Method and application of preparing ultra-small ferrite nanoparticles by ligand molecule-microwave assisted

The preparation of ultra-small ferrite nanoparticles through the collaborative microwave method of ligand molecules solves the problem that it is difficult to achieve controllable ultra-small ferrite nanoparticles and active group modification by preparation methods in the existing technology, and realizes the size of the nanoparticles. and biologically targeted control for multiple biomedical applications.

CN115367805BActive Publication Date: 2024-10-11XIAN SUPERMAG BIO NANOTECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211003093.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-08-19
Publication Date
2024-10-11
Estimated Expiration
2042-08-19

AI Technical Summary

Technical Problem

In the existing technology, the preparation method of ultra-small ferrite nanoparticles is difficult to achieve controllable macro-preparation and active group modification, resulting in uneven size and poor crystallinity, which affects the magnetic resonance T1 enhancement performance.

Method used

Using the ligand molecule collaborative microwave method, the metal precursor and ligand molecules are mixed in proportion, reacted under microwave conditions, and the pH value is adjusted to form ultra-small ferrite nanoparticles with a diameter of 2 to 5 nm, and pass through different PEG derivatives disubstituted with functional groups modify the surface to achieve biological targeting.

Benefits of technology

The ultra-small ferrite nanoparticles have controllable size components, short production cycle, good monodispersity, high crystallinity, and bioactive groups, making them suitable for magnetic resonance imaging, magnetic hyperthermia and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115367805B_ABST
    Figure CN115367805B_ABST
Patent Text Reader

Abstract

The present invention discloses a method and application of preparing ultra-small ferrite nanoparticles by ligand molecules in coordination with microwaves. The method comprises mixing a metal precursor and a ligand molecule in proportion, adding a pH regulator to adjust the pH value, and then reacting under microwave conditions, wherein the metal precursor forms ferrite nanoparticles, and the ligand molecules are modified on the surface of the ferrite nanoparticles to obtain ultra-small ferrite nanoparticles with a diameter of 2 to 5 nm. The metal precursor is composed of an iron-containing salt and a salt of metal M, and the metal M is any one of Fe, Mn, Co, Ni, Zn, Cu, and Mg. The molar ratio of the iron-containing salt, the salt of metal M to the ligand molecule is 2:1:60 to 150. The ultra-small ferrite nanoparticles modified by the ligand molecules of the present invention can provide biological targeting functions or provide targeting active sites. Moreover, the particles have good monodispersity and high crystallinity, and are widely used in biomedical fields such as magnetic resonance imaging and magnetic hyperthermia.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of biomedical materials and imaging materials, and specifically relates to a method for preparing ultra-small ferrite nanoparticles by using ligand molecules in coordination with microwaves and an application thereof. Background Art

[0002] Ferrite nanomaterials (MFe 2 O 4 , M=Fe, Mn, Co, Ni, Zn, Cu, etc.) can be used as medical materials such as magnetic resonance imaging contrast agents, magnetic hyperthermia agents, and drug delivery carriers due to their unique magnetic properties and excellent biocompatibility, and are widely used in the biomedical field [Advanced Healthcare Materials, 2020, 9(9): 1901058; Materials Today, 2016, 19(3): 157-168; Chemical Society Reviews, 2015, 44(14): 4501-4516; Chemical Reviews, 2015, 115(19): 10637-10689]. The latest research found that when the size of ferrite particles is reduced to below 5nm, they can form a core-shell structure consisting of a high proportion of surface paramagnetic amorphous layers and an internal extremely small ferromagnetic core, and show excellent magnetic resonance T1 enhancement effect [Nano Letters, 2009, 9 (12): 4434-4440; Langmuir, 2007, 23 (8): 4583-458]. At present, the research on ultra-small ferrite nanoparticles in the field of magnetic resonance T1 contrast agents has made great progress, but the method of controllable large-scale preparation of water-soluble monodisperse ultra-small ferrite nanoparticles modified with active groups is still lacking.

[0003] Currently, the main preparation methods of monodisperse ultrasmall ferrite nanoparticles are generally divided into two categories: high-temperature organic phase synthesis method and aqueous phase reduction of metal salt method [Drug Discovery Today, 2019, 24(3): 835-844; Advanced Materials, 2018, 30(49): 1802309].

[0004] When preparing ferrite nanoparticles by the traditional method of reducing metal salts in water, the growth rate of the process is fast and difficult to control, so the prepared ferrite nanoparticles are usually large and uneven in size. In addition, controlling the growth rate by adding stabilizers to the water phase is a commonly used method for preparing monodisperse ferrite nanoparticles, but the stabilizers bound to the surface of the particles make it difficult to subsequently modify the active groups. At the same time, due to the low reaction temperature in the water phase, the ferrite particles have poor crystallinity, which affects their magnetic resonance T1 enhancement performance.

[0005] The high-temperature organic phase synthesis method can obtain monodisperse, highly crystalline ultrasmall ferrite nanoparticles. However, it can only obtain oil-soluble nanoparticles. The oil phase particles need to be modified with water-soluble molecules before they can be used in biomedical applications. The operation is complicated and the cost is high. Summary of the invention

[0006] In order to solve the above problems existing in the prior art, the present invention provides a method and application of preparing ultra-small ferrite nanoparticles by ligand molecules in cooperation with microwaves. The technical problem to be solved by the present invention is achieved by the following technical solutions:

[0007] A method for preparing ultrasmall ferrite nanoparticles by ligand molecules in coordination with microwaves, comprising: mixing a metal precursor and a ligand molecule in proportion, adding a pH regulator to adjust the pH value, and then reacting under microwave conditions, wherein the metal precursor forms ferrite nanoparticles, and the ligand molecules are modified on the surface of the ferrite nanoparticles to obtain ultrasmall ferrite nanoparticles with a diameter of 2 to 5 nm; wherein the metal precursor is composed of an iron-containing salt and a salt of a metal M, and the metal M is any one of Fe, Mn, Co, Ni, Zn, Cu, and Mg; and the molar ratio of the iron-containing salt to the salt of the metal M to the ligand molecule is 2:1:60 to 150.

[0008] In one embodiment of the present invention, the ligand molecule is a heterofunctional disubstituted PEG derivative, including a first group X and a second group Y, forming an X-PEG-Y structure; the first group X is bound to the surface of the ferrite nanoparticles, and the surface energy of the particles is regulated by regulating the type of the first group X to control the size of the ferrite nanoparticles to meet the ultra-small range; the second group Y is bound to the ferrite nanoparticles through X-PEG-, and provides a biological targeting function or a targeting active site for the ferrite nanoparticles, so that the ultra-small ferrite nanoparticles modified by the ligand molecule are targeted and bound to specific biological tissues.

[0009] In one embodiment of the present invention, the first group X is any one of a hydroxamic acid group, a phosphate group, a carboxyl group, and a catechol group.

[0010] In one embodiment of the present invention, the second group Y is any one of a thiol group, a maleimide group, a carboxyl group, a catechol group, an anilino group, and a hydroxamic acid group.

[0011] In one embodiment of the present invention, the concentration of the ligand molecule is 20-50 mM.

[0012] In one embodiment of the present invention, the iron-containing salt includes at least one of ferric chloride, ferric nitrate, ferric sulfate and ferric carbonate.

[0013] In one embodiment of the present invention, the salt of the metal M includes at least one of ferric nitrate, cobalt nitrate, manganese nitrate, nickel nitrate, copper nitrate, zinc nitrate, magnesium nitrate, ferric sulfate, cobalt sulfate, nickel sulfate, manganese sulfate, zinc sulfate, ferric chloride, cobalt chloride, manganese chloride, nickel chloride, copper chloride, zinc chloride, and magnesium chloride.

[0014] In one embodiment of the present invention, the microwave conditions are as follows: the microwave temperature control range is 100-150° C., the microwave power control range is 100-2800 W, and the microwave time control range is 5-15 min.

[0015] The present invention also provides a ligand molecule modified ultra-small ferrite nanoparticle, comprising ferrite nanoparticles and ligand molecules modified on the surface of the ferrite nanoparticles; the ferrite nanoparticles are formed by a metal precursor, the metal precursor is composed of an iron-containing salt and a metal M salt, and the metal M is any one of Fe, Mn, Co, Ni, Zn, Cu, and Mg; the ultra-small ferrite nanoparticles modified by the ligand molecules are mixed by a molar ratio of 2:1:60 to 150 with an iron-containing salt, a metal M salt, and a metal ligand molecule, and a pH regulator is added to adjust the pH value, and then reacted under microwave conditions to obtain the ultra-small ferrite nanoparticles modified by the ligand molecules; the diameter size of the ultra-small ferrite nanoparticles modified by the ligand molecules is 2 to 5 nm;

[0016] The ligand molecule is a heterofunctional disubstituted PEG derivative, wherein the PEG derivative comprises a first group X and a second group Y to form an X-PEG-Y structure;

[0017] The first group X is bound to the surface of the ferrite nanoparticles, and the surface energy of the particles is regulated by regulating the type of the first group X, thereby controlling the size of the nanoparticles to meet an ultra-small range; the second group Y is bound to the ferrite nanoparticles through X-PEG-, and provides a biological targeting function or a targeting active site for the ferrite nanoparticles, so that the ferrite nanoparticles can be targetedly bound to specific biological tissues.

[0018] The present invention also provides an application of ultrasmall ferrite nanoparticles modified by ligand molecules. The ultrasmall ferrite nanoparticles modified by ligand molecules are prepared by any of the preparation methods described above and are applied to the fields of magnetic resonance imaging, long-term cell tracking or magnetic nanoparticle imaging.

[0019] Beneficial effects of the present invention: The method of preparing ultrasmall ferrite nanoparticles by ligand molecules in cooperation with microwaves of the present invention has controllable size components, short production cycle, good monodispersity and high crystallinity; and the ultrasmall ferrite nanoparticles have biologically active groups, through which targeted binding with specific biological tissues can be achieved, providing biological targeting functions or providing targeted active sites, and can be applied in multiple fields such as magnetic resonance imaging, magnetic hyperthermia and other biomedical fields.

[0020] The present invention will be further described in detail below with reference to the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 It is a structural schematic diagram of a ligand molecule-modified ultra-small ferrite nanoparticle and its components provided in an embodiment of the present invention;

[0022] Figure 2 Schematic diagram of a one-pot method for preparing ultra-small ferrite nanoparticles modified with ligand molecules provided in an embodiment of the present invention;

[0023] Figure 3 1 is a transmission electron microscope image and a particle size distribution diagram of ultra-small manganese ferrite nanoparticles prepared in Example 1 of the present invention;

[0024] Figure 4 is an XRD diagram of ultra-small ferrite nanoparticles prepared in Example 1 of the present invention;

[0025] Figure 5 It is a transmission electron microscope image and a particle size distribution diagram of ferrite nanoparticles prepared by the preparation method provided in Comparative Example 1;

[0026] Figure 6 This is a graph showing the size of ferrite nanoparticles obtained by adjusting the type of active groups of the ligand molecule;

[0027] Figure 7 This is a graph showing the size of ferrite nanoparticles obtained by adjusting the concentration of ligand molecules. DETAILED DESCRIPTION

[0028] The present invention is further described in detail below with reference to specific embodiments, but the embodiments of the present invention are not limited thereto.

[0029] See also Figure 1 , Figure 1 is a schematic diagram of the structure of a ligand molecule-modified ultra-small ferrite nanoparticle and its components provided in an embodiment of the present invention, such as Figure 1As shown, the ultra-small ferrite nanoparticle 1 modified by a ligand molecule includes a ferrite nanoparticle 2 and a ligand molecule 3 modified on the surface of the ferrite nanoparticle 2, wherein the ligand molecule 3 is a PEG (polyethylene glycol) derivative with a heterofunctional disubstituted structure, including a first group X and a second group Y, forming an X-PEG-Y structure; the first group X is bound to the surface of the ferrite nanoparticle, and the surface energy of the particle is regulated by regulating the type of the first group X to control the diameter size of the nanoparticle to meet the ultra-small range; the second group Y is bound to the ferrite nanoparticle through X-PEG-, and provides a biological targeting function or a targeting active site for the ferrite nanoparticle, so that the ferrite nanoparticle can be targetedly combined with a specific biological tissue.

[0030] The molecular weight of PEG in the heterofunctional disubstituted PEG derivative X-PEG-Y is in the range of 200 to 20,000. As an embodiment, the reaction kinetics can be regulated by changing the viscosity of the reaction solvent by selecting PEG of different molecular weights. It should be noted that in all embodiments of the present invention, the X group in X-PEG-Y can be a polymer containing an X group, and the Y group can be a polymer containing a Y group.

[0031] The first group X active group in the heterofunctional disubstituted PEG derivative is any one of a hydroxamic acid group, a phosphate group, a carboxyl group, and a catechol group, which acts to bind to the surface of the ferrite nanoparticles to reduce the surface energy, while passivating the ferrite nanoparticles, slowing down the growth, and controlling the size of the nanoparticles. For example, the catechol group in dopamine can coordinate with the iron on the surface of manganese ferrite. Further, during the microwave thermal decomposition process, when the ligand molecule 3 is tightly bound to the surface of the ferrite nanoparticle 2, the surface energy of the particles can be regulated by changing different X groups, thereby regulating the growth kinetics and thermodynamics of the nanoparticles, and then stabilizing the size of the nanoparticles within an ultra-small size range. After testing, the hydroxamic acid group, the phosphate group, the carboxyl group, and the catechol group provided in the embodiment of the present invention as the X active group can make the prepared ferrite nanoparticles meet the ultra-small size range.

[0032] In addition, due to the hard and soft acid-base principle, hard acids preferentially bind to hard bases, and soft acids preferentially bind to soft bases. For example, the phosphate group in the phosphate-PEG-carboxyl group preferentially binds to the iron on the surface of the manganese ferrite than the catechol group in the dopamine-PEG-carboxyl group, reducing the surface energy of the nanoparticles and limiting their growth. Therefore, under the same reaction conditions, the size of the ferrite nanoparticles modified by the dopamine-PEG-carboxyl ligand is larger than that modified by the phosphate-PEG-carboxyl ligand. Therefore, it can be obtained that the size rule of the nanoparticles modified by the first type of group X ligand molecules is carboxyl>hydroxamic acid>catechol>phosphate. This rule can be used to adjust the type of the first type of group X so that the size of the ultra-small ferrite nanoparticles 1 modified by the ligand molecules obtained in the final stage can be regulated within the range of 2 to 5 nm. As a preferred embodiment, the first type of group X selects a phosphate group, and the particle size distribution of the final ferrite nanoparticles obtained by using a phosphate group as the PEG derivative of the first type of group X is narrow, and the difference between the synthetic batches is small.

[0033] The second group Y in the heterofunctional disubstituted PEG derivative is any one of thiol, maleimide, carboxyl, catechol, aniline, and hydroxamic acid groups, which acts to provide biological targeting function or targeted active sites for ferrite nanoparticles so that they can be targeted to specific biological tissues. For example, ethoxybenzene (EOB) in phosphate-PEG-EOB is a hepatocyte-specific ligand used in clinical practice for a long time, which can target hepatocytes and give nanoparticles the function of targeting hepatocytes; another example: the carboxyl group in phosphate-PEG-carboxyl can modify some targeted amino acids (CREKA) and antibodies (PMSA) on the surface of nanoparticles through amide reaction, giving them a targeting function, so that they can be targeted to breast cancer and prostate cancer. As an object of the present invention, the targeting performance of ferrite nanoparticles can be changed by regulating the type of the second group Y.

[0034] The heterofunctional disubstituted PEG derivative used in the embodiment of the present invention is a water-soluble polymer material. Since it has very low interfacial free energy in water and its molecular chain is flexible and highly active, it has good water solubility, so that the prepared ligand molecule-modified ultrasmall ferrite nanoparticles can be evenly dispersed in an aqueous solution.

[0035] The ferrite nanoparticles 2 of the embodiment of the present invention are formed by a metal precursor, which is composed of an iron-containing salt and a salt of a metal M, and the metal M is any one of Fe, Mn, Co, Ni, Zn, Cu, and Mg; the ligand-modified ultrasmall ferrite nanoparticles are obtained by mixing an iron-containing salt, a salt of a metal M, and a metal ligand in a molar ratio of 2:1:60 to 150, and then reacting under microwave conditions.

[0036] Among them, the iron-containing salt includes: at least one of ferric chloride, ferric nitrate, ferric sulfate, and ferric carbonate, that is, it can be any single iron salt, or it can be two or more iron salts at the same time; the salt of metal M includes: at least one of ferric nitrate, cobalt nitrate, manganese nitrate, nickel nitrate, copper nitrate, zinc nitrate, magnesium nitrate, ferric sulfate, cobalt sulfate, nickel sulfate, manganese sulfate, zinc sulfate, ferric chloride, cobalt chloride, manganese chloride, nickel chloride, copper chloride, zinc chloride, and magnesium chloride, that is, it can be any single salt of metal M, or it can be two or more salts of metal M at the same time.

[0037] Since the spherical shape has the lowest surface energy, the spinel ferrite nanoparticles composed of iron-containing salts and metal M salts are easy to form a spherical structure. Figure 1 This is just an example of a structure of the present invention. The number of ligand molecules bound to a ferrite nanoparticle does not necessarily have to be six. As the concentration of the ligand molecules increases, the number of ligand molecules bound to the ferrite nanoparticle increases accordingly.

[0038] The ligand-modified ultrasmall ferrite nanoparticles provided in an embodiment of the present invention have biologically active groups, through which targeted binding with specific biological tissues can be achieved, thereby providing biological targeting functions or providing targeted active sites; and the particle size components are controllable and meet the requirements of 2 to 5 nm, the particles have good monodispersity and high crystallinity, and are widely used in biomedical fields such as magnetic resonance imaging and magnetic hyperthermia.

[0039] See also Figure 2 , Figure 2 It is a schematic diagram of a one-pot method for preparing ultra-small ferrite nanoparticles modified by ligand molecules provided in an embodiment of the present invention. The ultra-small ferrite nanoparticles modified by ligand molecules in an embodiment of the present invention are different from the traditional method of reducing metal salts in aqueous phase of ultra-small ferrite nanoparticles. All reactants including iron precursor, metal M precursor, pH regulator, and ligand molecules are added to an aqueous solution and reacted in one pot under microwave conditions to prepare the ultra-small ferrite nanoparticles. The ultra-small ferrite nanoparticles obtained by this method have controllable size components, short production cycle, good monodispersity, and high crystallinity. The preparation method of the present invention can achieve controllable, rapid, and large-scale preparation, providing a feasible method for the preparation of water-soluble ultra-small ferrite nanoparticles.

[0040] An embodiment of the present invention provides a method for preparing ultrasmall ferrite nanoparticles by using ligand molecules in conjunction with microwaves. The method comprises mixing a metal precursor and a ligand molecule in proportion, adding a pH adjuster to adjust the pH value, and then reacting the mixture under microwave conditions. The metal precursor forms ferrite nanoparticles, and the ligand molecules are modified on the surface of the ferrite nanoparticles to obtain ultrasmall ferrite nanoparticles with a diameter of 2 to 5 nm. The metal precursor is composed of an iron-containing salt and a salt of a metal M, and the metal M is any one of Fe, Mn, Co, Ni, Zn, Cu, and Mg. The molar ratio of the iron-containing salt, the salt of the metal M, and the ligand molecule is 2:1:60 to 150.

[0041] The ligand molecule is a PEG derivative with a heterofunctional group disubstituted, including a first group X and a second group Y, forming an X-PEG-Y structure; the first group X is combined with the surface of the ferrite nanoparticle, and the surface energy of the particle is regulated by regulating the type of the first group X, thereby controlling the size of the ferrite nanoparticle to meet an ultra-small range; the second group Y is combined with the ferrite nanoparticle through X-PEG-, and provides a biological targeting function or a targeting active site for the ferrite nanoparticle, so that the ultra-small ferrite nanoparticle modified by the ligand molecule is targetedly combined with a specific biological tissue.

[0042] The first group X is any one of a hydroxamic acid group, a phosphoric acid group, a carboxyl group, and a catechol group. The second group Y is any one of a thiol group, a maleimide group, a carboxyl group, a catechol group, an aniline group, and a hydroxamic acid group.

[0043] The iron-containing salt is any one of ferric chloride, ferric nitrate, ferric sulfate, and ferric carbonate. The salt of metal M includes at least one of ferric nitrate, cobalt nitrate, manganese nitrate, nickel nitrate, copper nitrate, zinc nitrate, magnesium nitrate, ferric sulfate, cobalt sulfate, nickel sulfate, manganese sulfate, zinc sulfate, ferric chloride, cobalt chloride, manganese chloride, nickel chloride, copper chloride, zinc chloride, and magnesium chloride.

[0044] It should be noted that the structure of the ultrasmall ferrite nanoparticles modified by ligand molecules involved in the preparation method of the embodiment of the present invention, the specific requirements of each raw material and the overall efficacy achieved are the same as the ultrasmall ferrite nanoparticles modified by ligand molecules provided in the aforementioned embodiment of the present invention, and will not be repeated here.

[0045] In the preparation method provided in the embodiment of the present invention, the concentration of the ligand molecule is preferably 20 to 50 mM. In some embodiments, by adjusting the concentration of the ligand molecule 3, the size of the ultra-small ferrite nanoparticles 1 modified by the ligand molecule can be adjusted. On the one hand, due to the different binding amounts of ligand molecules in the nanoparticles of different concentrations, the surface energy of the particles is different, thereby regulating the size of the prepared particles; on the other hand, different concentrations of ligand molecules in the reaction system change the viscosity of the reaction mixture differently, thereby regulating the diffusion dynamics of the reactants and achieving controllable preparation of nanoparticles of different sizes. When the concentration of the ligand molecule 3-phospho-PEG-carboxyl is 0.01 to 1 mM, the size of the ferrite nanoparticles is about 15 nm; when the concentration of the ligand molecule 3-phospho-PEG-carboxyl is 1 to 20 mM, the size is about 10 nm; in a preferred embodiment of the present invention, when the concentration of the ligand molecule 3-phospho-PEG-carboxyl is 20 to 50 mM, the size range of the ferrite nanoparticles is 3 nm.

[0046] The preparation method of the present invention needs to be carried out under microwave conditions, the microwave temperature control range is 100-150°C, the microwave power control range is 100-2800W, and the microwave time control range is 5-15min. The microwave hydrothermal method used in the present invention is different from the general microwave hydrothermal method, and does not need to add a stabilizer separately, and will not cause the ferrite nanoparticles to have large size distribution and poor dispersibility due to the presence of the stabilizer, and it is very difficult to further modify the active groups with biological functions. Therefore, the use of heterofunctional disubstituted polyethylene glycol derivative ligand molecules not only acts as a stabilizer in the reaction, but also can make the nanoparticles targeted by changing the type of active groups, and the prepared nanoparticles have an ultra-small size range and good dispersibility.

[0047] In the preparation method provided in the embodiment of the present invention, after the reaction is completed, a washing step and a step of dispersing the washed product in deionized water may also be included.

[0048] The preparation method of ultra-small ferrite nanoparticles prepared by the preparation method provided by the present invention is described in detail below in conjunction with specific embodiments, comparative examples and drawings.

[0049] Embodiment 1

[0050] Preparation of Ultrasmall Ferrite Nanoparticles Modified with Phospho-PEG1500-Carboxyl

[0051] (1) Weigh 5.406 g of ferric chloride, 1.979 g of manganese chloride, and 25 mM phosphate-PEG1500-carboxyl in a molar ratio of 2:1:75, add 30 mL of deionized water, slowly add urea at a constant temperature on a magnetic stirrer to adjust the pH to 8.5, then transfer to a microwave instrument, maintain the temperature at 120°C, the microwave instrument power at 400 W, maintain for 10 min, and the reaction is completed;

[0052] (2) Cooling to below 50° C., washing the product three times by deionized water dispersion-centrifugation to obtain the product. The final product was dispersed in 10 mL of deionized water.

[0053] Embodiment 2

[0054] Preparation of Ultrasmall Ferrite Nanoparticles Modified with Phospho-PEG1500-Carboxyl

[0055] (1) Weigh 5.406 g of ferric chloride, 1.979 g of manganese chloride, and 50 mM dopamine-PEG1500-carboxyl in a molar ratio of 2:1:150, then add 30 mL of deionized water, slowly add urea at a constant temperature on a magnetic stirrer to adjust the pH to 8.5, then transfer to a microwave instrument, maintain the temperature at 120°C, the microwave instrument power at 400 W, maintain for 10 min, and the reaction is completed;

[0056] (2) Cooling to below 50° C., washing the product three times by deionized water dispersion-centrifugation to obtain the product. The final product was dispersed in 10 mL of deionized water.

[0057] Embodiment 3

[0058] Preparation of Ultrasmall Ferrite Nanoparticles Modified with Phospho-PEG1500-Carboxyl

[0059] (1) Weigh 5.406 g of ferric chloride, 1.979 g of manganese chloride, and 20 mM dopamine-PEG1500-carboxyl in a molar ratio of 2:1:60, add 30 mL of deionized water, slowly add urea at a constant temperature on a magnetic stirrer to adjust the pH to 8.5, then transfer to a microwave instrument, maintain the temperature at 120°C, the microwave instrument power at 400 W, maintain for 10 min, and the reaction is completed;

[0060] (2) Cooling to below 50° C., washing the product three times by deionized water dispersion-centrifugation to obtain the product. The final product was dispersed in 10 mL of deionized water.

[0061] Embodiment 4

[0062] Preparation of Ultrasmall Ferrite Nanoparticles Modified with Catechol-PEG1500-Maleimide

[0063] (1) Weigh 4.840 g of ferric nitrate, 2.564 g of magnesium nitrate, and 25 mM of catechol-PEG1500-maleimide, with a molar ratio of 2:1:75. Add 30 mL of deionized water, slowly add urea at a constant temperature on a magnetic stirrer to adjust the pH to 8.5, then transfer to a microwave, keep the temperature at 120°C, the microwave power at 400 W, and keep for 10 min. The reaction is complete.

[0064] (2) Cooling to below 50° C., washing the product three times by deionized water dispersion-centrifugation to obtain the product. The final product was dispersed in 10 mL of deionized water.

[0065] Embodiment 5

[0066] Preparation of Ultrasmall Ferrite Nanoparticles Modified with Hydroxamic Acid-PEG1500-Catechol

[0067] (1) Weigh 3.078 g of ferric sulfate, 1.614 g of zinc sulfate, and 25 mM of hydroxamic acid-PEG1500-catechol in a molar ratio of 2:1:75, add 30 mL of deionized water, slowly add urea at a constant temperature on a magnetic stirrer to adjust the pH to 8.5, then transfer to a microwave instrument, maintain the temperature at 150°C, the microwave instrument power at 100 W, maintain for 10 min, and the reaction is completed;

[0068] (2) Cooling to below 50° C., washing the product three times by deionized water dispersion-centrifugation to obtain the product. The final product was dispersed in 10 mL of deionized water.

[0069] Embodiment 6

[0070] Preparation of Ultrasmall Ferrite Nanoparticles Modified with Dopamine-PEG1500-aniline

[0071] (1) Weigh 2.317 g of iron carbonate, 1.344 g of copper chloride, and 25 mM dopamine-PEG1500-aniline, with a molar ratio of 2:1:75, add 30 mL of deionized water, slowly add urea at a constant temperature on a magnetic stirrer to adjust the pH to 8.5, then transfer to a microwave instrument, maintain the temperature at 100°C, the microwave instrument power at 2800 W, maintain for 15 min, and the reaction is completed;

[0072] (2) Cooling to below 50° C., washing the product three times by deionized water dispersion-centrifugation to obtain the product. The final product was dispersed in 10 mL of deionized water.

[0073] Comparative Example 1

[0074] (1) Weigh 5.406 g of ferric chloride, 1.979 g of manganese chloride, and 25 mM PEG1500, with a molar ratio of 2:1:75. Add 30 mL of deionized water, slowly add urea at a constant temperature on a magnetic stirrer to adjust the pH to 8.5, then transfer to a microwave, maintain the temperature at 120°C, the microwave power at 400 W, maintain for 10 min, and the reaction is complete;

[0075] (2) Cooling to below 50°C, washing the product three times by deionized water dispersion-centrifugation. The final product was dispersed in 10 mL of deionized water.

[0076] Take 100 μL of the product obtained in Example 1, disperse it in anhydrous ethanol, take 2 μL of the anhydrous ethanol solution with dispersed nanoparticles and drop it on the copper mesh, dry it naturally and then characterize it. Use transmission electron microscopy to verify the size and morphology of the obtained product. Figure 3 , Figure 3 1 is a transmission electron microscope image and a particle size distribution diagram of ultra-small manganese ferrite nanoparticles prepared in Example 1 of the present invention. Figure 3 It can be seen from the transmission electron microscopy image (a) that the size and morphology of the ferrite nanoparticles are uniform; the particle size statistics of the particles in the image are performed using image J ( Figure 3 (b)), it can be seen that the size of ferrite nanoparticles is about 3 nm and the size distribution is narrow.

[0077] An appropriate amount of ultra-small ferrite nanoparticles prepared in the embodiment of the present invention was freeze-dried, and the crystal structure of the ultra-small ferrite nanoparticles was characterized by XRD. Figure 4 This is the XRD diagram of the ultrasmall ferrite nanoparticles prepared in Example 1 of the present invention. The results show that the prepared manganese ferrite particles are completely matched with the standard spinel structure manganese ferrite powder (JCPDS standard card number 10-0319), no other impurity phases such as manganese oxide or ferrous oxide are present, and the ultrasmall ferrite nanoparticles have good crystallinity.

[0078] For comparison, 100 μL of the product obtained in Comparative Example 1 was dispersed in anhydrous ethanol, and 2 μL of the anhydrous ethanol solution containing dispersed nanoparticles was dropped on a copper mesh. After natural drying, the product was characterized and the size and morphology of the product were verified by transmission electron microscopy. Figure 5 , Figure 5 The transmission electron microscope image and particle size distribution diagram of ferrite nanoparticles prepared by the preparation method provided in Comparative Example 1 are shown. Figure 5 It can be seen from the transmission electron microscopy image (a) that the size and morphology of the ferrite nanoparticles are not uniform; the particle size statistics of the particles in the image were performed using image J ( Figure 5(b)), it can be seen that the size of ferrite nanoparticles is about 8 nm and the size distribution is wide.

[0079] The embodiment of the present invention also provides a method for controlling the size of the obtained ultra-small ferrite nanoparticles 1 by regulating the type of active groups in the ligand molecules 3. The size of the nanoparticles modified by the ligand molecules follows the rule of carboxyl>hydroxamic acid>catechol>phosphate. The active group can be selected according to the required size of the nanoparticles. For details, please refer to Figure 6 The statistical results in . Figure 6 The result of adjusting the type of active groups of ligand molecules to obtain the size of ferrite nanoparticles. The vertical axis in the figure is the size of ferrite nanoparticles, and the horizontal axis is the type of active groups of ligand molecule 3. The methyl group in the figure is for comparison. The size rule of nanoparticles modified by ligand molecules is carboxyl group>hydroxamic acid>catechol>phosphate group.

[0080] In addition, by adjusting the concentration of the ligand molecule 3, the size of the final ligand molecule-modified ultra-small ferrite nanoparticles 1 can also be adjusted. Figure 7 The statistical results in . Figure 7 FIG. 3 is a graph showing the size of ferrite nanoparticles obtained by adjusting the concentration of ligand molecule 3. The ordinate in the graph is the size of the ferrite nanoparticles, and the abscissa is the concentration of ligand molecule 3. Figure 7 As shown, when the ligand concentration is in the range of 20 to 50 mM, ultra-small nanoparticles can be prepared, and as the ligand concentration increases, the particle size gradually decreases.

[0081] The embodiment of the present invention proposes a method for preparing ultra-small ferrite nanoparticles by ligand molecules in coordination with microwaves. The preparation of water-soluble ultra-small ferrite nanoparticles with high crystallinity and good monodispersity is achieved by controlling the type of ligand molecules, the ratio of ligand molecules to precursors, and the microwave heating time. The regulation of the size and components of the nanoparticles can also be achieved, and they are ultimately applied to biomedical fields such as magnetic resonance imaging and magnetic hyperthermia. The water-soluble ultra-small ferrite nanoparticles prepared by the preparation method of the present invention have biologically active groups, through which targeted binding with specific biological tissues can be achieved, providing biological targeting functions or targeted active sites for them; and the particle size components are controllable and meet the requirements of 2 to 5 nm, the particles have good monodispersity and high crystallinity, and are widely used in biomedical fields such as magnetic resonance imaging and magnetic hyperthermia.

[0082] The embodiment of the present invention also provides an application of ultra-small ferrite nanoparticles modified by ligand molecules, which are prepared by the preparation method described in any of the above embodiments and are applied to the fields of magnetic resonance imaging, long-term cell tracking or magnetic nanoparticle imaging. The specific preparation process and the function of the prepared ultra-small ferrite nanoparticles are the same as those of the above preparation method, and will not be repeated here.

[0083] The above contents are further detailed descriptions of the present invention in combination with specific preferred embodiments, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. For ordinary technicians in the technical field to which the present invention belongs, several simple deductions or substitutions can be made without departing from the concept of the present invention, which should be regarded as falling within the protection scope of the present invention.

Claims

1. A method for preparing ultra-small ferrite nanoparticles by using ligand molecules in cooperation with microwaves, characterized in that: The metal precursor and the ligand molecule with a concentration of 20 to 50 mM are mixed in proportion, a pH adjuster is added to adjust the pH value, and then the mixture is reacted under microwave conditions with a microwave temperature control range of 100 to 150° C., a microwave power control range of 100 to 2800 W, and a microwave time control range of 5 to 15 min, so that the metal precursor forms ferrite nanoparticles, and the ligand molecule is modified on the surface of the ferrite nanoparticles to obtain ultra-small ferrite nanoparticles with a diameter of 2 to 5 nm. The metal precursor is composed of an iron-containing salt and a salt of a metal M, and the metal M is any one of Fe, Mn, Co, Ni, Zn, Cu, and Mg; the molar ratio of the iron-containing salt, the salt of the metal M, and the ligand molecule is 2:1:60-150; The ligand molecule is a heterofunctional disubstituted PEG derivative, comprising a first group X and a second group Y, forming an X-PEG-Y structure; The first group X is combined with the surface of the ferrite nanoparticles, and under the synergistic effect of the microwave conditions, the surface energy of the particles can be regulated by regulating the type of the first group X, thereby controlling the size of the ferrite nanoparticles to meet an ultra-small range; the first group X is any one of a hydroxamic acid group, a phosphate group, a carboxyl group, and a catechol group; the size rule of the nanoparticles modified with the ligand molecules of the first group X is carboxyl group>hydroxamic acid>catechol group>phosphate group; The second type of group Y is bound to the ferrite nanoparticles through X-PEG, and provides biological targeting function or targeted active sites for the ferrite nanoparticles, so that the ultrasmall ferrite nanoparticles modified with the ligand molecules can be targetedly bound to specific biological tissues; the second type of group Y is any one of thiol, maleimide, carboxyl, catechol, aniline, and hydroxamic acid groups.

2. The method according to claim 1, characterized in that The iron-containing salt includes at least one of ferric chloride, ferric nitrate and ferric sulfate.

3. The method according to claim 1, characterized in that The salt of the metal M includes at least one of cobalt nitrate, manganese nitrate, nickel nitrate, copper nitrate, zinc nitrate, magnesium nitrate, cobalt sulfate, nickel sulfate, manganese sulfate, zinc sulfate, cobalt chloride, manganese chloride, nickel chloride, copper chloride, zinc chloride and magnesium chloride.

4. A ligand molecule-modified ultra-small ferrite nanoparticle for use in the field of imaging, characterized in that: Prepared by the method according to any one of claims 1 to 3.

5. An application of ultra-small ferrite nanoparticles modified by ligand molecules, characterized in that: The ligand molecule-modified ultrasmall ferrite nanoparticles are prepared by the method according to any one of claims 1 to 3, and are applied in the fields of magnetic resonance imaging, long-term cell tracking or magnetic nanoparticle imaging.