Gel electrolyte, preparation method thereof and lithium ion battery

Through the copolymerization preparation of a variety of functional monomers and crosslinking agents, the safety and interface compatibility problems of lithium-ion batteries are solved, and efficient flame retardant performance and electrochemical performance are achieved, suitable for high energy and high power density application.

CN115312835BActive Publication Date: 2024-11-01ZHEJIANG GEELY HLDG GRP CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211027624.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-08-25
Publication Date
2024-11-01
Estimated Expiration
2042-08-25

AI Technical Summary

Technical Problem

Safety issues of existing lithium-ion batteries, especially the flammability of gel electrolytes and poor interface compatibility with electrode materials, lead to the risk of combustion and liquid leakage, insufficient flame retardant performance, and affect the high energy and high power density applications of the battery.

Method used

Flame-retardant gel electrolytes are prepared by thermally initiating in situ copolymerization, including organic solvents, lithium salts, crosslinking agents, first monomers, second monomers and third monomers , through chain polymerization, the flame retardant and electrochemical properties are improved.

Benefits of technology

It effectively improves the flame retardant and electrochemical properties of lithium-ion batteries, reduces the flash point, enhances the interface compatibility with electrode materials, reduces the risk of liquid leakage, and improves the safety and circulation performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115312835B_ABST
    Figure CN115312835B_ABST
Patent Text Reader

Abstract

The present invention provides a gel electrolyte and a preparation method thereof and a lithium ion battery, and specifically relates to the field of electrolytes. The gel electrolyte comprises the following raw material components: 60-90% of an organic solvent, 5-20% of a lithium salt, 0.5-5% of a crosslinking agent, 1-15% of a first monomer, 0.5-15% of a second monomer, 0.5-15% of a third monomer, and 0.005-5% of an initiator; wherein the first monomer, the second monomer, the third monomer, the crosslinking agent, the initiator, the organic solvent and the lithium salt are in situ copolymerized by thermal initiation to prepare the gel electrolyte. The present invention introduces a variety of functional monomers so that the copolymer has a variety of functional groups and gives the copolymer a variety of functionalities, thereby improving the safety of the battery of the gel electrolyte.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of electrolytes, and in particular to a gel electrolyte and a preparation method thereof, and a lithium ion battery. Background Art

[0002] In recent years, with the rapid development and popularization of electric vehicles, people have put forward higher standards for the safety of power lithium-ion batteries. At present, lithium-ion batteries are mainly composed of three parts: pole pieces, diaphragms and electrolytes. The organic solvents in the electrolyte have the characteristics of low flash point, flammability and volatility, which leads to safety problems such as combustion and explosion in traditional liquid lithium-ion batteries. Especially with the development of high-energy and high-power density lithium-ion secondary batteries, the safety problem of batteries has become more prominent. Safety has always been a key factor restricting the application of lithium-ion batteries in the field of high energy and high power density.

[0003] At present, the methods for solving the safety problem of lithium batteries mainly include: all-solid-state lithium-ion battery solution, adding flame retardants to the electrolyte solution and gel electrolyte solution. Among them, the all-solid-state lithium-ion battery solution can effectively solve the safety problem of lithium batteries, but the interface impedance of all-solid-state lithium-ion batteries is large and the low-temperature performance is poor, which leads to poor rate and cycle performance, making it unable to meet the current power battery needs. Although adding flame retardants to the electrolyte can effectively improve the safety performance of lithium batteries, the presence of free flame retardants increases the internal resistance of the battery, reduces the electrochemical stability, and still has the risk of leakage. Gel electrolytes can improve the safety of lithium batteries to a certain extent while taking into account excellent ionic conductivity, but gel electrolyte lithium-ion batteries still have the risk of combustion due to the flammability of the gel electrolyte polymer matrix. Patent CN113234195A discloses the use of a gel electrolyte or lithium battery with a flame-retardant phosphorus-containing monomer. However, the flame retardancy of the phosphorus-containing monomer is limited. Therefore, the proportion of the phosphorus-containing monomer introduced needs to be more than 20% to have a certain flame retardancy. However, the introduction of a large amount of phosphorus-containing monomers will inevitably reduce the ionic conductivity and electrochemical properties of the lithium battery. At the same time, the phosphorus-containing monomer gel electrolyte has poor liquid absorption and liquid retention, so that the lithium battery still has the risk of leakage, and there is a problem of poor interface compatibility between it and the electrode material.

[0004] Therefore, it is necessary to develop a new gel electrolyte to solve the above problems. Summary of the invention

[0005] In view of the above shortcomings of the prior art, the present invention provides a gel electrolyte and a preparation method thereof and a battery to improve the safety problem of the gel electrolyte battery in the prior art and the compatibility problem between the gel electrolyte and the electrode material.

[0006] To achieve the above-mentioned object and other related objects, the present invention provides a gel electrolyte, which comprises the following raw material components, measured by mass percentage of raw materials for preparing the gel electrolyte: 60-90% of organic solvent, 5-20% of lithium salt, 0.5-5% of cross-linking agent, 1-15% of first monomer, 0.5-15% of second monomer, 0.5-15% of third monomer and 0.005-5% of initiator; wherein the first monomer, the second monomer, the third monomer, the cross-linking agent, the initiator, the organic solvent and the lithium salt are in-situ copolymerized by thermal initiation to prepare the gel electrolyte.

[0007] In one example of the present invention, the organic solvent is selected from a mixture of one or more of ethylene carbonate, propylene carbonate, dimethyl carbonate, dimethyl carbonate, ethyl methyl carbonate, diethyl carbonate, carboxylates, sulfites, and fluorinated solvents.

[0008] In one example of the present invention, the lithium salt is selected from one or a combination of lithium hexafluorophosphate, lithium bis(trifluoromethanesulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium tetrafluoroborate, lithium bis(oxalatoborate), lithium difluorooxalatoborate, lithium difluorophosphate, and lithium perchlorate.

[0009] In one example of the present invention, the cross-linking agent is a polyalkenyl phosphonate cross-linking agent.

[0010] In one example of the present invention, the cross-linking agent includes one or more of di(methacryloyloxyethyl) hydrogen phosphate, triallyl phosphate, di(methacryloyloxy)ethyl phosphate, di[2-(methacryloyloxy)ethyl]phosphate, and di[2-(acryloyloxy)ethyl]phosphate.

[0011] In an example of the present invention, the first monomer includes alkenyl acrylate monomers and / or alkenyl carbonate monomers and / or allyl ether monomers.

[0012] In one example of the present invention, the first monomer includes one or more of methyl methacrylate, ethyl methacrylate, isopropylene acetate, vinylene carbonate, allyl methyl carbonate, allyl phenyl carbonate, allyl carbonate, acrylamide, N,N-dimethylallylamine, and allyl ethers.

[0013] In one example of the present invention, the second monomer includes a fluorine-containing alkenyl carboxylate monomer and / or a fluorine-containing alkenyl carbonate monomer.

[0014] In one example of the present invention, the second monomer includes one or more of trifluoroethyl acrylate, trifluoroethyl methacrylate, 2,2,2-trifluoroethyl acrylate, methyl trifluoromethacrylate, trifluoroethyl trifluoromethacrylate, allyl trifluoromethyl carbonate, 2,2,2-trifluoroallylphenyl carbonate, and 2,2,2-trifluoroallyl carbonate.

[0015] In one example of the present invention, the third monomer includes a halogen-containing alkenyl phosphate monomer and / or a halogen-containing alkenyl phosphazene monomer composite flame retardant monomer.

[0016] In one example of the present invention, the third monomer includes one or more of allyl bis(2,2,2-trifluoroethyl) phosphate, allyl bis(trifluoromethyl) phosphate, vinyl bis(2,2,2-trifluoroethyl) phosphate, vinyl bis(trifluoromethyl) phosphate, 2,2,2-trifluoropropylene diphosphate, allyl bis(2,2,2-tribromoethyl) phosphate, allyl bis(tribromomethyl) phosphate, vinyl bis(2,2,2-tribromoethyl) phosphate, 2,2,2-trifluoropropylene (pentamethylphosphazene), and 2,2,2-tribromopropylene (pentamethylphosphazene).

[0017] In one example of the present invention, the initiator includes one or more of azobisisoheptanenitrile, azobisisobutyronitrile, dimethyl azobisisobutyrate, tert-butyl peroxy-2-ethylhexanoate, dibenzoyl peroxide, dilauroyl peroxide, dodecyl peroxide, and diisopropylbenzene peroxide.

[0018] Another aspect of the present invention provides a lithium ion battery, which comprises the gel electrolyte of the present invention or the gel electrolyte prepared by the preparation method of the present invention.

[0019] The present invention also provides a method for preparing a lithium ion battery, comprising the following steps:

[0020] Adding lithium salt to an organic solvent and stirring until the lithium salt is completely dissolved to obtain a reference electrolyte;

[0021] Under an inert atmosphere, adding a crosslinking agent, a first monomer, a second monomer and a third monomer to a portion of the reference electrolyte, stirring and mixing the mixture to obtain a first mixed solution;

[0022] Under an inert atmosphere, adding an initiator to another portion of the reference electrolyte, stirring and mixing, and obtaining a second mixed solution;

[0023] Under an inert atmosphere, mixing the second mixed solution and the first mixed solution, and stirring them uniformly to obtain a third mixed solution;

[0024] The third mixed solution is injected into a dry lithium-ion battery cell, and then vacuum heat-sealed and heated for polymerization and curing to obtain a gel electrolyte.

[0025] In one example of the present invention, the positive electrode material of the lithium-ion battery cell is one or more of lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium cobalt oxide, lithium nickel oxide, and lithium manganese oxide; the negative electrode material of the lithium-ion battery cell is one or more of natural graphite, artificial graphite, hard carbon, soft carbon, mesophase carbon microbeads, nano-silicon, silicon oxide, and lithium metal.

[0026] In one example of the present invention, the temperature of the heating polymerization curing is 40 to 80° C., and the curing time is 1 to 72 hours.

[0027] The various functional monomers and crosslinking agents in the gel electrolyte of the present invention form a network polymer by heat-induced chain polymerization under the action of an initiator, and gel with a reference electrolyte to obtain a flame-retardant gel electrolyte. The introduction of various functional monomers allows the copolymer to have various functional groups, thereby giving the copolymer multiple functions. And due to the differences in polarity, functional groups and molecular structures of various monomers, the physical and chemical properties such as polarity, configuration, melting point, glass transition temperature of the copolymer molecular chain can be adjusted by adjusting the ratio between monomers and the interaction between different monomers, thereby utilizing the synergistic effect between various functional monomers to design the desired in-situ copolymer gel electrolyte.

[0028] Introducing a first monomer with excellent liquid absorption and liquid retention into the gel electrolyte can effectively improve the liquid absorption rate and liquid retention rate of the gel electrolyte, effectively reduce the flash point of the organic solvent in the reference electrolyte to improve its flame retardant properties, and at the same time solve the leakage problem of a single flame retardant monomer gel electrolyte, and can also effectively improve the interface compatibility between the gel electrolyte and the electrode material.

[0029] Introducing a second monomer of fluorinated alkenyl carboxylates and / or fluorinated alkenyl carbonates into the gel electrolyte can effectively promote the dissociation and desolvation of lithium salts, improve the ionic conductivity and electrochemical properties of lithium batteries, broaden the electrochemical window of the gel electrolyte matrix polymer, and improve the flame retardant properties of the gel electrolyte.

[0030] A composite flame-retardant third monomer of halogen-containing alkenyl phosphate and / or halogen-containing alkenyl phosphazene with high flame retardancy is introduced into the gel electrolyte. This composite flame-retardant monomer will produce hydrogen halide (HX), phosphorus oxide free radical (PO·), ammonia (NH3), nitrogen (N2), deep nitrogen oxides, etc. when the polymer molecular chain burns at high temperature. Among them, HX and PO· can capture hydrogen free radical (H·) and hydroxyl free radical (HO·) produced during the combustion of the material to achieve a flame retardant effect, while non-flammable gases NH3, N2, deep nitrogen oxides, etc. can dilute the flammable gas and combustion-supporting gas on the surface of the material, thereby achieving a flame retardant effect. Since the composite flame-retardant monomer has the above three types of flame-retardant factors and modes, a small amount of this composite monomer can achieve an excellent flame retardant effect, and a small amount of non-free composite flame-retardant monomer will not reduce the ionic conductivity and electrochemical properties of the lithium battery.

[0031] The crosslinking agent in the gel electrolyte of the present invention is a flame retardant phosphorus-containing monomer, which can further improve the flame retardant performance of the gel electrolyte. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0033] Figure 1 is a flow chart of the preparation method of the gel electrolyte of the present invention;

[0034] Figure 2 This is a schematic diagram of the chain polymerization of the gel electrolyte of the present invention;

[0035] Figure 3 A flow chart of a gel electrolyte according to an embodiment of the present invention;

[0036] Figure 4 This is a photo of the gel electrolyte of the present invention after polymerization and curing;

[0037] Figure 5 The first cycle charge and discharge curves of the gel electrolyte lithium ion battery of the present invention and the reference electrolyte lithium ion battery;

[0038] Figure 6 The cycle performance of the gel electrolyte lithium ion battery of the present invention;

[0039] Figure 7 Benchmark electrolyte lithium-ion battery cycling performance. DETAILED DESCRIPTION

[0040] The following is an explanation of the embodiments of the present invention by specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention. It should be noted that the features in the following embodiments and the embodiments can be combined with each other without conflict. It should also be understood that the terms used in the embodiments of the present invention are intended to describe specific embodiments, rather than to limit the scope of protection of the present invention. The test methods for which specific conditions are not specified in the following examples are usually carried out under conventional conditions or according to the conditions recommended by the manufacturers.

[0041] It should be noted that the terms such as "upper", "lower", "left", "right", "middle" and "one" etc. used in this specification are only for the convenience of description and are not intended to limit the scope of implementation of the present invention. Changes or adjustments to their relative relationships, without substantially changing the technical content, should also be regarded as the scope of implementation of the present invention.

[0042] See also Figures 1 to 7 The present invention provides a gel electrolyte, a preparation method thereof and a lithium ion battery. By introducing a variety of functional monomers, the copolymer has a variety of functional groups, giving the copolymer a variety of functionalities, thereby improving the safety of the battery with the gel electrolyte.

[0043] The invention provides a gel electrolyte, comprising the following raw material components and the percentage of each component in the total mass of the raw materials is: 60-90% of an organic solvent, 5-20% of a lithium salt, 0.5-5% of a crosslinking agent, 1-15% of a first monomer, 0.5-15% of a second monomer, 0.5-15% of a third monomer and 0.005-5% of an initiator; wherein the first monomer, the second monomer, the third monomer, the crosslinking agent, the initiator, the organic solvent and the lithium salt are in situ copolymerized by thermal initiation to prepare the gel electrolyte.

[0044] The organic solvent and the lithium salt are mixed in a certain mass ratio to obtain a reference electrolyte. The first monomer, the second monomer, the third monomer, the initiator and the cross-linking agent initiate a chain reaction in the reference electrolyte through heat and in situ copolymerize with the reference electrolyte to form a gel electrolyte.

[0045] The mass percentage of the organic solvent in the raw material for preparing the gel electrolyte is 60-90%, for example, it can be any value within the above range such as 60%, 70%, 80% or 90%. The organic solvent includes a mixture of one or more of ethylene carbonate, propylene carbonate, dimethyl carbonate, dimethyl carbonate, ethyl methyl carbonate, diethyl carbonate, carboxylates, sulfites, and fluoro solvents. That is, the organic solvent can be any one of the organic solvents listed above, for example, the organic solvent is ethylene carbonate or propylene carbonate or dimethyl carbonate or dimethyl carbonate or ethyl methyl carbonate or diethyl carbonate or carboxylates or sulfites or fluoro solvents; the organic solvent can also be any two or more combinations of the organic solvents listed above, for example, the organic solvent is a mixture of ethylene carbonate and propylene carbonate or a mixture of dimethyl carbonate, dimethyl carbonate and ethyl methyl carbonate or a mixture of diethyl carbonate, carboxylates, sulfites and fluoro solvents or a mixture of propylene carbonate, dimethyl carbonate and dimethyl carbonate, etc., which are not listed one by one here. When the organic solvent is a mixture of multiple components, there is no restriction on the ratio between the components in the mixture, and they can be mixed in any ratio.

[0046] The mass percentage of lithium salt in the raw material for preparing the gel electrolyte is 5-20%, for example, it can be any value within the above range such as 5%, 10%, 15% or 20%. The lithium salt includes one or a combination of lithium hexafluorophosphate, lithium bis(trifluoromethanesulfonyl)imide, lithium bis(fluorosulfonyl)imide, lithium tetrafluoroborate, lithium bis(oxalatoborate), lithium difluorooxalatoborate, lithium difluorophosphate, and lithium perchlorate. That is, the lithium salt can be any one of the lithium salts listed above, for example, the lithium salt can be lithium hexafluorophosphate or lithium bis(trifluoromethanesulfonyl)imide or lithium bisfluoro yellow imide or lithium tetrafluoroborate or lithium bisoxalate borate or lithium difluoro oxalate borate or lithium difluorophosphate or lithium perchlorate; the lithium salt can be a combination of any two, any three or more of the lithium salts listed above, for example, the lithium salt is a combination of lithium hexafluorophosphate and lithium bis(trifluoromethanesulfonyl)imide, or a combination of lithium bisfluoro yellow imide, lithium tetrafluoroborate and lithium bisoxalate borate, or a combination of lithium difluoro oxalate borate, lithium difluorophosphate and lithium perchlorate, or a combination of lithium bisfluoro yellow imide, lithium tetrafluoroborate, lithium bisoxalate borate and lithium difluoro oxalate borate, etc., which are not listed one by one here. When the lithium salt is a combination of multiple lithium salts, the ratio between the components in the composition is not limited here, and it can be mixed in any proportion. The lithium salt includes but is not limited to the types listed above. The preparation process of the reference electrolyte may refer to the preparation method of the conventional liquid electrolyte in the art.

[0047] The mass percentage of the first monomer in the raw material for preparing the gel electrolyte is 1 to 15%, for example, it can be any value within the above range such as 1%, 5%, 10% or 15%. The first monomer has excellent liquid absorption and liquid retention, which can effectively improve the liquid absorption rate and liquid retention rate of the gel electrolyte, reduce the flash point of the organic solvent in the electrolyte to improve its flame retardant performance, and solve the leakage problem of the single flame retardant monomer gel electrolyte, and can also effectively improve the interface compatibility between the gel electrolyte and the electrode material. The first monomer includes alkenyl acrylate monomers and / or alkenyl carbonate monomers and / or allyl ether monomers, that is, the first monomer can be an alkenyl acrylate monomer, an alkenyl carbonate monomer or an allyl ether monomer, or a combination of any two or three of alkenyl acrylate monomers, alkenyl carbonate monomers and allyl ether monomers.

[0048] Further, the first monomer includes one or more of methyl methacrylate, ethyl methacrylate, isopropenyl acetate, vinylene carbonate, allyl methyl carbonate, allyl phenyl carbonate, allyl carbonate, acrylamide, N,N-dimethylallylamine, and allyl ethers. That is to say, the first monomer can be any one of the monomers listed above, for example, the first monomer is methyl methacrylate or ethyl methacrylate or isopropenyl acetate or vinylene carbonate or allyl methyl carbonate or allyl phenyl carbonate or allyl carbonate or acrylamide or N,N-dimethylallylamine or allyl ethers; the first monomer can also be any two or more combinations of the monomers listed above, for example, the first monomer is a combination of methyl methacrylate and ethyl methacrylate, or a combination of allyl phenyl carbonate and allyl carbonate, or a combination of methyl methacrylate, N,N-dimethylallylamine and allyl ethers, or a combination of allyl methyl carbonate, allyl phenyl carbonate, allyl carbonate and acrylamide, etc., which are not listed one by one here. When the first monomer is a composition, there is no restriction on the ratio of the components in the composition, and the components can be mixed in any ratio.

[0049] The mass percentage of the second monomer in the raw material for preparing the gel electrolyte is 0.5-15%, for example, it can be any value within the above range such as 0.5%, 5%, 10% or 15%. The second monomer is a fluorine-containing monomer, which can effectively promote the dissociation and desolvation of lithium salts, improve the ionic conductivity and electrochemical properties of lithium batteries, and can also broaden the electrochemical window of the gel electrolyte matrix polymer, while improving the flame retardant properties of the gel electrolyte. The second monomer includes fluorine-containing alkenyl carboxylate monomers and / or fluorine-containing alkenyl carbonate monomers, that is, the second monomer can be a fluorine-containing alkenyl carboxylate monomer or a fluorine-containing alkenyl carbonate monomer or a combination of a fluorine-containing alkenyl carboxylate monomer and a fluorine-containing alkenyl carbonate monomer.

[0050] Further, the second monomer includes one or more of trifluoroethyl acrylate, trifluoroethyl methacrylate, 2,2,2-trifluoroethyl acrylate, methyl trifluoromethacrylate, trifluoroethyl trifluoromethacrylate, allyl trifluoromethyl carbonate, 2,2,2-trifluoroallylphenyl carbonate, and 2,2,2-trifluoroallyl carbonate. That is, the second monomer can be any one of the monomers listed above, for example, the second monomer is trifluoroethyl acrylate or trifluoroethyl methacrylate or 2,2,2-trifluoroethyl acrylate or methyl trifluoromethacrylate or trifluoroethyl trifluoromethacrylate or allyl trifluoromethyl carbonate or 2,2,2-trifluoroallylphenyl carbonate or 2,2,2-trifluoroallyl carbonate; the second monomer can also be any two or more combinations of the monomers listed above, for example, the second monomer is a combination of trifluoroethyl acrylate and trifluoroethyl methacrylate. A composition, or a composition of trifluoroethyl acrylate and 2,2,2-trifluoroethyl acrylate, or a composition of 2,2,2-trifluoroethyl acrylate, methyl trifluoromethacrylate and trifluoroethyl trifluoromethacrylate, or a composition of trifluoroethyl trifluoromethacrylate, allyl trifluoromethyl carbonate, 2,2,2-trifluoroallylphenyl carbonate and 2,2,2-trifluoroallyl carbonate, etc., which are not listed one by one here. When the second monomer is a composition, there is no restriction on the proportion of each component in the composition, and they can be mixed in any proportion.

[0051] The mass percentage of the third monomer in the raw material for preparing the gel electrolyte is 0.5-15%, for example, it can be any value within the above range such as 0.5%, 5%, 10% or 15%. The third monomer is a composite flame retardant monomer with high efficiency flame retardancy, for example, the third monomer includes a halogen-containing alkenyl phosphate monomer and / or a halogen-containing alkenyl phosphazene monomer, and this composite flame retardant monomer will produce hydrogen halide (HX), phosphorus oxide free radical (PO·) and ammonia (NH3), nitrogen (N2), deep nitrogen oxides, etc. when the polymer molecular chain burns at high temperature, wherein HX and PO· can capture hydrogen free radicals (H·) and hydroxyl free radicals (HO·) generated during the combustion of the material to achieve a flame retardant effect, while non-flammable gas NH3, nitrogen N2, deep nitrogen oxides, etc. can dilute the combustible gas and combustion-supporting gas on the surface of the material, thereby achieving a flame retardant effect. Since the composite flame retardant monomer has the above three types of flame retardant factors and modes, a small amount of this composite monomer (1-10%) can be added to achieve an excellent flame retardant effect. At the same time, a small amount of non-free composite flame retardant monomer will not reduce the ionic conductivity and electrochemical properties of lithium batteries.

[0052] Further, the third monomer includes one or more of allyl bis(2,2,2-trifluoroethyl) phosphate, allyl bis(trifluoromethyl) phosphate, vinyl bis(2,2,2-trifluoroethyl) phosphate, vinyl bis(trifluoromethyl) phosphate, 2,2,2-trifluoropropylene diphosphate, allyl bis(2,2,2-tribromoethyl) phosphate, allyl bis(tribromomethyl) phosphate, vinyl bis(2,2,2-tribromoethyl) phosphate, 2,2,2-trifluoropropylene (pentamethylphosphazene), and 2,2,2-tribromopropylene (pentamethylphosphazene). That is to say, the third monomer can be any one of the monomers listed above, for example, the third monomer is allyl phosphate di(2,2,2-trifluoroethyl) ester, or allyl phosphate di(trifluoromethyl) ester, or vinyl phosphate di(2,2,2-trifluoroethyl) ester, or vinyl phosphate di(trifluoromethyl) ester or 2,2,2-trifluoropropylene diphosphate, and the like; the third monomer can also be any two or more combinations of the monomers listed above, for example, the third monomer is a combination of allyl phosphate di(2,2,2-trifluoroethyl) ester and allyl phosphate di(trifluoromethyl) ester, or a combination of vinyl phosphate di(2,2,2-trifluoroethyl) ester and vinyl phosphate di(trifluoromethyl) ester, or a combination of allyl phosphate di(2,2,2-tribromoethyl) ester, allyl phosphate di(tribromomethyl) ester and vinyl phosphate di(2,2,2-tribromoethyl) ester, and the like, which are not listed one by one here. When the third monomer is a composition of several monomers, the ratio between the components in the composition is not limited here, and they can be mixed in any ratio.

[0053] The mass percentage of the crosslinking agent in the raw material for preparing the gel electrolyte is 0.5-5%, for example, it can be any value within the above range such as 0.5%, 2%, 3% or 5%. The crosslinking agent is a flame retardant phosphorus-containing monomer, which can further improve the flame retardancy of the gel electrolyte. Furthermore, the crosslinking agent is a polyolefin phosphonate, preferably, the crosslinking agent includes one or more of di(methacryloyloxyethyl) hydrogen phosphate, triallyl phosphate, di(methacryloyloxy)ethyl phosphate, di[2-(methacryloyloxy)ethyl] phosphate, and di[2-(acryloyloxy)ethyl] phosphate. That is, the crosslinking agent can be any one of the crosslinking agents described above, for example, the crosslinking agent is di(methacryloyloxyethyl) hydrogen phosphate or triallyl phosphate or di(methacryloyloxy)ethyl phosphate or di[2-(methacryloyloxy)ethyl] phosphate or di[2-(acryloyloxy)ethyl] phosphate; the crosslinking agent can also be any two or more combinations of the crosslinking agents described above, for example, the crosslinking agent is a combination of di(methacryloyloxyethyl) hydrogen phosphate and triallyl phosphate, or a combination of triallyl phosphate and di(methacryloyloxy)ethyl phosphate, or a combination of di(methacryloyloxy)ethyl phosphate, di[2-(methacryloyloxy)ethyl] phosphate and di[2-(acryloyloxy)ethyl] phosphate, etc., which are not listed one by one here. When the crosslinking agent is a composition, there is no restriction on the proportion of each component in the composition, and it can be mixed in any proportion.

[0054] The mass percentage of the initiator in the raw material for preparing the gel electrolyte is 0.005-5%, for example, any value within the above range such as 0.005%, 1%, 3% or 5%. The initiator includes one or more of azobisisoheptanenitrile, azobisisobutyronitrile, dimethyl azobisisobutyrate, tert-butyl peroxy-2-ethylhexanoate, dibenzoyl peroxide, dilauroyl peroxide, dodecyl peroxide, and diisopropylbenzene peroxide. That is, the initiator can be any one of the above-mentioned types, for example, the initiator can be azobisisoheptanitrile or azobisisobutyronitrile or dimethyl azobisisobutyrate or peroxy-2-ethylhexanoic acid tert-butyl ester or dibenzoyl peroxide or dilauroyl peroxide or dodecanoyl peroxide or dicumyl peroxide; it can also be a combination of any two or more of the above-mentioned types, for example, the initiator is a composition of azobisisoheptanitrile and azobisisobutyronitrile, or a composition of dimethyl azobisisobutyrate and peroxy-2-ethylhexanoic acid tert-butyl ester, or a composition of dilauroyl peroxide, dodecanoyl peroxide and dicumyl peroxide, etc., which are not listed one by one here. When the initiator is several combinations, the ratio of each component in the composition is not limited here, and it can be mixed in any proportion.

[0055] Another aspect of the present invention provides a method for preparing a gel electrolyte, comprising the following steps:

[0056] S1. Adding lithium salt into an organic solvent and stirring until the lithium salt is completely dissolved to obtain a reference electrolyte;

[0057] S2, taking a portion of the reference electrolyte, adding the cross-linking agent, the first monomer, the second monomer and the third monomer to the reference electrolyte under an inert atmosphere, stirring and mixing to obtain a first mixed solution;

[0058] S3, taking another portion of the reference electrolyte, adding the initiator to the reference electrolyte under an inert atmosphere, stirring and mixing to obtain a second mixed solution;

[0059] S4. Under an inert atmosphere, the first mixed solution and the second mixed solution are mixed and stirred to obtain a third mixed solution;

[0060] S5. Inject the third mixed solution into a dry lithium-ion battery cell, heat-seal it in vacuum, and then heat and polymerize it to obtain a gel electrolyte.

[0061] Before performing step S1, the raw material components are weighed according to the following mass percentages: 60-90% organic solvent, 5-20% lithium salt, 0.5-5% cross-linking agent, 1-15% first monomer, 0.5-15% second monomer, 0.5-15% third monomer and 0.005-5% initiator.

[0062] Preferably, the injection process of step S1 to step S5 is carried out at room temperature to prevent the organic solvent from volatilizing during the stirring process. During the preparation process, there is no restriction on the stirring method, and conventional stirring methods in the art can be used, with the principle of mixing the components evenly.

[0063] Preferably, steps S2 to S4 are performed under an inert atmosphere, such as stirring and mixing in an argon environment, to prevent the air from affecting the polymerization reaction.

[0064] In step S5, the polymerization curing process can also be carried out in other temperature control devices, as long as the curing temperature is reached. Preferably, curing is carried out in a dry lithium-ion battery cell without liquid injection, and a gel electrolyte lithium battery can be obtained at the same time as the gel electrolyte. Compared with curing first and then assembling the battery, the matching degree of the interface between the gel electrolyte and the electrode material can be improved.

[0065] The positive electrode material of the lithium-ion battery cell is one or more combinations of lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium cobalt oxide, lithium nickel oxide, and lithium manganese oxide. For example, the positive electrode material is lithium nickel cobalt manganese oxide or lithium manganese oxide or a combination of lithium nickel cobalt aluminum oxide and lithium cobalt oxide, etc. The negative electrode material of the lithium-ion battery cell is one or more combinations of natural graphite, artificial graphite, hard carbon, soft carbon, mesophase carbon microspheres, nano silicon, silicon oxide, and lithium metal. For example, the negative electrode material is nano silicon or natural graphite or hard carbon or a combination of nano silicon and silicon oxide, etc. The assembly method of the lithium-ion battery cell is not limited here, and the conventional assembly method in the art can be used.

[0066] The heating polymerization curing temperature in step S5 is 40 to 80°C, for example, 40°C, 60°C or 80°C, etc.; the heating polymerization curing time is 1 to 72 hours, and further, the curing time is 10 to 60 hours, for example, 10 hours, 30 hours, 50 hours or 60 hours, etc., etc. Figure 2 That is, the first monomer (M1), the second monomer (M2), the third monomer (M3) and the crosslinking agent (M4) undergo chain polymerization under the action of high temperature and an initiator to form a network polymer.

[0067] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solution of the present invention. The described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. The preparation process of the following embodiments can be found in Figure 3 .

[0068] Example 1

[0069] The raw materials were weighed according to the following mass ratio: 75% organic solvent (ethylene carbonate, ethyl methyl carbonate, diethyl carbonate in a mass ratio of 1:1:1, and 8% of the mass content of organic solvent was added to fluoroethylene carbonate), 7% lithium hexafluorophosphate (lithium salt), 5% methyl methacrylate (first monomer), 2% di(methacryloyloxyethyl) hydrogen phosphate (cross-linking agent), 2% trifluoroethyl acrylate (second monomer) and 8% di(trifluoromethyl) vinyl phosphate (third monomer), and 1% azobisisoheptonitrile (initiator).

[0070] Preparation process see Figure 3 :

[0071] (1) Ethylene carbonate, ethyl methyl carbonate, and diethyl carbonate are mixed in a mass ratio of 1:1:1, and then fluoroethylene carbonate having a mass content of 8% of an organic solvent is added, and then lithium hexafluorophosphate is added at room temperature, and mechanically stirred until the lithium salt is completely dissolved to obtain a reference electrolyte;

[0072] (2) dividing the reference electrolyte into two parts, adding 2% by weight of di(methacryloyloxyethyl) hydrogen phosphate, 5% by weight of methyl methacrylate, 2% by weight of trifluoroethyl acrylate and 8% by weight of di(trifluoromethyl) vinyl phosphate to one part of the reference electrolyte at room temperature and in an argon environment, and mixing them uniformly with mechanical stirring to obtain a first mixed solution;

[0073] (3) at room temperature and in an argon atmosphere, adding 1% by weight of azobisisoheptanenitrile to another portion of the reference electrolyte and mechanically stirring until completely dissolved to obtain a second mixed solution;

[0074] (4) at room temperature and in an argon environment, adding the first mixed solution obtained in step (2) to the second mixed solution obtained in step (3), and mixing them uniformly with mechanical stirring to obtain a third mixed solution;

[0075] (5) At room temperature, the third mixed solution obtained in step (4) is injected into a dry lithium-ion battery cell without liquid injection, and then heated for polymerization and curing after vacuum heat sealing, wherein the heating temperature is 70° C. and the heating time is 5 h. The negative electrode material of the battery cell is silicon carbon, and the positive electrode material is LiNi 0.8 Co 0.1 Mn 0.1 O2(NCM811).

[0076] Example 2

[0077] The raw materials were weighed according to the following mass ratio: 60% organic solvent (ethylene carbonate, ethyl methyl carbonate, diethyl carbonate in a mass ratio of 1:1:1, and 8% of the mass content of organic solvent was added to fluoroethylene carbonate), 15% lithium hexafluorophosphate (lithium salt), 10% methyl methacrylate (first monomer), 4% di(methacryloyloxyethyl) hydrogen phosphate (cross-linking agent), 8% trifluoroethyl acrylate (second monomer) and 1% di(trifluoromethyl) vinyl phosphate (third monomer), and 2% azobisisoheptonitrile (initiator).

[0078] The preparation process is the same as that in Example 1.

[0079] Example 3

[0080] The raw materials were weighed according to the following mass ratio: 90% organic solvent (ethyl methyl carbonate and diethyl carbonate in a mass ratio of 1:1, and 8% of the mass content of organic solvent fluoroethylene carbonate was added), 5% lithium hexafluorophosphate (lithium salt), 1% isopropenyl acetate (first monomer), 0.5% triallyl phosphate (cross-linking agent), 1% 2,2,2-trifluoroethyl acrylate (second monomer) and 1% vinyl bis(2,2,2-trifluoroethyl) phosphate, 1.5% dimethyl azobisisobutyrate (initiator).

[0081] The preparation process is the same as that in the example.

[0082] Example 4

[0083] The raw materials were weighed according to the following mass ratio: 60% organic solvent (ethylene carbonate, ethyl methyl carbonate, diethyl carbonate in a mass ratio of 1:1:1, and 8% of the mass content of organic solvent was added to fluoroethylene carbonate), 20% lithium hexafluorophosphate (lithium salt), 15% ethyl methacrylate (first monomer), 2% di(methacryloyloxy)ethyl phosphate (cross-linking agent), 0.5% trifluoroethyl methacrylate (second monomer) and 0.5% di(trifluoromethyl) allyl phosphate (third monomer), and 2% dimethyl azobisisobutyrate (initiator).

[0084] The preparation process is the same as that in Example 1.

[0085] Example 5

[0086] The raw materials were weighed according to the following mass ratio: 60% organic solvent (ethylene carbonate, ethyl methyl carbonate, diethyl carbonate in a mass ratio of 1:1:1, and 8% of fluoroethylene carbonate was added as the organic solvent), 10% lithium hexafluorophosphate (lithium salt), 3% allyl carbonate (first monomer), 1.5% di[2-(methacryloyloxy)ethyl] phosphate (cross-linking agent), 15% 2,2,2-trifluoroallyl carbonate (second monomer) and 10% 2,2,2-tribromopropylene (pentamethylphosphazene) (third monomer), and 0.5% dodecanoyl peroxide (initiator).

[0087] The preparation process is the same as that in Example 1.

[0088] Example 6

[0089] The raw materials were weighed according to the following mass ratio: 60% organic solvent (ethylene carbonate, ethyl methyl carbonate, diethyl carbonate in a mass ratio of 1:1:1, and 8% of the mass content of organic solvent fluoroethylene carbonate was added), 10% lithium hexafluorophosphate (lithium salt), 7% ethyl methacrylate (first monomer), 1% di(methacryloyloxyethyl) hydrogen phosphate (cross-linking agent), 15% trifluoroethyl acrylate (second monomer), 5% trifluorovinyl bis(2,2,2-trifluoroethyl) phosphate (third monomer), and 2% azobisisobutyronitrile (initiator).

[0090] Example 7

[0091] The raw materials were weighed according to the following mass ratio: 60% organic solvent (ethylene carbonate, ethyl methyl carbonate, diethyl carbonate in a mass ratio of 1:1:1, and 8% of the mass content of organic solvent fluoroethylene carbonate was added), 10% lithium hexafluorophosphate (lithium salt), 8% methyl methacrylate (first monomer), 5% di(methacryloyloxyethyl) hydrogen phosphate (cross-linking agent), 10% trifluoroethyl acrylate (second monomer) and 5% di(trifluoromethyl) vinyl phosphate (third monomer), and 2% azobisisoheptonitrile (initiator).

[0092] The preparation process is the same as that in Example 1.

[0093] Example 8

[0094] The raw materials were weighed according to the following mass ratio: 60% organic solvent (ethylene carbonate, ethyl methyl carbonate, diethyl carbonate in a mass ratio of 1:1:1, and 8% of the mass content of organic solvent fluoroethylene carbonate was added), 10% lithium hexafluorophosphate (lithium salt), 5% methyl methacrylate (first monomer), 2% di(methacryloyloxyethyl) hydrogen phosphate (cross-linking agent), 8% trifluoroethyl acrylate (second monomer) and 10% di(trifluoromethyl) vinyl phosphate (third monomer), and 5% azobisisoheptonitrile (initiator).

[0095] The preparation process is the same as that in Example 1.

[0096] Comparative Example

[0097] As a control, the difference between the comparative example and Example 1 is that steps (2)-(4) are omitted, di(methacryloyloxyethyl) hydrogen phosphate, methyl methacrylate, trifluoroethyl acrylate, di(trifluoromethyl) vinyl phosphate and azobis(isoheptylonitrile) are not added, and in step (5), the reference electrolyte in step (1) of Example 1 is injected into the uninjected dry battery cell and vacuum heat-sealed.

[0098] See also Figure 4After the third mixed solution prepared in Example 1 (mixed solution of the reaction system for preparing the gel electrolyte) was cured by heating at 70° C. for 5 hours, it was cured into a gel state and could not flow.

[0099] Acupuncture safety performance tests were performed on Examples 1 to 8 and the comparative example. The test results are shown in Table 1.

[0100] Table 1: Acupuncture test results of Examples 1 to 8 and Comparative Examples

[0101]

[0102]

[0103] From the test results in Table 1, it can be seen that the gel electrolyte lithium ion battery of the present invention can safely pass through the metal puncture 30 times in most cases without combustion or explosion, and only one or two combustion phenomena occur, indicating that the gel electrolyte lithium battery of the present invention has excellent flame retardant safety performance. However, after being punctured by a needle, the reference electrolyte lithium batteries in the comparative example all exploded and burned without exception.

[0104] See also Figure 5 , Figure 5 Compared with the reference electrolyte lithium battery obtained in the comparative example, the first cycle 0.1C charge and discharge curves of the gel electrolyte lithium battery obtained in Example 1 are almost completely overlapped, and the capacity decrease is less than 3%, indicating that the capacity of the gel electrolyte lithium battery prepared in the present invention is comparable to that of a liquid lithium ion battery, and the addition of monomer polymers does not affect the flow of conductive ions in the battery.

[0105] See also Figure 6 and Figure 7 , Figure 6 is the cycle curve of the gel electrolyte in Example 1 of the present invention, Figure 7 is the cycle curve of the reference electrolyte lithium battery in the comparative example, through Figure 6 and Figure 7 It can be seen that the gel electrolyte lithium battery in Example 1 has the same cycling performance at 1C rate as the reference electrolyte lithium battery in the comparative example, and the capacity retention rate is about 95% after 600 cycles.

[0106] In summary, the present invention uses multiple functional monomers and cross-linking agents to copolymerize in situ under the action of an initiator to prepare a multifunctional gel electrolyte, and improves the comprehensive properties of the gel electrolyte such as flame retardancy and electrochemical properties through the synergistic effect of multiple functional monomers. Therefore, the present invention effectively overcomes some practical problems in the prior art and has high utilization value and use significance.

[0107] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.

Claims

1. A gel electrolyte, characterized in that: The raw materials for preparing the gel electrolyte include the following raw material components in terms of mass percentage: Organic solvent 60~90%; Lithium salt 5~20%; The first monomer is 1~15%; The second monomer is 0.5~15%; The third monomer is 0.5~15%; Cross-linking agent 0.5~5%; Initiator 0.005~5%; Wherein, the first monomer includes one or more of alkenyl acrylate monomers and / or alkenyl carbonate monomers and / or allyl ether monomers; The second monomer includes a fluorine-containing alkenyl carboxylate monomer and / or a fluorine-containing alkenyl carbonate monomer; The third monomer includes a halogen-containing alkenyl phosphate monomer and / or a halogen-containing alkenyl phosphazene monomer composite flame retardant monomer; The gel electrolyte is prepared by in-situ copolymerization of the first monomer, the second monomer, the third monomer, the crosslinking agent, the initiator, the organic solvent and the lithium salt through thermal initiation.

2. The gel electrolyte according to claim 1, characterized in that The crosslinking agent is a polyolefin phosphonate crosslinking agent, and the crosslinking agent includes one or more of di(methacryloyloxyethyl) hydrogen phosphate, triallyl phosphate, di(methacryloyloxy)ethyl phosphate, di[2-(methacryloyloxy)ethyl]phosphate, and di[2-(acryloyloxy)ethyl]phosphate.

3. The gel electrolyte according to claim 1, characterized in that The first monomer includes one or more of methyl methacrylate, ethyl methacrylate, isopropylene acetate, vinylene carbonate, allyl methyl carbonate, allyl phenyl carbonate, allyl carbonate, acrylamide, N,N-dimethylallylamine, and allyl ethers.

4. The gel electrolyte according to claim 1, characterized in that The second monomer includes one or more of trifluoroethyl acrylate, trifluoroethyl methacrylate, 2,2,2-trifluoroethyl acrylate, methyl trifluoromethacrylate, trifluoroethyl trifluoromethacrylate, allyl trifluoromethyl carbonate, 2,2,2-trifluoroallylphenyl carbonate, and 2,2,2-trifluoroallyl carbonate.

5. The gel electrolyte according to claim 1, characterized in that The third monomer includes one or more of allyl bis(2,2,2-trifluoroethyl) phosphate, allyl bis(trifluoromethyl) phosphate, vinyl bis(2,2,2-trifluoroethyl) phosphate, vinyl bis(trifluoromethyl) phosphate, 2,2,2-trifluoropropylene diphosphate, allyl bis(2,2,2-tribromoethyl) phosphate, allyl bis(tribromomethyl) phosphate, vinyl bis(2,2,2-tribromoethyl) phosphate, 2,2,2-trifluoropropylene (pentamethylphosphazene), and 2,2,2-tribromopropylene (pentamethylphosphazene).

6. The gel electrolyte according to claim 1, characterized in that: The initiator includes one or more of azobisisoheptanenitrile, azobisisobutyronitrile, dimethyl azobisisobutyrate, tert-butyl peroxy-2-ethylhexanoate, dibenzoyl peroxide, dilauroyl peroxide, dodecyl peroxide, and dicumyl peroxide.

7. The gel electrolyte according to claim 1, characterized in that The organic solvent includes one or more mixtures of ethylene carbonate, propylene carbonate, dimethyl carbonate, ethyl methyl carbonate, diethyl carbonate, carboxylates, sulfites, and fluorinated solvents; the lithium salt is selected from one or more combinations of lithium hexafluorophosphate, lithium bis(trifluoromethanesulfonyl)imide, lithium bis(fluorosulfonyl)imide, lithium tetrafluoroborate, lithium bis(oxalatoborate), lithium difluorooxalatoborate, lithium difluorophosphate, and lithium perchlorate.

8. A method for preparing the gel electrolyte according to claim 1, characterized in that: The following steps are involved: Adding lithium salt to an organic solvent and stirring until the lithium salt is completely dissolved to obtain a reference electrolyte; Under an inert atmosphere, adding a crosslinking agent, a first monomer, a second monomer and a third monomer to a portion of the reference electrolyte, stirring and mixing the mixture to obtain a first mixed solution; Under an inert atmosphere, adding an initiator to another portion of the reference electrolyte, mixing and stirring to obtain a second mixed solution; Under an inert atmosphere, the second mixed solution and the first mixed solution are mixed and stirred uniformly to obtain a third mixed solution; The third mixed solution is injected into a dry lithium-ion battery cell, and then vacuum heat-sealed and heated for polymerization and curing to obtain a gel electrolyte.

9. The preparation method according to claim 8, characterized in that The temperature of the heating polymerization curing is 40-80° C., and the curing time is 1-72 h.

10. A lithium ion battery, characterized in that: The invention comprises the gel electrolyte according to claim 1.