A semi-solid composite diaphragm and preparation method thereof
By using a semi-solid composite separator combining polyethylene and ceramic aerogel in lithium-ion batteries, the challenges of traditional lithium-ion battery solid electrolytes in terms of mechanical strength and conductivity are solved, achieving high safety and excellent battery performance. The preparation process is simplified.
Patent Information
- Application Number
- CN202210719857.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-06-23
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-06-23
AI Technical Summary
The solid electrolyte of traditional lithium-ion batteries has challenges in achieving high ionic conductivity, uniform lithium ion flux, excellent interfacial compatibility and mechanical strength, and excessive use of liquid electrolyte poses safety risks.
It adopts a semi-solid composite separator, which is composed of polyethylene, ceramic aerogel and solid electrolyte mother liquor. Through the combination of polymethyl methacrylate, lithium salt and dibutyl phthalate, it has excellent mechanical properties and high ionic conductivity. High-efficiency separators are prepared through sheet casting, stretching and heat setting processes to reduce the use of liquid electrolyte.
It achieves high battery safety, excellent mechanical strength, liquid absorption and retention ability and interface compatibility, inhibits the growth of lithium dendrites, improves the overall performance and safety of the battery, while simplifying the preparation process and improving efficiency.
Smart Images

Figure BDA0003710031840000091
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of battery separators, and in particular to a semi-solid composite separator and a preparation method thereof. Background Art
[0002] Lithium-ion batteries have become an indispensable part of our daily lives, from daily consumer electronics to electric vehicles. However, conventional battery systems composed of organic or inorganic liquid electrolytes have certain limitations (e.g., flammability, etc.), which hinder the widespread application of lithium-ion batteries in energy storage and conversion systems. In order to solve the safety problem, all-solid-state batteries have been developed. However, it is difficult to achieve high ionic conductivity, uniform lithium ion (Li-ion) + ) flux, excellent interfacial compatibility and enhanced mechanical strength are still the severe challenges faced by solid electrolytes. Combining the advantages and disadvantages of the two, a semi-solid composite membrane and its preparation method are proposed. Summary of the invention
[0003] In order to solve the above technical problems, the present invention provides a semi-solid composite membrane and a preparation method thereof; the semi-solid composite membrane provided by the present invention has excellent mechanical strength, liquid absorption and retention capacity, ionic conductivity, and interface compatibility, and uses less liquid electrolyte, inhibits the growth of lithium dendrites, and can achieve high safety of the battery; at the same time, the preparation process of the semi-solid composite membrane provided by the present invention is simple and efficient.
[0004] To achieve the above object, the present invention is implemented through the following technical solutions:
[0005] A semi-solid composite diaphragm, characterized in that the semi-solid composite diaphragm is composed of polyethylene raw material (PE), ceramic aerogel and solid electrolyte mother solution;
[0006] The solid electrolyte mother solution comprises polymethyl methacrylate (PMMA), lithium salt, dibutyl phthalate and a solvent.
[0007] The semi-solid composite diaphragm provided by the present invention has excellent mechanical strength, liquid absorption and retention capacity, ionic conductivity, and interface compatibility. In addition, the semi-solid composite diaphragm of the present invention uses less liquid electrolyte, inhibits the growth of lithium dendrites, and can achieve high safety of the battery.
[0008] The semi-solid composite diaphragm of the invention uses PE and PMMA as a skeleton, which provides excellent mechanical properties for the semi-solid composite diaphragm, and has high puncture strength, tensile strength and elongation.
[0009] Furthermore, a semi-solid composite diaphragm: the mass ratio between the polyethylene, the ceramic aerogel and the solid electrolyte mother solution is 1: (0.05-0.1): (6-10).
[0010] Furthermore, a semi-solid composite diaphragm: the molecular weight of the polyethylene raw material is 100,000-1,000,000.
[0011] Furthermore, a semi-solid composite diaphragm: the thickness of the semi-solid composite diaphragm is 0.2-1.0 mm.
[0012] Furthermore, a semi-solid composite diaphragm: the ceramic aerogel is selected from one or a mixture of aluminum oxide aerogel, silicon dioxide aerogel, and titanium dioxide aerogel.
[0013] Furthermore, a semi-solid composite membrane: the ceramic aerogel has a porosity of 90-99% and a specific surface area of ≥300m 2 / g.
[0014] Furthermore, a semi-solid composite separator: the mass ratio of the polymethyl methacrylate (PMMA), the lithium salt and the dibutyl phthalate is (10-15):1:(0.2-0.8).
[0015] Further, a semi-solid composite diaphragm: the lithium salt is selected from LiClO 4 , LiBF 4 、LiAsF 6 、LiPF 6 , Li 3 PO 4 , Li 2 SiO 3 、LiSiO 3 Any one of the above; the solvent is N-methylpyrrolidone (NMP, chemical formula C 5 H 9 NO).
[0016] A method for preparing a semi-solid composite diaphragm, characterized in that the method comprises the following steps:
[0017] 1. Preparation of solid electrolyte mother solution:
[0018] S1. Weigh the polymethyl methacrylate and the lithium salt according to the mass ratio, add them to the solvent, and stir them evenly to form a first mixed material;
[0019] S2, adding the dibutyl phthalate to the first mixed material, and continuing stirring to obtain the solid electrolyte mother solution;
[0020] 2. Preparation of semi-solid composite diaphragm:
[0021] S1, heating and melting the polyethylene raw material in an extruder, then adding the ceramic aerogel, and mixing evenly to form a second mixed material;
[0022] S2, adding the solid electrolyte mother solution to the second mixed material and stirring evenly, and then removing the solvent to obtain a third mixed material;
[0023] S3, casting the third mixed material into sheets → longitudinal stretching → primary transverse stretching → secondary transverse stretching → heat setting → slitting and winding to obtain a semi-solid composite diaphragm.
[0024] Furthermore, a method for preparing a semi-solid composite diaphragm comprises the following specific steps:
[0025] 1. Preparation of solid electrolyte mother solution:
[0026] S1. Weigh the polymethyl methacrylate and the lithium salt according to the mass ratio, add them to the solvent, and then stir them magnetically at 70-90° C. for 2-5 hours to form a first mixed material;
[0027] S2, adding the dibutyl phthalate to the first mixed material, and continuing stirring for 1-3 hours to obtain the solid electrolyte mother solution;
[0028] 2. Preparation of semi-solid composite diaphragm:
[0029] S1, heating and melting the polyethylene raw material at 150-160° C. in an extruder, then adding the ceramic aerogel and mixing them evenly to form a second mixed material;
[0030] S2, adding the solid electrolyte mother solution to the second mixed material and stirring evenly, then heating to 200-210° C., removing the solvent, and obtaining a third mixed material;
[0031] S3, casting the third mixed material → longitudinal stretching → primary transverse stretching → secondary transverse stretching → heat setting → slitting and winding to obtain a semi-solid composite diaphragm;
[0032] Among them: the longitudinal stretching ratio is (6-10):1, the first transverse stretching ratio is (9-13):1, and the second transverse stretching ratio is (1.3-1.6):1.
[0033] Beneficial effects of the present invention:
[0034] (1) The semi-solid composite diaphragm provided by the present invention has excellent mechanical strength, liquid absorption and retention capacity, ionic conductivity, and interface compatibility, and uses less liquid electrolyte, inhibits the growth of lithium dendrites, and can achieve high safety of the battery. At the same time, the preparation process of the semi-solid composite diaphragm provided by the present invention is simple and efficient.
[0035] (2) The semi-solid composite diaphragm of the present invention has polyethylene (PE) and polymethyl methacrylate (PMMA) as the skeleton, which provides the semi-solid composite diaphragm with excellent mechanical properties, such as high puncture strength, tensile strength and elongation.
[0036] (3) The semi-solid composite diaphragm of the present invention reduces the crystallinity of polymethyl methacrylate (PMMA) by introducing dibutyl phthalate and ceramic aerogel with high porosity and large specific surface area, thereby greatly improving the ionic conductivity of the semi-solid composite diaphragm. At the same time, the addition of ceramic aerogel also improves the thermal shrinkage performance of the diaphragm.
[0037] (4) The semi-solid composite diaphragm of the present invention uses polymethyl methacrylate (PMMA) as the main solid electrolyte, which greatly improves the material's ability to absorb and retain liquid, and greatly reduces the internal resistance of the diaphragm through ion conduction between the solid and liquid phases.
[0038] (5) The thickness of the semi-solid composite diaphragm of the present invention is thicker than that of the currently commercialized wet-process PE diaphragm, which effectively prevents the puncture of the diaphragm due to the generation of lithium dendrites. In addition, even if a short circuit occurs, the diaphragm still retains the thermal shutdown characteristics of the PE diaphragm, providing double protection and achieving high safety of the battery. Among them: The principle of the thermal shutdown characteristic: the PE diaphragm has holes for the passage of lithium ions. When the battery temperature rises, the PE begins to melt and blocks the holes, preventing lithium ions from passing through, so that the battery no longer works, preventing further temperature increases and avoiding safety problems. DETAILED DESCRIPTION
[0039] The technical solution of the present invention will be clearly and completely described below in conjunction with specific embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present invention and its application or use. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0040] Example 1
[0041] A semi-solid composite diaphragm, characterized in that the semi-solid composite diaphragm is composed of polyethylene (PE), aluminum oxide aerogel (ceramic aerogel) and solid electrolyte mother solution; wherein the mass ratio of PE, aluminum oxide aerogel and solid electrolyte mother solution is 1:0.05:8;
[0042] The solid electrolyte mother solution includes: polymethyl methacrylate (PMMA), LiClO 4 (lithium salt), dibutyl phthalate, and N-methylpyrrolidone solvent (NMP);
[0043] Wherein: the mass ratio of polymethyl methacrylate, lithium salt and dibutyl phthalate is 12:1:0.4.
[0044] The preparation process of the semi-solid composite diaphragm of the above-mentioned embodiment 1 comprises the following specific steps:
[0045] 1. Preparation of solid electrolyte mother solution:
[0046] S1. According to the mass ratio, weigh 12 kg of polymethyl methacrylate (PMMA) and 1 kg of LiClO 4 (lithium salt) is added into N-methylpyrrolidone solvent, and then magnetically stirred at 80° C. for 3 hours to form a first mixed material;
[0047] S2, adding 0.4 kg of dibutyl phthalate to the first mixed material, and continuing stirring for 1 hour to obtain a solid electrolyte mother solution;
[0048] 2. Preparation of semi-solid composite diaphragm:
[0049] S1. 10 kg of polyethylene raw material was heated and melted at 155°C in an extruder, and then 0.5 kg of alumina aerogel (with a porosity of about 99% and a specific surface area of ≥300 m 2 / g), uniformly mixed for 1 hour to form a second mixed material;
[0050] S2, adding 80 kg of solid electrolyte mother solution to the second mixed material and stirring for 0.5 hours to mix evenly, then heating to 205° C., evaporating and removing the N-methylpyrrolidone solvent, to obtain a third mixed material;
[0051] S3, casting the obtained third mixed material → longitudinal stretching → primary transverse stretching → secondary transverse stretching → heat setting → slitting and winding to obtain a semi-solid composite diaphragm;
[0052] Among them: the longitudinal stretching ratio is 8:1, the first transverse stretching ratio is 10:1, and the second transverse stretching ratio is 1.4:1.
[0053] Example 2
[0054] A semi-solid composite diaphragm, characterized in that the semi-solid composite diaphragm is composed of polyethylene, titanium dioxide aerogel and solid electrolyte mother solution; wherein the mass ratio of polyethylene, titanium dioxide aerogel and solid electrolyte mother solution is 1:0.1:10;
[0055] The solid electrolyte mother solution includes: polymethyl methacrylate (PMMA), LiBF 4 (lithium salt), dibutyl phthalate, and N-methylpyrrolidone solvent (NMP);
[0056] Wherein: the mass ratio of polymethyl methacrylate, lithium salt and dibutyl phthalate is 10:1:0.2.
[0057] The preparation process of the semi-solid composite diaphragm of the above-mentioned embodiment 2 comprises the following specific steps:
[0058] 1. Preparation of solid electrolyte mother solution:
[0059] S1. According to the mass ratio, weigh 10 kg of polymethyl methacrylate (PMMA) and 1 kg of LiBF 4 (lithium salt) is added into N-methylpyrrolidone solvent, and then magnetically stirred at 70° C. for 5 hours to form a first mixed material;
[0060] S2, adding 0.2 kg of dibutyl phthalate to the first mixed material, and continuing stirring for 2 hours to obtain a solid electrolyte mother solution;
[0061] 2. Preparation of semi-solid composite diaphragm:
[0062] S1. 10 kg of polyethylene raw material was heated and melted at 150°C in an extruder, and then 1 kg of titanium dioxide aerogel (with a porosity of about 90% and a specific surface area of ≥300 m 2 / g), uniformly mixed for 1 hour to form a second mixed material;
[0063] S2, adding 100 kg of solid electrolyte mother solution to the second mixed material and stirring for 0.5 hours to mix evenly, then heating to 210° C., evaporating and removing the N-methylpyrrolidone solvent, to obtain a third mixed material;
[0064] S3, casting the obtained third mixed material → longitudinal stretching → primary transverse stretching → secondary transverse stretching → heat setting → slitting and winding to obtain a semi-solid composite diaphragm;
[0065] Among them: the longitudinal stretching ratio is 10:1, the first transverse stretching ratio is 9:1, and the second transverse stretching ratio is 1.6:1.
[0066] Example 3
[0067] A semi-solid composite diaphragm, characterized in that the semi-solid composite diaphragm is composed of polyethylene, silica aerogel and solid electrolyte mother solution; wherein the mass ratio of polyethylene, silica aerogel and solid electrolyte mother solution is 1:0.7:6;
[0068] The solid electrolyte mother solution includes: polymethyl methacrylate (PMMA), Li 3 PO 4 (lithium salt), dibutyl phthalate, and N-methylpyrrolidone solvent (NMP);
[0069] Wherein: the mass ratio of polymethyl methacrylate, lithium salt and dibutyl phthalate is 15:1:0.8.
[0070] The preparation process of the semi-solid composite diaphragm of the above-mentioned embodiment 3 comprises the following specific steps:
[0071] 1. Preparation of solid electrolyte mother solution:
[0072] S1. According to the mass ratio, weigh 15 kg of polymethyl methacrylate (PMMA) and 1 kg of Li 3 PO 4 (lithium salt) is added into N-methylpyrrolidone solvent, and then magnetically stirred at 90° C. for 4 hours to form a first mixed material;
[0073] S2. Add 0.8 kg of dibutyl phthalate to the first mixed material, and continue stirring for 3 hours to obtain a solid electrolyte mother solution;
[0074] 2. Preparation of semi-solid composite diaphragm:
[0075] S1. 10 kg of polyethylene raw material was heated and melted at 160°C in an extruder, and then 0.7 kg of silica aerogel (with a porosity of about 95% and a specific surface area of ≥300 m 2 / g), uniformly mixed for 1 hour to form a second mixed material;
[0076] S2, adding 60 kg of solid electrolyte mother solution to the second mixed material and stirring for 0.5 hours to mix evenly, then heating to 200° C., evaporating and removing the N-methylpyrrolidone solvent, to obtain a third mixed material;
[0077] S3, casting the obtained third mixed material → longitudinal stretching → primary transverse stretching → secondary transverse stretching → heat setting → slitting and winding to obtain a semi-solid composite diaphragm;
[0078] Among them: the longitudinal stretching ratio is 6:1, the first transverse stretching ratio is 13:1, and the second transverse stretching ratio is 1.3:1.
[0079] Comparative Example 1
[0080] The membrane of Comparative Example 1 is set to be a commercial wet-process PE membrane.
[0081] test:
[0082] The performance of the diaphragms of Examples 1-3 and Comparative Example 1 was tested, and the results are shown in Table 1 below:
[0083] Table 1 shows the performance test results of the diaphragms of Examples 1-3 and Comparative Example 1.
[0084]
[0085] It can be seen from the test results in Table 1 that the semi-solid composite membrane of the present invention is significantly superior to the current commercial membrane (Comparative Example 1) in terms of puncture strength, 120°C / 1h thermal shrinkage, and liquid absorption rate, and there is no obvious difference in tensile strength and ionic conductivity, further demonstrating the superiority of the semi-solid composite membrane of the present invention.
[0086] The semi-solid composite diaphragm of the present invention has excellent mechanical strength, liquid absorption and retention capacity, ionic conductivity and interface compatibility, and the semi-solid composite diaphragm of the present invention uses less liquid electrolyte, inhibits the growth of lithium dendrites, and can achieve high safety of the battery.
[0087] The above are preferred embodiments of the present invention and are only used to explain the present invention, not to limit the present invention. Any obvious changes or modifications derived from the technical solution of the present invention are still within the protection scope of the present invention.
Claims
1. A method for preparing a semi-solid composite diaphragm, characterized in that: The method comprises the following steps:
1. Preparation of solid electrolyte mother solution: S1. Weigh polymethyl methacrylate and lithium salt according to mass ratio, add them to the solvent, and stir evenly to form a first mixed material; S2, adding dibutyl phthalate to the first mixed material, and continuing stirring to obtain a solid electrolyte mother solution; 2. Preparation of semi-solid composite diaphragm: S1, heating and melting the polyethylene raw material in an extruder, then adding the ceramic aerogel and mixing them evenly to form a second mixed material; S2, adding the solid electrolyte mother solution to the second mixed material and stirring evenly, and then removing the solvent to obtain a third mixed material; S3, casting the third mixed material into sheets → longitudinal stretching → primary transverse stretching → secondary transverse stretching → heat setting → slitting and winding to obtain a semi-solid composite diaphragm.
2. The method for preparing a semi-solid composite diaphragm according to claim 1, characterized in that: The method comprises the following specific steps:
1. Preparation of solid electrolyte mother solution: S1. Weigh the polymethyl methacrylate and the lithium salt according to the mass ratio, add them to the solvent, and stir them magnetically at 70 to 90° C. for 2 to 5 hours to form a first mixed material; S2, adding the dibutyl phthalate to the first mixed material, and continuing stirring for 1 to 3 hours to obtain the solid electrolyte mother solution; 2. Preparation of semi-solid composite diaphragm: S1, heating and melting the polyethylene raw material at 150-160° C. in an extruder, then adding the ceramic aerogel and mixing them evenly to form a second mixed material; S2, adding the solid electrolyte mother solution to the second mixed material and stirring evenly, then heating to 200-210° C., removing the solvent, and obtaining a third mixed material; S3, casting the third mixed material → longitudinal stretching → primary transverse stretching → secondary transverse stretching → heat setting → slitting and winding to obtain a semi-solid composite diaphragm; Among them: the longitudinal stretching ratio is (6-10):1, the first transverse stretching ratio is (9-13):1, and the second transverse stretching ratio is (1.3-1.6):
1.
3. The method for preparing a semi-solid composite diaphragm according to claim 1, characterized in that: The mass ratio of the polyethylene, the ceramic aerogel and the solid electrolyte mother solution is 1: (0.05-0.1): (6-10).
4. The method for preparing a semi-solid composite diaphragm according to claim 1, characterized in that: The molecular weight of the polyethylene is 100,000 to 1,000,000.
5. The method for preparing a semi-solid composite diaphragm according to claim 1, characterized in that: The thickness of the semi-solid composite diaphragm is 0.2-1.0 mm.
6. The method for preparing a semi-solid composite diaphragm according to claim 1, characterized in that: The ceramic aerogel is selected from one or a mixture of aluminum oxide aerogel, silicon dioxide aerogel and titanium dioxide aerogel.
7. The method for preparing a semi-solid composite diaphragm according to claim 1 or 6, characterized in that: The porosity of ceramic aerogel is 90-99% and the specific surface area is ≥300m 2 / g.
8. The method for preparing a semi-solid composite diaphragm according to claim 1, characterized in that: The mass ratio of the polymethyl methacrylate, the lithium salt and the dibutyl phthalate is (10-15):1:(0.2-0.8).
9. The method for preparing a semi-solid composite diaphragm according to claim 1, characterized in that: The lithium salt is selected from any one of LiClO4, LiBF4, LiAsF6, LiPF6, Li3PO4, Li2SiO3, and LiSiO3; and the solvent is N-methylpyrrolidone.
10. A semi-solid composite diaphragm, characterized in that: The semi-solid composite diaphragm is prepared by the preparation method according to any one of claims 1 to 9, and the semi-solid composite diaphragm is composed of polyethylene raw material, ceramic aerogel and solid electrolyte mother solution; The solid electrolyte mother solution comprises polymethyl methacrylate, lithium salt, dibutyl phthalate and a solvent.
Citation Information
Patent Citations
Ceramic diaphragm taking aerogel as powder body, and applications of ceramic diaphragm in lithium ion battery
CN106784558A
Dopamine-modified polyimide battery diaphragm as well as preparation method and application thereof