Resin composition, molded product, modifier for polyamide resin, and method for modifying polyamide resin
By adding a specific proportion of aliphatic polyester-modified ethylene-vinyl alcohol resin grafted into the polyamide resin, the problem of reduced transparency and solvent resistance caused by the olefin elastomer in the polyamide resin is solved, and the problem is improved. Improves the mechanical strength and formability of the molded article.
Patent Information
- Application Number
- CN202180022206.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-03-26
- Filing Date
- 2021-03-09
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2041-03-09
Smart Images

Figure BDA0003846647970000071 
Figure BDA0003846647970000231
Abstract
Description
Technical Field
[0001] The present invention relates to a resin composition containing a polyamide resin and a modified ethylene-vinyl alcohol resin grafted with an aliphatic polyester, and more particularly to a resin composition having excellent molding processability and forming a molded product having excellent transparency, tensile fracture strain characteristics and solvent resistance, and a molded product thereof, as well as a modifier for a polyamide resin used therein and a method for modifying a polyamide resin. Background Art
[0002] Conventionally, polyamide resins have been widely used as engineering plastics in various industrial fields including the automobile industry due to their excellent impact resistance, chemical resistance, abrasion resistance, and the like.
[0003] Furthermore, recently, the demand has also been expanding in applications under more severe environments, and various proposals have been made for further improving the mechanical strength of molded products made of polyamide-based resins.
[0004] For example, in order to obtain a molded product that exhibits excellent impact resistance even at an extremely low temperature of -40°C or lower, a technique of blending an olefin-based elastomer or the like into a polyamide-based resin has been proposed (see Patent Document 1).
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent Application Publication No. 2009-191871 Summary of the invention
[0008] Problem that the invention aims to solve
[0009] However, when a molded product is obtained by mixing an olefin elastomer with a polyamide resin as described above, the transparency of the molded product is reduced because the polyamide resin and the olefin elastomer are incompatible. In addition, the solvent resistance is reduced, so there is also a problem of limited use.
[0010] The present invention has been made in view of such circumstances, and provides a resin composition containing a polyamide resin as a main component which can improve the mechanical strength, especially the tensile break strain characteristics, without impairing the transparency and solvent resistance of the molded product, as well as a molded product formed from the resin composition, a modifier for a polyamide resin used in modifying the polyamide resin, and a method for modifying the polyamide resin.
[0011] Solutions for solving problems
[0012] Therefore, the present inventors have conducted in-depth research on a modification method for improving the mechanical strength of a resin composition having a polyamide resin as a main component without impairing the transparency and solvent resistance of its molded product. As a result, it was found that if a specific modified ethylene-vinyl alcohol resin that is compatible with the polyamide resin is mixed with the polyamide resin in a specific ratio, the molding processability is excellent and the reduction in the transparency of the molded product is suppressed. In addition, the tensile break strain characteristics and solvent resistance are improved.
[0013] That is, the present invention provides the following [1] to [9].
[0014] [1] A resin composition, characterized in that it contains a polyamide resin (A) and a modified ethylene-vinyl alcohol resin (B) grafted with an aliphatic polyester, wherein when the total content of the polyamide resin (A) and the modified ethylene-vinyl alcohol resin (B) is set to 100 parts by weight, the content of the modified ethylene-vinyl alcohol resin (B) is not less than 1 part by weight and less than 50 parts by weight.
[0015] [2] The resin composition according to the above [1] is characterized in that when the total content of the above polyamide resin (A) and the above modified ethylene-vinyl alcohol resin (B) is set to 100 parts by weight, the content of the above modified ethylene-vinyl alcohol resin (B) is 1 to 45 parts by weight.
[0016] [3] The resin composition according to [1] or [2] above, wherein the modification rate of the modified ethylene-vinyl alcohol-based resin (B) is 0.1 to 30 mol%.
[0017] [4] A resin composition according to any one of [1] to [3] above, characterized in that in the modified ethylene-vinyl alcohol resin (B), the grafted aliphatic polyester is a ring-opening polymer of a lactone ring, and the number of carbon atoms constituting the lactone ring is 3 to 10.
[0018] [5] A resin composition according to any one of [1] to [4] above, wherein a single-layer film having a thickness of 30 μm obtained using the resin composition has a total haze of 2% or less as measured using a haze meter (NDH2000 manufactured by Nippon Denshoku Co., Ltd.) in accordance with JIS K7105.
[0019] [6] A molded product formed from the resin composition according to any one of [1] to [5] above.
[0020] [7] The formed article according to [6] above, wherein the formed article is a sheet or a film.
[0021] [8] A modifier for a polyamide-based resin, comprising a modified ethylene-vinyl alcohol-based resin (B) grafted with an aliphatic polyester.
[0022] [9] A method for modifying a polyamide resin, wherein the polyamide resin (A) is modified by allowing the polyamide resin (A) to contain a modified ethylene-vinyl alcohol resin (B) grafted with an aliphatic polyester, and when the total content of the polyamide resin (A) and the modified ethylene-vinyl alcohol resin (B) is set to 100 parts by weight, the content of the modified ethylene-vinyl alcohol resin (B) is set to be greater than 1 part by weight and less than 50 parts by weight.
[0023] As described above, the resin composition of the present invention contains a specific modified ethylene-vinyl alcohol resin (B) in a specific ratio relative to the above-mentioned polyamide resin (A) in order to modify the resin composition containing the polyamide resin (A) as the main component, and the modified ethylene-vinyl alcohol resin (B) is compatible with the above-mentioned polyamide resin (A).
[0024] In addition, hereinafter, “ethylene-vinyl alcohol-based resin” may be abbreviated as “EVOH”, and “modified EVOH grafted with an aliphatic polyester” may be abbreviated as “aliphatic polyester-modified EVOH” or “modified EVOH”.
[0025] Effects of the Invention
[0026] According to the resin composition, since the polyamide resin (A) and the aliphatic polyester modified EVOH (B) are compatible, the amorphous part of the polyamide resin (A) and the modified EVOH (B) are compatible, and as a result, the glass transition temperature (Tg) is reduced, and excellent tensile fracture strain characteristics are exhibited, and excellent molding processability is possessed. Therefore, the molded product obtained by the resin composition has the advantage of maintaining excellent quality without losing the original transparency and solvent resistance.
[0027] Furthermore, according to the modifier for a polyamide resin and the method for modifying a polyamide resin of the present invention, a polyamide resin having the above-mentioned excellent physical properties can be provided simply by incorporating the modifier into the polyamide resin. DETAILED DESCRIPTION
[0028] Hereinafter, although the form for implementing this invention is demonstrated concretely, this invention is not limited to these descriptions.
[0029] First, the resin composition of the present invention contains a polyamide-based resin (A) and an aliphatic polyester-modified EVOH (B), and these will be described below in order.
[0030] <Polyamide Resin (A)>
[0031] The polyamide resin (A) used in the present invention is not particularly limited. Examples of general polyamide resins include homopolymers such as polycaproamide (nylon 6), poly-ω-aminoheptanoic acid (nylon 7), poly-ω-aminononanoic acid (nylon 9), polyundecamide (nylon 11), and polylaurolactam (nylon 12). Examples of the copolymer polyamide resin include polyethylene adipamide (nylon 26), polybutylene adipamide (nylon 46), polyhexamethylene adipamide (nylon 66), polyhexamethylene sebacate (nylon 610), polyhexamethylene dodecanoate (nylon 612), polyoctylene adipamide (nylon 86), polydecamethylene adipamide (nylon 108), caprolactam / laurolactam copolymer (nylon 6 / 12), caprolactam / ω-aminononanoic acid copolymer (nylon 6 / 9), caprolactam / hexamethylenediamine adipate copolymer (nylon 6 / 66), laurolactam / hexamethylenediamine adipate copolymer (nylon 12 / 66), and polyethylene adipamide / hexamethylenediamine adipate copolymer. (nylon 26 / 66), caprolactam / hexamethylenediamine adipate / hexamethylenediamine sebacate copolymer (nylon 66 / 610), ethylamine adipate / hexamethylenediamine adipate / hexamethylenediamine sebacate copolymer (nylon 6 / 66 / 610) and the like; aromatic polyamides such as poly(hexamethylene isophthalamide), poly(hexamethylene terephthalamide), poly(m-phenylene adipamide), hexamethylene isophthalamide / hexamethylene terephthalamide copolymer, poly(p-phenylene terephthalamide), poly(3,4'-diphenyl ether terephthalamide); amorphous polyamide; those obtained by modifying these polyamide resins with aromatic amines such as methylenebenzylamine and m-phenylenediamine; m-phenylenediamine adipate, etc. Alternatively, they may be terminal-modified polyamide resins, preferably terminal-modified polyamide resins. These polyamide-based resins may be used alone or in combination of two or more.
[0032] The melting point of the polyamide resin (A) is preferably 160 to 270° C., more preferably 180 to 250° C., and particularly preferably 200 to 230° C. When the melting point of the polyamide resin (A) is too low, the heat resistance of the resin composition tends to decrease. On the other hand, if the melting point of the polyamide resin (A) is too high, when the polyamide resin (A) and the aliphatic polyester-modified EVOH (B) are blended using a twin-screw extruder, the mold temperature tends to be too high, and the blended resin composition tends to be thermally degraded.
[0033] From the above viewpoints, as a preferable polyamide-based resin (A), for example, nylon 6 (melting point: about 220° C.) and nylon 6 / 66 (melting point: about 200° C.) are preferable.
[0034] <Aliphatic polyester modified EVOH (B)>
[0035] Next, the aliphatic polyester-modified EVOH (B) used together with the above-mentioned polyamide-based resin (A) will be described.
[0036] The aliphatic polyester-modified EVOH (B) is a resin in which an aliphatic polyester is grafted onto the hydroxyl group of EVOH.
[0037] The EVOH is generally a resin obtained by saponifying a copolymer of ethylene and a vinyl ester monomer, that is, an ethylene-vinyl ester copolymer, and is a water-insoluble thermoplastic resin.
[0038] As the polymerization method of the above-mentioned ethylene and vinyl ester monomers, any known polymerization method, such as solution polymerization, suspension polymerization, and emulsion polymerization, can be used for the polymerization, and solution polymerization using methanol as a solvent is usually used. In addition, the saponification of the obtained ethylene-vinyl ester copolymer can also be carried out using a known method.
[0039] EVOH produced in this manner mainly contains structural units derived from ethylene and vinyl alcohol, and generally contains a certain amount of vinyl ester structural units that remain without being saponified.
[0040] As the above-mentioned vinyl ester monomer, vinyl acetate is typically used from the viewpoint of market availability and good impurity treatment efficiency during production. As other vinyl ester monomers, for example, aliphatic vinyl esters such as vinyl formate, vinyl propionate, vinyl valerate, vinyl butyrate, vinyl isobutyrate, vinyl pivalate, vinyl caprate, vinyl laurate, vinyl stearate, and vinyl versatate; aromatic vinyl esters such as vinyl benzoate, etc., can be listed. Generally, aliphatic vinyl esters having 3 to 20 carbon atoms, preferably 4 to 10 carbon atoms, and particularly preferably 4 to 7 carbon atoms can be used. These can be used alone or in combination of two or more.
[0041] The content of the ethylene structural unit in the above EVOH can be controlled by the ethylene pressure when copolymerizing the vinyl ester monomer and ethylene, and is usually 20 to 60 mol%, preferably 25 to 50 mol%, and particularly preferably 30 to 45 mol%. When the content is too low, the melt moldability tends to decrease. On the contrary, when it is too high, the gas barrier properties tend to decrease.
[0042] It should be noted that the content of the ethylene structural unit can be measured according to ISO14663.
[0043] The saponification degree of the vinyl ester component in the EVOH can be controlled by the amount of the saponification catalyst (usually a basic catalyst such as sodium hydroxide) used when saponifying the ethylene-vinyl ester copolymer, the temperature, the time, etc., and is usually 90 to 100 mol%, preferably 95 to 100 mol%, and particularly preferably 99 to 100 mol%. When the saponification degree is too low, there is a tendency for gas barrier properties, thermal stability, moisture resistance, etc. to decrease.
[0044] The saponification degree of EVOH can be measured in accordance with JIS K6726 (wherein EVOH is used in the form of a solution uniformly dissolved in a water / methanol solvent).
[0045] The EVOH described above may further contain a structural unit derived from a comonomer shown below within a range (for example, 10 mol% or less of EVOH) that does not impair the effects of the present invention.
[0046] Examples of the comonomer include olefins such as propylene, 1-butene, and isobutylene; hydroxyl-containing α-olefins such as 3-butene-1-ol, 3-butene-1,2-diol, 4-pentene-1-ol, and 5-hexene-1,2-diol, and their derivatives such as esters and acylates; hydroxyalkyl vinylides such as 2-methylenepropane-1,3-diol and 3-methylenepentane-1,5-diol; 1,3-diacetoxy-2-methylenepropane, 1,3-dipropionyloxy-2-methylenepropane unsaturated acids such as acrylic acid, methacrylic acid, crotonic acid, phthalic acid (anhydride), maleic acid (anhydride), itaconic acid (anhydride), or salts thereof or mono- or di-alkyl esters in which the alkyl group has 1 to 18 carbon atoms; acrylamide, N-alkyl acrylamide in which the alkyl group has 1 to 18 carbon atoms, N,N-dimethylacrylamide, 2-acrylamidopropanesulfonic acid or its salts, acrylamidopropyl dimethyl Acrylic amides such as amine or its acid salt or quaternary salt; methacrylamide, N-alkyl methacrylamide with 1 to 18 carbon atoms in the alkyl group, N,N-dimethyl methacrylamide, 2-methacrylamide propanesulfonic acid or its salt, methacrylamide propyl dimethylamine or its acid salt or quaternary salt; N-vinyl amides such as N-vinyl pyrrolidone, N-vinyl formamide, N-vinyl acetamide; vinyl cyanides such as acrylonitrile and methacrylonitrile; carbon atoms in the alkyl group Vinyl ethers such as alkyl vinyl ethers, hydroxyalkyl vinyl ethers, and alkoxyalkyl vinyl ethers having 1 to 18 moieties; halogenated vinyl compounds such as vinyl chloride, vinylidene chloride, vinyl fluoride, vinylidene fluoride, and vinyl bromide; vinyl silanes such as trimethoxyvinylsilane; allyl halides such as allyl acetate and allyl chloride; allyl alcohols such as allyl alcohol and dimethoxyallyl alcohol; comonomers such as trimethyl-(3-acrylamide-3-dimethylpropyl)ammonium chloride and acrylamide-2-methylpropanesulfonic acid. These may be used alone or in combination of two or more.
[0047] In particular, EVOH having a primary hydroxyl group in a side chain is preferred, and EVOH having a 1,2-diol structure in a side chain is particularly preferred, from the viewpoint of good secondary moldability such as stretching processing and vacuum / pressure molding.
[0048] The EVOH used in the present invention may be EVOH that has been "post-modified" by urethanization, acetalization, cyanoethylation, oxyalkylenation, acylation, or the like.
[0049] Furthermore, the EVOH used in the present invention may be a mixture with other EVOHs. Examples of the other EVOHs include EVOHs with different saponification degrees, EVOHs with different polymerization degrees, and EVOHs with different copolymer components.
[0050] Next, a method for obtaining the aliphatic polyester-modified EVOH (B) used in the present invention using the above-mentioned EVOH will be described.
[0051] Methods for modifying the above-mentioned EVOH include: (1) a method of subjecting lactones to ring-opening polymerization in the presence of EVOH; (2) a method of first subjecting aliphatic polyesters and lactones to ring-opening polymerization and condensation polymerization to obtain a polyester having a carboxyl group at the terminal, and then reacting the polyester having a carboxyl group at the terminal with EVOH.
[0052] Among them, the method of ring-opening polymerization of lactones in the presence of EVOH can easily obtain a resin in which an aliphatic polyester is grafted onto EVOH through a one-stage reaction. Therefore, compared with the method of previously generating an aliphatic polyester through ring-opening polymerization and condensation polymerization and then reacting the aliphatic polyester with EVOH, it has fewer steps and is simpler, so it is preferred.
[0053] The lactones are preferably lactones having 3 to 10 carbon atoms constituting a ring which forms an aliphatic polyester by ring-opening polymerization. When such lactones have no substituent, they are represented by the following general formula (1).
[0054]
[0055] In the above general formula (1), n is an integer of 2 to 9, preferably 4 to 5. In addition, the alkylene chain -(CH 2 ) n Any carbon atom in - may have at least one substituent such as a lower alkyl group or lower alkoxy group having about 1 to 8 carbon atoms, a cycloalkyl group, a phenyl group, or an aralkyl group.
[0056] Specific examples of such lactones include β-propiolactones, γ-butyrolactones, ε-caprolactones, and δ-valerolactones.
[0057] Examples of the β-propiolactones include β-propiolactone and dimethylpropiolactone.
[0058] Examples of the γ-butyrolactones include gamma-butyrolactone, gamma-valerolactone, gamma-caprolactone, gamma-decanolactone, gamma-laurolactone, gamma-palmitolactone, gamma-stearoyllactone, crotonyllactone, α-angelica lactone, and β-angelica lactone.
[0059] As the above-mentioned ε-caprolactones, there can be listed monoalkyl-ε-caprolactones such as ε-caprolactone, monomethyl-ε-caprolactone, monoethyl-ε-caprolactone, monodecyl-ε-caprolactone, monopropyl-ε-caprolactone, and monodecyl-ε-caprolactone; dialkyl-ε-caprolactones having two alkyl groups substituted on carbon atoms other than the ε position; trialkyl-ε-caprolactones having three alkyl groups substituted on carbon atoms other than the ε position; alkoxy-ε-caprolactones such as ethoxy-ε-caprolactone; cycloalkyl-lactones such as cyclohexyl-ε-caprolactone; aralkyl-ε-caprolactones such as benzyl-ε-caprolactone; aryl-ε-caprolactones such as phenyl-ε-caprolactone, and the like.
[0060] Examples of the δ-valerolactones include 5-valerolactone, 3-methyl-5-valerolactone, 3,3-dimethyl-5-valerolactone, 2-methyl-5-valerolactone, and 3-ethyl-5-valerolactone.
[0061] These lactones may be used alone or in combination of two or more.
[0062] Among these, ε-caprolactones and δ-valerolactones are particularly preferred, and ε-caprolactone is particularly preferred from the viewpoint of being inexpensive and easily available.
[0063] In addition, in the case of a reaction accompanied by ring-opening polymerization, it is preferred to add a conventionally known ring-opening polymerization catalyst. Examples of the ring-opening polymerization catalyst include titanium compounds and tin compounds. Specifically, examples include titanium alkoxides such as titanium tetra-n-butoxide, titanium tetraisobutoxide, and titanium tetraisopropoxide; tin alkoxides such as dibutyltin dibutoxide; and tin ester compounds such as dibutyltin diacetate. Among these, titanium tetra-n-butoxide is preferred from the viewpoint of being cheap and easily available.
[0064] The above reaction can also be carried out in a heated melt state in a kneading machine such as a single-screw extruder, a twin-screw extruder, a Banbury mixer, a kneader, or a Brabender.
[0065] In addition, the reaction time and temperature in the ring-opening polymerization are not particularly limited, and can be appropriately selected. It is preferably carried out while stirring at 50 to 250° C. for 10 seconds to 24 hours, and more preferably carried out while stirring at 150 to 230° C. for 5 minutes to 10 hours. If the reaction time is too short compared to the lower limit or the reaction temperature is too low compared to the lower limit, the grafting reaction rate will decrease, and therefore, there is a tendency for unreacted compounds to ooze out of the molded product and cause deterioration of the surface appearance. If the reaction time is too long compared to the upper limit or the reaction temperature is too high compared to the upper limit, there is a tendency for cross-linking to occur between the modified EVOHs, resulting in poor appearance of the molded product such as fish eyes.
[0066] In the aliphatic polyester modified EVOH (B) obtained by such operation, the content of EVOH units forming the main chain of the modified EVOH (B) is usually 40 to 99% by weight, preferably 45 to 95% by weight, and particularly preferably 50 to 90% by weight, and the content of aliphatic polyester units grafted on the main chain is usually 1 to 60% by weight, preferably 5 to 55% by weight, and particularly preferably 10 to 50% by weight. If the amount of EVOH units is too much, the mechanical strength, especially the tensile breaking strain, will not be improved, and the compatibility with the polyamide resin (A) will be reduced. Therefore, there is a tendency that the effect of the present invention cannot be obtained. On the other hand, if the amount of EVOH units is too little, there is a tendency that the adhesion is strong and the molded product is easily blocked. It should be noted that the content of EVOH units in the aliphatic polyester modified EVOH (B) and the content of grafted aliphatic polyester units can be adjusted according to 1 Calculated based on the results of H-NMR measurement.
[0067] In addition, the number average molecular weight (measured by GPC and standard polystyrene conversion) of the above-mentioned aliphatic polyester modified EVOH (B) is usually 5000 to 300000, preferably 10000 to 200000, and particularly preferably 10000 to 100000. If the number average molecular weight of the above-mentioned modified EVOH (B) is too high, there is a tendency that its melt viscosity is too high and its dispersibility in the polyamide resin (A) as the main component is reduced. On the other hand, if the number average molecular weight of the modified EVOH (B) is too low, there is a tendency that its melt viscosity is too low and stable melt molding is difficult. It should be noted that the number average molecular weight of the above-mentioned modified EVOH (B) can be calculated based on the GPC measurement results.
[0068] Furthermore, the modification rate of the grafted aliphatic polyester in the aliphatic polyester-modified EVOH (B) (hereinafter referred to as "grafted modification rate" or simply "modification rate") is generally 0.1 to 30 mol%, more preferably 1 to 25 mol%, and particularly preferably 5 to 20 mol%. If the modification rate is too low, the mechanical strength, especially the tensile breaking strain, of the modifier is poor, and the compatibility with the polyamide resin (A) is reduced. Therefore, there is a tendency that the effect of the present invention cannot be obtained. On the other hand, if the modification rate is too high, there is a tendency that the adhesiveness is strong and the molded product is easily blocked. It should be noted that the modification rate can be adjusted according to the following conditions: 1 Calculated based on the results of H-NMR measurement.
[0069] Furthermore, in the above-mentioned aliphatic polyester modified EVOH (B), the average chain length of the aliphatic polyester unit grafted on its main chain is usually 1 to 15 mol, preferably 1 to 10 mol, and particularly preferably 1 to 8 mol. If the average chain length of the above-mentioned grafted aliphatic polyester unit is too long, there is a tendency that the adhesiveness is strong and the molded product is easily blocked. It should be noted that the average chain length of the above-mentioned aliphatic polyester unit can be 1 Calculated based on the results of H-NMR measurement.
[0070] Specifically, by using the following conditions 1 By H-NMR measurement, the modification ratio of the grafted aliphatic polyester in the aliphatic polyester-modified EVOH (B) and the average chain length of the grafted aliphatic polyester can be calculated.
[0071] (a) 1 H-NMR measurement conditions
[0072] Internal standard substance: tetramethylsilane
[0073] Solvent: d6-DMSO
[0074] Measured polymer concentration: 5 wt% (sample 0.1 g, solvent 2 mL)
[0075] Measurement temperature: 50℃(323K)
[0076] Irradiation pulse: 45° pulse
[0077] Pulse interval: 10sec
[0078] Cumulative times: 16 times
[0079] (b) Attribution of resonance absorption peak
[0080] (I) 0.8 to 0.9 ppm: -CH 3
[0081] (II) 1.0~1.9ppm: -CH 2 - and -CH adjacent to the aliphatic polyester 2 -
[0082] (III) 2.0 ppm: -CH 3
[0083] (IV) 2.1 to 2.3 ppm: -CH adjacent to the carboxyl group of the aliphatic polyester 2 -
[0084] (V) 3.3 to 4.0 ppm: -CH- adjacent to -OH of aliphatic polyester-modified EVOH and -CH- adjacent to -OH of aliphatic polyester 2 -
[0085] (VI) 4.0 to 4.7 ppm: -OH of aliphatic polyester-modified EVOH and aliphatic polyester, and -CH adjacent to the ester bond of aliphatic polyester 2 -
[0086] (c) Calculation of grafting modification rate and average chain length of aliphatic polyester
[0087] The integrated values of the resonance absorption peaks of (I) to (VI) above are used to establish the following simultaneous equations of formulas (i) to (vi), and the amount C (mol) of the grafted modified groups and the average chain length n (mol) of the aliphatic polyester are calculated based on the solutions of the simultaneous equations. Furthermore, the grafted modified ratio X (mol %) of the aliphatic polyester is calculated based on formula (vii).
[0088] Formula (i): 3×M=[integral value of peak (I)]
[0089] Formula (ii): (2×M)+(2×A)+(4×E)+(2×O)+(6×n+2)×C=[integral value of peak (II)]
[0090] Formula (iii): 3×A=[integral value of peak (III)]
[0091] Formula (vi): 2×n×C=[integral value of peak (IV)]
[0092] Formula (v): O + (2 × C) = [integral value of peak (V)]
[0093] Formula (vi): O+(2×n-1)×C=[integral value of peak (VI)]
[0094] Formula (vii): X=C / (M+A+O+C+E)×100
[0095] Here, M, A, O, C, n, E, and X represent the following values.
[0096] M: The amount of terminal methyl groups of aliphatic polyester-modified EVOH (mole)
[0097] A: Acetyl group content of aliphatic polyester modified EVOH (mole)
[0098] O: Hydroxyl content of aliphatic polyester modified EVOH (mole)
[0099] C: The amount of aliphatic polyester grafted modification groups in aliphatic polyester modified EVOH (mole)
[0100] n: average chain length of aliphatic polyester (mole)
[0101] E: Vinyl content of aliphatic polyester modified EVOH (mole)
[0102] X: Graft modification ratio of aliphatic polyester-modified EVOH (mol%)
[0103] In addition, the glass transition temperature (Tg) of the aliphatic polyester-modified EVOH (B) used in the present invention is usually -50 to 60°C, preferably -30 to 45°C, and particularly preferably -10 to 35°C. If the glass transition temperature is too low, there is a tendency that the molded product is easily blocked, while on the other hand, if the glass transition temperature is too high, there is a tendency that the effect of the present invention cannot be obtained. It should be noted that the above-mentioned glass transition temperature can be measured using a differential scanning calorimeter.
[0104] Specifically, the glass transition temperature of the aliphatic polyester-modified EVOH (B) can be calculated by measuring using a differential scanning calorimeter under the following conditions.
[0105] (a) Conditioning of the test piece: After melting at 230°C for 1 minute, the sample was cooled to -30°C at a cooling rate of 10°C / min.
[0106] (b) Analysis of glass transition temperature: The sample cooled in (a) was heated to 230° C. at a heating rate of 10° C. / min.
[0107] (c) Calculation of glass transition temperature: Based on the DSC curve obtained in (b), the midpoint temperature of the step-change portion of the glass transition was calculated as the glass transition temperature.
[0108] In addition, the MFR (melt flow rate) of the aliphatic polyester modified EVOH (B) is usually 0.5 to 100 g / 10 minutes, preferably 1 to 50 g / 10 minutes, and particularly preferably 3 to 35 g / 10 minutes. When the MFR is too large, the melt viscosity of the modified EVOH (B) tends to be too low, making it difficult to perform stable melt molding, and when the MFR is too small, the melt viscosity of the modified EVOH (B) tends to be too high, and the dispersibility in the polyamide resin (A) tends to decrease.
[0109] The MFR is an index of the degree of polymerization of EVOH forming the main chain of the modified EVOH (B), and can be adjusted by the amount of the polymerization initiator and the amount of the solvent when copolymerizing the monomers.
[0110] <Resin composition>
[0111] Next, the resin composition of the present invention will be described.
[0112] The resin composition of the present invention is a resin composition comprising the aforementioned polyamide-based resin (A) and the aforementioned aliphatic polyester-modified EVOH (B).
[0113] The content ratio of the above-mentioned polyamide resin (A) and the aliphatic polyester modified EVOH (B) is set so that when the total content of the above-mentioned polyamide resin (A) and the above-mentioned modified EVOH (B) is set to 100 parts by weight, the content of the above-mentioned modified EVOH (B) is greater than 1 part by weight and less than 50 parts by weight.
[0114] That is, the lower limit of the content of the modified EVOH (B) is 1 part by weight, preferably 5 parts by weight or more, and more preferably 10 parts by weight or more. The upper limit of the content of the modified EVOH (B) is less than 50 parts by weight, preferably 45 parts by weight or less, more preferably 40 parts by weight or less, further preferably 30 parts by weight or less, and particularly preferably 20 parts by weight or less. And, in particular, the content of the modified EVOH (B) is preferably 1 part by weight or more and 45 parts by weight or less, more preferably 1 part by weight or more and less than 40 parts by weight, and further preferably 1 part by weight or more and less than 20 parts by weight.
[0115] That is, if the content of the modified EVOH (B) is more than the above range, the compatibility of the two resins (A) and (B) will be unbalanced, the transparency, solvent resistance and molding processability of the obtained molded product will tend to be reduced, and the effect of improving the tensile break strain characteristics will tend not to be obtained. In addition, if the content of the modified EVOH (B) is too small, the effect of modifying the polyamide resin (A) will tend not to be obtained.
[0116] It should be noted that the resin composition of the present invention may contain, as other components, carboxylic acid-modified polyolefin resin (C), hydrocarbon resin having a number average molecular weight of 100 to 3000 and a softening point of 60° C. or higher and less than 170° C., antioxidants, lubricants, antistatic agents, colorants, ultraviolet absorbers, plasticizers, heat stabilizers, light stabilizers, surfactants, antibacterial agents, desiccants, antiblocking agents, flame retardants, crosslinking agents, curing agents, foaming agents, crystal nucleating agents, antifogging agents, biodegradable additives, silane coupling agents and other additives as appropriate within a range that does not impair the effects of the present invention (e.g., less than 5% by weight of the entire resin composition).
[0117] <Preparation of resin composition>
[0118] Next, the method for obtaining the resin composition of the present invention will be described.
[0119] The resin composition of the present invention can be obtained by mixing the above-mentioned polyamide resin (A), modified EVOH (B), and optional components blended as required.
[0120] The above-mentioned mixing method is not particularly limited, and the components can also be directly used by dry mixing. The following method is usually used: after mixing by a melt mixing method, a solution mixing method, etc., the mixture is formed into a shape that is easy to handle, such as pellets, and prepared in the form of a resin composition. From the viewpoint of productivity, the melt mixing method is preferably used.
[0121] The above-mentioned melt mixing method can be a method in which the components are dry-mixed and then melt-mixed. This can be done using a known mixing device such as a Kneader-Ruder, an extruder, an open roll, a Banbury mixer, a Plastomill, etc. In general, a single-screw or twin-screw extruder is preferably used in industry. In addition, a vent suction device, a gear pump device, a screen device, etc. are also preferably provided as needed.
[0122] The melt kneading temperature is usually in the range of 160 to 300° C., preferably 200 to 260° C., and particularly preferably 210 to 240° C., based on the set temperature of the extruder and the die. If the temperature is too low, the resin tends to be in an unmelted state and the processing state tends to be unstable, while if the temperature is too high, the resin composition tends to be thermally degraded and the quality of the obtained molded article tends to be reduced.
[0123] <Molded article>
[0124] Next, a molded product obtained by using the resin composition of the present invention will be described.
[0125] The resin composition of the present invention is usually provided in the form of a molded article having various shapes in accordance with the target, such as a film, a sheet, a container, a fiber, a rod, a tube, etc., by melt molding, etc. Its use includes a variety of uses such as packaging materials, fibers, daily necessities, home appliance parts, automobile parts, medical components, civil engineering / construction materials, etc.
[0126] As described above, the amorphous part of the polyamide resin (A) as the resin component in the molded product obtained using the resin composition of the present invention is compatible with the modified EVOH (B), and as a result, the glass transition temperature (Tg) of the resin composition is reduced, and excellent tensile fracture strain characteristics are exhibited. In addition, the original transparency and solvent resistance are not impaired and the excellent quality is maintained.
[0127] It should be noted that the total haze of a 30 μm-thick single-layer film obtained using the resin composition of the present invention is preferably 3.5% or less, more preferably 2% or less, and further preferably 1.5% or less, as measured using a haze meter (NDH2000 manufactured by Nippon Denshoku Co., Ltd.) in accordance with JIS K7105. If the total haze exceeds 3.5%, the transparency of the film tends to decrease.
[0128] The above-mentioned “total haze (%)” represents the value obtained by dividing the diffuse light transmittance of the test piece by the total light transmittance in the form of percentage. The lower the total haze value, the better the transparency of the film.
[0129] Incidentally, the glass transition temperature of the resin composition of the present invention is usually preferably about 3 to 50°C lower, particularly preferably about 8 to 20°C lower, than the glass transition temperature of the polyamide resin (A) alone.
[0130] It should be noted that the molded product obtained using the resin composition of the present invention can not only be used as a virgin product, but also (when the recycled product is reused, etc.) a crushed product formed by the molded product can be used again for melt molding. As the above-mentioned melt molding method, extrusion molding (T-die extrusion, inflation extrusion, blow molding, melt spinning, profile extrusion, etc.) and injection molding are mainly used. The melt molding temperature is usually in the range of 160 to 300°C, preferably 200 to 260°C, and particularly preferably 210 to 240°C. If the above-mentioned melt molding temperature is too low, there is a tendency for the melt moldability to be reduced due to insufficient fluidity. If the above-mentioned melt molding temperature is too high, there is a tendency for the resin composition to undergo thermal degradation, produce fish eyes, and have poor appearance such as coloring.
[0131] When the resin composition of the present invention is formed into a single-layer film or sheet, the thickness thereof varies depending on the intended use, but is generally 5 to 2000 μm, preferably 10 to 500 μm, and more preferably 10 to 200 μm.
[0132] Furthermore, when the resin composition of the present invention is formed into a film or sheet, it can be formed not only into a single molded product but also into a multilayer structure having at least one layer formed of the resin composition of the present invention, and can be formed into various molded products for use.
[0133] Examples of methods for producing the multilayer structure include a method of melt-extruding a thermoplastic resin onto a film or sheet comprising the resin composition of the present invention; a method of melt-extruding the resin composition of the present invention onto a substrate such as a thermoplastic resin; a method of co-extruding the resin composition of the present invention with other thermoplastic resins; and a method of dry laminating a film or sheet comprising the resin composition of the present invention with a film or sheet of another substrate using a known adhesive such as an organic titanium compound, an isocyanate compound, a polyester compound, or a polyurethane compound.
[0134] Among the above methods, the method of co-extruding the resin composition of the present invention with other thermoplastic resins is easy to operate and manage, and is suitable. In addition, as the thermoplastic resins that become the object during co-extrusion, for example, polyolefin resins, polyester resins, polyamide resins, copolyamides, polystyrene resins, polyvinyl chloride resins, polyvinylidene chloride, acrylic resins, vinyl ester resins, polyester elastomers, polyurethane elastomers, chlorinated polyethylene, chlorinated polypropylene, aromatic and aliphatic polyketones, aliphatic polyols, etc. can be listed. Among them, from the viewpoint of having excellent mechanical properties, extrusion processability, and being able to cope with a variety of molding, it is suitable to use polyolefin resins.
[0135] The polyolefin resin is not particularly limited, but from the viewpoint of excellent bending fatigue resistance, vibration fatigue resistance, etc. of the obtained laminated packaging material, preferably, for example, linear low-density polyethylene (LLDPE), low-density polyethylene (LDPE), ultra-low-density polyethylene (VLDPE), ethylene-vinyl acetate copolymer (EVA), and ionomer.
[0136] Furthermore, regarding the layer structure when a multilayer structure is obtained by using the resin composition of the present invention, when the layer containing the resin composition of the present invention is set as a (a1, a2, ...), and the other substrate, for example, the layer formed by a thermoplastic resin is set as b (b1, b2, ...), if it is a film, a sheet, a bottle, a pipe, or a duct, it can be not only a two-layer structure of a / b, but also any combination of b / a / b, a / b / a, a1 / a2 / b, a / b1 / b2, b2 / b1 / a / b1 / b2, b1 / b2 / a / b3 / b4, a1 / b1 / a2 / b2, etc. In addition, when a fiber-like or filament-like molded product is made, the resin composition of the present invention and other substrates can be used in combination in the same manner, and a and b can be any combination of bimetallic type, core (a)-sheath (b) type, core (b)-sheath (a) type, or eccentric core-sheath type.
[0137] It should be noted that in the above-mentioned multilayer structure, an adhesive resin layer can be provided between the respective layers as required. The resin used in the above-mentioned adhesive resin layer varies depending on the type of resin used as the other layer in the above-mentioned b, and therefore cannot be generalized. Examples thereof include modified olefin polymers containing carboxyl groups obtained by chemically bonding unsaturated carboxylic acids or their anhydrides to olefin polymers through addition reactions, grafting reactions, etc.
[0138] Specifically, as suitable substances, one or a mixture of two or more selected from maleic anhydride grafted modified polyethylene, maleic anhydride grafted modified polypropylene, maleic anhydride grafted modified ethylene-propylene (block or random) copolymer, maleic anhydride grafted modified ethylene-ethyl acrylate copolymer, maleic anhydride grafted modified ethylene-vinyl acetate copolymer, etc. can be listed. The amount of unsaturated carboxylic acid or its anhydride contained in the olefin polymer at this time is preferably 0.001 to 3 weight%, more preferably 0.01 to 1 weight, and particularly preferably 0.03 to 0.5 weight. If the amount of modification in the above-mentioned modified product is small, there is a tendency for insufficient adhesion. On the other hand, if the amount of modification in the above-mentioned modified product is large, there is a tendency for cross-linking reaction to occur and poor formability.
[0139] In addition, the resin composition of the present invention, other rubber / elastomer components such as EVOH, polyisobutylene, and ethylene-propylene rubber may be blended into these adhesive resins, and further the resin of the above-mentioned b layer (the layer to be bonded) may be blended. In particular, a polyolefin resin different from the polyolefin resin serving as the matrix of the adhesive resin may be blended.
[0140] The thickness of each layer of the multilayer structure cannot be generalized due to the layer composition, the type of b, the purpose, the shape of the molded product, the required physical properties, etc. Usually, the a layer is appropriately selected from the range of 5 to 2000 μm, further 10 to 500 μm, and particularly 10 to 200 μm, the b layer is appropriately selected from the range of 5 to 5000 μm, further 30 to 1000 μm, and the adhesive resin layer is appropriately selected from the range of 5 to 400 μm, further 10 to 150 μm. In addition, regarding the thickness ratio of the a layer to the adhesive resin layer, the a layer is usually thicker, and the ratio of the a layer / adhesive resin layer (thickness ratio) is usually 1 to 100, preferably 1 to 50, and particularly preferably 1 to 10.
[0141] In addition, in the above-mentioned multilayer structure, regarding the thickness ratio of the a layer and the b layer, when the thickness of all the layers of the same type in the multilayer structure are added together, the b layer is usually thicker, and the ratio of the b layer / a layer (thickness ratio) is usually 1 to 100, preferably 3 to 20, and particularly preferably 6 to 15. When the above-mentioned a layer is too thin, there is a tendency that the mechanical properties such as rigidity and impact resistance are insufficient or the thickness control thereof becomes unstable. On the contrary, when it is too thick, there is a tendency that the bending fatigue resistance is poor and there is an uneconomical tendency. In addition, when the b layer is too thin, there is a tendency that the rigidity is insufficient. On the contrary, when it is too thick, there is a tendency that the bending fatigue resistance is poor or there is a tendency that the weight becomes large. On the other hand, when the adhesive resin layer is too thin, there is a tendency that the interlayer adhesion is insufficient or there is a tendency that the thickness control thereof is unstable. On the contrary, when it is too thick, there is a tendency that the weight becomes large and there is an uneconomical tendency. In addition, in order to improve the molding processability and various physical properties, the aforementioned various additives, various modifiers other than the aforementioned modified EVOH (B) used in the present invention, fillers, other resins, etc. may be added to each layer of the multilayer structure within a range that does not impair the effects of the present invention.
[0142] Furthermore, in order to improve the physical properties of the above-mentioned multilayer structure, a stretching treatment may also be implemented. The stretching treatment may be any one of uniaxial stretching and biaxial stretching. When the stretching is performed at a high ratio as much as possible, a stretched film, a stretched sheet, a stretched container, a stretched bottle and other formed products with good physical properties and no pinholes, cracks, uneven stretching, delamination, etc., can be obtained during stretching. As a stretching method, in addition to a roller stretching method, a tenter stretching method, a tube stretching method, a stretching blow molding method, etc., a method with a high stretching ratio among deep drawing forming, vacuum pressure forming, etc. may also be adopted. In the case of biaxial stretching, any method of a simultaneous biaxial stretching method or a sequential biaxial stretching method may be adopted. The stretching temperature is usually selected from a range of about 40 to 170°C, preferably about 60 to 160°C. When the stretching temperature is less than 40°C, the stretchability becomes poor. If it exceeds 170°C, there is a tendency to be difficult to maintain a stable stretched state.
[0143] After the stretching is completed, heat fixing is preferably performed for the purpose of imparting dimensional stability to the stretched film. Heat fixing can be performed by known means, for example, the stretched film is kept in a tensioned state while being heat treated at 80 to 180°C, preferably 100 to 165°C, for about 2 to 600 seconds. In addition, when used for heat shrink packaging of raw meat, processed meat, cheese, etc., the finished film can be made without heat fixing after stretching. After the raw meat, processed meat, cheese, etc. are placed in the film, heat treatment is performed at 50 to 130°C, preferably 70 to 120°C, for about 2 to 300 seconds, so that the film is heat-shrunk for sealing packaging.
[0144] The above-mentioned multilayer structure can be directly used for objects of various shapes, for example, films, sheets, tapes, bottles, pipes, filaments, irregular cross-section extrudates, etc. In addition, when a cup or tray-shaped multilayer container is obtained from a multilayer sheet or multilayer film, a deep drawing method can be used, specifically, vacuum forming method, pressure forming method, vacuum pressure forming method, pressure-assisted plug vacuum pressure forming method, etc. Furthermore, when a catheter or bottle-shaped multilayer container is obtained from a multilayer parison (a hollow tubular preform before blow molding), a blow molding method can be used, specifically, extrusion blow molding method (double-head type, mold moving type, parison moving type, rotary type, accumulator type, horizontal parison type, etc.), cold parison blow molding method, injection blow molding method, biaxial stretch blow molding method (extrusion type cold parison biaxial stretch blow molding method, injection type cold parison biaxial stretch blow molding method, injection molding in-line biaxial stretch blow molding method, etc.) and the like can be used. The obtained multilayer structure may be subjected to heat treatment, cold treatment, calendaring treatment, printing treatment, dry lamination treatment, solution or melt coating treatment, bag making process, deep drawing process, box processing, tube processing, slit processing, etc. as required.
[0145] <Modifier for polyamide resin>
[0146] Next, the polyamide resin modifier of the present invention will be described.
[0147] The modifier for a polyamide-based resin of the present invention is obtained by using the aliphatic polyester-modified EVOH (B) itself used in the resin composition of the present invention as a modifier for a polyamide-based resin.
[0148] As described above, the modified EVOH (B) is compatible with the polyamide resin (A). Therefore, when the modified EVOH (B) is used as a modifier and is compounded into a resin composition formed by the polyamide resin (A), the amorphous part of the polyamide resin (A) is compatible with the modified EVOH (B), and as a result, the glass transition temperature (Tg) is reduced, and excellent tensile fracture strain characteristics are exhibited, and excellent molding processability is possessed. Therefore, the molded product obtained by the above resin composition has the advantage of maintaining excellent quality without damaging the original transparency and solvent resistance.
[0149] The details of the polyamide resin modifier of the present invention, namely, the modified EVOH (B), have been described above, and the description thereof will be omitted.
[0150] The details of the polyamide resin to be modified in the polyamide resin modifier of the present invention, namely, the modified EVOH (B), have also been described as the polyamide resin (A), and the description thereof will be omitted.
[0151] It should be noted that when the modifier for polyamide resin of the present invention, i.e., modified EVOH (B), is mixed into polyamide resin (A) to modify its physical properties, the mixing ratio is appropriately set according to the required degree of modification, the shape / application of the resulting molded product, etc. Usually, when the total content of the above-mentioned polyamide resin (A) and the above-mentioned modified EVOH (B) is set to 100 parts by weight, it is suitable to set the content of the above-mentioned modified EVOH (B) to be greater than 1 part by weight and less than 50 parts by weight.
[0152] If described in more detail, the lower limit of the content of the modified EVOH (B) is preferably set to 1 part by weight, more preferably 5 parts by weight or more, and further preferably 10 parts by weight or more. In addition, the upper limit of the content of the modified EVOH (B) is preferably less than 50 parts by weight, more preferably 45 parts by weight or less, further preferably 40 parts by weight or less, particularly preferably 30 parts by weight or less, and further preferably 20 parts by weight or less. And, in particular, the content of the modified EVOH (B) is preferably from 1 part by weight to 45 parts by weight, more preferably from 1 part by weight to less than 40 parts by weight, and further preferably from 1 part by weight to less than 20 parts by weight.
[0153] That is, if the content of the modified EVOH (B) is too much compared to the above range, the compatibility of the two resins (A) and (B) will be unbalanced, the transparency, solvent resistance and molding processability of the obtained molded product will tend to be reduced, and the effect of improving the tensile break strain characteristics will tend not to be obtained. In addition, if the content of the modified EVOH (B) is too little, the effect of modifying the polyamide resin (A) will tend not to be obtained.
[0154] The form of the polyamide resin modifier of the present invention, namely, the modified EVOH (B) is not particularly limited, and may be, for example, a powder or pellet, a solution, or a dispersion.
[0155] Example
[0156] Hereinafter, examples of the present invention will be described in detail together with comparative examples. However, the present invention is not limited to the following examples unless the gist of the present invention is exceeded.
[0157] <Materials>
[0158] First, details of materials used in Examples and Comparative Examples are shown below.
[0159] Polyamide resin (A1): Nylon 6 (manufactured by Mitsubishi Engineering-Plastics Corporation, grade: NOVAMID (registered trademark) 1022BLMJ)
[0160] Polyamide resin (A2): Nylon 6 (manufactured by DSM, grade: NOVAMID (registered trademark) 1020)
[0161] Aliphatic polyester modified EVOH (B1): ethylene content 32 mol%, saponification degree 99.6%, graft modification rate 12.5 mol%, average chain length of aliphatic polyester 1.4 mol, glass transition temperature 18°C
[0162] Aliphatic polyester modified EVOH (B2): ethylene content 44 mol%, saponification degree 99.6%, graft modification rate 7.3 mol%, average chain length of aliphatic polyester 1.4 mol, glass transition temperature 20°C
[0163] Unmodified EVOH: Ethylene content 32 mol%, saponification degree 99.6%, glass transition temperature 61°C
[0164] · Polyolefin elastomer: Mitsui Chemicals, Inc., Tafmer MH7010, glass transition temperature -50°C
[0165] · Polyester elastomer: GQ430 manufactured by Mitsubishi Chemical Corporation, glass transition temperature: -50°C
[0166] ·Styrene elastomer: Asahi Kasei Chemicals Co., Ltd., Tuftec M1913, glass transition temperature: -45°C
[0167] <Explanation of evaluation items (evaluation method, evaluation criteria)>
[0168] Next, details of evaluation items for Example products and Comparative example products are shown below.
[0169] (1) Tensile fracture strain
[0170] Using pellets formed from the resin compositions used in the Examples and Comparative Examples, ISO3167 A-type test pieces were prepared by injection molding as samples for measuring tensile fracture strain. Furthermore, a tensile test was performed using a tensile testing machine (manufactured by Shimadzu Corporation, Autograph AGS-H) under the following conditions to measure the strain (%) at fracture.
[0171] Test conditions: ISO527
[0172] Temperature / humidity conditions: 23°C, 50% RH
[0173] ·Stretching speed: 50mm / min
[0174] (2) Transparency (internal haze, total haze)
[0175] A single-layer film with a thickness of 30 μm was prepared using pellets formed from the resin composition used in the examples and comparative examples. In addition, regarding the transparency of the single-layer film, a haze meter (NDH2000 manufactured by Nippon Denshoku Co., Ltd.) was used to measure the total haze (%) in accordance with JIS K7105. The above-mentioned "total haze (%)" has been explained. It is expressed as a percentage of the diffuse light transmittance of the test piece divided by the total light transmittance. The lower the total haze value, the better the transparency of the film. It should be noted that in order to evaluate the haze inside the film, a sample coated with liquid paraffin on both sides of the film was used during the measurement, and the internal haze (%) was measured in a state where the influence caused by the unevenness of the film surface was removed.
[0176] (3)Solvent resistance: Toluene
[0177] The pellets formed from the resin compositions used in the examples and comparative examples were used to prepare test pieces of 50 mm in length × 25 mm in width × 2 mm in thickness using an injection molding machine. The obtained test pieces were immersed in toluene in a constant temperature room at 23°C / 50%RH and allowed to stand, and the weight increase rate (g / per 100 g of resin) after one week of immersion was evaluated.
[0178] (4) Glass transition temperature
[0179] The state of the samples (pellets) formed of the resin compositions used in Examples and Comparative Examples was observed by heating using a differential scanning calorimeter (Diamond DSC manufactured by Perkin Elmer) to calculate the glass transition temperature.
[0180] (a) Conditioning of the test piece: After heating to 250°C, the sample was cooled to -30°C at a cooling rate of 10°C / min.
[0181] (b) Analysis of glass transition temperature: The sample cooled in (a) was heated to 250° C. at a heating rate of 10° C. / min.
[0182] (c) Calculation of glass transition temperature: Based on the DSC curve obtained in (b), the midpoint temperature of the step-change portion of the glass transition was calculated as the glass transition temperature.
[0183] (5) Formability (adhesion)
[0184] The sample (pellet) formed by the resin composition used in Examples 3, 4 and Comparative Example 6 was heated at 150°C for 5 hours. The pellets after heating were visually observed to see if they were sticky. The situation where no sticking occurred was evaluated as "0", and the situation where sticking occurred was evaluated as "×". In the case of sticking, the pellets lose fluidity, which becomes a cause of clogging in the hopper tank, hopper, etc. during the forming process, and the forming processability is reduced.
[0185] [Example 1]
[0186] The polyamide resin (A1) and the aliphatic polyester-modified EVOH (B1) were introduced into a barrel from the raw material supply port of a twin-screw kneading extruder (TEX32, manufactured by The Nippon Steel Works, Ltd.) at a weight ratio shown in the following Table 1, and transported to a kneading zone set at a temperature of 240° C. for melt blending, and the molten blend was extruded into a strand from a die attached to a nozzle. The obtained strand-shaped extrudate was pelletized using a resin pelletizer to obtain a pelletized resin composition.
[0187] [Example 2]
[0188] A pelletized resin composition was obtained in the same manner as in Example 1 except that the polyamide resin (A1) was changed to 80 parts by weight and the aliphatic polyester-modified EVOH (B1) was changed to 20 parts by weight.
[0189] [Examples 3, 4, Comparative Examples 1 to 7]
[0190] A pelletized resin composition was obtained in the same manner as in Example 1 except that the types and weight ratios of the resins to be combined were changed as shown in Table 1 described later.
[0191] The obtained products of Examples 1 to 4 and Comparative Examples 1 to 7 were measured and evaluated for the aforementioned evaluation items (tensile strain at break, transparency [internal haze, total haze], solvent resistance, glass transition temperature, and molding processability [blocking]). The results are collectively shown in Table 1 below.
[0192] [Table 1]
[0193]
[0194] According to the above results, the products of Examples 1 to 4 all showed good properties in any evaluation item, but the products of Comparative Examples 1 to 7 were poorly evaluated in at least any item of tensile fracture strain, solvent resistance, transparency, glass transition temperature, and molding processability, indicating that the effect of modifying the polyamide resin (A) was insufficient.
[0195] It should be noted that the above embodiments show specific aspects of the present invention, but the above embodiments are merely illustrative and are not to be construed as limiting. It should be considered that various modifications obvious to those skilled in the art are within the scope of the present invention.
[0196] Industrial Applicability
[0197] The present invention relates to a resin composition containing a polyamide resin (A) and an aliphatic polyester-modified EVOH (B), a molded product thereof, a modifier thereof and a method for modifying a polyamide resin. The resin composition has excellent molding processability, and the obtained molded product has excellent transparency, tensile fracture strain characteristics and solvent resistance, and therefore, they can be widely used.
Claims
1. A resin composition, characterized in that It contains a polyamide resin (A) and a modified ethylene-vinyl alcohol resin (B) grafted with an aliphatic polyester, wherein the content of the modified ethylene-vinyl alcohol resin (B) is 1 part by weight or more and less than 50 parts by weight, when the total content of the polyamide resin (A) and the modified ethylene-vinyl alcohol resin (B) is 100 parts by weight, The modification rate of the modified ethylene-vinyl alcohol resin (B) grafted with aliphatic polyester is 0.1 to 30 mol%. The modification rate is calculated by the following formula (vii): Formula (vii): X=C / (M+A+O+C+E)×100 Here, M, A, O, C, E, and X represent the following values: M, in moles: the amount of terminal methyl groups in aliphatic polyester-modified EVOH A, in moles: acetyl content of aliphatic polyester modified EVOH O, in moles: hydroxyl content of aliphatic polyester modified EVOH C, in moles: the amount of aliphatic polyester grafted modified groups in aliphatic polyester modified EVOH E, in moles: vinyl content of aliphatic polyester-modified EVOH X, in mol %: graft modification ratio of aliphatic polyester-modified EVOH.
2. The resin composition according to claim 1, characterized in that When the total content of the polyamide resin (A) and the modified ethylene-vinyl alcohol resin (B) is 100 parts by weight, the content of the modified ethylene-vinyl alcohol resin (B) is 1 to 45 parts by weight.
3. The resin composition according to claim 1 or 2, characterized in that In the modified ethylene-vinyl alcohol-based resin (B), the grafted aliphatic polyester is a ring-opening polymer of a lactone ring, and the number of carbon atoms constituting the lactone ring is 3 to 10.
4. The resin composition according to claim 1 or 2, characterized in that The total haze of a 30 μm-thick single-layer film obtained by using the resin composition, measured using a haze meter (NDH2000 manufactured by Nippon Denshoku Industries) in accordance with JIS K7105, was 2% or less.
5. A formed article, characterized in that: The resin composition is formed from the resin composition according to any one of claims 1 to 4.
6. The formed article according to claim 5, characterized in that The formed article is a sheet or a film.
7. Use of a modified ethylene-vinyl alcohol resin (B) grafted with an aliphatic polyester as a modifier for a polyamide resin, wherein the modified ethylene-vinyl alcohol resin (B) grafted with an aliphatic polyester and a polyamide resin form a resin composition as claimed in any one of claims 1 to 4.
8. A method for modifying a polyamide resin, characterized in that: The invention relates to a method for modifying a polyamide resin (A) by making the polyamide resin (A) contain a modified ethylene-vinyl alcohol resin (B) grafted with an aliphatic polyester, wherein the content of the modified ethylene-vinyl alcohol resin (B) is set to 1 part by weight or more and less than 50 parts by weight when the total content of the polyamide resin (A) and the modified ethylene-vinyl alcohol resin (B) is set to 100 parts by weight, The modification rate of the modified ethylene-vinyl alcohol resin (B) grafted with aliphatic polyester is 0.1 to 30 mol%. The modification rate is calculated by the following formula (vii): Formula (vii): X=C / (M+A+O+C+E)×100 Here, M, A, O, C, E, and X represent the following values: M, in moles: the amount of terminal methyl groups in aliphatic polyester-modified EVOH A, in moles: acetyl content of aliphatic polyester modified EVOH O, in moles: hydroxyl content of aliphatic polyester modified EVOH C, in moles: the amount of aliphatic polyester grafted modified groups in aliphatic polyester modified EVOH E, in moles: vinyl content of aliphatic polyester-modified EVOH X, in mol %: graft modification ratio of aliphatic polyester-modified EVOH.
Citation Information
Patent Citations
Hydrogen tank liner material and hydrogen tank liner
JP2009191871A
Pneumatic tire
CN104334634A
Ethylene-vinyl alcohol copolymer composition, pellet and multilayered structure
CN110637059A
Resin composition and film using the same
JP2013209588A
Thermoplastic resin composition for pneumatic tire inner liner
JP2019104828A