Coordination polymer solid electrolyte and preparation method thereof, solid-state battery

By using coordination polymer solid electrolytes in lithium-ion batteries, combined with the reaction of lithium salts and transition metal fluorides with ether oxygen bond-containing polymers, a solid electrolyte with high conductivity and high stability is formed, which solves the problem of lithium-ion batteries. The problems of low conductivity and poor mechanical properties at room temperature are achieved by stable operation and high energy density at 30°C.

CN115332623BActive Publication Date: 2024-10-11HUAZHONG UNIV OF SCI & TECH
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202210999562.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-08-19
Publication Date
2024-10-11
Estimated Expiration
2042-08-19

AI Technical Summary

Technical Problem

The solid electrolyte of existing lithium-ion batteries has low conductivity and poor mechanical properties at room temperature, which can easily lead to lithium dendrite puncture and battery short circuit, and cannot meet the energy density requirements of long-range electric vehicles.

Method used

Using the preparation method of coordination polymer solid electrolyte, the lithium salt and transition metal fluoride are reacted with the ether oxygen bond-containing polymer in a dimethyl sulfoxide mixed solution to form a solid electrolyte layer rich in lithium fluoride, which improves the The migration number and conductivity of lithium ions are controlled, and by controlling the amount of transition metal fluoride and the drying process, agglomeration and energy density reduction are avoided.

Benefits of technology

It has achieved a lithium ion conductivity of 10-4S/cm at room temperature, a migration number of 0.42, and high stability for lithium metal anodes, reducing the battery operating temperature and maintaining a high capacity retention rate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115332623B_ABST
    Figure CN115332623B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field related to solid electrolytes, and discloses a coordination polymer solid electrolyte and a preparation method thereof, and a solid-state battery. The preparation method comprises: adding an organic solvent to a dimethyl sulfoxide mixed solution of a lithium salt and a transition metal fluoride and stirring for a first preset time to obtain a first mixed solution, then adding an ether oxygen bond-containing polymer to the first mixed solution and continuing to stir for a second preset time to obtain a second mixed solution, and drying the second mixed solution to obtain a coordination polymer solid electrolyte. The solid electrolyte and solid-state battery prepared by the method of the present application have high ionic conductivity at room temperature and high stability to a lithium metal negative electrode, so the operating temperature of the polymer solid-state battery can be greatly reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field related to solid electrolytes, and more specifically, relates to a coordination polymer solid electrolyte and a preparation method thereof, and a solid-state battery. Background Art

[0002] The continuous consumption of fossil energy by human beings has brought about serious environmental pollution problems. Therefore, people are paying more and more attention to green and sustainable clean energy. Lithium-ion batteries are green, environmentally friendly and sustainable. Compared with lead-acid batteries, they have the advantages of low cost and high energy density, so they have received widespread attention. At present, commercial lithium-ion batteries use ethylene carbonate-based organic matter as electrolyte, which brings many safety problems, such as flammability and easy leakage. In addition, the energy density of lithium-ion batteries has reached a bottleneck and cannot meet the requirements of long-range electric vehicles. In order to solve the above problems, solid electrolytes are used to replace organic electrolytes, and the assembled all-solid-state batteries have high safety and high energy density.

[0003] Polymer solid electrolytes have good flexibility and electrode interface compatibility. Among various solid electrolytes, poly(ethylene oxide) (PEO) and its derivatives have high stability to lithium metal and good dissociation ability to lithium salts, making them one of the most popular polymer solid electrolytes. However, the room temperature conductivity of pure PEO electrolyte is low (10 -6 ~10 -5 S / cm), low migration number (<0.2), poor mechanical properties, unstable interface with lithium metal, easy to produce lithium dendrites, puncture the electrolyte, and cause battery short circuit. At the same time, the electrochemical window of PEO electrolyte is narrow (<4V), which cannot match high-voltage positive electrode materials. At present, the modification of PEO electrolyte mainly focuses on the introduction of second-phase nano-ceramic particles. The mechanism of improving conductivity is as follows: (1) Through Lewis acid-base chemical action, the crystallinity of PEO is reduced; (2) For lithium-containing ceramics, in addition to reducing the crystallinity, it can also conduct lithium ions and provide a rich ceramic / polymer interface, which is conducive to the migration of lithium ions. However, the introduction of nano-ceramics is prone to agglomeration, making the transmission of lithium ions discontinuous. In order to construct a three-dimensional continuous lithium-ion conductive network, it is usually necessary to add a large amount of ceramic particles (>50%) to the polymer. Although the room temperature conductivity of the polymer can be improved to a certain extent (10 -5 S / cm) and the stability of the metal lithium anode, but the addition of excessive ceramic nanoparticles seriously reduces the energy density of solid-state batteries. Since the room temperature conductivity of polymer solid electrolytes cannot reach 10 -4 S / cm, the battery still needs to operate at a temperature above 50°C. At this temperature, the mechanical properties of PEO are poor and lithium dendrites can easily pierce the PEO electrolyte membrane. Therefore, the design has high room temperature ionic conductivity (>10-4 S / cm) and solid electrolytes that are stable to metallic lithium anodes are of great significance to the development of solid-state batteries. Summary of the invention

[0004] In view of the above defects or improvement needs of the prior art, the present invention provides a coordination polymer solid electrolyte and a preparation method thereof, and a solid-state battery. The solid-state electrolyte and solid-state battery of the present application have high ionic conductivity at room temperature and high stability to the lithium metal negative electrode, and thus can significantly reduce the operating temperature of the polymer solid-state battery.

[0005] To achieve the above-mentioned purpose, according to one aspect of the present invention, a method for preparing a coordination polymer solid electrolyte is provided, the preparation method comprising: adding an organic solvent to a mixed solution of dimethyl sulfoxide containing a lithium salt and a transition metal fluoride and stirring for a first preset time to obtain a first mixed solution, then adding an ether oxygen bond-containing polymer to the first mixed solution and continuing to stir for a second preset time to obtain a second mixed solution, and drying the second mixed solution to obtain a coordination polymer solid electrolyte.

[0006] Preferably, the mass ratio of the lithium salt, the transition metal fluoride and the ether oxygen bond-containing polymer is 240:(1-5):600.

[0007] Preferably, the dimethyl sulfoxide mixed solution of lithium salt and transition metal fluoride is obtained by the following method: dissolving transition metal fluoride and lithium salt in dimethyl sulfoxide solution, and then placing on a heated stirring table and stirring for a preset time to obtain the dimethyl sulfoxide mixed solution of lithium salt and transition metal fluoride.

[0008] Preferably, the boiling point of the organic solvent is less than 100°C.

[0009] Preferably, the concentration of lithium salt in the dimethyl sulfoxide mixed solution of lithium salt and transition metal fluoride is 0.1-0.2M.

[0010] Preferably, the drying is carried out under an argon atmosphere with a vacuum degree of less than 0.1 MPa, and the organic solvent is first dried at 30-40° C., and then continued to dry at 50-60° C. for a preset time.

[0011] Preferably, the lithium salt includes at least one of lithium bis(trifluoromethylsulfonyl)imide, lithium bis(fluorosulfonyl)imide, lithium perchlorate, lithium dioxalatoborate and lithium difluorooxalatoborate; the ether oxygen bond-containing polymer includes at least one of polyethylene oxide, polypropylene oxide, polyethylene glycol dimethyl ether and polyethylene glycol; the transition metal fluoride includes at least one of copper fluoride, zinc fluoride, magnesium fluoride, aluminum fluoride, strontium fluoride and stannous fluoride; and the organic solvent is acetonitrile.

[0012] On the other hand, the present application provides a coordination polymer solid electrolyte prepared by the preparation method of the above-mentioned coordination polymer solid electrolyte.

[0013] Preferably, the mass fraction of the lithium salt in the coordination polymer solid electrolyte is 25.0% to 35.0%, the mass fraction of the ether oxygen bond-containing polymer in the polymer solid electrolyte is 65.0% to 75.0%, and the mass fraction of the metal fluoride in the polymer solid electrolyte is 0.048% to 0.5%.

[0014] On the other hand, the present application provides a solid-state battery, comprising a positive electrode, a negative electrode and the above-mentioned coordination polymer solid electrolyte, wherein the coordination polymer solid electrolyte is arranged between the positive electrode and the negative electrode.

[0015] In general, compared with the prior art, the coordination polymer solid electrolyte and preparation method thereof, and solid-state battery provided by the present invention have the following beneficial effects:

[0016] 1. The present application adds transition metal fluoride, wherein the transition metal ions can chelate with the oxygen atoms in the ether oxygen bond polymer and the lithium salt to form a strong coordination ability, thereby releasing more free lithium ions and weakening the binding of the ether oxygen of the ether oxygen bond polymer to the lithium ions, thereby improving the conductivity and migration number of the polymer solid electrolyte, and the lithium ion conductivity can reach 10 -4 S / cm, and the migration number is 0.42; the fluorine element participates in the formation process of the solid electrolyte interface film to form a solid electrolyte layer rich in lithium fluoride. Due to the low electronic conductivity, good hardness and stability of lithium fluoride, the solid electrolyte layer has high strength, so it can inhibit the growth of lithium dendrites and reduce interface side reactions. Therefore, it can maintain a high ionic conductivity at room temperature and has high stability to the lithium metal negative electrode. Therefore, the operating temperature of the polymer solid-state battery can be greatly reduced, and after multiple cycles, it still has a high capacity retention rate.

[0017] 2. This application needs to control the amount of transition metal fluoride to between 0.048% and 0.5%, because the introduction of too much transition metal fluoride will inevitably be accompanied by the addition of too much dimethyl sulfoxide solvent; and the boiling points of acetonitrile and dimethyl sulfoxide are quite different, so phase separation is likely to occur during the drying process, making the final membrane present a porous structure.

[0018] 3. Two-stage drying is adopted in the drying process. Low-temperature drying is first performed to avoid the melting of the low-melting-point ether-oxygen bond-containing polymer affecting the drying of the organic solvent, thereby facilitating the complete removal of the organic solvent.

[0019] 4. The transition metal fluoride of the present application is completely dissolved in the dimethyl sulfoxide solution, so it is evenly distributed when added to the polymer solid electrolyte, and the content is extremely low (<1wt%), which will not reduce the energy density of the battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 is a photograph of the coordination polymer solid electrolyte prepared in Example 1 of the present application;

[0021] Figure 2 is the distribution of copper fluoride nanoparticles in the coordination polymer solid electrolyte prepared in Example 1 of the present application;

[0022] Figure 3 is the Cu 2p peak of the X-ray photoelectron spectrum of the polymer solid electrolyte prepared in Example 1 of the present application;

[0023] Figure 4 It is the Fourier infrared spectra of polymer solid electrolytes obtained by adding different contents of copper fluoride to Comparative Example 1 and Examples 1 to 4 of the present application;

[0024] Figure 5 The lithium-lithium symmetric battery of the coordination polymer solid electrolyte prepared in Example 1 of the present application is at 30°C and 0.1 mA / cm 2 , 0.5mAh / cm 2 The cycle curve below;

[0025] Figure 6 It is the charge and discharge curve of the Li / LiFePO4 button cell of the coordination polymer solid electrolyte prepared in Example 1 of the present application at 30° C. and 0.3C for the 100th cycle;

[0026] Figure 7 It is the charge and discharge curve of the Li / LiFePO4 button cell of the coordination polymer solid electrolyte prepared in Example 1 of the present application at 30° C. and 0.15C for the 100th cycle;

[0027] Figure 8 The Li / LiNi coordination polymer solid electrolyte prepared in Example 1 of the present application 0.83 Co 0.12 Mn 0.05 The charge and discharge curve of the 100th cycle of O2 button battery at 30℃ and 0.6C;

[0028] Fig. 9 The Li / LiNi coordination polymer solid electrolyte prepared in Example 1 of the present application 0.83 Co 0.12 Mn 0.05 The charge and discharge curves of the O2 button battery at 30°C and 0.15C for the 100th cycle. DETAILED DESCRIPTION

[0029] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. In addition, the technical features involved in the various embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.

[0030] The first aspect of the present invention provides a method for preparing a coordination polymer solid electrolyte, which comprises: adding an organic solvent to a mixed solution of dimethyl sulfoxide containing a lithium salt and a transition metal fluoride and stirring for a first preset time to obtain a first mixed solution, then adding an ether oxygen bond-containing polymer to the first mixed solution and continuing to stir for a second preset time to obtain a second mixed solution, and drying the second mixed solution to obtain a coordination polymer solid electrolyte.

[0031] During the preparation process, the transition metal fluoride can be first added to the auxiliary solvent dimethyl sulfoxide to dissolve. In order to increase the dissolution of the transition metal fluoride, part or all of the lithium salt required for the configuration is added to the above solution and then placed on a heated stirring table for stirring. The temperature of the stirring table is preferably 60°C. Stirring is carried out for about 24 hours to completely dissolve the lithium salt and the transition metal fluoride. Then, the solution is added to the organic solvent acetonitrile and stirred for a certain period of time to obtain a first mixed solution. Then, the ether oxygen bond-containing polymer is added to the first mixed solution and continued to stir for a second preset time, for example, stirring on a heated stirring table at 20 to 30°C for 24 hours to completely dissolve the ether oxygen bond-containing polymer to obtain a second mixed solution. The second mixed solution is dried to remove the auxiliary solvent dimethyl sulfoxide and the organic solvent acetonitrile to obtain a coordination polymer solid electrolyte.

[0032] In order to better dissolve the transition metal fluoride, the particle size is nanometer-sized, less than 50 nm.

[0033] In a further preferred embodiment, the mass ratio of the lithium salt, the transition metal fluoride and the ether oxygen bond-containing polymer is 240:(1-5):600. It can be seen that the content of the transition metal fluoride in the present application is relatively small and soluble, thus ensuring that the transition metal ions react with the oxygen atoms while avoiding the generation of agglomeration.

[0034] In a further preferred embodiment, the concentration of the lithium salt in the mixed solution of the lithium salt and the transition metal fluoride in dimethyl sulfoxide is 0.1-0.2M.

[0035] The drying process is preferably vacuum drying with a vacuum degree of less than 0.1 MPa. The drying atmosphere is an argon atmosphere. The organic solvent is first dried at 30-40°C and then continued to dry at 50-60°C for a preset time to obtain a high conductivity coordination polymer solid electrolyte.

[0036] The lithium salt includes at least one of lithium bis(trifluoromethylsulfonyl)imide, lithium bis(fluorosulfonyl)imide, lithium perchlorate, lithium dioxalatoborate and lithium difluorooxalatoborate; the ether oxygen bond-containing polymer includes at least one of polyethylene oxide, polypropylene oxide, polyethylene glycol dimethyl ether and polyethylene glycol; the metal fluoride includes at least one of copper fluoride, zinc fluoride, magnesium fluoride, aluminum fluoride, strontium fluoride and stannous fluoride, and copper fluoride is more preferred.

[0037] On the other hand, the present application provides a coordination polymer solid electrolyte prepared by the above-mentioned preparation method of the coordination polymer solid electrolyte.

[0038] The mass fraction of the lithium salt in the coordination polymer solid electrolyte is 25.0% to 35.0%, the mass fraction of the ether oxygen bond-containing polymer in the polymer solid electrolyte is 65.0% to 75.0%, and the mass fraction of the metal fluoride in the polymer solid electrolyte is 0.048% to 0.5%.

[0039] On the other hand, the present application provides a solid-state battery, including a positive electrode, a negative electrode and the above-mentioned coordination polymer solid electrolyte, wherein the coordination polymer solid electrolyte is arranged between the positive electrode and the negative electrode. The negative electrode of the solid-state battery is lithium metal or lithium alloy, and the prepared battery needs to be placed in a heat preservation oven for heat treatment during the preparation process, and the heat treatment temperature is preferably 45°C to 50°C.

[0040] Example 1

[0041] Under the condition that the water and oxygen concentrations are less than 0.1ppm, 0.01g of copper fluoride nanoparticles are dissolved in 10mL of dimethyl sulfoxide solution. In order to increase the dissolution of CuF2, 2.4g of lithium bis(trifluoromethylsulfonyl)imide is added to the solution. The mixed solution is placed on a heated stirring table at 60°C and stirred for 24h to obtain a completely dissolved copper fluoride solution. Take 0.5mL of the above solution and add it to acetonitrile, then add 0.24g of lithium bis(trifluoromethylsulfonyl)imide and stir at room temperature for 2h. Finally, add 0.6g of PEO and stir for 24h to obtain a uniformly mixed PEO solution. The PEO solution is dried at room temperature to remove acetonitrile; in order to further remove residual acetonitrile, the obtained PEO film is placed in a vacuum oven at 50°C for 12h to obtain a high-conductivity PEO coordination polymer solid electrolyte, such as Figure 1 As shown, the conductivity is 0.20 mS / cm.

[0042] Example 2

[0043] Under the condition that the water oxygen concentration is less than 0.1ppm, 0.005g of copper fluoride nanoparticles are dissolved in 10mL of dimethyl sulfoxide solution. In order to increase the dissolution of CuF2, 2.4g of lithium bis(trifluoromethylsulfonyl)imide is added to the solution, and the mixed solution is placed on a heated stirring table at 60°C and stirred for 24h to obtain a completely dissolved copper fluoride solution. Except for the different CuF2 concentration, the other material operations are the same as in Example 1. The obtained polymer solid-state conductivity is 0.02mS / cm.

[0044] Example 3

[0045] Under the condition that the water oxygen concentration is less than 0.1ppm, 0.025g of copper fluoride nanoparticles are dissolved in 10mL of dimethyl sulfoxide solution. In order to increase the dissolution of CuF2, 2.4g of lithium bis(trifluoromethylsulfonyl)imide is added to the solution, and the mixed solution is placed on a heated stirring table at 60°C and stirred for 24h to obtain a completely dissolved copper fluoride solution. Except for the different CuF2 concentration, the other material operations are the same as in Example 1. The obtained polymer solid-state conductivity is 0.09mS / cm.

[0046] Example 4

[0047] Under the condition that the water oxygen concentration is less than 0.1ppm, 0.05g of copper fluoride nanoparticles are dissolved in 10mL of dimethyl sulfoxide solution. In order to increase the dissolution of CuF2, 2.4g of lithium bis(trifluoromethylsulfonyl)imide is added to the solution, and the mixed solution is placed on a heated stirring table at 60°C and stirred for 24h to obtain a completely dissolved copper fluoride solution. Except for the different CuF2 concentration, the other material operations are the same as in Example 1. The obtained polymer solid-state conductivity is 0.047mS / cm.

[0048] Example 5

[0049] Under the condition that the water and oxygen concentrations are less than 0.1ppm, 0.01g of copper fluoride nanoparticles are dissolved in 10mL of dimethyl sulfoxide solution. In order to increase the dissolution of CuF2, 2.4g of lithium bis(fluorosulfonyl)imide is added to the solution. The mixed solution is placed on a heated stirring table at 60°C and stirred for 24h to obtain a completely dissolved copper fluoride solution. Take 0.5mL of the above solution and add it to acetonitrile, then add 0.24g of lithium bis(fluorosulfonyl)imide, stir at room temperature for 2h, and finally add 0.6g of PEO and stir for 24h to obtain a uniformly mixed PEO solution. The PEO solution is dried at room temperature to remove acetonitrile; in order to further remove residual acetonitrile, the obtained PEO film is placed in a vacuum oven at 50°C for 12h, thereby obtaining a high-conductivity PEO polymer solid electrolyte with a conductivity of 0.13mS / cm.

[0050] Example 6

[0051] The operation of preparing the PEO polymer electrolyte membrane is the same as that in Example 1; in order to further remove the residual acetonitrile, the obtained PEO membrane is placed in a vacuum oven at 60° C. for 12 hours, thereby obtaining a PEO polymer solid electrolyte with high conductivity.

[0052] Comparative Example 1

[0053] Under the condition that the water and oxygen concentrations are less than 0.1ppm, 0.24g of lithium bis(trifluoromethylsulfonyl)imide was added to acetonitrile, stirred at room temperature for 2h, and finally 0.6g of PEO was added and stirred for 24h to obtain a uniformly mixed PEO solution. The PEO solution was dried at room temperature to remove acetonitrile; in order to further remove the residual acetonitrile, the obtained PEO film was placed in a vacuum oven at 50°C for 12h, thereby obtaining a PEO polymer solid electrolyte with high conductivity.

[0054] Comparative Example 2

[0055] Under the condition that the water and oxygen concentrations are less than 0.1ppm, 0.5mL of dimethyl sulfoxide is added to acetonitrile, followed by 0.24g of lithium bis(trifluoromethylsulfonyl)imide, stirred at room temperature for 2h, and finally 0.6g of PEO is added and stirred for 24h to obtain a uniformly mixed PEO solution. The PEO solution is dried at room temperature to remove acetonitrile; in order to further remove residual acetonitrile, the obtained PEO film is placed in a vacuum oven at 50°C for 12h, thereby obtaining a PEO polymer solid electrolyte with high conductivity.

[0056] The distribution state of copper fluoride nanoparticles in the PEO coordination polymer solid electrolyte prepared in Example 1 was observed using a transmission electron microscope. Figure 2 As shown, copper fluoride nanoparticles are evenly distributed in the PEO coordination polymer solid electrolyte without agglomeration.

[0057] The PEO coordination polymer solid electrolyte prepared in Example 1 was subjected to X-ray photoelectron spectroscopy (XPS) test. Figure 3 As shown, it is found that the Cu 2p peak has an obvious shift toward the low binding energy direction, indicating that there is a coordination effect between Cu and the ether bond oxygen of PEO, which can weaken the effect between the ether bond oxygen of PEO and lithium ions and accelerate the transmission of lithium ions in the PEO polymer electrolyte.

[0058] The coordination polymer solid electrolytes prepared in Examples 1 to 4 and Comparative Example 1 were tested by Fourier transform infrared spectroscopy. Figure 4 As shown, with the increase of copper fluoride content, the peak corresponding to TFSI (bis(trifluoromethylsulfonyl)imide) ion shifts to the right, proving that copper fluoride has a coordination effect with lithium bis(trifluoromethylsulfonyl)imide, which can release more lithium ions.

[0059] Ionic conductivity test:

[0060] The conductivity of the prepared coordination polymer solid electrolyte was tested by AC impedance spectroscopy. Specifically, a PEO coordination polymer solid electrolyte membrane with a diameter of 18 mm was taken as a sample, and a stainless steel with a diameter of 15.8 mm was used as a blocking electrode. The PEO electrolyte was sandwiched between two stainless steel sheets and sealed in a button cell. The battery was placed in a 50°C oven for 1 hour and cooled to 30°C. The electrochemical workstation was connected via a wire and the frequency was or 10 6 -1Hz, bias voltage 10mV, test to get the impedance diagram of the electrolyte; the thickness of the coordination polymer solid electrolyte is obtained by scanning electron microscopy. The ionic conductivity of the electrolyte is calculated according to the formula: σ=L / (R×S). Among them, L is the thickness of the polymer electrolyte, R is the resistance value of the electrolyte, and S is the area of ​​the stainless steel sheet.

[0061] Example battery performance test results:

[0062] The PEO coordination polymer solid electrolyte prepared in Example 1 was subjected to a lithium-lithium symmetric battery cycle test at 30°C and 0.1 mA / cm 2 , 0.5mAh / cm 2 Charge and discharge under the conditions of Figure 5 As shown, the battery has a stable cycle within 700 h and the overpotential does not increase significantly.

[0063] The PEO coordination polymer solid electrolyte prepared in Example 1 was subjected to charge and discharge tests, and a button cell was assembled with metallic lithium as the negative electrode and LiFePO4 as the positive electrode. Figure 6 As shown, after the battery is cycled 100 times at 30°C and 0.3C, the positive electrode discharge specific capacity can reach 138mAh / g.

[0064] The PEO coordination polymer solid electrolyte prepared in Example 1 was subjected to charge and discharge tests, and a soft pack battery was assembled with metallic lithium as the negative electrode and LiFePO4 as the positive electrode. Figure 7 As shown, after the battery is cycled 100 times at 30°C and 0.15C, the positive electrode discharge specific capacity can reach 130mAh / g.

[0065] The PEO coordination polymer solid electrolyte prepared in Example 1 was subjected to charge and discharge tests, with lithium metal as the negative electrode and LiNi 0.83 Co 0.12 Mn 0.05 O2 is the positive electrode, and button cells are assembled. Figure 8 As shown, after the battery is cycled 100 times at 30°C and 0.6C, the positive electrode discharge specific capacity can reach 157mAh / g.

[0066] The PEO coordination polymer solid electrolyte prepared in Example 1 was subjected to charge and discharge tests, with lithium metal as the negative electrode and LiNi 0.83 Co 0.12 Mn 0.05 O2 is used as the positive electrode and a soft pack battery is assembled. Fig. 9 As shown, after the battery is cycled 100 times at 30°C and 0.15C, the positive electrode discharge specific capacity can reach 175mAh / g.

[0067] The positive electrode preparation methods in the above embodiments were tested as follows: LiFePO4, conductive carbon, PEO, and lithium bis(trifluoromethylsulfonyl)imide were uniformly dispersed in acetonitrile in a mass ratio of 6:1:2.2:0.8, the slurry was scraped onto carbon-rich aluminum foil, and dried to obtain a LiFePO4 positive electrode sheet. 0.83 Co 0.12 Mn 0.05 O2, conductive carbon, polyvinylidene fluoride, succinonitrile / bis(trifluoromethylsulfonyl)imide lithium are uniformly dispersed in N-methylpyrrolidone in a mass ratio of 6:1:2.5:0.5, and the slurry is scraped on a carbon-rich aluminum foil and dried to obtain LiNi 0.83 Co 0.12 Mn 0.05 O2 positive electrode sheet. Succinonitrile / lithium bis(trifluoromethylsulfonyl)imide are prepared in a molar ratio of 20:1.

[0068] It can be seen from the above examples that nano copper fluoride can coordinate with the ether oxygen of the PEO chain, and can also coordinate with the bistrifluoromethylsulfonyl imide anion, thereby weakening the bondage of the ether oxygen to the lithium ions, and releasing more lithium ions to jointly improve the ionic conductivity of the PEO coordination polymer solid electrolyte. Fluoride ions can participate in the formation of the negative electrode interface, stabilize the lithium negative electrode, and inhibit lithium dendrites. The combined effect of these two aspects allows the PEO-based all-solid-state battery to operate stably at a temperature of 30°C. Since the amount of copper fluoride added is very small, it will not affect the energy density of the battery.

[0069] It will be easily understood by those skilled in the art that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a coordination polymer solid electrolyte, characterized in that: The preparation method comprises: An organic solvent is added to a mixed solution of lithium salt and transition metal fluoride in dimethyl sulfoxide, and the mixture is stirred for a first preset time to obtain a first mixed solution, wherein the transition metal fluoride is completely dissolved in the dimethyl sulfoxide solution, and the transition metal ions in the transition metal fluoride are chelated with the ether oxygen bond-containing polymer and the oxygen atoms in the lithium salt, and then the ether oxygen bond-containing polymer is added to the first mixed solution and the mixture is stirred for a second preset time to obtain a second mixed solution, and the second mixed solution is dried to obtain a coordination polymer solid electrolyte; The transition metal fluoride includes at least one of copper fluoride, zinc fluoride, magnesium fluoride, aluminum fluoride, strontium fluoride and stannous fluoride; the mass ratio of the lithium salt, the transition metal fluoride and the ether oxygen bond-containing polymer is 240:(1-5):

600.

2. The preparation method according to claim 1, characterized in that: The dimethyl sulfoxide mixed solution of the lithium salt and the transition metal fluoride is obtained by the following method: The transition metal fluoride and the lithium salt are dissolved in a dimethyl sulfoxide solution, and then placed on a heated stirring table and stirred for a preset time to obtain a dimethyl sulfoxide mixed solution of the lithium salt and the transition metal fluoride.

3. The preparation method according to claim 1, characterized in that: The boiling point of the organic solvent is less than 100°C.

4. The preparation method according to claim 3, characterized in that: The concentration of lithium salt in the dimethyl sulfoxide mixed solution of lithium salt and transition metal fluoride is 0.1-0.2M.

5. The preparation method according to claim 1, characterized in that: Drying is carried out under an argon atmosphere with a vacuum degree of less than 0.1 MPa. The organic solvent is first dried at 30-40°C, and then continued to dry at 50-60°C for a preset time.

6. The preparation method according to claim 1, characterized in that: The lithium salt includes at least one of lithium bis(trifluoromethylsulfonyl)imide, lithium bis(fluorosulfonyl)imide, lithium perchlorate, lithium dioxalatoborate and lithium difluorooxalatoborate; the ether oxygen bond-containing polymer includes at least one of polyethylene oxide, polypropylene oxide, polyethylene glycol dimethyl ether and polyethylene glycol; and the organic solvent is acetonitrile.

7. A coordination polymer solid electrolyte prepared by the method for preparing a coordination polymer solid electrolyte according to any one of claims 1 to 6.

8. The coordination polymer solid electrolyte according to claim 7, characterized in that: The mass fraction of the lithium salt in the coordination polymer solid electrolyte is 25.0% to 35.0%, the mass fraction of the ether oxygen bond-containing polymer in the polymer solid electrolyte is 65.0% to 75.0%, and the mass fraction of the metal fluoride in the polymer solid electrolyte is 0.048% to 0.5%.

9. A solid-state battery, characterized in that: The invention comprises a positive electrode, a negative electrode and the coordination polymer solid electrolyte according to claim 7 or 8, wherein the coordination polymer solid electrolyte is arranged between the positive electrode and the negative electrode.

Citation Information

Patent Citations

  • Open framework fluorine-based solid-state electrolyte material and preparation method of open framework fluorine-based solid-state electrolyte material

    CN106887639A

  • Preparation method of all-solid-state battery, and obtained all-solid-state battery

    CN109921097A

  • Solid electrolyte material, fluorine ion battery and preparation methods of solid electrolyte material and fluorine ion battery

    CN112456536A

  • Composite solid electrolyte, preparation method thereof, application and solid-state lithium battery

    CN113540556A

  • Solid electrolyte, preparation method of solid electrolyte, lithium ion battery and preparation method of lithium ion battery