A kind of polythioetherimide modified epoxy resin and preparation method thereof
By adding a small amount of thermoplastic polythioetherimide to epoxy resin and using melt blending and thermal insulation curing processes, the problems of insufficient fatigue resistance and impact resistance of epoxy resin are solved, and its performance and glass transition are significantly improved. temperature, suitable for industrial production and reducing costs.
Patent Information
- Application Number
- CN202211005458.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-22
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2042-08-22
AI Technical Summary
After curing, epoxy resin has problems such as high internal stress, brittleness, and poor fatigue resistance and impact resistance, resulting in poor peel strength and shear strength, making it unable to meet the requirements of some industrial fields that require high performance.
By adding a small amount of thermoplastic polysulfide imide to epoxy resin, using melt blending and three-stage thermal insulation curing process, it can be evenly dispersed and improve toughness and impact strength. At the same time, appropriate curing agent and release agent can be selected to control Phase structure and properties.
The impact properties, flexural strength and tensile modulus of epoxy resin are significantly improved, and the glass transition temperature is increased by more than 10°C. The process is simple and the equipment requirements are low. It is suitable for industrial production and reduces modification costs.
Smart Images

Figure BDA0003808495070000021 
Figure BDA0003808495070000022 
Figure BDA0003808495070000031
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of epoxy resin composite materials, and particularly relates to a polythioetherimide-modified epoxy resin and a preparation method thereof. Background Art
[0002] Epoxy resin (EP) is an epoxy oligomer. It must be added with a curing agent to react in order to form a three-dimensional network thermosetting plastic with application value. The cured EP has good physical and chemical properties, excellent bonding strength to the surface of metal and non-metallic materials, small shrinkage, good product dimensional stability, high hardness, good stress transmission, stability to alkali and most solvents, easy processing and low cost. However, since EP forms a three-dimensional network structure with a very high cross-linking density after curing, it has the disadvantages of large internal stress, brittleness, poor fatigue resistance and impact resistance, resulting in its poor peel strength, shear strength, low cracking strain and other shortcomings. Therefore, although unmodified EP is relatively widely used in many industrial fields, it cannot meet the requirements of certain fields of use.
[0003] By modifying epoxy resin and increasing its toughness, the disadvantage of poor impact resistance can be overcome and the performance of composite materials can be greatly improved. There are many ways to modify it, such as modifying epoxy resin with rubber, but its glass transition temperature is low, especially when the rubber content is increased to obtain better toughness and fracture strength, the glass transition temperature of the modified epoxy resin is particularly significantly reduced; in addition, the use of thermoplastic resin to modify epoxy resin has a better effect. Thermoplastic resin not only has good toughness, but also has high modulus and heat resistance. Adding it to epoxy resin as a toughening agent can improve the toughness of epoxy resin without affecting the modulus and heat resistance of epoxy cured product. Commonly used thermoplastic resins include polyether sulfone, polysulfone, etc., but the use of polysulfone to modify epoxy resin will affect other mechanical properties while improving the heat resistance and toughness of epoxy resin, and the heat resistance is not improved enough.
[0004] The Chinese patent document with publication number CN105907040A discloses an epoxy resin composition suitable for low temperature use, which includes a multifunctional epoxy resin, a bisphenol A polyether epoxy resin, a thermoplastic resin, a curing agent and an interface modifier, wherein the thermoplastic resin is selected from polyether sulfone or polyaryletherketone. In the application, the thermoplastic resin is used as a low temperature anti-microcrack modifier to further improve the low temperature performance and adjust the rheological properties of the epoxy composition. However, more thermoplastic resin needs to be added to the epoxy resin composition to achieve good use effect.
[0005] The Chinese patent document with publication number CN1263909A discloses a method for preparing a polyetherimide-modified epoxy resin, in which the epoxy resin is modified by a blending method, the amount of polyetherimide added is 5-45 Phr, and the flexural modulus is increased to 2.6 GPa. However, the effect of improving the toughness and modulus of the epoxy resin modified by this method is not obvious, and the amount of polyetherimide added is relatively large, which is expensive. Summary of the invention
[0006] The invention provides a polythioetherimide-modified epoxy resin. The modified epoxy resin has a simple preparation process and mild modification conditions. By adding a small amount of thermoplastic resin polythioetherimide, the comprehensive properties of the epoxy resin, especially the impact strength, are effectively improved.
[0007] The specific technical solutions adopted are as follows:
[0008] A polythioetherimide-modified epoxy resin comprises the following raw materials in parts by weight:
[0009]
[0010] Polythioetherimide is an excellent thermoplastic heat-resistant polymer material with excellent mechanical properties and heat resistance. When the addition amount is 0.5-4.5 parts, the impact properties of modified epoxy resin can be improved. The addition amount of polythioetherimide is limited by the solubility performance. Too much addition will result in excessive viscosity and affect the processing performance. Too little addition will have a poor effect.
[0011] The epoxy resin includes bisphenol A epoxy resin or 4,4'-diaminodiphenylmethane tetraglycidyl ether (TGDDM), wherein the bisphenol A epoxy resin includes E-42, E-51 or E-55.
[0012] The polythioetherimide is a mixture having three structural units of formula (I), formula (II) and formula (III):
[0013]
[0014]
[0015] Wherein, x, y and z are positive integers, 10<x+y+z<100; R is a diamine residue derived from a diamine monomer, and the diamine monomer includes an aliphatic diamine or an aromatic diamine.
[0016] Specifically, the diamine monomer is selected from at least one of p-phenylenediamine, m-phenylenediamine, 4,4'-diaminodiphenyl ether, 4,4'-diaminobenzophenone, 3,4'-diaminobenzophenone, 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenyl sulfone, 3,3'-dichloro-4,4'-diaminodiphenylmethane, 4,4'-bis(4-aminophenoxy)biphenyl, 2,4-toluenediamine and 3,3'-dimethyl-4,4'-diaminodiphenylmethane.
[0017] The polythioetherimide is a mixed material, and the thioether bond is located at the 3-bond or 4-bond of the polymer, wherein the 3-bond and the 4-bond refer to the isomeric positions on the phthalimide ring in the structural unit containing phthalimide.
[0018] The curing agent is at least one of an anhydride curing agent, an aliphatic amine curing agent or an aromatic amine curing agent. Anhydride curing agents include phthalic anhydride, trimellitic anhydride, pyromellitic dianhydride, etc.; aliphatic amine curing agents include hexamethylenediamine, butanediamine, diethylmethyltriamine, etc.; aromatic amine curing agents include 4,4'-diaminodiphenylmethane (DDM), 4.4-diaminodiphenyl ether (ODA), 4,4'-diaminodiphenyl sulfone (DDS), etc.
[0019] Taking heat resistance and solubility into consideration, the curing agent is preferably an aromatic amine curing agent.
[0020] The release agent can prevent the molded epoxy resin-based products from sticking to the mold, resulting in incomplete product appearance and quality defects, and can make the products easily removed from the mold while ensuring the surface quality of the product and the mold are intact. The release agent is at least one of HD-1915, HD-9182 and HD-9185 of Shanghai Dongheng Chemical Co., Ltd.
[0021] The present invention also provides a method for preparing the polythioetherimide-modified epoxy resin, comprising the following steps:
[0022] (1) Under the protection of nitrogen atmosphere, after heating the epoxy resin, adding polysulfide etherimide, stirring, and melt blending;
[0023] (2) Cooling the blend obtained in step (1) to 115-135° C., adding a curing agent and a release agent, stirring until uniform and transparent, vacuum degassing, and then pouring into a mold, and obtaining the polysulfide etherimide-modified epoxy resin after curing.
[0024] In the above preparation method, the epoxy resin and the polythioetherimide are melt blended, and the epoxy resin is heated to 140-160°C before the polythioetherimide is added, and the temperature of the melt blending is 140-160°C. The modified epoxy resin obtained by physical blending needs to effectively control the system phase structure in the polymerization reaction induced phase separation process to greatly improve its performance, and has the disadvantages of uneven mixing, difficulty in phase structure control, and poor toughening effect; while the method of the present invention introduces polythioetherimide soluble in epoxy resin, and makes it uniformly dispersed in epoxy resin under molten conditions, which can improve toughness and impact strength without affecting the thermal properties of epoxy resin.
[0025] Preferably, the curing process is a three-stage heat preservation curing process, wherein the first stage heat preservation curing parameters are: 80-210°C, 1-2h; the second stage heat preservation curing parameters are: 160-240°C, 1-3h; the third stage heat preservation curing parameters are: 200-260°C, 1-3h. The heat curing time is short, less than 8 hours; the above parameters can make the curing complete, which is very suitable for the polythioetherimide modified epoxy resin in this application.
[0026] Preferably, the impact resistance of the polythioetherimide modified epoxy resin is 7-10 kJ / m 2 , the flexural strength is 106-130MPa, the tensile modulus is 3.0-4.0GPa, and the glass transition temperature is 230-240℃.
[0027] The polysulfide imide-modified epoxy resin can be used as an adhesive, molding powder, etc.
[0028] Compared with the prior art, the present invention has the following beneficial effects:
[0029] (1) The preparation process of the present invention is simple, the equipment requirements are low, the reaction conditions are mild, and it is easy to industrialize the production. The epoxy resin is modified by using thermoplastic polythioetherimide soluble in the epoxy resin. By adding the polythioetherimide, the impact property, bending strength, and tensile modulus performance indicators of the modified epoxy resin are improved by about 80%, 20%, and 20%, respectively; and the glass transition temperature is increased by more than 10°C.
[0030] (2) In the polythioetherimide-modified epoxy resin provided by the present invention, the addition amount of polythioetherimide is low, and only 0.5-4.5 parts of the addition amount is required to greatly improve the comprehensive performance of the epoxy resin. DETAILED DESCRIPTION
[0031] The present invention will be further described below in conjunction with the examples. It should be understood that these examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention.
[0032] In the following examples, the raw materials are selected as follows:
[0033] The preparation process of polythioetherimide PTEI is as follows: a mixture of 3-chlorophthalic anhydride and 4-chlorophthalic anhydride and 4,4'-diaminodiphenyl ether are reacted in a solvent system of DMF and toluene to obtain a crude dichloromonomer; the crude product is recrystallized with DMSO and used for the next polymerization reaction; under an argon atmosphere, a system of dichloromonomer, anhydrous lithium sulfide, anhydrous potassium carbonate and DMSO is reacted to obtain a light yellow polyimide powder. The light yellow polyimide powder has a logarithmic viscosity of 0.48 dL / g measured in m-cresol with a concentration of 0.5 g / dL at 30°C, and is a mixture having the following three structural units:
[0034]
[0035] Wherein, x, y and z are positive integers, 10<x+y+z<100;
[0036] The curing agent is an aromatic amine curing agent 4,4'-diaminodiphenyl sulfone (DDS);
[0037] The release agent is HD-1915 or HD-9182 (product of Shanghai Dongheng Chemical Co., Ltd.).
[0038] Example 1
[0039] (1) Under nitrogen atmosphere, 100 parts by weight of epoxy resin (4,4'-diaminodiphenylmethane tetraglycidyl ether) was heated to 150° C., and 0.8 parts by weight of polysulfide ether imide was added, and stirred at the temperature for 4 hours to melt blend;
[0040] (2) The blend obtained in step (1) is cooled to 130° C., 54 parts by weight of a curing agent and 2 parts by weight of a release agent are added, the mixture is stirred until uniform and transparent, and then vacuum degassing is performed, and the mixture is poured into a mold preheated at 180° C. After curing, the mixture is naturally cooled to obtain the polysulfide etherimide-modified epoxy resin; the curing process is: keeping warm at 180° C. for 1 hour, keeping warm at 200° C. for 2 hours, and keeping warm at 240° C. for 2 hours.
[0041] Example 2
[0042] (1) Under nitrogen atmosphere, 100 parts by weight of epoxy resin (4,4'-diaminodiphenylmethane tetraglycidyl ether) was heated to 160° C., and 1.6 parts by weight of polysulfide imide was added, and stirred at the temperature for 4 hours to melt blend;
[0043] (2) The blend obtained in step (1) is cooled to 130° C., 60 parts by weight of a curing agent and 1.5 parts by weight of a release agent are added, the mixture is stirred until uniform and transparent, and then vacuum degassing is performed, and the mixture is poured into a mold preheated at 180° C. After curing, the mixture is naturally cooled to obtain the polysulfide etherimide-modified epoxy resin; the curing process is: keeping warm at 190° C. for 1 hour, keeping warm at 210° C. for 2 hours, and keeping warm at 240° C. for 2 hours.
[0044] Example 3
[0045] (1) Under nitrogen atmosphere, 100 parts by weight of epoxy resin (4,4'-diaminodiphenylmethane tetraglycidyl ether) was heated to 150° C., and 3.1 parts by weight of polysulfide imide was added, and stirred at the temperature for 4 hours to melt blend;
[0046] (2) The blend obtained in step (1) is cooled to 135° C., 54 parts by weight of a curing agent and 2 parts by weight of a release agent are added, the mixture is stirred until uniform and transparent, and then vacuum degassing is performed, and then the mixture is poured into a mold preheated at 180° C., and the mixture is naturally cooled after curing to obtain the polysulfide etherimide-modified epoxy resin; the curing process is: keeping warm at 180° C. for 1 hour, keeping warm at 200° C. for 2 hours, and keeping warm at 240° C. for 2 hours.
[0047] Example 4
[0048] (1) Under nitrogen atmosphere, 100 parts by weight of epoxy resin (bisphenol A epoxy resin-E51) was heated to 150° C., and then 4 parts by weight of polysulfide imide was added and stirred at the temperature for 4 hours to melt blend;
[0049] (2) The blend obtained in step (1) is cooled to 130° C., 54 parts by weight of a curing agent and 2 parts by weight of a release agent are added, the mixture is stirred until uniform and transparent, and then vacuum degassing is performed, and the mixture is poured into a mold preheated at 180° C. After curing, the mixture is naturally cooled to obtain the polysulfide etherimide-modified epoxy resin; the curing process is: keeping warm at 180° C. for 1 hour, keeping warm at 200° C. for 2 hours, and keeping warm at 240° C. for 2 hours.
[0050] Example 5
[0051] (1) Under nitrogen atmosphere, 100 parts by weight of epoxy resin (bisphenol A epoxy resin-E51) was heated to 150° C., and 4.5 parts by weight of polysulfide imide was added, and stirred at the temperature for 4 hours to melt blend;
[0052] (2) The blend obtained in step (1) is cooled to 125° C., 50 parts by weight of a curing agent and 3 parts by weight of a release agent are added, the mixture is stirred until uniform and transparent, and then vacuum degassing is performed, and the mixture is poured into a mold preheated at 180° C. After curing, the mixture is naturally cooled to obtain the polysulfide etherimide-modified epoxy resin; the curing process is: keeping warm at 180° C. for 1 hour, keeping warm at 220° C. for 2 hours, and keeping warm at 250° C. for 2 hours.
[0053] Comparative Example 1
[0054] The preparation method of the modified epoxy resin in this comparative example is the same as that in Example 1, except that polysulfide ether imide is not added in step (1).
[0055] Sample analysis
[0056] The performance tests were conducted on the modified epoxy resin materials in Examples 1-5 and Comparative Example 1. The test results are shown in Table 1 below.
[0057] Table 1 Properties of modified epoxy resins in Examples 1-5 and Comparative Example 1
[0058]
[0059] From the data in the table above, it can be seen that as the amount of polythioetherimide added increases, the impact performance of the modified epoxy resin increases with the addition of PTEI, reaching a maximum of 9.3 KJ / m at 4.5 parts. 2 The flexural modulus and flexural strength increased first and then decreased with the increase of PTEI addition, reaching the highest value when the PTEI addition was 3.1 parts.
[0060] The solubility of polyimide resin in epoxy resin is relatively poor. The use of polysulfide ether imide to modify epoxy resin not only solves the problem of polyimide solubility in epoxy resin, but also does not reduce the glass transition temperature of epoxy resin when added in small amounts, significantly improves the impact resistance, bending resistance and tensile resistance of epoxy resin, reduces the modification cost, and better meets market demand.
[0061] The embodiments described above provide a detailed description of the technical solutions of the present invention. It should be understood that the above are only specific embodiments of the present invention and are not intended to limit the present invention. Any modifications, supplements or similar substitutions made within the scope of the principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A polythioetherimide-modified epoxy resin, characterized in that: The following raw materials in parts by weight composition: Epoxy resin 100 parts; Polythioetherimide 0.8-4.5 parts; 30-70 parts of curing agent; 1-10 parts of release agent; The polythioetherimide is a mixture of three structural units of formula (I), formula (II) and formula (III): ; Formula (I); ; Formula (II); ; Formula (III); Wherein, x, y and z are positive integers, 10<x+y+z<100; R is a diamine residue derived from a diamine monomer, and the diamine monomer includes an aliphatic diamine or an aromatic diamine.
2. The polythioetherimide-modified epoxy resin according to claim 1, characterized in that The epoxy resin includes bisphenol A epoxy resin or 4,4'-diaminodiphenylmethane tetraglycidyl ether, and the bisphenol A epoxy resin includes E-42, E-51 or E-55.
3. The polythioetherimide-modified epoxy resin according to claim 1, characterized in that: In formula (I), formula (II) and formula (III), the diamine monomer is selected from at least one of p-phenylenediamine, m-phenylenediamine, 4,4'-diaminodiphenyl ether, 4,4'-diaminobenzophenone, 3,4'-diaminobenzophenone, 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenyl sulfone, 3,3'-dichloro-4,4'-diaminodiphenylmethane, 4,4'-bis(4-aminophenoxy)biphenyl, 2,4-toluenediamine and 3,3'-dimethyl-4,4'-diaminodiphenylmethane.
4. The polythioetherimide-modified epoxy resin according to claim 1, characterized in that: The curing agent is at least one of anhydride curing agent, aliphatic amine curing agent or aromatic amine curing agent.
5. The method for preparing a polythioetherimide-modified epoxy resin according to any one of claims 1 to 4, characterized in that: The following steps are involved: (1) Under the protection of nitrogen atmosphere, after heating the epoxy resin, add polysulfide etherimide and stir to melt blend; (2) The blend obtained in step (1) is cooled to 115-135° C., a curing agent and a release agent are added, and the mixture is stirred until uniform and transparent, and then vacuum degassing is performed, and then poured into a mold, and the polysulfide ether imide-modified epoxy resin is obtained after curing.
6. The method for preparing a polythioetherimide-modified epoxy resin according to claim 5, characterized in that: The epoxy resin is heated to 140-160°C and then polysulfide is added. The temperature of melt blending is 140-160°C.
7. The method for preparing a polythioetherimide-modified epoxy resin according to claim 5, characterized in that: The curing process is a three-stage insulation curing process. The first stage insulation curing parameters are: 80-210 ℃, 1-2 h; the second stage insulation curing parameters are: 160-240 ℃, 1-3 h; the third stage insulation curing parameters are: 200-260 ℃, 1-3h.