to 8,000,000 g / mol (Abs) ; and / or

[0122] (ii) Mw of 1.3 to 3.0, or 1.4 to 2.9, or 1.5 to 2.8, or 2.1 to 2.7, or 2.2 to 2.6 (Abs) / Mn (Abs) ; and / or

[0123] (iii) residual amounts of germanium, or greater than 0 ppm, or 1 ppm to less than 300 ppm, or 10 ppm to 200 ppm, or 12 ppm to 150 ppm, or 14 ppm to 130 ppm, or 14 ppm to 125 ppm of germanium; and / or

[0124] (iv) residual amounts of zirconium, or greater than 0 ppm, or 1 ppm to less than 300 ppm, or 10 ppm to 200 ppm, or 15 ppm to 180 ppm, or 20 ppm to 170 ppm, or 30 ppm to 160 ppm zirconium (Polymer 3);

[0125] (B) 20 to 90 wt %, or 75 to 55 wt %, of a liquid carrier that is an aliphatic hydrocarbon; and

[0126] The drag reducer has:

[0127] (i)2.9014*10 +05 m-Pas to 3.573*10 +07 Viscosity in m-Pas.

[0128] In one embodiment, the drag reducer comprises:

[0129] (A) 10 to 80 wt. %, or 25 to 45 wt. % of a hexene homopolymer,

[0130] The hexene homopolymer has one, some or all of the following properties:

[0131] (i) Mw greater than 1,300,000 g / mol to 12,000,000 g / mol, or 1,400,000 g / mol to 10,000,000 g / mol, or 1,400,000 g / mol to 9,000,000 g / mol, or 1,500,000 g / mol to 8,000,000 g / mol (Abs) ; and / or

[0132] (ii) Mw of 1.3 to 3.0, or 1.4 to 2.9, or 1.5 to 2.8, or 2.1 to 2.7, or 2.2 to 2.6 (Abs) / Mn (Abs) ; and / or

[0133] (iii) residual amounts of germanium, or greater than 0 ppm, or 1 ppm to less than 300 ppm, or 10 ppm to 200 ppm, or 12 ppm to 150 ppm, or 14 ppm to 130 ppm, or 14 ppm to 125 ppm of germanium; and / or

[0134] (iv) residual amounts of zirconium, or greater than 0 ppm, or 1 ppm to less than 300 ppm, or 10 ppm to 200 ppm, or 15 ppm to 180 ppm, or 20 ppm to 170 ppm, or 30 ppm to 160 ppm zirconium (Polymer 4);

[0135] (B) 20 to 90 wt %, or 75 to 55 wt %, of a liquid carrier that is an aliphatic hydrocarbon; and

[0136] The viscosity of the drag reducer is 2.9014*10 +05 m-Pas to 3.573*10 +07 m-Pas.

[0137] By way of example and not limitation, some embodiments of the present disclosure will now be described in detail in the following examples.

[0138] Example

[0139] The catalysts used in the comparative samples (CS) and the inventive examples (IE) are provided in Table 1 below.

[0140] Table 1

[0141]

[0142]

[0143] A. Polymerization of 1-hexene and 1-octene

[0144] For comparative sample 1 (CS1), polymerization was carried out with Ziegler-Natta catalyst (ZN) in a 40 mL vial containing 4 mL 1-octene and 8 mL solvent (Isopar E), 4 μmol catalyst (ZN) and 5 equivalents of Et3Al (as activator) at a temperature of 23° C.-25° C. for a period of twelve hours. Then, the solvent was removed under vacuum.

[0145] CS2 was polymerized in the same manner as CS1, but the solution temperature was maintained at -35°C for a period of 48 hours during the polymerization.

[0146] For Inventive Examples 1-4 (IE1-4), a bis-biphenyl phenoxy catalyst (BBP1) was used in a reaction mixture containing 8 mL of 1-octene and 12 mL of Isopar-E (in Isopar E), 4 μmol of catalyst (BBP1) and 1.2 equivalents of RIBS-2 (R2N(H)MeB(C6F5)4, wherein R is a hydrogenated tallow alkyl (C6F5) 14–18The polymerization was carried out in a 40 mL vial containing 2-(4-(4-(2-(4-(2-(4-(2-alkyl)-1-oxo-2-yl)-4-oxo-2-yl)-1 ...

[0147] For Inventive Example 5 (IE5), a bis-biphenyl phenoxy catalyst (BBP2) was used in a reaction mixture containing 8 mL of 1-octene and 12 mL of Isopar-E (in Isopar E), 4 μmol of catalyst (BBP2) and 1.2 equivalents of RIBS-2 (R2N(H)MeB(C6F5)4, where R is a hydrogenated tallow alkyl (C6F5) 14–18 The polymerization was carried out in a 40 mL vial containing 2-(4-(4-(2-(4-(2-(4-(2-alkyl)-1-oxo-2-yl)-4-oxo-2-yl)-1 ...

[0148] For Inventive Example 6 (IE6), bis-biphenyl phenoxy catalyst (BBP1) was used in a reaction mixture containing 8 mL 1-hexene and 12 mL Isopar-E, 1 μmol-4 μmol catalyst (BBP1) and 1.2 equivalents of RIBS-2 (R2N(H)MeB(C6F5)4, where R is a hydrogenated tallow alkyl (C 14–18 The polymerization was carried out in a 40 mL vial containing 2-(4-(4-(2 ...

[0149] The properties of the resulting C6-C8 alpha-olefin homopolymers are provided in Table 2 below.

[0150] Table 2

[0151]

[0152] 1 The ppm of residual catalyst metal present in the homopolymer is based on the total weight of the homopolymer.

[0153] 2 The polymerization was carried out at -35°C.

[0154] Drag reduction test

[0155] use Figure 1 and Figure 2 The experimental apparatus shown in is used to evaluate the drag reducing performance of the drag reducer.

[0156] A one meter long, 0.25 inch diameter stainless steel pipe or "test section" was used to evaluate the drag reduction of the drag reducer. The flow rate (Q) through the test section of the pipeline was measured downstream of the test section using a Coriolis flow meter, and the pressure drop (ΔP) was measured using a differential pressure sensor across the length of the test section of the pipeline. A schematic diagram of the construction of the test section is shown in Figure 1 middle.

[0157] The flow circuit directs fluid between two pressure vessels or "paint cans" (PP1 and PP2). Liquid movement is created by a pressure differential applied between the two paint cans, which is set using nitrogen at approximately 70 psig-80 psig. Figure 1 The valve assembly shown allows fluid to shuttle back and forth between PP1 and PP2 without requiring any piping or equipment openings. Also, in the back and forth operation, the fluid flows in the same direction ( Figure 1 ) travels across the test section, allowing consistent ΔP measurements.

[0158] Each paint tank is equipped with a vent valve, pressure gauge, pressure regulator and safety valve. Nitrogen maintains a positive gauge pressure in both paint tanks to rule out any problems associated with flammable and combustible materials. The entire unit is placed in a fume hood for added safety. In addition, the PP1 is equipped with a funnel assembly, which is used to introduce liquids in the unit without the need for pipelines or equipment openings.

[0159] The pressure drop over the length of the test section was measured using a wet-wet differential pressure sensor (Omega PX459-050DWUI). The sensor was connected to the pressure taps (1m apart) at both ends of the test section using 3 / 8” diameter SS tubing - a schematic diagram of the complete assembly is shown in Figure 2 The pressure tap (blue cross) is specially designed so as not to disrupt the structure of the turbulent boundary layer, which is necessary to obtain an accurate measurement of the coefficient of friction, key to quantifying drag reduction performance. The 3 / 8 inch connection to the pressure sensor is 30 ° Bend to horizontal in order to prevent air bubbles from accumulating in the line and to allow the line to be easily emptied via valves 3-P and 4-P. Valves 1-P and 2-P are used to degas the pressure tap after the line is first filled with liquid (before the first run).

[0160] The flow rate of the liquid is measured using a Coriolis flow sensor (MicroMotion CMF050) placed downstream of the test section. A control valve is used to limit the flow rate for each run. Ideally, this device can be used in conjunction with LabVIEW to accurately regulate the flow rate to a set value. The opening of the control valve is manually set by the user using the LabVIEW software and does not utilize an automatic flow control feedback loop.

[0161] The tests were conducted in an organic liquid carrier (to simulate the hydrophobicity of crude oil). The organic liquid carrier had a lower viscosity than crude oil in order to achieve a sufficiently high flow rate (Reynolds number) in the test section so that the flow could be in a fully turbulent state. As a result, Isopar L (Exxon Mobil ISOPAR TM L fluid) as solvent (and further simulates the hydrophobicity of crude oil). The polyoctenes synthesized in vials were premixed in Isopar L, using heating and stirring to accelerate dissolution, thereby preparing concentrated solutions. Drag reduction measurements were made at polymer concentrations ranging from 10 ppm to 400 ppm; these solutions were prepared by initially introducing 2 gallons of Isopar L into the apparatus and adding increasing amounts of the polymer concentrated solution thereto. Drag reduction measurements were made on water and pure Isopar L (verification) as well as four solutions of each polyoctene.

[0162] Results and discussion

[0163] Drag reduction measurements were made using the homopolymer dissolved in Isopar L at concentrations of 10 ppm, 20 ppm, 50 ppm, 100 ppm, 200 ppm and 400 ppm.

[0164] Figure 4 A comparison of broad MWD (Comparative Sample 2) and narrow MWD (Inventive Example 2) at higher MW is shown. Here, the deviation is significantly larger; the narrow MWD polyoctenes of IE2 are consistently significantly better than the broad MWD polyoctenes of CS2: about 84% at 10 ppm, about 72% at 20 ppm, about 79% at 50 ppm, and about 42% at 100 ppm.

[0165] Drag Reduction Performance. Table 3 shows the drag reduction in % (65% theoretical maximum drag reduction).

[0166] Table 3 - Percent drag reduction in a flow loop system at various polyoctene or polyhexene dosages.

[0167] CS 1 CS 2 IE1 Internet Explorer 2 Internet Explorer 3 IE4 Internet Explorer 5 Internet Explorer 6 10ppm DRA --- 11% --- 21% --- --- 7% --- 20ppm DRA --- 15% --- 26% --- --- 10% --- 50ppm DRA 19% 27% 37% 49% 42% 35% 17% 11% 100ppm DRA 26% 40% 45% 57% 50% 53% 24% 17% 200ppm DRA 42% --- 57% 66% 62% 65% --- --- 400ppm DRA 47% --- 64% 65% 65% 65% --- ---

[0168] In all cases, the drag reducers produced using the BBP catalysts (BBP1 / BBP2) performed well and consistently outperformed those made with Ziegler-Natta catalysts. At the same molecular weight, the polyoctenes and / or polyhexenes with narrow molecular weight distributions (IE 1-6) outperformed the broad molecular weight distribution and polyoctenes comparative samples (CS 1-2).

[0169] It is particularly intended that the present disclosure is not limited to the embodiments and descriptions contained herein, but includes modifications of those embodiments including parts of the embodiments and combinations of elements of different embodiments as appear within the scope of the following claims.

Claims

1. A drag reducer, comprising: 10 to 80 wt. % of a polymer consisting of: (i) one or more C6-C 14 an α-olefin monomer, and (ii) a residual amount of a component selected from the group consisting of zirconium, germanium, and combinations thereof, the polymer having an absolute weight average molecular weight (Mw) greater than 1,300,000 g / mol (Abs) ) and Mw of 1.3 to 3.0 (Abs) / Mn (Abs) ; 20 wt % to 90 wt % of a liquid carrier; and The viscosity of the drag reducer at 100°C is 2.9014*10 +05 mPas to 3.573*10 +07 mPas.

2. The drag reducer of claim 1, wherein the polymer has 0 ppm titanium.

3. The drag reducer according to any one of claims 1 to 2, wherein the polymer has greater than 0 ppm to 300 ppm zirconium.

4. The drag reducer according to any one of claims 1 to 2, wherein the polymer has greater than 0 ppm to 300 ppm of germanium.

5. The drag reducer according to any one of claims 1 to 2, wherein the polymer is selected from the group consisting of octene homopolymers and hexene homopolymers.

6. The drag reducer according to any one of claims 1 to 2, wherein the liquid carrier is selected from the group consisting of: a linear C4-C 16 Aliphatic hydrocarbons, branched C4-C 14 Aliphatic hydrocarbons, cyclic C4-C 16 Aliphatic hydrocarbons and combinations thereof.

Citation Information

Patent Citations

  • Anti-drag composition and preparation method of anti-drag composition

    CN103030855A

  • A polyolefin composition

    CN104870488A

  • Methods for forming amorphous ultra-high molecular weight polyolefins for use as drag reducing agents

    CN1527846A

  • Process for preparing and method of using a drag reducing agent

    EP1335941A1

  • Low-viscosity drag reducer

    US20090227729A1