N-type doped germanium single crystal and wafer derived therefrom

The Czochralski crystal pulling method uses GeP as a single dopant to produce n-type doped germanium single crystals with no dislocation and a resistivity less than 10mOhm.cm, which solves the problems of complex processes and difficult resistivity control in the existing technology, and improves performance of optoelectronic devices.

CN115279955BActive Publication Date: 2024-10-29UMICORE(BE)
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202180020388.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-03-12
Publication Date
2024-10-29
Estimated Expiration
2041-03-12

AI Technical Summary

Technical Problem

It is difficult to produce dislocation-free low-resistivity n-type doped germanium single crystals with existing technology. Especially when phosphorus doping is used, the process is complicated and it is difficult to accurately control the resistivity, which affects the performance of optoelectronic devices.

Method used

Using the Czochralski crystal pulling method, germanium and phosphorus are fed into the furnace at a dopant level of 1×1018/cm3. By pulling the crystal, GeP is used as a single dopant to simplify the process and achieve more accurate resistivity predictions. , ensure that the crystal has no dislocations and the resistivity is less than 10mOhm.cm.

Benefits of technology

The combination of high n-type doping and no dislocation is achieved, which improves the performance of optoelectronic devices, simplifies the process flow, and allows more precise resistivity control, which is suitable for vertical cavity surface emitting lasers and infrared plasma sensors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003840030490000091
    Figure BDA0003840030490000091
Patent Text Reader

Abstract

The present invention relates to single-crystalline dislocation-free Ge with n-type doping and a resistivity of less than 10 mOhm.cm, characterized in that phosphorus is the only dopant. Such a crystal can be obtained by using the Czochralski crystal pulling method with GeP as the dopant.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for producing dislocation-free single crystal Ge, which is n-doped with phosphorus and has a resistivity of less than 10 mOhm.cm. It also relates to n-doped materials in the form of large-diameter bulk crystals, and wafers derived from these crystals. Background Art

[0002] Manufacturers of electronic and optoelectronic devices require commercially grown, large, uniform single crystals of semiconductor germanium, which, when sliced ​​and polished, provide a substrate for the production of microelectronic devices. The market for n-type Ge wafers is mainly used for optoelectronic devices such as vertical cavity surface emitting lasers (VCSELs) or mid-infrared plasma sensors. VCSELs are semiconductor laser diodes in which the laser beam is emitted vertically from the top surface. VCSELs are used in a variety of laser products, including computer mice, fiber-optic communications, laser printers, facial recognition, and smart glasses. Plasmonic sensors are based on the collective oscillation of free electrons and are suitable for a variety of applications, such as molecular detection.

[0003] These applications require n-type doping and low resistivity because the high electron densities achieved in these highly doped wafers enable plasmon effects in germanium films. However, dislocations often degrade performance.

[0004] On the other hand, p-type doped germanium wafers are not suitable for infrared plasma due to large plasma losses, Frigerio et al., Physical Review B 94, 085202, 2016.

[0005] Low-resistivity dislocation-free semiconductor wafers are described in US Pat. No. 7,341,787. Very low resistivities, for example below 2 mOhm.cm, are envisaged. To this end, at least two electrically active dopants belonging to the same group in the periodic table are added simultaneously. This is said to be to avoid the problem that above a certain concentration some of the dopant atoms incorporated into the semiconductor material may be electrically deactivated. Although the document mentions Si, Ge and Si-Ge alloys, it is clearly specifically aimed at doping Si. No detailed information on Ge is disclosed, in particular no source of the dopant used is disclosed.

[0006] Spitzer et al., J. Appl. Phys., 32, 1822, 1961, describe the preparation of Ge single crystals heavily doped with Sb, As and P. Resistivity well below 2 mOhm.cm is reported. Here, the phosphorus-doped samples were all obtained by pulling single crystals with calcium orthophosphate as the source. However, the use of calcium orthophosphate as a dopant necessarily prevents the obtaining of dislocation-free crystals, as shown in the following comparative examples.

[0007] US8,574,363 teaches that high doping levels in silicon-based semiconductor crystals can also be obtained by using a so-called doping chamber, which contains phosphorus, for example. The chamber is brought very close to the melt. When the temperature rises to the melting point of phosphorus, the phosphorus is released as a gas, part of which is incorporated into the melt, while the rest is lost to the environment. Therefore, this gas phase operation requires additional attention and calculations to predict the amount of phosphorus released into the melt. In the case of doping silicon with phosphorus and germanium, US8,574,363 also teaches the use of two separate chambers, one for phosphorus supplied by evaporation and the other for germanium supplied by liquefaction. US7,132,091 indicates the use of a doping chamber, the lid of which partially dissolves when it is lowered into the melt. The use of such a chamber can introduce undesirable contaminants into the melt. Summary of the invention

[0008] To this end, the present invention provides a doped n-type germanium single crystal and a wafer derived from said germanium single crystal. In a first aspect, the present invention provides an n-type doped Ge single crystal, wherein phosphorus is the sole dopant. This simplifies the process and allows for better process control, but also allows for a more accurate prediction of the resistivity of the formed ingot. The high n-type doping combined with the fact that the wafer is dislocation-free opens up the possibility of enhancing the performance of the aforementioned optoelectronic devices.

[0009] In a second aspect, the present invention provides a wafer comprising an n-type doped Ge single crystal according to the first aspect of the present invention. More specifically, the n-type doped single crystal Ge wafer comprises phosphorus as a single dopant. Such a single crystal is dislocation-free and preferably has a resistivity of less than 10 mOhm.cm.

[0010] In a third aspect, the present invention provides a method for manufacturing an n-type doped Ge single crystal according to the first aspect of the present invention, the method comprising the following steps:

[0011] - Provide Czochralski crystal pulling furnace;

[0012] - germanium and phosphorus to obtain at least 1×10 18 / cm 3 The relative amounts of dopant levels fed into the furnace; and

[0013] -Pulled crystals. DETAILED DESCRIPTION

[0014] Unless otherwise defined, all terms used to disclose the present invention, including technical and scientific terms, have the meanings commonly understood by ordinary technicians in the field to which the present invention belongs. By further guidance, term definitions are included to better understand the teachings of the present invention.

[0015] As used herein, the following terms have the following meanings:

[0016] As used herein, "a", "an", and "the" refer to both singular and plural referents unless the context clearly dictates otherwise. For example, "a compartment" refers to one or more than one compartment.

[0017] As used herein, "about" for measurable values ​​such as parameters, amounts, time periods, etc., is intended to include variations of + / -20% or less, preferably + / -10% or less, more preferably + / -5% or less, even more preferably + / -1% or less, and still more preferably + / -0.1% or less, and such variations from the specified value within this range are suitable for implementation in the disclosed invention. However, it is to be understood that the value to which the modifier "about" refers itself is also specifically disclosed.

[0018] As used herein, "comprising" is synonymous with "including" or "containing", and is an inclusive or open-ended term that specifies what follows, such as the presence of a component, and does not exclude or prevent the presence of additional unrecited components, features, elements, members, steps known in the art or disclosed herein.

[0019] Numerical ranges recited by endpoints include all numbers and fractions contained within the range, as well as the recited endpoints. All percentages are understood to be percentages by weight, abbreviated as "wt. %", unless otherwise defined or unless a different meaning is apparent to one skilled in the art from its use and the context in which it is used.

[0020] Semiconductor crystal growth according to the present invention includes heating a raw material to its melting point to generate a crystalline raw material melt, contacting the melt with a high quality seed crystal, and causing the melt to crystallize when in contact with the seed crystal. Many different methods are known for accomplishing this process. These methods include the Czochralski (Cz) method and its variant Liquid Encapsulated Czochralski (LEC) method, the Horizontal Bridgman and Bridgman-Stockbarger method (HB) and its vertical variant (VB), and the gradient solidification method (GF) and its variant vertical gradient solidification (VGF) method. Such methods are described in "Bulk Crystal Growth of Electronic, Optical and Optoelectronic Materials" (P. Clapper, Ed., John Wiley and Sons Ltd, Chichester, England, 2005).

[0021] The crystallization of the melt forms a substantially cylindrical crystal along a vertical axis with a seed crystal located below one or more crystallization feedstocks, called an ingot. The equipment necessary to form semiconductor crystals includes a crystal growth furnace, a crucible, and sometimes a crucible support.

[0022] In a first aspect, the present invention provides an n-type doped Ge single crystal in which phosphorus is the sole dopant. This simplifies the process and allows for better process control, but also allows for more accurate prediction of the resistivity of the formed ingot. The high n-type doping combined with the fact that the wafer is dislocation-free opens up the possibility of enhancing the performance of the aforementioned optoelectronic devices.

[0023] Preferably, the Ge single crystal is substantially free of dislocations. In the context of the present invention, the term "substantially free of dislocations" is interpreted as having less than 0.025 dislocations / cm 2 , preferably less than 0.005 dislocations / cm 2 , more preferably less than 0.001 dislocation / cm 2 . Most preferably, the Ge single crystal has no dislocations and is therefore dislocation-free. Dislocations present in crystals grown by the Czochralski method can be determined by etching and / or copper decoration techniques. Sources of dislocations include thermal shock due to surface damage or residual dislocations in the seed; poor seed epitaxy; the generation of plasticity in the ingot; the effects of impurity segregation. The skilled person will appreciate that the residual dislocations can be eliminated and then dislocation-free crystals can be grown, for example by the Dash necking method. In a preferred embodiment, the Ge single crystal of the present invention is produced in a procedure in which a crystal growth furnace produces an ingot without dislocations or embedded crystals. Preferably, the ingot is grown by a vertical growth method.

[0024] In a preferred embodiment, the present invention provides an n-type doped Ge single crystal, wherein the content of the dopant is at least 5×10 17 / cm 3 , preferably 5×10 17 / cm 3 Up to 2.5×10 19 / cm 3 , and the more preferred content is 1×10 18 / cm 3 Up to 2.5×10 19 / cm 3 , more preferably the content is 1×10 18 / cm 3 Up to 6×10 18 / cm 3 , or any value in between.

[0025] In a preferred embodiment, the present invention provides an n-type doped Ge single crystal, wherein the resistivity of the Ge single crystal is less than 10mOhm.cm, preferably between 1mOhm.cm and 10mOhm.cm, more preferably between 1mOhm.cm and 7mOhm.cm. Most preferably, the resistivity is between 2mOhm.cm and 6mOhm.cm, for example 2.0mOhm.cm, 3.0mOhm.cm, 4.0mOhm.cm, 5.0mOhm.cm, 6.0mOhm.cm, or any value therebetween.

[0026] The single crystal may have In a preferred embodiment, the present invention provides an n-type doped Ge single crystal, wherein the single crystal is substantially cylindrical and has a diameter of 1 cm to 50 cm, more preferably 5 cm to 35 cm. Most preferably, the diameter is about 100 mm or 4 inches, about 150 mm or 6 inches, about 200 mm or 8 inches, or about 300 mm or 12 inches, or any diameter therebetween. Preferably, the Ge single crystal is in the form of an ingot, more preferably in the form of a Czochralski grown ingot.

[0027] In a preferred embodiment, the present invention provides an n-type doped Ge single crystal, wherein the single crystal is substantially cylindrical and has a length of 1 cm to 300 cm, preferably a length of 5 cm to 200 cm, more preferably a length of 10 cm to 150 cm, for example 30 cm, 45 cm, 60 cm, 75 cm, 90 cm, 105 cm, 120 cm or 135 cm, or any length therebetween.

[0028] In a second aspect, the present invention provides a wafer comprising a Ge single crystal preferably doped n-type according to the first aspect of the present invention. More specifically, the n-doped single crystal Ge wafer comprises phosphorus as a single dopant. Such a single crystal is dislocation-free and preferably has a resistivity of less than 10mOhm.cm. Preferably, the resistivity is between 1mOhm.cm and 10mOhm.cm, more preferably between 1mOhm.cm and 7mOhm.cm. Most preferably, the resistivity is between 2mOhm.cm and 6mOhm.cm, for example 2.0mOhm.cm, 3.0mOhm.cm, 4.0mOhm.cm, 5.0mOhm.cm, 6.0mOhm.cm, or any value therebetween.

[0029] In a preferred embodiment, the present invention provides a wafer according to the second aspect of the present invention, wherein the wafer is obtained by cutting from a single crystal ingot, preferably a single crystal grown by the Czochralski method, the ingot having a diameter of 1 cm to 50 cm, more preferably a diameter of 5 cm to 35 cm. Most preferably, the diameter is about 100 mm or 4 inches, about 150 mm or 6 inches, about 200 mm or 8 inches, or about 300 mm or 12 inches, or any diameter therebetween. The length of the ingot is 1 cm to 300 cm.

[0030] In a preferred embodiment, the present invention provides a wafer according to the second aspect of the present invention, wherein the thickness of the wafer is 25 μm to 1000 μm. More preferably, the thickness of the wafer is 100 μm to 750 μm, more preferably, the thickness of the wafer is about 140 μm, 180 μm, 220 μm, 260 μm, 300 μm, 450 μm, 650 μm, or any thickness therebetween.

[0031] In a third aspect, the present invention provides a method for manufacturing an n-type doped Ge single crystal according to the first aspect of the present invention, the method comprising the following steps:

[0032] - Provide Czochralski crystal pulling furnace;

[0033] - germanium and phosphorus to obtain at least 1×10 18 / cm 3 The relative amounts of dopant levels fed into the furnace; and

[0034] -Pulled crystals.

[0035] In a preferred embodiment, the present invention provides a method according to the third aspect of the present invention, wherein phosphorus is fed into the furnace in the form of GeP.

[0036] In a preferred embodiment, the present invention provides a method according to the third aspect of the present invention, the method comprising the following additional steps:

[0037] - cutting the crystal into wafers;

[0038] - grinding the wafer with coarse sand;

[0039] - chemically-mechanically polishing the wafer;

[0040] - Cleaning the surface of the wafer.

[0041] In another aspect, the present invention provides an electronic or optoelectronic device comprising an n-doped Ge single crystal according to the first aspect of the present invention, or a wafer comprising single crystal dislocation-free Ge according to the first aspect of the present invention according to the second aspect of the present invention.

[0042] In another aspect, the present invention provides a vertical cavity surface emitting laser or an infrared plasma sensor, which comprises an n-type doped Ge single crystal according to the first aspect of the present invention - directly included or included after being cut into a size suitable for use in a vertical cavity surface emitting laser or an infrared plasma sensor, or comprises a wafer according to the second aspect of the present invention - directly included or included after being cut into a size suitable for use in a vertical cavity surface emitting laser or an infrared plasma sensor.

[0043] In another aspect, the present invention provides use of the single crystal dislocation-free Ge according to the first aspect of the present invention in a vertical cavity surface emitting laser or an infrared plasma sensor.

[0044] In other words, the present invention aims to prepare and provide single-crystalline dislocation-free Ge with n-type doping and a resistivity of less than 10 mOhm.cm, characterized in that phosphorus is the sole dopant. This simplifies the process and allows better process control, but also allows a more accurate prediction of the resistivity of the formed ingot. The high n-type doping combined with the fact that the wafer is dislocation-free opens the possibility of enhancing the performance of the aforementioned optoelectronic devices.

[0045] Another embodiment according to any of the foregoing embodiments relates to the above-mentioned dislocation-free single-crystalline Ge obtainable by supplying phosphorus in the form of GeP. This ensures that a phosphorus-doped, single-crystalline and dislocation-free product is obtained. The use of GeP as a dopant source is far superior to, for example, red or white phosphorus, which require safety precautions when handling the latter two. Furthermore, high purity GeP (99,999%) is available, minimizing the addition of undesirable impurities to the melt.

[0046] Another embodiment according to any of the preceding embodiments relates to dislocation-free single crystal Ge in the form of an ingot grown by the Czochralski method.

[0047] Another embodiment according to any of the preceding embodiments relates to dislocation-free single-crystalline Ge in the form of wafers derived from an ingot grown by the Czochralski method. Such wafers may preferably have a thickness of 140 μm to 1000 μm and a diameter of 5 cm to 35 cm.

[0048] Another embodiment according to any of the preceding embodiments relates to the use of dislocation-free single crystal Ge for vertical cavity surface emitting lasers or infrared plasma sensors.

[0049] To this end, a method was developed comprising the following steps:

[0050] - Provide Czochralski crystal pulling furnace;

[0051] - Ge and GeP to obtain at least 1×10 18 / cm 3 The relative amounts of dopant levels fed into the furnace; and

[0052] -Pulled crystals.

[0053] Optional additional steps are:

[0054] - cutting the crystal into wafers by means of a wire saw;

[0055] - grinding the wafer with coarse sand;

[0056] -Chemical-mechanical polishing;

[0057] - Cleaning the wafer surface.

[0058] The method is illustrated in the following examples. The following examples are intended to further illustrate the present invention and are in no way intended to limit the scope of the present invention.

[0059] Example

[0060] A loading of 100 kg of high purity germanium was introduced into a graphite crucible in a Czochralski furnace, to which 62.3 g of GeP as a dopant was added.

[0061] This doping level corresponds to 1×10 18 / cm 3 and 6×10 18 / cm 3 The doping levels varied between 2 and 6 mOhm.cm, corresponding to a change in resistivity between 2 and 6 mOhm.cm. This variation is due to the well-known fact that impurities segregate at solid interfaces during crystal growth. As a result, the concentration of phosphorus increases towards the tail of the crystal, resulting in a lower resistivity there.

[0062] The furnace is first heated to 1000°C in a nitrogen environment to melt the germanium. At around 725°C, germanium phosphide dissociates into solid Ge and liquid phosphorus. At 1000°C, germanium also melts and phosphorus is incorporated into the melt. When the germanium is completely melted, the furnace temperature is lowered to 950°C. After 6 hours, the temperature is stabilized, so the germanium seed crystal descends through the furnace body of the furnace until it contacts the molten pool. Then a procedure known to technicians as the "Dash necking method" is implemented to start growth. More specifically, a thin crystal with a diameter of 5 mm grows to a length of 150 mm. The crystal is then slowly pulled up at a controlled rate of 10 mm / h to increase its diameter to 150 mm. The diameter of the crystal is then stabilized by controlling the heater temperature and / or the crystal pulling rate. This stage is generally referred to as crystal body growth. The crystal pulling rate reaches about 10 mm / h.

[0063] At the end of the growth of the body, the crystal forms a tail on the crystal by steadily reducing its diameter, which separates the crystal from the melt. This procedure can be used to minimize thermal shock to help avoid dislocations. The crystal is pulled up into the body of the furnace and slowly cooled to below 50°C for 28 hours. It is then unloaded from the furnace.

[0064] The crystal was sawn into cylindrical pieces perpendicular to the crystal axis and the resistivity was measured at 6 different locations along the length of the crystal using a 4-point probe. The results are reported in Table 1.

[0065]

[0066] Table 1: Resistivity function as a function of position along the body of the crystal.

[0067] This shows that doping the germanium melt with GeP effectively produces low-resistance n-type germanium crystals with resistivity between 2 and 6 mOhm.cm. This variation in resistivity is perfectly acceptable for the intended application. Theoretical calculations further show that with these amounts of dopant added, almost all of the phosphorus atoms are electrically active within the germanium lattice.

[0068] It was then verified that a dislocation-free crystal had been obtained. This was done by etching a cross section taken from the crystal tail with a dislocation-indicating chemical. In this case, a solution consisting of 75 g of Cu(NO3)2·3H2O, 300 mL of H2O, 300 mL of HNO3 (69%) and 600 mL of HF (49%) was prepared to etch the crystal piece. The surface was then analyzed with a microscope to confirm the absence of dislocations.

[0069] Analyzing the tail of a crystal is sufficient to ensure that the crystal as a whole is dislocation-free, since dislocations created in the body of the crystal multiply and propagate toward the tail.

[0070] To obtain wafers, the crystal can be further processed as follows.

[0071] The crown and tail of the crystal are trimmed off and the crystal is subsequently ground to the desired diameter using cylindrical grinding. Flats or notches are then machined on the rounded crystal to mark the crystal orientation. Afterwards, a wire saw cuts the crystal into individual wafers. These wafers are laser marked with a unique identification code for tracking purposes. The edges of the wafers are rounded to prevent the wafers from breaking during further processing. In order to eliminate the thickness variations present after sawing, the wafer surface is ground with coarse sand. Any sub-surface damage caused by this process is removed by chemical etching. Then, chemical-mechanical polishing is performed until a mirror-like surface is obtained. The final cleaning ensures an "epitaxial-ready" surface for the growth of various epitaxial layers.

[0072] Comparative Example

[0073] In a Czochralski furnace, a crucible was filled with 2500 g of germanium and 5 g of calcium orthophosphate as a dopant. The furnace was then heated to its normal operating temperature of 1100°C. However, it was observed that a considerable portion of the dopant did not dissolve, forming particles floating on the surface of the germanium melt. The same crystal growth and analysis procedures as in the above example were implemented. Analysis of the crystals showed multiple dislocations, probably due to particle absorption near the solid-liquid interface.

[0074] It is therefore inevitable to conclude that the use of calcium orthophosphate as dopant necessarily prevents the obtaining of dislocation-free crystals.

Claims

1. An n-type doped dislocation-free Ge single crystal, wherein the resistivity of the n-type doped dislocation-free Ge single crystal is less than 10 mOhm.cm, characterized in that Phosphorus is the single dopant.

2. The n-type doped dislocation-free Ge single crystal according to claim 1, wherein the content of the dopant is 5×10 17 / cm 3 Up to 2.5×10 19 / cm 3 . 3 . The n-type doped dislocation-free Ge single crystal according to claim 1 , wherein the resistivity of the n-type doped dislocation-free Ge single crystal is 2.0 mOhm.cm to 6.0 mOhm.cm. 4 . The n-type doped dislocation-free Ge single crystal according to claim 1 , wherein the single crystal is cylindrical and has a diameter of 1 cm to 50 cm. 5 . The n-type doped dislocation-free Ge single crystal according to claim 1 , wherein the single crystal is cylindrical and has a length of 1 cm to 300 cm.

6. The n-type doped dislocation-free Ge single crystal according to claim 1 or 2, wherein the single crystal is in the form of an ingot.

7. A wafer comprising an n-type doped dislocation-free Ge single crystal, wherein the resistivity of the n-type doped dislocation-free Ge single crystal is less than 10 mOhm.cm, characterized in that Phosphorus is the single dopant. The wafer according to claim 7 , wherein the resistivity of the Ge single crystal is 2.0 mOhm.cm to 6.0 mOhm.cm. 9 . The wafer according to claim 7 , wherein the wafer has a thickness of 25 μm to 1000 μm.

10. A method for manufacturing an n-type doped dislocation-free Ge single crystal according to any one of claims 1 to 6, the method comprising the following steps: - Provide Czochralski crystal pulling furnace; - germanium and phosphorus to obtain at least 1×10 18 / cm 3 The relative amounts of dopant levels fed into the furnace; and -Pulled crystals.

11. The method of claim 10, wherein phosphorus is fed into the furnace in the form of GeP.

12. The method according to claim 10 or 11, comprising the following additional steps: - cutting the crystal into wafers; - grinding the wafer with coarse sand; - chemically-mechanically polishing the wafer; - Cleaning the surface of the wafer.

13. An electronic or optoelectronic device comprising the n-type doped Ge single crystal according to any one of claims 1 to 3. 14 . A vertical cavity surface emitting laser or an infrared plasma sensor, comprising the n-type doped Ge single crystal according to claim 1 .

15. Use of the single crystal dislocation-free Ge according to any one of claims 1 to 3 in a vertical cavity surface emitting laser or an infrared plasma sensor.

Citation Information

Patent Citations

  • Single crystal silicon ingot having a high arsenic concentration

    US7132091B2

  • Process for producing highly doped semiconductor wafers, and dislocation-free highly doped semiconductor wafers

    US7341787B2

  • Process for production of silicon single crystal, and highly doped N-type semiconductor substrate

    US8574363B2

  • Doping method for growth of germanium single crystals for solar cells

    CN102877121A

  • P-type gaas single crystal and method for producing the same

    JP2003206200A