Backfill type friction stir spot welding stirring head, spot welding device and spot welding method

By designing the nested structure of the stirring head, using rotation and reciprocating motion to generate uniform heat, the problem of uneven heat-force of the solder joints in backfill friction stir spot welding is solved, the uniformity and mechanical properties of the joint are improved, and the welding is simplified Optimization of parameters.

CN115283814BActive Publication Date: 2024-10-25NORTHWESTERN POLYTECHNICAL UNIV +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202210792363.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-07-07
Publication Date
2024-10-25
Estimated Expiration
2042-07-07

AI Technical Summary

Technical Problem

In backfill friction stir spot welding, the uneven heat-force of the solder joint leads to uneven joint structure, prone to defects, reducing the mechanical properties of the joint, and the welding process window is narrow, requiring repeated exploration and testing to optimize the welding parameters.

Method used

A mixing head including an inner compression column, a first stirring sleeve, a second mixing sleeve and an outer compression sleeve is designed. The rotation and reciprocating motion of these components generates uniform heat, softening the plates to be welded and passing through the metal. The extrusion and backfilling form a metallurgical bond to form a flat spot welded joint.

Benefits of technology

It achieves a more uniform thermal-mechanical effect at the solder joint position, reduces joint defects, improves the uniformity of the structure and performance of the spot welded joint, expands the welding process window, and simplifies the optimization process of welding parameters.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115283814B_ABST
    Figure CN115283814B_ABST
Patent Text Reader

Abstract

The present application discloses a backfill type friction stir spot welding stirring head, a spot welding device and a spot welding method. The backfill type friction stir spot welding stirring head comprises an inner compression column, a first stirring sleeve, a second stirring sleeve and an outer compression sleeve. The inner compression column is used to compress and fix the plate to be welded; the first stirring sleeve is rotatably sleeved on the outer periphery of the inner compression column, and the first stirring sleeve can also reciprocate along the axial direction of the inner compression column; the second stirring sleeve is rotatably sleeved on the outer periphery of the first stirring sleeve, and the second stirring sleeve can also reciprocate along the axial direction of the inner compression column; the outer compression sleeve is sleeved on the outer periphery of the second stirring sleeve, and the outer compression sleeve is used to compress and fix the plate to be welded. The present invention can at least solve the problem of uneven heat and force of the weld during friction welding.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of backfill friction stir spot welding, and in particular to a backfill friction stir spot welding stirring head, a spot welding device and a spot welding method. Background Art

[0002] Refill friction stir spot welding (RFSSW) is a new type of solid phase spot welding technology developed on the basis of friction stir welding (FSW) and friction stir spot welding (FSSW). The welding tool consists of a clamping ring, a sleeve and a stirring pin. The clamping ring is used to fix the workpiece and prevent the overflow of plastic materials during welding. The sleeve and the stirring pin can move up and down independently. During the welding process, the friction heat generated by the high-speed rotation of the welding tool is used to make the metal to be welded reach a viscoplastic state. Then, the reciprocating motion of the stirring pin and the sleeve is used to form a metallurgical bond through the extrusion and backfilling of the metal at the lap interface. This welding method can successfully eliminate the exit hole and obtain a spot welding joint without a keyhole. As an advanced solid phase welding technology, it can effectively avoid the inherent defects of liquid phase welding and has irreplaceable advantages in the field of spot connection of lightweight metals such as aluminum alloys and magnesium alloys.

[0003] However, the existing backfill friction stir spot welding also has the problem of uneven heat and force at the weld. Since all the heat in the spot welding process comes from the friction heat generated by the welding tool, the heat generation is related to the linear speed of the stirring needle and the sleeve. The linear speed of the outer side of the stirring needle is relatively large, the heat generation is large, and the temperature is high; the linear speed of the inner side is small, the heat generation is small, and the temperature is low. Especially at the center of the stirring needle, the linear speed is 0 during the friction process and the temperature is the lowest. This significant heat difference causes the unevenness of the joint structure, making the joint prone to various defects and reducing the mechanical properties of the joint. Therefore, the current backfill friction stir spot welding has a narrow welding process window, and repeated exploration and testing are required to obtain the optimal welding process parameters to optimize the mechanical properties of the joint. Summary of the invention

[0004] The main purpose of the present application is to provide a backfill type stir friction spot welding stirring head, a spot welding device and a spot welding method, which can solve the problem of uneven heat and force at the welding point during friction welding.

[0005] According to one aspect of an embodiment of the present application, a backfill type friction stir spot welding stirring head is provided, comprising:

[0006] An internal pressing column, which is used to press and fix the plate to be welded;

[0007] A first stirring sleeve, wherein the first stirring sleeve is rotatably sleeved on the outer periphery of the inner pressing column, and the first stirring sleeve can also reciprocate along the axial direction of the inner pressing column;

[0008] a second stirring sleeve, wherein the second stirring sleeve is rotatably sleeved on the outer periphery of the first stirring sleeve, and the second stirring sleeve can also reciprocate along the axial direction of the inner compression column; and

[0009] An outer compression sleeve is arranged on the outer periphery of the second stirring sleeve, and is used for compressing and fixing the plate to be welded.

[0010] Furthermore, a first friction reinforcing portion is provided at the bottom end and / or the side wall of the first stirring sleeve.

[0011] Furthermore, a second friction reinforcing portion is provided at the bottom end and / or the side wall of the second stirring sleeve.

[0012] Furthermore, the rotation speed of the first stirring sleeve and the second stirring sleeve is 600 rpm to 2000 rpm.

[0013] Furthermore, the speed at which the first stirring sleeve and the second stirring sleeve are pressed down and retracted along the axis of the inner pressing column is 0.5 mm / s to 2 mm / s.

[0014] Furthermore, the backfill friction stir spot welding stirring head satisfies the following formula:

[0015]

[0016] Wherein, P is the limit extrusion pressure provided by the robot arm of the backfill friction stir spot welding device, in units of Pa, P is the pressure required for the backfill friction stir spot welding stirring head to be inserted into the plate to be welded, in units of MPa, and d is the maximum diameter of the backfill friction stir spot welding stirring head, in units of mm.

[0017] Furthermore, the inner compression column, the first stirring sleeve, the second stirring sleeve and the outer compression sleeve are all made of H13 tool steel.

[0018] Furthermore, the lengths of the inner compression column, the first stirring sleeve, the second stirring sleeve and the outer compression sleeve decrease in sequence.

[0019] On the other hand, the present invention further provides a backfill type friction stir spot welding device, comprising the above-mentioned backfill type friction stir spot welding stirring head.

[0020] On the other hand, the present invention further provides a backfilling friction stir spot welding method, the backfilling friction stir spot welding method is performed using the above-mentioned backfilling friction stir spot welding device, and the backfilling friction stir spot welding method comprises:

[0021] Step S1: Move the backfill friction stir spot welding stirring head to the welding position and press it down closely to the surface of the plate to be welded;

[0022] Step S2: rotating the first stirring sleeve and the second stirring sleeve at high speed to soften the plate to be welded;

[0023] Step S3: the second stirring sleeve is pushed down to enter the softened plate to be welded, and at the same time, the first stirring sleeve is retracted to accommodate the extruded high-temperature plastic metal;

[0024] Step S4: retracting the second stirring sleeve, and at the same time, pulling the first stirring sleeve down to refill the high-temperature plastic metal extruded in step S3 into the joint;

[0025] Step S5: the backfill friction stir spot welding stirring head is withdrawn from the weldment surface to end the welding.

[0026] Compared with the prior art, the technical solution of this application has at least the following technical effects:

[0027] When in use, the stirring head of the present invention is installed on the backfill type friction stir spot welding device. During the actual working process, the inner clamping column and the outer clamping sleeve will not rotate, and both are clamped and fixed on the plate to be welded. There are two forms of movement of the first stirring sleeve and the second stirring sleeve, one is rotational movement, and the other is downward and back movement (i.e., axial reciprocating movement along the inner clamping column). During the rotational movement, the first stirring sleeve and the second stirring sleeve rub against the plate to be welded, generating a large amount of heat to soften the plate; then, the downward and back movement of the first stirring sleeve and the second stirring sleeve are utilized, and the metal is extruded and backfilled to form a metallurgical bond at the overlapping interface of the plate, thereby forming a smooth stirring spot welding joint without a keyhole.

[0028] In addition, compared with the traditional backfill stir friction spot welding, the thermal-mechanical effect at the weld point is more uniform. The linear velocity at the center of the traditional stirring needle is zero, and the temperature is the lowest; the linear velocity at the outside is larger, and the temperature is the highest. This significant difference in heat causes the unevenness of the joint structure, which is prone to welding defects. The stirring head of the present invention has a first stirring sleeve and a second stirring sleeve that are nested. By rotating the first stirring sleeve and the second stirring sleeve on the surface of the plate to be welded, the temperature of the first stirring sleeve and the second stirring sleeve on the friction interface with the plate to be welded is more uniform, and the difference in thermal-mechanical effect at the weld point is smaller. In other words, the present invention solves the problem of uneven thermal-mechanical effect at the weld point during friction welding to a large extent, and it is easier to obtain a spot welding joint with uniform and stable structure and performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] The drawings described herein are used to provide a further understanding of the present application and constitute a part of the present application. The illustrative embodiments of the present application and their descriptions are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:

[0030] Figure 1 It is a structural schematic diagram of the backfill type friction stir spot welding stirring head disclosed in the embodiment of the present application when it is in a first viewing angle;

[0031] Figure 2 is a structural schematic diagram of the backfill type friction stir spot welding stirring head disclosed in the embodiment of the present application when it is at a second viewing angle;

[0032] Figure 3 It is a front view of a backfill type friction stir spot welding stirring head disclosed in an embodiment of the present application;

[0033] Figure 4 is a cross-sectional view of a friction stir spot welding stirring head during backfilling disclosed in an embodiment of the present application;

[0034] Figure 5 It is a flow chart of the stir friction spot welding method during backfilling disclosed in the embodiment of the present application.

[0035] The above drawings include the following reference numerals:

[0036] 10. Inner compression column; 20. First stirring sleeve; 30. Second stirring sleeve; 40. Outer compression sleeve. DETAILED DESCRIPTION

[0037] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present application will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.

[0038] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit the exemplary embodiments according to the present application. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprise" and / or "include" are used in this specification, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.

[0039] Unless otherwise specifically stated, the relative arrangement, numerical expressions and numerical values ​​of the parts and steps set forth in these embodiments do not limit the scope of the present application. At the same time, it should be understood that, for ease of description, the sizes of the various parts shown in the accompanying drawings are not drawn according to the actual proportional relationship. The technology, methods and equipment known to those of ordinary skill in the relevant art may not be discussed in detail, but in appropriate cases, the technology, methods and equipment should be considered as a part of the authorization specification. In all examples shown and discussed here, any specific value should be interpreted as being merely exemplary, rather than as a limitation. Therefore, other examples of exemplary embodiments may have different values. It should be noted that similar reference numerals and letters represent similar items in the following drawings, and therefore, once a certain item is defined in an accompanying drawing, it does not need to be further discussed in subsequent drawings.

[0040] See also Figures 1 to 4 As shown, according to one aspect of the present application, a backfilling friction stir spot welding stirring head is provided, hereinafter referred to as a stirring head. The stirring head is particularly suitable for realizing hollow annular backfilling friction stir spot welding of lightweight materials such as aluminum alloys and magnesium alloys.

[0041] Specifically, the stirring head in this embodiment includes an inner compression column 10 , a first stirring sleeve 20 , a second stirring sleeve 30 and an outer compression sleeve 40 .

[0042] Among them, the inner clamping column 10 is used to compress and fix the plate to be welded; the first stirring sleeve 20 can be rotatably mounted on the outer periphery of the inner clamping column 10, and the first stirring sleeve 20 can also reciprocate along the axial direction of the inner clamping column 10; the second stirring sleeve 30 can be rotatably mounted on the outer periphery of the first stirring sleeve 20, and the second stirring sleeve 30 can also reciprocate along the axial direction of the inner clamping column 10; the outer clamping sleeve 40 is mounted on the outer periphery of the second stirring sleeve 30, and the outer clamping sleeve 40 is used to compress and fix the plate to be welded.

[0043] When in use, the stirring head in this embodiment is installed on the backfill type friction stir spot welding device. During the actual working process, the inner clamping column 10 and the outer clamping sleeve 40 will not rotate, and both are clamped and fixed on the plate to be welded. There are two forms of movement of the first stirring sleeve 20 and the second stirring sleeve 30, one is rotational movement, and the other is downward and retracting movement (i.e., axial reciprocating movement along the inner clamping column 10). During the rotational movement, the first stirring sleeve 20 and the second stirring sleeve 30 rub against the plate to be welded, generating a large amount of heat to soften the plate; then, the downward and reciprocating movement of the first stirring sleeve 20 and the second stirring sleeve 30 is utilized, and through the extrusion and backfilling of the metal, the overlapping interface of the plate forms a metallurgical bond, forming a smooth stirring spot welding joint without a keyhole.

[0044] In addition, compared with the traditional backfill stir friction spot welding, the heat-mechanical effect at the welding spot is more uniform. The linear velocity of the center position of the traditional stirring needle is 0, and the temperature is the lowest; the linear velocity of the outer side is larger, and the temperature is the highest. This significant difference in heat causes the unevenness of the joint structure, which is prone to welding defects. The stirring head of the present invention has a first stirring sleeve 20 and a second stirring sleeve 30 that are nested. By rotating the first stirring sleeve 20 and the second stirring sleeve 30 on the surface of the plate to be welded, the temperature of the first stirring sleeve 20 and the second stirring sleeve 30 on the friction interface with the plate to be welded is more uniform, and the difference in heat-mechanical effect at the welding spot is smaller. In other words, the present invention solves the problem of uneven heat-mechanical effect at the welding spot during friction welding to a large extent, and it is easier to obtain a spot welding joint with uniform and stable structure and performance.

[0045] Specifically, the inner compression column 10, the first stirring sleeve 20, the second stirring sleeve 30 and the outer compression sleeve 40 in this embodiment are all cylindrical structures. When assembled, the four parts of the inner compression column 10, the first stirring sleeve 20, the second stirring sleeve 30 and the outer compression sleeve 40 are put together with an inner outer sleeve, and the matching form is a gap match, which can ensure that the two adjacent parts can move independently. The structure is simple and easy to process, and is suitable for the rotation of the first stirring sleeve 20 and the second stirring sleeve 30.

[0046] Furthermore, the bottom end and / or side wall of the first stirring sleeve 20 in this embodiment is provided with a first friction reinforcement part (not shown in the figure), that is, the first friction reinforcement part can be provided at the bottom end (the end for contacting the plate to be welded) of the first stirring sleeve 20, and the first friction reinforcement part can also be provided on the side wall (the side wall for contacting the welding plate) of the first stirring sleeve 20, and the first friction reinforcement part can also be provided on both the bottom end and the side wall of the first stirring sleeve 20 at the same time. Through the action of the first friction reinforcement part, good friction can be provided during the friction welding process, and the high-temperature plastic metal can be promoted to flow. Optionally, the first friction reinforcement part can be a thread, a corrugation or other uneven structure, as long as it is other deformation methods under the conception of the present application, it is within the protection scope of the present application.

[0047] Similarly, the bottom end and / or side wall of the second stirring sleeve 30 in this embodiment is provided with a second friction reinforcement part (not shown in the figure). That is to say, the second friction reinforcement part can be provided at the bottom end of the second stirring sleeve 30 (the end for contacting the plate to be welded), and the second friction reinforcement part can also be provided on the side wall of the second stirring sleeve 30 (the side wall for contacting the welding plate), and the second friction reinforcement part can also be provided on both the bottom end and the side wall of the second stirring sleeve 30. Through the action of the second friction reinforcement part, good friction can be provided during the friction welding process, and the high-temperature plastic metal can be promoted to flow. Optionally, the second friction reinforcement part can be a thread, a corrugation or other uneven structure. As long as it is other deformation methods under the conception of this application, it is within the protection scope of this application.

[0048] Of course, in other embodiments of the present application, the first friction reinforcement portion and the second friction reinforcement portion may not be provided on the first stirring sleeve 20 and the second stirring sleeve 30, that is, the surfaces of the first stirring sleeve 20 and the second stirring sleeve 30 are smooth surfaces, and the specific structure may be determined according to the properties of the plate to be welded.

[0049] Optionally, the rotation speed of the first stirring sleeve 20 and the second stirring sleeve 30 in this embodiment is 600rpm to 2000rpm, for example, 600rpm, 1000rpm, 1400rpm or 2000rpm, and the speed of the first stirring sleeve 20 and the second stirring sleeve 30 axially pressing down and retracting along the inner compression column 10 is 0.5mm / s to 2mm / s, for example, 0.5mm / s, 1.0mm / s, 1.5mm / s or 2mm / s, so that it can be suitable for different welding processes.

[0050] In addition, compared with the traditional backfill friction stir spot welding, the stirring head of the present invention is easier to achieve welding for thick plates and easier to develop large-diameter stirring tools. Since the first stirring sleeve 20 and the second stirring sleeve 30 in the present invention are both cylindrical in design, while the traditional stirring needle is a solid cylindrical structure. When the stirring spot welding device provides equal welding pressure, the first stirring sleeve 20 and the second stirring sleeve 30 in the present invention can be made with a larger diameter, which is more advantageous for welding thick plates and large areas. The specific reasons are as follows:

[0051] The backfill friction stir spot welding stirring head in this embodiment satisfies the following formula:

[0052]

[0053] Among them, P is the ultimate extrusion pressure provided by the mechanical arm of the backfill friction stir spot welding, the unit is Pa, P is the pressure required for the backfill friction stir spot welding stirring head to be inserted into the plate to be welded, the unit is MPa, and d is the maximum diameter of the stirring head, the unit is mm.

[0054] When using the commonly used units in engineering, and assuming that the ultimate extrusion pressure is F = 100kg (1kN), P = 100MPa, and the maximum supported stirring head diameter is d (unit: mm), then there is the equation:

[0055]

[0056] If a conventional solid stirring head is used, after calculation, the maximum stirring head diameter allowed is d = 11 mm. When the cylindrical stirring head of the present invention is used, assuming that its outer diameter is d and the wall thickness is 3 mm, the formula is Substituting the numerical value, the maximum diameter of the stirring head allowed to be used is calculated to be d=22mm, which is twice the diameter of the former. It can be seen that the diameter of the stirring head provided by the present invention can be significantly larger when the stirring friction spot welding device provides the same maximum welding pressure, so that the stirring tool has better rigidity. This is more advantageous for welding thick plates and large areas.

[0057] Optionally, the inner compression column 10, the first stirring sleeve 20, the second stirring sleeve 30 and the outer compression sleeve 40 in this embodiment are all made of H13 tool steel, with high structural strength and good stability.

[0058] Furthermore, the lengths of the inner compression column 10, the first stirring sleeve 20, the second stirring sleeve 30 and the outer compression sleeve 40 are successively reduced, which is more suitable for assembly and control. In a specific embodiment, the outer diameter of the inner compression column 10 is 10 mm and the height is 100 mm; the first stirring sleeve 20 has a wall thickness of 2.5 mm, an outer diameter of 15 mm, and a height of 85 mm; the second stirring sleeve 30 has a wall thickness of 2.5 mm, an outer diameter of 20 mm, and a height of 70 mm; and the outer compression sleeve 40 has a wall thickness of 5 mm, an outer diameter of 30 mm, and a height of 50 mm.

[0059] On the other hand, an embodiment of the present application also provides a backfill type stir friction spot welding device, which includes the above-mentioned backfill type stir friction spot welding stirring head. Therefore, the backfill type stir friction spot welding device in this embodiment includes all the technical effects of the backfill type stir friction spot welding stirring head in the above-mentioned embodiment. Since the technical effects of the backfill type stir friction spot welding stirring head have been described in detail in the previous article, they will not be repeated here.

[0060] See also Figure 5 As shown, the embodiment of the present application also provides a backfilling friction stir spot welding method, which is performed using the above-mentioned backfilling friction stir spot welding device. Specifically, the backfilling friction stir spot welding method in this embodiment includes the following steps:

[0061] Step S1: Use the backfill type friction stir spot welding device to move the stirring head to the welding position and press it down closely to the surface of the plate to be welded. At this time, the lower end surfaces of the inner clamping column 10, the first stirring sleeve 20, the second stirring sleeve 30 and the outer clamping sleeve 40 are flush (such as Figure 2 As shown), and are pressed tightly against the surface of the plate to be welded.

[0062] Step S2: Using the backfill type friction stir spot welding device, the first stirring sleeve 20 and the second stirring sleeve 30 are rotated at high speed to soften the plate to be welded. At this time, the first stirring sleeve 20 and the second stirring sleeve 30 are in contact with the plate to be welded. The position generates intense friction, and a large amount of heat is generated within a few seconds, so that the temperature of the plate to be welded rises rapidly and softens.

[0063] Step S3: using the backfill type friction stir spot welding device to push the second stirring sleeve 30 down into the softened plate to be welded, and at the same time, using the backfill type friction stir spot welding device to retract the first stirring sleeve 20 to accommodate the extruded high-temperature plastic metal.

[0064] Step S4: Use the backfilling friction stir spot welding device to retract the second stirring sleeve 30 and return it to the initial interface position. At the same time, the first stirring sleeve 20 is also returned to the initial interface position, so that the high-temperature plastic metal extruded in step S3 can be refilled into the joint.

[0065] Step S5: Using the backfill friction stir spot welding device to withdraw the stirring head from the weldment surface, and end the welding. In this step, the first stirring sleeve 20 and the second stirring sleeve 30 stop rotating, and the entire stirring head is withdrawn from the weldment surface, and the welding process ends. At this time, a flat stirring spot welding joint without a keyhole can be formed.

[0066] For ease of description, spatially relative terms such as "above", "above", "on the upper surface of", "above", etc. may be used here to describe the spatial positional relationship between a device or feature and other devices or features as shown in the figure. It should be understood that spatially relative terms are intended to include different orientations of the device in use or operation in addition to the orientation described in the figure. For example, if the device in the accompanying drawings is inverted, the device described as "above other devices or structures" or "above other devices or structures" will be positioned as "below other devices or structures" or "below other devices or structures". Thus, the exemplary term "above" can include both "above" and "below". The device can also be positioned in other different ways (rotated 90 degrees or in other orientations), and the spatially relative descriptions used here are interpreted accordingly.

[0067] In addition, it should be noted that the use of terms such as "first" and "second" to limit components is only for the convenience of distinguishing the corresponding components. Unless otherwise stated, the above terms have no special meaning and therefore cannot be understood as limiting the scope of protection of this application.

[0068] The above are only preferred embodiments of the present application and are not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.

Claims

1. A backfill type friction stir spot welding stirring head, characterized in that: include: An internal pressing column (10), the internal pressing column (10) being used to press and fix the plate to be welded; a first stirring sleeve (20), the first stirring sleeve (20) being rotatably sleeved on the outer circumference of the inner pressing column (10), and the first stirring sleeve (20) being further capable of reciprocating along the axial direction of the inner pressing column (10); a second stirring sleeve (30), the second stirring sleeve (30) being rotatably sleeved on the outer periphery of the first stirring sleeve (20), and the second stirring sleeve (30) being further capable of reciprocating along the axial direction of the inner compression column (10); and An outer compression sleeve (40), the outer compression sleeve (40) being sleeved on the outer circumference of the second stirring sleeve (30), the outer compression sleeve (40) being used to compress and fix the plate to be welded; The first stirring sleeve (20) and the second stirring sleeve (30) are nested and have two forms of movement, namely rotational movement and downward and backward reciprocating movement; When rotating, the first stirring sleeve (20) and the second stirring sleeve (30) rub against the plate to be welded, generating a large amount of heat, thereby softening the plate to be welded; When performing the reciprocating motion of pushing down and pulling back, the first stirring sleeve (20) and the second stirring sleeve (30) form a metallurgical bond at the overlapping interface of the plates to be welded through metal extrusion and backfilling, thereby forming a smooth stirring spot welding joint without a keyhole.

2. The backfill friction stir spot welding stirring head according to claim 1, characterized in that: The bottom end and / or the side wall of the first stirring sleeve (20) is provided with a first friction reinforcement portion.

3. The backfill friction stir spot welding stirring head according to claim 1, characterized in that: The bottom end and / or the side wall of the second stirring sleeve (30) is provided with a second friction reinforcement portion.

4. The backfill friction stir spot welding stirring head according to claim 1, characterized in that: The rotation speed of the first stirring sleeve (20) and the second stirring sleeve (30) is 600 rpm to 2000 rpm.

5. The backfill friction stir spot welding stirring head according to claim 1, characterized in that: The speed at which the first stirring sleeve (20) and the second stirring sleeve (30) are pressed down and retracted along the axial direction of the inner pressing column (10) is 0.5 mm / s to 2 mm / s.

6. The backfill friction stir spot welding stirring head according to any one of claims 1 to 5, characterized in that: The inner compression column (10), the first stirring sleeve (20), the second stirring sleeve (30) and the outer compression sleeve (40) are all made of H13 tool steel.

7. The backfill friction stir spot welding stirring head according to any one of claims 1 to 5, characterized in that: The lengths of the inner compression column (10), the first stirring sleeve (20), the second stirring sleeve (30), and the outer compression sleeve (40) decrease in sequence.

8. A backfill type friction stir spot welding device, characterized in that: A backfill friction stir spot welding stirring head comprising any one of claims 1 to 7.

9. A backfill friction stir spot welding method, characterized in that: The backfill type friction stir spot welding method is performed by using the backfill type friction stir spot welding device described in claim 8, and the backfill type friction stir spot welding method comprises: Step S1: Move the backfill friction stir spot welding stirring head to the welding position and press it down closely to the surface of the plate to be welded; Step S2: rotating the first stirring sleeve (20) and the second stirring sleeve (30) at a high speed to soften the plate to be welded; Step S3: the second stirring sleeve (30) is pushed down to enter the softened plate to be welded, and at the same time, the first stirring sleeve (20) is retracted to accommodate the extruded high-temperature plastic metal; Step S4: retracting the second stirring sleeve (30) and, at the same time, pulling the first stirring sleeve (20) downward to refill the high-temperature plastic metal extruded in step S3 into the joint; Step S5: the backfill friction stir spot welding stirring head is withdrawn from the weldment surface to end the welding.

Citation Information

Patent Citations

  • Three-moving-ring stirring friction spot-welding tool and spot welding method using same

    CN102554454A

  • A filling friction spot welding method with outer sleeve shaft rotation

    CN106342013B

  • Method for improving welding efficiency of backfill type friction stir spot welding

    CN113369670A

  • Combined tool for improving fluidity of stirring friction spot welding molded metal

    CN216829132U

  • Method and apparatus for joining metallic workpieces by means of friction stir welding

    DE102020108503A1