Method for preparing patterned QLED based on electrostatic adsorption of quantum dots
By combining electrostatic adsorption technology with P4VP film and dip pen nanolithography, the problem of alignment and fixation of quantum dots in nanopatterning is solved, and high-brightness, high-resolution quantum dot light-emitting diode devices are realized, which are suitable for the next generation. display device.
Patent Information
- Application Number
- CN202211162470.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-23
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-09-23
AI Technical Summary
When manufacturing high-resolution and uniform quantum dot light-emitting diode devices with existing technologies, nanopatterning technology has solution/substrate interface complexity, which makes it difficult to achieve precise alignment and fixation of quantum dots at designed positions, leading to non-specific deposition problems.
The electrostatic adsorption technology combining P4VP film and dip pen nanolithography (DPN) method is used to form a pattern through local protonation, adsorb the ionized quantum dots to achieve precise fixation, and transfer the patterned quantum dot film through transfer technology. Transfer to QLED base functional layer to prepare QLED device.
The pixel size of the quantum dot device is reduced to the nanometer level, and a high-brightness, high-resolution display pixel unit is obtained. The process is safe, pollution-free, and simple and easy to operate.
Smart Images

Figure CN115377339B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of nano-LED preparation, and in particular relates to a method for preparing patterned QLED based on electrostatic adsorption of quantum dots. Background Art
[0002] Colloidal quantum dots are particles with a radius size range of about the Bohr radius, and their special size effect gives them excellent optoelectronic properties. For example, continuous high-brightness spectral regulation can be achieved by controlling the size of the particles. In addition, it also has a core-shell structure, which gives quantum dots extremely high quantum yields and good stability. These advantages make quantum dots have broad prospects in the development of next-generation displays. At present, although there have been major breakthroughs in quantum dot-based quantum dot light-emitting diode devices, there is still a lack of technology for manufacturing high-resolution and uniform patterns. The difficulty in achieving nano-patterning of quantum dot light-emitting diode devices lies in the complexity at the solution / substrate interface. In order to align at a defined position with nanometer precision, it requires a series of interactions between quantum dots and substrates. It requires long-range particle-substrate attraction to enrich the quantum dots on the substrate for efficient and rapid assembly, strong short-range attraction to fix the quantum dots at the designed position, and counteraction to avoid nonspecific deposition of quantum dots in undesirable areas. Summary of the invention
[0003] In view of the defects and shortcomings of the prior art, the present invention proposes a method for preparing patterned QLEDs based on electrostatic adsorption of quantum dots. The DPN (dip pen nanolithography) method is used to prepare patterned films and combined with ligand modification. The principle of electrostatic adsorption is used to precisely fix the quantum dots at the designed positions, thereby obtaining high-brightness, high-PPI display pixel units that can be applied to the next generation of displays.
[0004] First, a P4VP (4-vinylpyridine diblock copolymer) film is prepared, and then a patterned P4VP film is prepared using the DPN (dip pen nanolithography) method. Finally, quantum dots modified with ligands (such as carboxylic acid, phosphonic acid, and thiol-terminated ligands) are spin-coated on the P4VP film.
[0005] The pattern on the P4VP film is formed due to local protonation. The quantum dots that are negatively charged due to ligand ionization can be adsorbed through electrostatic interaction to obtain a patterned quantum dot film.
[0006] Based on this, we can design and prepare patterns of different sizes on the P4VP film to obtain submicron and nanometer-level quantum dot film luminescent pixels, and transfer the patterned quantum dot film to the prefabricated QLED substrate functional layer through transfer technology to prepare QLED devices.
[0007] This method of preparing nano-LEDs based on electrostatic adsorption of quantum dots enables the pixel size of QLED devices to be reduced to the nanometer level, thereby obtaining high-brightness, high-PPI display pixel units that can be applied to the next generation of displays.
[0008] The present invention specifically adopts the following technical solutions:
[0009] A method for preparing patterned QLED based on electrostatic adsorption of quantum dots, characterized in that:
[0010] First, a P4VP film was prepared, then a patterned P4VP film was prepared using the DPN method, and finally, ligand-modified quantum dots were spin-coated on the P4VP film;
[0011] Among them, the pattern on the P4VP film is formed by local protonation, and the quantum dots that are negatively charged due to ligand ionization are adsorbed by electrostatic action to obtain a patterned quantum dot film; the patterned quantum dot film is transferred to the prefabricated QLED substrate functional layer through transfer technology to prepare a QLED device.
[0012] Further, it comprises the following steps:
[0013] Step S1: preparing a hole injection layer on an ITO glass substrate electrode;
[0014] Step S2: depositing a hole transport layer on the hole injection layer;
[0015] Step S3: depositing a patterned quantum dot film on the hole transport layer;
[0016] Step S4: depositing an electron transport layer on the quantum dot film;
[0017] Step S5: evaporating a metal electrode on the electron transport layer as a top electrode to obtain a QLED device;
[0018] In step S3, a P4VP film is first prepared, and then the P4VP film is patterned by a DPN method, and then quantum dots are spin-coated on the P4VP film, and finally the quantum dot film is transferred to the functional layer of the ITO substrate.
[0019] Furthermore, the hole injection functional layer material in step S1 is at least one of polymer PEDOT:PSS, molybdenum oxide, nickel oxide and cuprous thiocyanate;
[0020] The material of the hole transport functional layer in step S2 is at least one of polymers TFB, Poly-TPD, and PVK;
[0021] The quantum dot material in the quantum dot solution in step S3 is a quantum dot modified with one of the ligands at the end of carboxylic acid, phosphonic acid and thiol;
[0022] The gold electron transport layer material in step S4 is at least one of ZnO nanoparticles, ZnO nanoparticles doped with metal cations, and TiO nanoparticles;
[0023] In step S5, the top electrode is one of Al, Ag, Cu, Au or an alloy electrode, wherein the alloy is an alloy of at least two elements among Al, Ag, Cu and Au.
[0024] Furthermore, the preparation methods of the epitaxial layers corresponding to steps S1, S2 and S4 are all spin coating.
[0025] Furthermore, in the preparation process of step S3, the solvent of the quantum dot solution is at least one of chlorobenzene and toluene.
[0026] Furthermore, the thickness of the hole injection layer in step S1 is 5-10 nm;
[0027] The thickness of the hole transport layer in step S2 is 20-60 nm;
[0028] The thickness of the metal oxide film in step S3 is 100-150 nm;
[0029] The thickness of the top electrode in step S4 is 100-150 nm.
[0030] Furthermore, the formation of the quantum dot film in step S3 is annealed and cured to obtain a light-emitting layer, the annealing temperature is 70-110° C., and the curing time is 30 minutes. The preferred annealing temperature is 80° C.
[0031] Furthermore, in step S1, the IT0 glass substrate electrode needs to be cleaned before use, and the cleaning treatment is to use acetone, isopropyl alcohol, deionized water and ultrasonic vibration substrate electrode material for 10 to 15 minutes in sequence; in step S5, after the top electrode is prepared, it is packaged to obtain a QLED device.
[0032] Compared with the prior art, the present invention and its preferred embodiment:
[0033] (1) The ligand-modified quantum dots are fixed by local protonation on the P4VP film, so that the pixel size of the QLED device can be reduced to the nanometer level, thereby obtaining a high-brightness, high-PPI display pixel unit, which can be applied to the next generation of displays.
[0034] (2) The preparation process is safe and pollution-free, does not generate by-products, and is simple and easy to operate;
[0035] (3) The P4VP film used can be further designed into a pattern. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] The present invention is further described in detail below with reference to the accompanying drawings and specific embodiments:
[0037] Figure 1 This is a schematic diagram of the finished product structure of a nano-LED prepared by transferring patterned quantum dots according to an embodiment of the present invention;
[0038] Figure 2 Schematic diagram of the process flow of depositing a patterned quantum dot film on a hole transport layer according to an embodiment of the present invention. DETAILED DESCRIPTION
[0039] In order to make the features and advantages of this patent more obvious and easy to understand, the following embodiments are specifically described in detail as follows:
[0040] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present application. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present application belongs.
[0041] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit the exemplary embodiments according to the present application. As used herein, unless the context clearly indicates otherwise, the singular form is intended to include the plural form as well.
[0042] like Figure 2 As shown, the key process of the solution of the present invention, that is, the process flow of depositing a patterned quantum dot film on the hole transport layer, specifically includes the following steps:
[0043] (1) Preparation of P4VP film: P-type silicon wafers were cleaned by immersion in a piranha solution consisting of 35% hydrogen peroxide (H2O2) and 98% sulfuric acid (H2SO4) in a volume ratio of 3:7 and stirred at 80-90°C for 30 min to remove contaminants. Subsequently, the silicon wafers were cleaned with boiling water for 60 min and then dried under N2. The cleaned wafers were then immersed in an HF aqueous solution to remove the native oxide layer on the silicon surface, rinsed thoroughly with ultrapure water, and dried with N2. A solution of P4VP in n-butanol (10 mg / mL) was spin-coated onto the silicon substrate at 2000 rpm for 60 s. The polymer-coated substrate was irradiated with a 450 W medium-pressure mercury lamp for 15 min (the irradiation time included a preheating of about 2 min to allow the UV lamp to reach its maximum intensity). The sample was soaked in n-butanol for 3 h to remove unbound polymer, and the remaining film was dried with nitrogen.
[0044] (2) P4VP film patterning: Prior to the patterning process, the AFM (atomic force microscope) tip was immersed in a phosphate buffer solution for 1 min and then dried with N2. The phosphate buffer solution was prepared by dissolving appropriate proportions of sodium dihydrogen phosphate (NaH2PO4) and sodium hydrogen phosphate (Na2HPO4) in distilled water (pH 4.0 buffer solution ratios of 13.8 and 0.036 g / L). The sample was grounded while a bias voltage was applied to the tip. The AFM probe was immersed in an acidic phosphate buffer solution with a pH of 4.0. During the patterning operation, the ink pen tip was scanned over the polymer surface at a fixed writing speed of 80 nm / s while the contact force between the pen tip and the surface was kept constant.
[0045] (3) Preparation of quantum dot film: Spin-coating quantum dots on the patterned P4VP film. The quantum dots are carboxylic acid-modified CdSe / ZnS quantum dots. During spin coating, the quantum dot concentration is 10-30 mg / ml, the spin coating speed is 1000-2500 rpm / min, the time is 20-50 s, and after spin coating, the film is annealed at 50-100°C for 30-60 min.
[0046] like Figure 1 As shown, QLED devices are prepared based on the above process flow: the structure of the nano QLED device is ITO layer, hole injection layer, hole transport layer, patterned quantum dot film, electron transport layer, and metal cathode. The hole injection layer uses PEDOT:PSS solution, and the hole transport layer uses TFB solution, which are spin-coated using a coating machine at a speed of 3000rpm and a time of 40s. The patterned quantum dot film is transferred to the hole transport layer, and then the electron transport layer is spin-coated with a ZnO nanoparticle solution doped with an organic polymer PVP at a speed of 2000rpm and a time of 40s. The metal cathode is deposited with a 100nm Ag electrode by a vacuum coating machine.
[0047] This patent is not limited to the above-mentioned best implementation mode. Anyone can derive other various forms of methods for preparing patterned QLEDs based on electrostatic adsorption of quantum dots under the inspiration of this patent. All equal changes and modifications made according to the scope of the patent application of the present invention should be covered by this patent.
Claims
1. A method for preparing patterned QLED based on electrostatic adsorption of quantum dots, characterized in that: First, a P4VP film was prepared, then a patterned P4VP film was prepared using the DPN method, and finally, ligand-modified quantum dots were spin-coated on the P4VP film; Among them, the pattern on the P4VP film is formed by local protonation, and the quantum dots that are negatively charged due to ligand ionization are adsorbed by electrostatic action to obtain a patterned quantum dot film; the patterned quantum dot film is transferred to the prefabricated QLED substrate functional layer through transfer technology to prepare a QLED device.
2. The method for preparing patterned QLED based on electrostatic adsorption of quantum dots according to claim 1, characterized in that: The following steps are involved: Step S1: preparing a hole injection layer on an ITO glass substrate electrode; Step S2: depositing a hole transport layer on the hole injection layer; Step S3: depositing a patterned quantum dot film on the hole transport layer; Step S4: depositing an electron transport layer on the quantum dot film; Step S5: evaporating a metal electrode on the electron transport layer as a top electrode to obtain a QLED device; In step S3, a P4VP film is first prepared, and then the P4VP film is patterned by a DPN method, and then quantum dots are spin-coated on the P4VP film, and finally the quantum dot film is transferred to the functional layer of the ITO substrate.
3. The method for preparing patterned QLED based on electrostatic adsorption of quantum dots according to claim 2, characterized in that: The hole injection functional layer material in step S1 is at least one of polymer PEDOT:PSS, molybdenum oxide, nickel oxide and cuprous thiocyanate; The material of the hole transport functional layer in step S2 is at least one of polymers TFB, Poly-TPD, and PVK; The quantum dot material in the quantum dot solution in step S3 is quantum dots modified with one of the ligands at the ends of carboxylic acid, phosphonic acid and thiol; The electron transport layer material in step S4 is at least one of ZnO nanoparticles, ZnO nanoparticles doped with metal cations, and TiO nanoparticles; In step S5, the top electrode is one of Al, Ag, Cu, Au or an alloy electrode, wherein the alloy is an alloy of at least two elements among Al, Ag, Cu and Au.
4. The method for preparing patterned QLED based on electrostatic adsorption of quantum dots according to claim 2, characterized in that: The preparation methods of the epitaxial layers corresponding to steps S1, S2 and S4 are all spin coating.
5. The method for preparing patterned QLED based on electrostatic adsorption of quantum dots according to claim 2, characterized in that: During the preparation process of step S3, the solvent of the quantum dot solution is at least one of chlorobenzene and toluene.
6. The method for preparing patterned QLED based on electrostatic adsorption of quantum dots according to claim 2, characterized in that: The thickness of the hole injection layer in step S1 is 5-10 nm; The thickness of the hole transport layer in step S2 is 20-60 nm; The thickness of the quantum dot film in step S3 is 100-150 nm; The thickness of the top electrode in step S5 is 100-150 nm.
7. The method for preparing patterned QLED based on electrostatic adsorption of quantum dots according to claim 2, characterized in that: The quantum dot film formed in step S3 is annealed and cured to obtain a light-emitting layer, the annealing temperature is 70~110°C, and the curing time is 30min.
8. The method for preparing patterned QLED based on electrostatic adsorption of quantum dots according to claim 2, characterized in that: In step S1, the IT0 glass substrate electrode needs to be cleaned before use, and the cleaning treatment is to use acetone, isopropyl alcohol, deionized water and ultrasonic vibration substrate electrode material for 10 to 15 minutes in sequence; in step S5, after the top electrode is prepared, it is packaged to obtain a QLED device.
Citation Information
Patent Citations
Method of preparing carbon thin film, and electronic device and electrochemical devices each including the carbon thin film
CN102800774A
QLED device and preparation method thereof
CN109244252A
Quantum dot film, preparation method thereof, QLED (Quantum dot Light-Emitting Diode) device and preparation method thereof
CN109935709A
Quantum dot light emitting diode and preparation method thereof
CN114447237A
Organic memory device and method of manufacture
US20090146202A1