Curable composition and method for producing the same

By using a curable composition containing elastomers, epoxy resins and a variety of latent curing agents in the motor vehicle body process, the problems of low-temperature curing and property maintenance are solved, and high efficiency in the range of 130°C to 165°C is achieved. Cure and maintain properties.

CN115386321BActive Publication Date: 2024-10-25SUNSTAR GIKEN KK
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210564498.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-11-30
Filing Date
2022-05-23
Publication Date
2024-10-25
Estimated Expiration
2042-05-23

AI Technical Summary

Technical Problem

The existing technology is difficult to achieve curing of adhesives for automobile body processes at low temperatures, and it is difficult to maintain properties such as hardness, elongation, shear strength, peel strength and impact absorption.

Method used

A curable composition containing elastomer, epoxy resin and a variety of latent curing agents is used. The latent curing agent is pre-pulverized or dispersed, combined with the thermoplastic resin and cross-linking agent, and stirred under reduced pressure to improve the curing of the adhesive. performance.

Benefits of technology

The adhesive is cured at lower temperatures (such as 130°C to 165°C), maintaining hardness, elongation, shear strength and impact absorption, and has good storage stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003657304300000041
    Figure BDA0003657304300000041
  • Figure BDA0003657304300000131
    Figure BDA0003657304300000131
  • Figure BDA0003657304300000321
    Figure BDA0003657304300000321
Patent Text Reader

Abstract

The present invention provides a curable composition and a method for producing the curable composition, wherein the curable composition comprises an elastomer (A), an epoxy resin (B), a latent curing agent (C), a filler (D), a thermoplastic resin (E), a crosslinking agent (F) for the elastomer, and a plasticizer (G), wherein the latent curing agent (C) comprises a combination of two or more latent curing agents, and 0.1 to 10 parts by mass of the epoxy resin (B) are contained in every 100 parts by mass of the curable composition. The curable composition can be applied to adhesives for automobiles, more specifically, to adhesives for vehicle body processes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a curable composition, and more specifically, to a curable composition comprising an elastomer, an epoxy resin and a latent curing agent. The curable composition can be applied to, for example, automotive adhesives, more specifically, adhesives for vehicle body processes (e.g., structural adhesives, mastic adhesives, etc.). Background Art

[0002] The body of a motor vehicle is manufactured by a body process including stamping, welding and assembling steel plates to form a white body. The white body is painted by a coating process including electrodeposition coating, electrodeposition baking, painting and baking varnish. The adhesive for the body process is an adhesive used when the white body is manufactured by the body process. The adhesive for the body process is sometimes applied by people, but in recent years it is usually sent from a pail or drum and automatically applied without human intervention. The adhesive is usually required to have oil surface adhesion and rust resistance, and further required to have viscosity and drip resistance suitable for coating. The adhesive is a single-component thermosetting type and is cured in an electrodeposition baking furnace during the electrodeposition baking of the coating process of the next process.

[0003] For example, Patent Document 1 discloses a curable composition, which is prepared by mixing a diluent and a tackifier (which is a combination of an epoxy resin and a latent curing agent) in a composition containing synthetic rubber, a plasticizer, a filler, and a core-shell acrylic resin (see [Claims 1] to [Claim 3],

[0043] [Table 1]). According to Patent Document 1, the curable composition does not require vinyl chloride resin, has little harm to the environment, and exhibits excellent adhesion to alloyed aluminum materials, thereby expanding the application range of alloyed aluminum materials and achieving a significant effect of further reducing the weight of the vehicle body (see

[0008] ).

[0004] Patent Document 2 discloses an adhesive for bonding vehicle body panels, which is composed of synthetic rubber, polyvinyl chloride, a plasticizer, and a filler, and contains a titanium oxide pigment at a ratio of 0.2 wt% to 10 wt% (see claims, Table 1 on page 4). According to Patent Document 2, even when subjected to near-infrared heating at a temperature of 140°C to 270°C for less than 3 minutes, there is no problem of blistering or carbonization (see lines 11 to 16 on the right column on page 2).

[0005] Patent document 3 discloses that the adhesion of a curable resin composition comprising a urethane-rubber modified epoxy resin and a latent curing agent at low temperatures to room temperatures is improved. In addition, in particular, the adhesion of a curable composition comprising a urethane rubber modified epoxy resin, a blocked urethane and a latent curing agent at low temperatures to room temperatures and the tensile elongation at low temperatures are both excellent (see

[0065] [Table 1] to

[0067] ).

[0006] Prior art literature

[0007] Patent Literature

[0008] Patent Document 1: Japanese Patent Application Publication No. 2005-272712

[0009] Patent Document 2: Japanese Patent Application Laid-Open No. 2-84477

[0010] Patent Document 3: Japanese Patent Application Publication No. 2007-246648 Summary of the invention

[0011] Problems to be solved by the invention

[0012] In recent years, the requirements for protecting the earth's environment, improving the working environment, and reducing energy consumption have become increasingly stringent, and the electrodeposition baking temperature of the coating process has also been required to be further reduced. Therefore, the adhesive cured in the electrodeposition baking furnace of the coating process is also required to be cured at a relatively low temperature (e.g., 130°C to 165°C), but other properties such as hardness, elongation, shear strength, peel strength, impact absorption, and storage stability are also required to be maintained.

[0013] Specifically, regarding Patent Document 1, a test piece is cured by being held at 170° C. for 20 minutes (see

[0038] to

[0039] ).

[0014] Regarding Patent Document 2, no specific curing temperature is disclosed.

[0015] Regarding Patent Document 3, specifically, the test piece is cured by being held at 180° C. for 30 minutes (see

[0063] to

[0064] ).

[0016] Patent Documents 1 to 3 all disclose curable compositions that cure at 170° C. or higher, but it is difficult to meet the recent demand for lower temperatures.

[0017] Technical means to solve problems

[0018] The present inventors have repeatedly conducted intensive studies and, as a result, have found that a curable composition comprising an elastomer (A), an epoxy resin (B) and a latent curing agent (C) (the latent curing agent (C) comprises a combination of two or more latent curing agents) is suitable for use as an adhesive for automobiles, more specifically, for use as an adhesive for vehicle body processes, thereby completing the present invention.

[0019] This specification includes the following embodiments.

[0020] 1. A curable composition comprising an elastomer (A), an epoxy resin (B) and a latent curing agent (C), wherein the latent curing agent (C) comprises a combination of two or more latent curing agents.

[0021] 2. The curable composition according to item 1 above, wherein the elastomer (A) comprises at least one selected from styrene / butadiene copolymers, nitrile / butadiene copolymers, butadiene polymers, isoprene polymers, ethylene / propylene / diene rubbers, acrylic acid, and urethane.

[0022] 3. The curable composition according to item 1 above, wherein at least a part of the elastomer (A) contains a compound that has reacted in advance with the epoxy resin (B).

[0023] 4. The curable composition according to any one of 1 to 3 above, further comprising a thermoplastic resin (E).

[0024] 5. The curable composition according to 4 above, wherein the thermoplastic resin (E) comprises at least one selected from acrylic resins, PVC resins, vinyl acetate resins, and copolymers thereof.

[0025] 6. The curable composition according to any one of 1 to 5 above, comprising a crosslinking agent (F) for an elastomer.

[0026] 7. The curable composition according to 6 above, wherein the crosslinking agent (F) for the elastomer contains at least one selected from sulfur and a peroxide.

[0027] 8. The curable composition according to any one of 1 to 7 above, wherein the melting points of at least two latent curing (accelerating) agents contained in the latent curing agent (C) differ by 10° C. or more and 80° C. or less.

[0028] 9. The curable composition according to any one of 1 to 8 above, wherein at least one of the latent curing agents (C) has a C10 to C23 aliphatic alkane structure.

[0029] 10. The curable composition according to any one of 1 to 9 above, wherein at least one of the latent curing agents (C) comprises an aliphatic dihydrazide.

[0030] 11. The curable composition according to any one of 1 to 10 above, wherein at least one of the latent curing agents (C) comprises a latent curing (accelerating) agent satisfying formula (1).

[0031] [Chemical formula 1]

[0032]

[0033] [In formula (1), n=10 to 23]

[0034] 12. The curable composition according to any one of 1 to 11 above, wherein at least one of the latent curing agents (C) comprises dodecanedioic acid dihydrazide.

[0035] 13. The curable composition according to any one of 1 to 12 above, further comprising a filler (D).

[0036] 14. The curable composition according to any one of 1 to 13 above, further comprising a plasticizer (G).

[0037] 15. The curable composition according to any one of 1 to 14 above, further comprising a filler (D), a thermoplastic resin (E), an elastomer crosslinking agent (F), and a plasticizer (G).

[0038] 16. A method for producing a curable composition, the curable composition comprising an elastomer (A), an epoxy resin (B) and a latent curing agent (C),

[0039] The manufacturing method comprises mixing an elastomer (A), an epoxy resin (B) and a latent curing agent (C), and

[0040] Satisfies at least any one of the following (i) to (iii).

[0041] (i) The method comprises: pulverizing at least a portion of the latent curing agent (C) in advance to an average particle size of 25 μm or less, and / or dispersing at least a portion of the latent curing agent (C) in advance in the epoxy resin (B).

[0042] (ii) the curable composition further comprises a plasticizer (G),

[0043] The steps include:

[0044] Step 1, making at least a portion of the elastomer (A) solid, mixing and dissolving the portion of the elastomer (A) that is solid with at least a portion of the plasticizer (G) or the epoxy resin (B) that is a liquid component, thereby obtaining a mixture 1 containing the elastomer (A);

[0045] Step 2, mixing at least a portion of the latent curing (accelerating) agent (C) with at least a portion of the plasticizer (G) to obtain a mixture 2 containing the latent curing (accelerating) agent (C); and

[0046] In step 3, the mixture 1 obtained in step 1, the mixture 2 obtained in step 2, and other components of the curable composition other than the mixture 1 and the mixture 2 are mixed.

[0047] (iii) comprising: mixing a part or all of the components of the curable composition to obtain an intermediate mixture of the curable composition, and decompressing and stirring the intermediate mixture to obtain the curable composition;

[0048] Here, the decompression and stirring include: decompression and stirring for more than 20 minutes at a temperature between 3 mmHg and 150 mmHg; and no stirring when the pressure is reduced to less than 3 mmHg or decompression and stirring for less than 10 minutes when the pressure is less than 3 mmHg.

[0049] 17. The production method according to 16 above, wherein, in the case of (ii), the method comprises: in the mixing of the elastomer (A) and the plasticizer (G), adding the plasticizer (G) in batches to the elastomer (A) passing through a mixing roller.

[0050] 18. The production method according to 16 or 17 above, wherein the stirring includes using a twin-screw mixer, a planetary mixer or a sigma mixer.

[0051] 19. The production method according to any one of 16 to 18 above, wherein in the case of (iii), the lower limit of the degree of reduced pressure is 1 mmHg or more.

[0052] 20. The production method according to any one of 16 to 19 above, wherein, in the case of (iii), the latent curing agent (C) further comprises a combination of two or more latent curing agents.

[0053] 21. The production method according to any one of 16 to 20 above, which satisfies (i) and (iii) simultaneously.

[0054] 22. The method for producing a curable composition according to any one of 16 to 21 above, wherein the curable composition is the curable composition according to any one of 1 to 15 above.

[0055] Effects of the Invention

[0056] The curable composition of an embodiment of the present invention comprises an elastomer (A), an epoxy resin (B) and a latent curing agent (C), wherein the latent curing agent (C) comprises a combination of two or more latent curing agents, and the curable composition can be applied to adhesives for automobiles, more specifically, to adhesives for vehicle body processes. DETAILED DESCRIPTION

[0057] In one aspect of the present invention, a novel curable composition is provided, which comprises an elastomer (A), an epoxy resin (B) and a latent curing agent (C), wherein the latent curing agent (C) comprises a combination of two or more latent curing agents.

[0058] The curable composition according to the embodiment of the present invention includes an elastomer (A), an epoxy resin (B), and a latent curing agent (C).

[0059] In this specification, the elastomer (A) refers to a polymer having rubber elasticity, which is generally called an elastomer, and includes thermosetting elastomers and thermoplastic elastomers. There is no particular limitation as long as the target curable composition of the present invention can be obtained.

[0060] Examples of the elastomer (A) include styrene / butadiene copolymers, nitrile / butadiene copolymers, butadiene polymers, isoprene polymers, ethylene / propylene / diene polymers, acrylic polymers, and polymers containing urethane bonds.

[0061] As the elastomer (A), it is preferred to contain at least one selected from styrene / butadiene copolymers (styrene / butadiene rubber), nitrile / butadiene copolymers, butadiene polymers (butadiene rubber), isoprene polymers, ethylene / propylene / diene polymers, acrylic polymers, and polymers containing urethane bonds, and more preferably contains at least one selected from styrene / butadiene copolymers (styrene / butadiene rubber) and butadiene polymers (butadiene rubber).

[0062] In an embodiment of the present invention, at least a portion of the elastomer (A) may contain a compound that has reacted with the epoxy resin (B) in advance. In this case, the affinity (or compatibility) between the elastomer and the epoxy resin can be further improved, and it is possible to further improve the physical properties of the curable composition as a whole.

[0063] As the elastomer (A), a commercially available item can be used.

[0064] Examples include SBR1009 (trade name) manufactured by ASP Japan, SB-1009 (trade name) manufactured by Nitriflex, SBR 1009 (trade name) manufactured by Lion Elastomers, Nipol DN214 (trade name) manufactured by Nippon Zeon, BR 1220 (trade name) manufactured by Nippon Zeon, and N230S (trade name) manufactured by JSR.

[0065] The elastomer (A) may be used alone or in combination.

[0066] The curable composition according to the embodiment of the present invention may contain, for example, 2 to 20 parts by mass of the elastomer (A) per 100 parts by mass of the curable composition, preferably 3 to 15 parts by mass of the elastomer (A), more preferably 4 to 10 parts by mass of the elastomer (A), and even more preferably 5 to 9 parts by mass of the elastomer (A).

[0067] In the curable composition of the embodiment of the present invention, when 2 to 20 parts by mass of the elastomer (A) are contained per 100 parts by mass of the curable composition, more appropriate curability can be obtained, better workability can be obtained based on a more appropriate viscosity, and the hardness of the cured product can be more appropriately adjusted.

[0068] The curable composition according to the embodiment of the present invention may further contain a thermoplastic resin (E).

[0069] In this specification, the thermoplastic resin (E) refers to a resin as follows: a polymer that is solid and powdery or granular at room temperature, and exists in a dispersed state, i.e., a sol state, in liquid components such as epoxy resin and plasticizer (when a plasticizer is used), and is heated (e.g., above 80°C) to a state where the thermoplastic resin is swollen in the epoxy resin and plasticizer as liquid components, and solidifies when cooled. There are no particular restrictions as long as the above-mentioned elastomer (A) is not included and the target curable composition of the present invention can be obtained. In the case where the curable composition of an embodiment of the present invention also includes a thermoplastic resin (E), the curability can be further improved, and the physical properties can be more easily adjusted by changing the amount of the thermoplastic resin (E) added.

[0070] Examples of the thermoplastic resin (E) include acrylic resins, vinyl chloride (PVC) resins, vinyl acetate resins, and copolymers thereof.

[0071] The thermoplastic resin (E) is preferably a thermoplastic resin having a polar group and a non-polar group and having a polarizable structure, and is preferably at least one selected from acrylic resins, polyvinyl chloride (PVC) resins, vinyl acetate resins, and copolymers thereof. Furthermore, combinations of acrylic resins, polyvinyl chloride (PVC) resins, vinyl acetate resins, and copolymers thereof are exemplified, and combinations of acrylic resins and polyvinyl chloride resins, combinations of acrylic resins and vinyl acetate resins, and combinations of polyvinyl chloride resins and vinyl acetate resins are preferred.

[0072] Furthermore, the thermoplastic resin (E) may have a core-shell structure, and preferably contains a resin that is dispersed at room temperature and is soluble when heated (for example, an acrylic resin).

[0073] The thermoplastic resin (E) is preferably in a granular form. The average particle size of the thermoplastic resin (E) is preferably 0.01 μm to 100 μm, more preferably 0.05 μm to 10 μm, further preferably 0.1 μm to 5 μm, and further more preferably 0.2 μm to 2 μm.

[0074] When the thermoplastic resin (E) is in a granular form, it is more easily plasticized when heated, and can be mixed more uniformly with the elastomer (A) and the epoxy resin (B).

[0075] The average particle size of the thermoplastic resin can be measured by a laser particle size distribution measurement method using SALD-200VER (trade name) manufactured by Shimadzu Corporation.

[0076] As the thermoplastic resin (E), a commercially available item can be used.

[0077] Examples include: LP-3106 (trade name) manufactured by Mitsubishi Rayon Co., Ltd., LP-3102 (trade name) manufactured by Mitsubishi Rayon Co., Ltd., LP-3108 (trade name) manufactured by Mitsubishi Rayon Co., Ltd., LP-3109 (trade name) manufactured by Mitsubishi Rayon Co., Ltd., etc.; ZEFIAC F351 (trade name) manufactured by Aica Kogyo Co., Ltd., ZEFIAC F351 (trade name) manufactured by Aica Kogyo Co., Ltd.; PSH-10 (trade name) manufactured by Kaneka Corporation, PCH-72 (trade name) manufactured by Kaneka Corporation, PSH-24 (trade name) manufactured by Kaneka Corporation, PBM-6 (trade name) manufactured by Kaneka Corporation, etc.

[0078] The thermoplastic resin (E) can be used alone or in combination.

[0079] The curable composition according to the embodiment of the present invention may contain, for example, 0.2 to 20 parts by mass of a thermoplastic resin (E) per 100 parts by mass of the curable composition, preferably 0.4 to 15 parts by mass of a thermoplastic resin (E), more preferably 1 to 10 parts by mass of a thermoplastic resin (E), and even more preferably 2 to 9 parts by mass of a thermoplastic resin (E).

[0080] When the curable composition of the embodiment of the present invention contains 0.2 to 20 parts by mass of the thermoplastic resin (E) per 100 parts by mass of the curable composition, more appropriate physical properties can be obtained and the balance between curability and storage stability can be better achieved.

[0081] The curable composition according to the embodiment of the present invention may contain a cross-linking agent (F) for the elastomer.

[0082] In this specification, the crosslinking agent (F) for elastomer refers to a substance that can crosslink the elastomer (A) to adjust the rubber properties of the elastomer (A) (for example, making it harder), and there is no particular limitation as long as the target curable composition of the present invention can be obtained.

[0083] When the curable composition according to the embodiment of the present invention contains the crosslinking agent (F) for the elastomer, the following advantageous effects can be exhibited: the curability can be improved, the hardness can be improved, and the hardness can be adjusted by adjusting the amount.

[0084] Examples of the cross-linking agent (F) for the elastomer include sulfur, peroxides, and quinone compounds.

[0085] The crosslinking agent (F) for the elastomer preferably contains at least one selected from sulfur, peroxides, and quinone compounds, and more preferably contains at least one selected from peroxides and quinone compounds.

[0086] As the cross-linking agent (F) for the elastomer, a commercially available product can be used.

[0087] Examples include: peroxides such as Perhexa V (trade name) (4,4-di(tert-butylperoxy)valerate) and Perhexa C (1,1-di(tert-butylperoxy)cyclohexane) (trade name) manufactured by NOF Chemical Co., Ltd.; and quinone compounds such as (p-quinone dioxime) Vulnoc GM-P (trade name) and (O,O'-dibenzoyl-p-quinone dioxime) Vulnoc DGM (trade name) manufactured by Ouchi Shinko Chemical Co., Ltd.

[0088] The crosslinking agent (F) for the elastomer may be used alone or in combination.

[0089] The curable composition of the embodiment of the present invention may contain, for example, 0.03 to 5 parts by mass of a crosslinking agent (F) for an elastomer per 100 parts by mass of the curable composition, preferably 0.08 to 4 parts by mass of a crosslinking agent (F) for an elastomer, and more preferably 0.1 to 3 parts by mass of a crosslinking agent (F) for an elastomer.

[0090] When the curable composition of the embodiment of the present invention contains 0.3 to 5 parts by mass of the elastomer crosslinking agent (F) per 100 parts by mass of the curable composition, a cured product having more appropriate physical properties (eg, hardness) can be obtained more easily.

[0091] The curable composition according to the embodiment of the present invention contains an epoxy resin (B).

[0092] In this specification, "epoxy resin" refers to a compound containing two or more epoxy groups in the molecule, which is generally referred to as epoxy resin, and there is no particular limitation as long as the target curable composition of the present invention can be obtained. Examples of epoxy resins include glycidyl ether epoxy resins, glycidyl amine epoxy resins, glycidyl ester epoxy resins, and the like.

[0093] Examples of the epoxy resin contained in the curable composition according to the embodiment of the present invention include:

[0094] Bisphenol-type epoxy resins such as bisphenol A, bisphenol F, brominated bisphenol A, diglycidyl ether of bisphenol AD, and diglycidyl ether of alkylene oxide adduct of bisphenol A, and alicyclic epoxy resins obtained by hydrogenating aromatic rings contained in these epoxy resins;

[0095] Diglycidyl ether type epoxy resins with one aromatic ring, such as catechol, resorcinol, and hydroquinone;

[0096] Diglycidyl ester type epoxy resins based on dimer acid, phthalic acid, and hydrogenated phthalic acid;

[0097] A multifunctional novolac-type epoxy resin obtained by multi-nuclearizing bisphenol A and bisphenol F;

[0098] An acrylonitrile-butadiene copolymer-modified epoxy resin produced by mixing a carboxyl-terminated butadiene-acrylonitrile copolymer rubber with a bisphenol-type epoxy resin in a mass ratio of 1:5 to 4:1, preferably 1:3 to 3:2, and reacting them at a temperature of 80° C. to 180° C.;

[0099] Alkylene oxide-modified glycidyl ether type epoxy resins obtained by reacting polyhydroxy compounds [e.g., polyalkylene glycols (polyethylene glycol, polypropylene glycol, polyethylene propylene glycol, etc.); aliphatic polyhydroxy compounds such as hexanediol, butanediol, propylene glycol, ethylene glycol, neopentyl glycol, triethylene glycol, pentanediol, hexanetriol, glycerol, etc.] with epihalohydrin;

[0100] Urethane-modified epoxy resins obtained by reacting a polyurethane prepolymer obtained by adding polyisocyanate to the end of a polyalkylene glycol with a hydroxyl group of an epoxy resin (mixing ratio of 10:90 to 50:50), acrylic-modified epoxy resins obtained by reacting carboxyl groups on the surface of acrylic rubber particles with an epoxy resin (mixing ratio of 10:90 to 50:50), etc.

[0101] As the epoxy resin, commercial products can be used. Examples of these commercial products include "jER (registered trademark) 828" manufactured by Mitsubishi Chemical Corporation, "Adeka Resin EPR-4023", "Adeka Glycirol ED-506", "Adeka Resin EPU-73B", "Adeka Resin EPU-78-11" manufactured by ADEKA Corporation, "Kane Ace MX-257" manufactured by Kaneka Corporation, and "HBE-100" manufactured by Shin Nippon Chemical Co., Ltd.

[0102] The epoxy resins may be used alone or in combination.

[0103] The curable composition according to the embodiment of the present invention may contain, for example, 0.1 parts by mass or more of the epoxy resin (B), preferably 0.2 parts by mass or more of the epoxy resin (B), preferably 0.3 parts by mass or more of the epoxy resin (B), more preferably 0.5 parts by mass or more of the epoxy resin (B), and may contain 1.0 parts by mass or more of the epoxy resin (B), or may contain 1.5 parts by mass or more of the epoxy resin (B), per 100 parts by mass of the curable composition.

[0104] The curable composition according to the embodiment of the present invention may contain, for example, 50 parts by mass or less of the epoxy resin (B), 10 parts by mass or less of the epoxy resin (B), 8 parts by mass or less of the epoxy resin (B), more preferably 5 parts by mass or less of the epoxy resin (B), and more preferably 3 parts by mass or less of the epoxy resin (B), per 100 parts by mass of the curable composition.

[0105] For the curable composition of the embodiment of the present invention, for example, 0.1 to 50 parts by mass of epoxy resin (B) may be included per 100 parts by mass of the curable composition. If the adhesion to the aluminum plate during relatively low temperature curing (150° C.) is taken into account, 0.2 to 10 parts by mass of epoxy resin (B) is preferably included, more preferably 0.3 to 5 parts by mass of epoxy resin (B), and more preferably 0.5 to 3 parts by mass of epoxy resin (B). If impact strength is taken into account, 10 to 45 parts by mass of epoxy resin (B) is preferably included, more preferably 20 to 40 parts by mass of epoxy resin (B), and more preferably 25 to 35 parts by mass of epoxy resin (B) is preferably included.

[0106] When the curable composition according to the embodiment of the present invention contains 0.1 to 50 parts by mass of the epoxy resin (B) per 100 parts by mass of the curable composition, the adhesiveness to a substrate (eg, an aluminum plate) is more excellent.

[0107] When the curable composition according to the embodiment of the present invention contains 0.2 to 10 parts by mass of the epoxy resin (B) per 100 parts by mass of the curable composition, the adhesiveness to the aluminum plate during low temperature curing (150° C.) is more excellent.

[0108] The curable composition according to the embodiment of the present invention includes a latent curing agent (C), and the latent curing agent (C) includes a combination of two or more latent curing agents.

[0109] In this specification, "latent curing agent" refers to a compound as follows: although it is a curing agent for epoxy resin, it basically does not act as a curing agent at room temperature, but acts as a curing agent by heating (to, for example, 165°C, preferably 150°C). There are no particular restrictions as long as the target curable composition of the present invention can be obtained.

[0110] Specific examples of latent curing agents include: dicyandiamide, adipic acid dihydrazide, sebacic acid dihydrazide, isophthalic acid dihydrazide, dodecanedioic acid dihydrazide, 1,3-bis(hydrazinocarbonylethyl)-5-isopropylhydantoin, eicosanedioic acid dihydrazide, hydroquinone diglycolic acid dihydrazide, resorcinol diglycolic acid dihydrazide, 4,4'-ethylenebisphenol diglycolic acid dihydrazide and other dihydrazide compounds; 4,4'-diaminodiphenyl sulfone; imidazole compounds such as imidazole, 2-n-heptadecylimidazole, and 2-undecylimidazole; melamine; 2,4 ... Triazine compounds such as amino-6-(2'-methylimidazolyl(1'))-ethyl-o-triazine; benzoguanamine; N,N-dimethyl-N'-(3,4-dichlorophenyl)urea and other N,N-dialkylureas, dialkylurea compounds such as N,N'-dialkylurea compounds; N,N'-dialkylthiourea compounds; polyamines such as diaminodiphenylmethane, diaminobiphenyl, diaminobenzene, phenylenediamine, toluenediamine, dodecanediamine, decanediamine, octanediamine, tetradecanediamine, hexadecanediamine, polyoxypropylenediamine, and hydrazide polyamines; guanidine derivatives such as cyanoguanidine.

[0111] As the latent curing agent, commercially available products can be used, such as CG-NA (trade name) manufactured by Air Products, EH-4030s (trade name) manufactured by ADEKA Corporation, ADH (trade name) manufactured by Otsuka Chemical Co., Ltd., EH3731s (trade name) manufactured by ADEKA Corporation, Dyhard UR200 (trade name) manufactured by AlzChem, DDH (trade name) manufactured by Otsuka Chemical Co., Ltd., etc.

[0112] In an embodiment of the present invention, the melting points of at least two latent curing (accelerating) agents contained in the latent curing agent (C) preferably differ by 10°C to 80°C, more preferably by 13°C to 50°C, and further preferably by 15°C to 25°C.

[0113] When the melting points of at least two latent curing (accelerating) agents contained in the latent curing agent (C) differ by 10°C to 80°C, the balance among curability, physical properties (eg, adhesive strength, tensile strength, elongation, etc.) and storage stability is more excellent.

[0114] In an embodiment of the present invention, at least one compound contained in the latent curing agent (C) preferably includes at least one compound selected from dicyandiamide, dihydrazide compounds, imidazole compounds, triazine compounds, and dialkylurea compounds.

[0115] In the case where at least one compound contained in the latent curing agent (C) comprises at least one compound selected from dicyandiamide, dihydrazide compounds, imidazole compounds, triazine compounds, and dialkylurea compounds, the storage stability and the adhesiveness are more excellent.

[0116] In an embodiment of the present invention, at least one of the latent curing agents (C) preferably has a C10-C23 aliphatic alkane structure (or aliphatic alkyl), more preferably has a C10-C18 aliphatic alkane structure, and further preferably has a C12-C17 aliphatic alkane structure.

[0117] When at least one of the latent curing agents (C) has a C10-C23 aliphatic alkane structure, low-temperature adhesion is further excellent.

[0118] In the embodiment of the present invention, at least one of the latent curing agents (C) preferably has a C10-C23 aliphatic alkylene structure (or aliphatic alkylene group), and more preferably has a C10-C18 aliphatic alkylene structure.

[0119] In an embodiment of the present invention, at least one of the latent curing agents (C) preferably comprises a dihydrazide compound, preferably comprises an aliphatic dihydrazide compound, and more preferably comprises an aliphatic dicarboxylic acid dihydrazide. The aliphatic dicarboxylic acid dihydrazide preferably comprises an aliphatic alkylene structure having 10 to 23 carbon atoms, more preferably comprises an aliphatic alkylene structure having 10 to 18 carbon atoms, and even more preferably comprises dodecanedioic acid dihydrazide.

[0120] In the case where at least one of the latent curing agents (C) contains a dihydrazide compound, low-temperature adhesion is more excellent.

[0121] In the embodiment of the present invention, at least one of the latent curing agents (C) preferably comprises a latent curing (accelerating) agent represented by formula (1).

[0122] [Chemical formula 2]

[0123]

[0124] [In formula (1), n=10 to 23]

[0125] When at least one of the latent curing agents (C) comprises a latent curing (accelerating) agent represented by formula (1), a beneficial effect of further excellent low-temperature curing property can be obtained.

[0126] The curable composition of the embodiment of the present invention may contain, for example, 0.05 to 2.5 parts by mass of a latent curing agent (C) per 100 parts by mass of the curable composition, preferably 0.07 to 2.0 parts by mass of a latent curing agent (C), more preferably 0.1 to 1.6 parts by mass of a latent curing agent (C), and more preferably 0.2 to 1.0 parts by mass of a latent curing agent (C).

[0127] When the curable composition according to the embodiment of the present invention contains 0.05 to 2.5 parts by mass of the latent curing agent (C) per 100 parts by mass of the curable composition, the balance between curability and storage stability is further improved.

[0128] The curable composition according to the embodiment of the present invention may further contain a filler (D).

[0129] In this specification, the filler is a compound that can increase the volume of the curable composition of the embodiment of the present invention and impart a certain degree of strength to the film formed by the curable composition. Depending on the situation, it can help to adjust the viscosity or reduce the weight. As long as the target curable composition of the present invention can be obtained, there is no particular limitation.

[0130] Examples of fillers include calcium carbonate (heavy calcium carbonate, precipitated calcium carbonate, surface-treated calcium carbonate, etc.), magnesium carbonate, carbonates and sulfates of alkaline earth metals such as barium sulfate, mica, graphite, talc, clay, glass flakes (glass beads), vermiculite, kaolin, wollastonite (acicular calcium metasilicate), silicon dioxide, diatomaceous earth, gypsum, cement, converter slag, white sand, zeolite, cellulose powder, powdered rubber, burnt vermiculite (Zonolite), potassium titanate, bentonite, aluminum nitride, silicon nitride, zinc oxide, titanium oxide, aluminum oxide, zinc oxide , iron oxide, magnesium oxide, titanium oxide, magnesium hydroxide, aluminum hydroxide, calcium silicate, and calcium carbonate whiskers (needle-shaped calcium carbonate), ceramic short fibers or their whiskers, rock wool short fibers, glass fiber short fibers, potassium titanate short fibers, calcium silicate short fibers, aluminum silicate, carbon fiber short fibers, aramid fiber short fibers, mineral fibers such as sepiolite, various whiskers and other fibrous filling materials, glass balls, silica balls, resin balls, carbon inorganic hollow balls and other hollow filling materials, organic hollow filling materials such as plastic balls composed of organic synthetic resins such as vinylidene chloride and acrylonitrile, aluminum fillers and other metal fillers, etc.

[0131] The curable composition according to the embodiment of the present invention may contain, for example, 20 to 80 parts by mass of the filler (D) per 100 parts by mass of the curable composition, preferably 25 to 70 parts by mass of the filler (D), more preferably 30 to 60 parts by mass of the filler (D), and even more preferably 35 to 55 parts by mass of the filler (D).

[0132] When the curable composition according to the embodiment of the present invention contains 20 to 80 parts by mass of the filler (D) per 100 parts by mass of the curable composition, the workability can be further improved.

[0133] The curable composition according to the embodiment of the present invention may further contain a plasticizer (G).

[0134] In the present specification, the plasticizer (G) can increase plasticity and make the composition soft, and is not particularly limited as long as the target curable composition of the present invention can be obtained.

[0135] Examples of the plasticizer include alkyl benzyl phthalates such as butyl benzyl phthalate (BBP), octyl benzyl phthalate (OBP), and isononyl benzyl phthalate; di-methylcyclohexyl phthalate (DMCHP); phthalic acid polyester; benzoic acid esters; diisononyl phthalate (DINP), dioctyl phthalate (DOP), dimethyl phthalate (DMP), diethyl phthalate (DEP), dibutyl phthalate (DBP), diheptyl phthalate (DHEP), and dioctyl phthalate (DOP). Phthalate: DHP), nonyl phthalate (DNP), didecyl phthalate (DDP), di-n-octyl phthalate (DnOP), diisodecyl phthalate (DIDP), and di-2-ethylhexyl phthalate (DEHP); cyclohexanedicarboxylic acid dialkyl esters such as diisononyl cyclohexanedicarboxylate; trimellitic acid triesters such as trioctyl trimellitate (TOTM), trioctyl trimellitate (TOTN), triisooctyl trimellitate, and triisodecyl trimellitate.

[0136] The plasticizer preferably comprises a phthalic acid diester, and the phthalic acid diester more preferably comprises an alkylbenzyl phthalate and / or a dialkyl phthalate.

[0137] When the plasticizer contains a phthalic acid diester, it is preferred because it has moderate curability and excellent storage stability. When the plasticizer contains an alkylbenzyl phthalate and / or a dialkyl phthalate, it is more preferred because curability can be improved.

[0138] The curable composition of the embodiment of the present invention may contain, for example, 5 to 60 parts by mass of a plasticizer, preferably 10 to 55 parts by mass of a plasticizer, more preferably 15 to 50 parts by mass of a plasticizer, and even more preferably 20 to 40 parts by mass of a plasticizer, based on 100 parts by mass of the entire curable composition.

[0139] The curable composition according to the embodiment of the present invention may contain other components as appropriate. Examples of other components include a common curing agent (excluding the above-mentioned latent curing agent), a diluent, a surfactant, and other additives.

[0140] In the embodiment of the present invention, the curing agent is a compound that has no curing effect at room temperature but exhibits a curing effect when reaching a certain temperature. There is no particular limitation as long as the above-mentioned latent curing agent is not included and the target curable composition of the present invention can be obtained.

[0141] In the embodiment of the present invention, the diluent is not particularly limited as long as it can impart fluidity to the curable composition of the embodiment of the present invention and can obtain the target curable composition of the present invention.

[0142] Examples of the diluent include hydrocarbon solvents such as paraffin solvents, isoparaffin solvents, cycloparaffin solvents, and aromatic solvents.

[0143] In the embodiment of the present invention, other additives include, for example, hygroscopic agents (calcium oxide, molecular sieves, etc.), thixotropy imparting agents (organic bentonite, fumed silica, aluminum stearate, metal soaps, castor oil derivatives, etc.), stabilizers [2,6-di-tert-butyl-4-methylphenol, 2,2-methylene-bis(4-methyl-6-tert-butylphenol), nickel dibutyldithiocarbamate, etc.], curing accelerators (dibutyltin dilaurate, lead octanoate, bismuth octanoate, etc.), coupling agents such as silane or titanium, foaming agents, etc. As long as the target curable composition of the present invention can be obtained, other additives can be appropriately used without particular limitation.

[0144] The volume change rate of the curable composition according to the embodiment of the present invention is preferably 80% to 200%, preferably 90% to 180%, preferably 95% to 150%, and more preferably 96% to 120%.

[0145] When the volume change rate of the curable composition of the embodiment of the present invention is 80% to 200%, since the volume change rate is not large, the cured product of the curable composition is less likely to undergo cohesive failure and the adhesive force can be further improved.

[0146] The curable composition of the embodiment of the present invention may further include a filler (D), a thermoplastic resin (E), a crosslinking agent (F) for the elastomer, and a plasticizer (G) in addition to the elastomer (A), the epoxy resin (B), and the latent curing agent (C). When the curable composition of the embodiment of the present invention further includes a filler (D), a thermoplastic resin (E), a crosslinking agent (F) for the elastomer, and a plasticizer (G), the beneficial effect of being able to adjust the adhesiveness and physical properties according to the purpose of use can be exerted.

[0147] In the case where the curable composition of the embodiment of the present invention further comprises a filler (D), a thermoplastic resin (E), a crosslinking agent (F) and a plasticizer (G) for an elastomer, the sol-gel reaction of the thermoplastic resin (E) and the plasticizer (G) and the reaction of the elastomer (A) and the crosslinking agent (F) compete with the reaction of the epoxy resin (B) and the latent curing agent (C) (for example, an amine compound), and therefore, in the reaction of the epoxy resin (B) that contributes to adhesion, at least one of the latent curing agent (C) preferably comprises at least one selected from a dihydrazide compound and an imidazole compound, and the latent curing agent (C) preferably comprises both a dihydrazide compound and an imidazole compound. In this case, a balance between low temperature curability and storage stability can be achieved, and the beneficial effect of excellent adhesion performance can be exerted.

[0148] In the case where the curable composition of the embodiment of the present invention further includes a filler (D), a thermoplastic resin (E), an elastomer crosslinking agent (F) and a plasticizer (G), the sol-gel reaction of the thermoplastic resin (E) and the plasticizer (G) and the reaction of the elastomer (A) and the crosslinking agent (F) compete with the reaction of the epoxy resin (B) and the latent curing agent (C) (for example, an amine compound). Therefore, in the reaction of the epoxy resin (B) that contributes to adhesion, at least one of the latent curing agents (C) preferably has a C10-C23 aliphatic alkane structure. In this case, low-temperature adhesion is more excellent, and a high cohesive failure rate can be maintained even at low temperatures (for example, 150° C.). This effect can be observed in the case of containing a thermoplastic resin (E) and a plasticizer (G) and in the case of containing an elastomer (A) and an elastomer crosslinking agent (F), and it is considered that this effect is manifested by the interaction between the C10-C23 alkane structure and the acrylic structure of the latent curing agent (C) and the elastomer (A).

[0149] When the curable composition of the embodiment of the present invention further comprises a filler (D), a thermoplastic resin (E), an elastomer crosslinking agent (F) and a plasticizer (G), at least one of the latent curing agents (C) preferably comprises a latent curing agent represented by the above formula (1). In this case, a balance between low temperature curability and storage stability can be achieved, and the beneficial effect of excellent adhesive performance can be exerted.

[0150] The curable composition according to the embodiment of the present invention can be produced by mixing the above components.

[0151] In another aspect of the present invention, there is provided a method for producing a curable composition, wherein the curable composition comprises an elastomer (A), an epoxy resin (B) and a latent curing agent (C), wherein the method for producing the curable composition comprises mixing the elastomer (A), the epoxy resin (B) and the latent curing agent (C), and satisfies at least any one of the following (i) to (iii).

[0152] (i) The method comprises: pulverizing at least a portion of the latent curing agent (C) in advance to an average particle size of 25 μm or less, and / or dispersing at least a portion of the latent curing agent (C) in advance in the epoxy resin (B).

[0153] (ii) comprising the following steps:

[0154] Step 1, making at least a portion of the elastomer (A) solid, mixing and dissolving the portion of the elastomer (A) that is solid with at least a portion of the plasticizer (G) or the epoxy resin (B) that is a liquid component, thereby obtaining a mixture 1 containing the elastomer (A);

[0155] Step 2, mixing at least a portion of the latent curing (accelerating) agent (C) with at least a portion of the plasticizer (G) to obtain a mixture 2 containing the latent curing (accelerating) agent (C); and

[0156] Step 3, mixing the mixture 1 obtained in step 1 and the mixture 2 obtained in step 2 with other components of the curable composition other than mixture 1 and mixture 2 (for example: filler (D), thermoplastic resin (E), elastomer crosslinking agent (F) and / or plasticizer (G), etc.).

[0157] (iii) comprising: mixing a part or all of the components of the curable composition to obtain an intermediate mixture of the curable composition, and reducing the pressure and stirring the intermediate mixture to obtain the curable composition;

[0158] Here, the reduced pressure and stirring include: reducing pressure and stirring for more than 20 minutes at a temperature above 3 mmHg and below 150 mmHg; and not stirring when the pressure is reduced to below 3 mmHg or reducing pressure and stirring for less than 10 minutes when the pressure is below 3 mmHg (that is, the pressure can be reduced to below 3 mmHg, but in this case, the stirring time is less than 10 minutes and the stirring time can be 0 minutes).

[0159] As a method for producing a curable composition according to an embodiment, the present invention can provide a method for producing a curable composition, which is a method for producing a curable composition comprising an elastomer (A), an epoxy resin (B) and a latent curing agent (C).

[0160] The manufacturing method comprises mixing an elastomer (A), an epoxy resin (B) and a latent curing agent (C), and comprises:

[0161] (i) At least a portion of the latent curing agent (C) is pulverized in advance to an average particle size of 25 μm or less, and / or at least a portion of the latent curing agent (C) is dispersed in advance in the epoxy resin (B).

[0162] There are no particular limitations on the apparatus and method for mixing the elastomer (A), the epoxy resin (B) and the latent curing agent (C) as long as the objective curable composition of the present invention can be produced.

[0163] As the mixing device as described above, specifically, for example, a twin-screw mixer, a planetary mixer, a sigma mixer, a kneader, an attritor, a grinder, a roll, a dissolver and the like can be used.

[0164] The mixing is preferably performed using a twin-screw mixer, a planetary mixer or a sigma mixer. If a twin-screw mixer, a planetary mixer or a sigma mixer is used, a high-viscosity material can be dispersed more effectively.

[0165] Furthermore, mixing can be performed using a mixing vessel, for example, mixing can be performed in a tank, a container, or the like.

[0166] The method for producing a curable composition according to an embodiment of the present invention may include the above step (i).

[0167] When the production method according to the embodiment of the present invention includes the step (i) as described above, the latent curing agent (C) can be dispersed more uniformly in the curable composition, and a curable composition having better properties can be produced.

[0168] There are no particular limitations on the apparatus and method for pulverizing the latent curing agent (C) to an average particle size of 25 μm or less as long as the objective curable composition of the present invention can be produced.

[0169] As the above-mentioned pulverizing device and method, various pulverizing devices and methods can be used, and specifically, for example, KJ400 (trade name) manufactured by Kurimoto Iron Works Co., Ltd. can be used.

[0170] The average particle size of the latent curing agent (C) can be measured by a laser particle size distribution measurement method. Specifically, for example, it can be measured using SALD-200V ER (trade name) manufactured by Shimadzu Corporation.

[0171] The average particle size is preferably 50 μm or less, more preferably 30 μm or less, and further preferably 25 μm or less.

[0172] When the latent curing agent (C) is pulverized in advance to an average particle size of 25 μm or less, the adhesive strength can be further stabilized.

[0173] Furthermore, at least a portion of the latent curing agent (C) may be dispersed in advance in the epoxy resin (B). Preferably, 25% of the latent curing agent (C) is dispersed in the epoxy resin (B), more preferably, 50% of the latent curing agent (C) is dispersed in the epoxy resin (B), and even more preferably, all of the latent curing agent (C) is dispersed in the epoxy resin (B).

[0174] When at least a part of the latent curing agent (C) is dispersed in advance in the epoxy resin (B), the adhesive strength can be further stabilized.

[0175] As a method for producing a curable composition according to an embodiment, the present invention can provide a method for producing a curable composition, which is a method for producing a curable composition comprising an elastomer (A), an epoxy resin (B) and a latent curing agent (C).

[0176] The manufacturing method comprises mixing an elastomer (A), an epoxy resin (B) and a latent curing agent (C), and comprises the following steps 1 to 3 (in the case of (ii)):

[0177] (ii) Step 1, making at least a portion of the elastomer (A) solid, mixing and dissolving the portion of the elastomer (A) that is solid with at least a portion of the plasticizer (G) or the epoxy resin (B) that is a liquid component, thereby obtaining a mixture 1 containing the elastomer (A);

[0178] Step 2, mixing at least a portion of the latent curing (accelerating) agent (C) with at least a portion of the plasticizer (G) to obtain a mixture 2 containing the latent curing (accelerating) agent (C); and

[0179] Step 3, mixing the mixture 1 obtained in step 1 and the mixture 2 obtained in step 2 with other components of the curable composition other than mixture 1 and mixture 2 (for example: filler (D), thermoplastic resin (E), elastomer crosslinking agent (F) and / or plasticizer (G), etc.).

[0180] The method for producing a curable composition according to an embodiment of the present invention may include the above step (ii). In this case, the curable composition according to an embodiment of the present invention may further include a plasticizer (G), and the method for producing a curable composition as described above can be provided.

[0181] In the above step 1, it is preferable to use a method in which a part of the filler (D) is further added to reduce the cohesive force of the elastomer (A) and thereby promote the dissolution of the elastomer (A). In addition, the order of adding in step 3 may be changed as appropriate.

[0182] There are no particular limitations on the stirring device and method, and the mixing device and method performed in the above steps 1 to 3 as long as the objective curable composition of the present invention can be produced.

[0183] When the production method according to the embodiment of the present invention includes the step (ii) above, the following advantageous effects can be achieved: improved dispersibility, more efficient mixing, shortened process time, and improved adhesive strength.

[0184] If the dispersibility of the elastomer (A) is further improved, the mixing state with other components (such as epoxy resin (B), latent curing agent (C), thermosetting resin (E), etc.) can be further improved, and the adhesion can be further improved. In contrast, when the dispersion of the elastomer (A) is insufficient, the mixing state with other components will become insufficient, and the adhesion will become insufficient. Furthermore, if the dispersibility of the latent curing agent (C) is further improved, a more uniform curable composition can be obtained, and further, the aggregation of the latent curing agent (C) can be further prevented, and the mixing with the non-reactive components can be made easier, and long-term storage, long-term transportation (such as output), etc. can be easily carried out while preventing deterioration.

[0185] The production method according to the embodiment of the present invention may include adding the plasticizer (G) to the elastomer (A) passing through a mixing roll in batches during the mixing of the elastomer (A) and the plasticizer (G).

[0186] In the mixing of the elastomer (A) and the plasticizer (G), there are no particular restrictions on the apparatus and method for passing the elastomer through a mixing roll and the apparatus and method for adding the plasticizer (G) in batches, as long as the objective curable composition of the present invention can be produced.

[0187] In the case where the production method of the embodiment of the present invention includes adding the plasticizer (G) batchwise to the elastomer (A) passing through a mixing roll, it is possible to disperse the elastomer (A) more uniformly.

[0188] The solid elastomer (A) is preferably formed (or sheeted) into a thin sheet by passing it through a mixing roll. A plasticizer (G) is preferably used in the elastomer (A) sheeted (sheeted) by passing it through a mixing roll. The plasticizer (G) can be used to promote the softening of the elastomer (A). Usually, the elastomer (A) can be passed through the mixing roll multiple times.

[0189] In addition, the elastomer (A) already exemplified is suitable for sheeting by passing through a mixing roll.

[0190] As a method for producing a curable composition according to an embodiment, the present invention can provide a method for producing a curable composition, which is a method for producing a curable composition comprising an elastomer (A), an epoxy resin (B) and a latent curing agent (C).

[0191] The manufacturing method comprises mixing an elastomer (A), an epoxy resin (B) and a latent curing agent (C), and comprises:

[0192] (iii) mixing a part or all of the components of the curable composition to obtain an intermediate mixture of the curable composition, and reducing the pressure and stirring the intermediate mixture to obtain a curable composition;

[0193] Here, the decompression and stirring include: decompression and stirring for more than 20 minutes at a temperature between 3 mmHg and 150 mmHg; and no stirring when the pressure is reduced to less than 3 mmHg or decompression and stirring for less than 10 minutes when the pressure is less than 3 mmHg.

[0194] The method for producing a curable composition according to an embodiment of the present invention may include step (iii).

[0195] The manufacturing method of the embodiment of the present invention may include: mixing a part or all of the components of the curable composition to obtain an intermediate mixture of the curable composition, and decompressing and stirring the intermediate mixture. There is no particular limitation on the device and method for decompressing and stirring the intermediate mixture as long as the target curable composition of the present invention can be manufactured.

[0196] The reduced pressure stirring of the intermediate mixture can be carried out, for example, at a reduced pressure of 150 mmHg or less, preferably at a reduced pressure of 120 mmHg or less, preferably at a reduced pressure of 100 mmHg or less, and more preferably at a reduced pressure of 80 mmHg or less. There is no particular restriction on the time for reducing pressure and stirring as long as bubbles in the intermediate mixture can be removed and the physical properties are not reduced due to excessive foaming during heat curing, and it can usually be carried out for more than 20 minutes, and can be carried out for more than 20 minutes and less than 60 minutes.

[0197] When the intermediate mixture is decompressed and stirred, it is possible to exhibit a beneficial effect of preventing extremely violent foaming when the curable composition is heated and cured.

[0198] On the other hand, the reduced pressure of lower limit is, for example, more than 1mmHg, preferably more than 3mmHg, preferably more than 6mmHg, more preferably more than 10mmHg.If the reduced pressure is lower than 3mmHg, then preferably under this condition, it is less than 10 minutes, more preferably less than 5 minutes.When the intermediate mixture is decompressed to less than 3mmHg, the bubble from the intermediate mixture can be removed more, therefore the intensity of the cured product of curable composition can be further improved, but when the cured product is impacted, the cured product may be broken at once.It can be considered that the microbubble remaining in the cured product when cracks are generated inside the cured product can prevent the crack growth.

[0199] In the case of (iii) above, the decompression and stirring preferably include: decompression and stirring for more than 20 minutes at a temperature between 6 mmHg and 120 mmHg, and no stirring when the pressure is reduced to less than 6 mmHg, or decompression and stirring for less than 10 minutes when the pressure is less than 6 mmHg.

[0200] Furthermore, in the above-mentioned case (iii), the reduced pressure and stirring more preferably include: reducing pressure and stirring for more than 20 minutes at a pressure of more than 10 mmHg and less than 100 mmHg, and not stirring when the pressure is reduced to less than 10 mmHg, or reducing pressure and stirring for less than 10 minutes when the pressure is less than 10 mmHg.

[0201] In the case of (iii), when the intermediate mixture contains a part of the components of the curable composition, that is, does not contain all the components, the intermediate mixture is stirred under reduced pressure, and then the remaining components of the curable components are added to obtain a curable composition. It is preferred that the remaining components of the curable composition as described above do not substantially contain volatile substances even if the mixture is stirred under reduced pressure, and examples thereof include colorants, spherical particles (glass beads or glass balls), etc.

[0202] In the case of including (iii), the latent curing agent (C) preferably further comprises a combination of two or more latent curing agents. For the combination of two or more latent curing agents, reference can be made to the above-mentioned records of this specification, such as the melting points of at least two latent curing agents, the types of compounds contained, their chemical structures, etc. More specifically, the combination of two or more latent curing agents can be exemplified by examples such as: a combination of dicyandiamide and dodecanedioic acid dihydrazide, a combination of 2-heptadecanedioic acid dihydrazide and 2-undecyl imidazole, a combination of dodecanedioic acid dihydrazide and 2-heptadecanedioic acid dihydrazide, a combination of N,N-dimethyl-N'-(3,4-dichlorophenyl) urea (diuron) and dodecanedioic acid dihydrazide, a combination of dicyandiamide and 2-heptadecanedioic acid dihydrazide, and the like.

[0203] The manufacturing method of the embodiment of the present invention preferably satisfies both the features (i) and (iii). When the manufacturing method of the embodiment of the present invention satisfies both the features (i) and (iii), the beneficial effects of higher adhesion and impact absorption can be exerted.

[0204] Any curable composition according to the embodiment of the present invention can be produced using the method for producing a curable composition according to the embodiment of the present invention.

[0205] The present invention can provide a method for producing a curable composition according to any of the embodiments of the present invention, which has the characteristics of the curable composition according to any of the embodiments of the present invention.

[0206] The present invention can provide a curable composition produced by the method for producing a curable composition according to any one of the embodiments of the present invention.

[0207] Regarding the curable composition and its production method, etc. of the embodiments of this specification, each feature, the content of each embodiment, etc. can be combined arbitrarily as much as possible. Therefore, in order to avoid redundancy, the description of the detailed combination of features is omitted.

[0208] For the curable composition of the embodiment of the present invention, it is preferred to make the aluminum plate adhesion (cured at 150°C) (shear strength), aluminum plate adhesion (cured at 165°C) (shear strength), aluminum plate adhesion (cured at 150°C) (shear strength) after storage at 50°C for 5 days, elongation of the cured product (cured at 165°C), steel plate adhesion (cured at 165°C) (shear strength) and (peel strength), impact strength of the cured product, storage stability of the curable composition, and dripping of the curable composition excellent. The detailed evaluation method is described in the examples.

[0209] The curable composition of this embodiment can be applied to a desired location in any thickness and coating form using a known coating method, such as droplet coating, slit coating, spray coating, swirl coating, shot peening, etc., and can be cured by, for example, heating to a specified temperature using a hot air circulation drying furnace.

[0210] In an embodiment of the present invention, a method for manufacturing a motor vehicle including using the curable composition according to an embodiment of the present invention may be provided.

[0211] The curable composition according to the embodiment of the present invention can be used in the process of manufacturing the vehicle body of an automobile, and more specifically, can be suitably used as an adhesive for the vehicle body process (for example, a structural adhesive, a tackiness agent, etc.).

[0212] In the above-mentioned coating method, coating may also be performed by an automatic coater or a robot coater controlled by a computer.

[0213] In another aspect of the present invention, there is provided a method for lowering the curing temperature of a curable composition, comprising using the curable composition.

[0214] Example

[0215] Below, the present invention is specifically and in detail described by examples and comparative examples, but these examples are only one aspect of the present invention, and the present invention is not limited by these examples. It should be noted that, in the description of the examples, unless otherwise specified, the part without considering the solvent is measured by weight parts and weight %.

[0216] The components used in this example are shown below.

[0217] (A) Elastomer

[0218] (a1) Styrene / butadiene rubber (SBR1009 (trade name) manufactured by ISP Japan Co., Ltd.)

[0219] (a2) Butadiene rubber (BR1220 (trade name) manufactured by Zeon Co., Ltd. of Japan)

[0220] (B) Epoxy resin

[0221] (b1) Bisphenol A type epoxy resin (JER828 (trade name) manufactured by Mitsubishi Chemical Corporation)

[0222] (b2) Urethane-modified epoxy resin (EPU-78-11 (trade name) manufactured by ADEKA Corporation) (A part of the epoxy resin is modified with a urethane elastomer in advance, and contains (A). The amount of modification with the urethane elastomer is 10% to 20% by mass.)

[0223] (b3) Hydrogenated bisphenol A type epoxy resin (HBE-100 (trade name) manufactured by Shin Nippon Rika Co., Ltd.)

[0224] (b4) Polypropylene glycol diglycidyl ether (Adeka Glycirol ED-506 (trade name) manufactured by ADEKA Corporation)

[0225] (C) Latent curing (accelerating) agent

[0226] (c1) Dicyandiamide (CG-NA (trade name) manufactured by Air Products), melting point 207°C to 210°C, average particle size 30 μm or more

[0227] (c2) 2-heptadecylimidazole, melting point 88°C, average particle size 30 μm or more

[0228] (c3) 2-Undecyl imidazole, melting point 72°C, average particle size 30 μm or more

[0229] (c4) 2,4-diamino-6-(2'-methylimidazolyl (1'))-ethyl-o-triazine (2MZA (trade name) manufactured by Shikoku Chemical Co., Ltd.), melting point 248°C to 258°C, average particle size 25 μm or less

[0230] (c5) N,N-dimethyl-N'-(3,4-dichlorophenyl)urea (diuron) (Dyhard UR200 (trade name) manufactured by AlzChem), melting point 172°C to 182°C, average particle size 25 μm

[0231] (c6) Dodecanedioic acid dihydrazide (DDH (trade name) manufactured by Otsuka Chemical Co., Ltd.), melting point 188°C to 192°C, average particle size 25 μm or less

[0232] (D) Filling material

[0233] (d1) Surface treated calcium carbonate (Hakuenka CCR (trade name) manufactured by Shiraishi Industries)

[0234] (d2) Heavy calcium carbonate (BF200 (trade name) manufactured by Beihoku Powder Industry Co., Ltd.)

[0235] (d3) Crown clay (Crown clay (trade name) manufactured by SHIRAISHI CALCIUM KAISHA, LTD.)

[0236] (d4) Hydrophobic silica (TS720 (trade name) manufactured by Cabot Specialty Chemicals Inc.)

[0237] (E) Thermoplastic resin

[0238] (e1) Acrylic resin (LP-3102 (trade name) manufactured by Mitsubishi Rayon Co., Ltd.), average particle size 50 μm

[0239] (e2) Polymethacrylate resin (ZEFIAC F351 (trade name) manufactured by Aica Kogyo Co., Ltd.), average particle size 80 μm

[0240] (e3) Vinyl chloride resin (PSH-10 (trade name) manufactured by Kaneka Corporation), average particle size 1 μm

[0241] (F) Crosslinking agent for elastomer

[0242] (f1) 4,4-di(tert-butylperoxy)valerate (Perhexa V (trade name) manufactured by NOF Chemical Co., Ltd.)

[0243] (G) Plasticizer

[0244] (g1) Diisononyl phthalate

[0245] (H) Others

[0246] (h1) 3-Mercaptopropyltrimethoxysilane (KBM803 (trade name) manufactured by Shin-Etsu Chemical Co., Ltd.)

[0247] (h2) Calcium oxide (QCX (trade name) manufactured by Inoue Lime Co., Ltd.)

[0248] (h3) Hydrocarbon solvent (Isopar H (trade name) manufactured by ExxonMobil Corporation)

[0249] Average particle size

[0250] The latent curing agent (C) was pulverized using KJ400 (trade name) manufactured by Kurimoto Iron Works Co., Ltd. The average particle size thereof was measured by laser particle size distribution measurement using SALD-200V ER (trade name) manufactured by Shimadzu Corporation. The obtained average particle size is as described above.

[0251] These components were blended in the ratios shown in Table 1 and Table 2 to produce curable compositions of Examples 1 to 14 and Comparative Examples 1 to 3.

[0252] More specifically, the curable compositions of Examples 1 to 12 and Comparative Examples 1 and 2 were produced by the following operation.

[0253] The elastomer (A) is formed into sheets using a mixing roller, and the sheeted elastomer (A) is placed in a pressure kneader. Epoxy resin (B) or plasticizer (G) and calcium carbonate are added in small amounts successively, stirred and kneaded to dissolve the elastomer (A). The mixture containing the elastomer (A) is mixed and stirred with other components such as epoxy resin (B) and latent curing agent (C) using a planetary mixer, etc., to produce a curable composition.

[0254] Furthermore, in the method for producing the curable composition of Examples 1 to 12 and Comparative Examples 1 and 2, the following steps and the like were performed as necessary.

[0255] The latent curing agent (C) and part of the plasticizer (G) are mixed in advance (at a mass ratio of 1:1) before use. That is, the latent curing agent (C) is dispersed in the plasticizer (G) before use.

[0256] In the methods for producing curable compositions of Examples 1 to 12 and Comparative Examples 1 and 2, the mixture obtained by mixing all the components was stirred for 20 minutes to 60 minutes under a reduced pressure of 10 mmHg to 100 mmHg to obtain the target curable composition.

[0257] The curable compositions of Examples 13 to 16 and Comparative Example 3 were produced as follows.

[0258] Since (b2) containing the elastomer (A) component is used instead of the elastomer (A) component alone, the epoxy resin (including the elastomer (b2)), the latent curing agent (C) and other components are mixed and stirred using a planetary mixer or the like to produce a curable composition.

[0259] Furthermore, in the method for producing the curable composition of Examples 13 to 16, the following steps and the like were performed as necessary.

[0260] The latent curing agent (C) is mixed with a part of the filler (D) (equal to the amount of the latent curing agent (C)), and then crushed to an average particle size of 10 μm or less using a pulverizer. That is, the latent curing agent (C) mixed with a part of the filler (D) and crushed to an average particle size of 10 μm or less is used.

[0261] In the method for producing a curable composition of Example 13, the mixture obtained by mixing all the components is stirred under a reduced pressure of less than 60 mmHg for 30 minutes (during this period, it is stirred under a reduced pressure of less than 10 mmHg for 12 minutes, and the maximum reduced pressure is 4 mmHg) to obtain the target curable composition.

[0262] In the method for producing a curable composition of Example 14, the mixture obtained by mixing all the components is stirred under a reduced pressure of less than 60 mmHg for 30 minutes (during this period, the reduced pressure below 10 mmHg is 0 minutes, and the maximum reduced pressure is 15 mmHg) to obtain the target curable composition.

[0263] In the method for producing a curable composition of Example 15, the mixture obtained by mixing all the components is stirred under a reduced pressure of less than 60 mmHg for 30 minutes (during this period, the reduced pressure below 10 mmHg is 0 minutes, and the maximum reduced pressure is 15 mmHg) to obtain the target curable composition.

[0264] In the method for producing the curable composition of Example 16 and Comparative Example 3, the mixture obtained by mixing all the components is stirred under a reduced pressure of less than 60 mmHg for 60 minutes (during this period, the reduced pressure is less than 3 mmHg for 20 minutes and the maximum reduced pressure is 0.5 mmHg) to obtain the target curable composition.

[0265] For each of the above-mentioned curable compositions, the following methods were used to measure and evaluate the aluminum plate adhesion (cured at 150°C) (shear strength), aluminum plate adhesion (cured at 165°C) (shear strength), aluminum plate adhesion (cured at 150°C) (shear strength) after storage at 50°C for 5 days, the elongation of the cured product (cured at 165°C), steel plate adhesion (cured at 165°C) (shear strength) and (peel strength), the impact strength of the cured product, the storage stability of the curable composition, the volume change rate (%) of the curable composition, and the dripping property of the curable composition. The results are shown in Tables 1 and 2.

[0266] Aluminum plate adhesion (150℃ curing (low temperature))

[0267] The surface of the aluminum plate (1.0 mm × 25 mm × 100 mm) described in JIS A5182 was degreased with unleaded gasoline. A curable composition was applied to the surface of the aluminum plate. Then, the steel plates described in JIS G3141, which had also been degreased on the surface, were overlapped and adjusted with a partition so that the thickness of the curable composition was 3 mm. The curable composition was cured at 150°C for 30 minutes to obtain a sample. According to the shear strength test method of JASO M 323-77, the shear strength (kPa) was measured at a tensile speed of 50 mm / min using an autograph (Shimadzu Corporation, DSC-5000) as the aluminum plate adhesion (150°C curing (low temperature)).

[0268] Furthermore, the fracture state of the cured product of the curable composition was visually observed. The evaluation criteria for the fracture state are as follows. The shear strength (kPa) and the fracture state are shown in Tables 1 and 2.

[0269] ○: Less than 10% interfacial failure, more than 90% cohesive failure

[0270] ○-: 10% or more and less than 30% of interfacial failure / 70% or more and less than 90% of cohesive failure

[0271] ○△: 30% or more and less than 50% of interfacial failure / 50% or more and less than 70% of cohesive failure

[0272] △: 50% or more and less than 70% of interfacial failure / 30% or more and less than 50% of cohesive failure

[0273] ×: 70% or more of the interface is damaged

[0274] Aluminum plate adhesion (165℃ curing (standard))

[0275] The surface of the aluminum plate (1.0 mm × 25 mm × 100 mm) described in JIS A5182 was degreased with unleaded gasoline. The curable composition was applied to the surface of the aluminum plate. Then, the steel plates described in JIS G3141, which had been similarly degreased on the surface, were overlapped and adjusted with a partition so that the thickness of the curable composition was 3 mm. The curable composition was cured at 165°C for 30 minutes to obtain a sample. According to the shear strength test method of JASO M 323-77, the shear strength (kPa) was measured as the aluminum plate adhesion (165°C (standard)) using an autograph (Shimadzu Corporation, DSC-5000) at a tensile speed of 50 mm / min.

[0276] Furthermore, the fracture state of the cured product of the curable composition was visually observed. The evaluation criteria for the fracture state are as follows. The shear strength (kPa) and the fracture state are shown in Tables 1 and 2.

[0277] ○: Less than 10% interfacial failure, more than 90% cohesive failure

[0278] ○-: 10% or more and less than 30% of interfacial failure / 70% or more and less than 90% of cohesive failure

[0279] ○△: 30% or more and less than 50% of interfacial failure / 50% or more and less than 70% of cohesive failure

[0280] △: 50% or more and less than 70% of interfacial failure / 30% or more and less than 50% of cohesive failure

[0281] ×: 70% or more of the interface is damaged

[0282] Adhesion to aluminum plate after storage at 50°C for 5 days (cured at 150°C (low temperature))

[0283] The shear strength (kPa) was measured and the fracture state of the cured product was evaluated by the same method as described in the above aluminum plate adhesion (150°C curing (low temperature)) except that the curable composition was stored at 50°C for 5 days before use. The results are shown in Tables 1 and 2.

[0284] Elongation of cured product (cured at 165℃)

[0285] The elongation was measured according to JIS K 6251 "tensile test". The curable composition prepared as described above was coated into a sheet with a thickness of 3 mm, baked under specified conditions (165° C., 30 minutes), and then punched into a dumbbell shape of No. 2 to obtain a test specimen. The elongation at break measured at a tensile speed of 50 mm / min was recorded as the elongation.

[0286] The hardness is measured as follows.

[0287] The above-mentioned cured products were stacked so as to have a thickness of about 12 mm, and the hardness of the cured products was measured using a TYPE-A durometer in accordance with JIS K 6253.

[0288] Steel plate adhesion (165℃ cured (standard)) (shear strength)

[0289] The surface of the steel plate (1.6 mm × 25 mm × 100 mm) described in JIS G3141 was degreased with unleaded gasoline. A curable composition was applied to the surface of the steel plate. Then, the steel plates described in JIS G3141 whose surfaces were similarly degreased were overlapped and pressed, and the curable composition was cured at 165°C for 30 minutes to obtain a sample. According to the peel strength test method of JASOM 353, the shear strength (MPa) was measured as the adhesion of the steel plate (cured at 165°C (standard)) using an autograph (Shimadzu Corporation, DSC-5000) at a tensile speed of 50 mm / min.

[0290] Furthermore, the fracture state of the cured product was evaluated by visual observation. The evaluation criteria are as follows. The shear strength (MPa) and the fracture state are shown in Tables 1 and 2.

[0291] ○: Less than 10% interfacial failure, more than 90% cohesive failure

[0292] △: 10% or more and less than 70% of interfacial failure / 30% or more and less than 90% of cohesive failure

[0293] ×: More than 90% interface damage

[0294] Steel plate adhesion (165℃curing (standard)) (peel strength)

[0295] The surface of the steel plate (0.8 mm × 25 mm × 150 mm) described in JIS G3141 was degreased with toluene, and after the curable composition was applied to the surface, the steel plates whose surfaces were similarly degreased were overlapped and pressed, and cured at 165° C. for 30 minutes to obtain a sample. According to the peel strength test method of JASO M 353, the 180° peel strength (N / 25 mm) of the sample was measured at a tensile speed of 200 mm / min using an autograph (Shimadzu Corporation, DSC-5000).

[0296] Furthermore, the fracture state of the cured product was evaluated by visual observation. The evaluation criteria are as follows. The 180° peel strength (N / 25 mm) and the fracture state are shown in Tables 1 and 2.

[0297] ○: Less than 10% interfacial failure, more than 90% cohesive failure

[0298] △: 10% or more and less than 70% of interfacial failure / 30% or more and less than 90% of cohesive failure

[0299] ×: More than 90% interface damage

[0300] Impact strength of cured product (cured at 165℃ (standard))

[0301] Using the steel plate described in JIS G3141, the curable composition was cured at 165°C for 30 minutes according to the wedge impact test described in JIS K6865 to prepare a test piece. The impact test was carried out using a high-speed tensile tester. The test speed was 2m / s. The average strength in the range of 25% to 90% of the total displacement during the test was divided by the width of the test piece to obtain the impact strength (N / mm).

[0302] Storage stability of curable composition (40°C, 14 days)

[0303] The storage stability of the curable composition was evaluated by storing the composition at 40° C. for 14 days and measuring the change in viscosity during the storage period. Specifically, the evaluation was performed as follows.

[0304] The curable composition was filled in a 250cc bottle with a depth of 13cm, and the viscosity was measured using a rotational viscometer according to JIS K6833. The viscosity was measured using a No. 7 rotor for viscosity measurement at a rotation speed of 2 (2rpm). The material temperature during the measurement was 20°C. The viscosity (η) of the curable composition after storage at 20°C for 1 day from the time of manufacture was measured. 1 ) and the viscosity (η) of the curable composition after further storage at 40°C for 14 days 14 The viscosity (η) of the curable composition after storage at 20°C for 1 day after production was measured. 1 ) as a reference, and the viscosity (η) of the curable composition after further storage at 40°C for 14 days was determined. 14 )’s rate of increase (i.e., thickening rate).

[0305] Thickening rate (%) = η 14 / η 1 ×100-100

[0306] The evaluation criteria are as follows.

[0307] ○: Thickening rate less than 30%

[0308] ○-: Thickening rate is 30% or more and less than 40%

[0309] △: Thickening rate is 40% or more and less than 60%

[0310] ×: Thickening rate is 60% or more

[0311] Volume change rate of curable composition (%)

[0312] The volume change rate (%) of the curable composition was evaluated according to the volume change rate test method A described in 9.34 of JASO M323-86.

[0313] Drip properties of curable composition

[0314] The dripping property of the curable composition was evaluated according to the flowability test described in 9.10 of JASO M323-86. Specifically, the evaluation was performed as follows.

[0315] On a steel plate (100 mm in width, 300 mm in length, 0.8 mm in thickness), a curable composition stored at 20°C for 1 day from the time of manufacture was applied using a mold in an inverted L-shape of 50 mm in width, 100 mm in length, 10 mm in width, and 5 mm in thickness. After removing the mold, the steel plate was mounted on a fixture at an angle of 90°, and the sag after 10 minutes was measured. The sag after heating at 165°C for 20 minutes was further measured.

[0316] The evaluation criteria are as follows.

[0317] ○: Total sag length is less than 10mm

[0318] △: Total sag length is 10 mm or more and less than 20 mm

[0319] ×: Total sag length is 20 mm or more

[0320] [Table 1]

[0321]

[0322] a) Cured at 150℃ b) Cured at 165℃ c) Cured at 150℃ after 5 days storage

[0323] [Table 2]

[0324]

[0325] a) Cured at 150℃ b) Cured at 165℃ c) Cured at 150℃ after 5 days storage

[0326] For the curable compositions of Examples 1 to 16, the adhesion to aluminum plates (cured at 150°C, cured at 165°C, and cured at 150°C after storage at 50°C for 5 days), elongation at break (cured at 165°C), hardness, adhesion to steel plates (cured at 165°C) (shear strength and peel strength), impact strength, storage stability, volume change rate, and dripping properties are all excellent.

[0327] The curable compositions of Comparative Examples 1 to 3 were inferior in some of the above-mentioned properties.

[0328] Industrial Applicability

[0329] The curable composition of the embodiment of the present invention comprises an elastomer (A), an epoxy resin (B) and a latent curing agent (C), and the latent curing agent (C) comprises a combination of two or more latent curing agents, and the curable composition can be applied to adhesives for automobiles, more specifically, to adhesives for vehicle body processes. The curable composition can be applied to, for example, adhesives for automobiles, more specifically, to adhesives for vehicle body processes (e.g., structural adhesives, adhesives, etc.).

Claims

1. An adhesive composition for automobiles, comprising an elastomer (A), an epoxy resin (B), a latent curing agent (C), a filler (D), a thermoplastic resin (E), an elastomer crosslinking agent (F) and a plasticizer (G), wherein: The latent curing agent (C) comprises a combination of two or more latent curing agents, The latent curing agent (C) contains at least one imidazole compound having a C10-C23 aliphatic alkane structure, The latent curing agent (C) contains at least one dihydrazide compound having a C10-C23 aliphatic alkylene structure, The latent curing agent (C) comprises dicyandiamide, The epoxy resin (B) is contained in an amount of 0.2 to 10 parts by mass per 100 parts by mass of the adhesive composition.

2. The adhesive composition for automobiles according to claim 1, wherein: The elastomer (A) comprises at least one selected from the group consisting of styrene / butadiene copolymers, nitrile / butadiene copolymers, butadiene polymers, isoprene polymers, ethylene / propylene / diene rubbers, acrylic acid, and urethane.

3. The automotive adhesive composition according to claim 1 or 2, wherein: The thermoplastic resin (E) includes at least one selected from acrylic resins, PVC resins, vinyl acetate resins, and copolymers thereof.

4. The automotive adhesive composition according to claim 1 or 2, wherein: The crosslinking agent (F) for the elastomer comprises at least one selected from sulfur and peroxide.

5. The automotive adhesive composition according to claim 1 or 2, wherein: The melting points of at least two latent curing (accelerating) agents contained in the latent curing agent (C) differ by 10° C. or more and 80° C. or less.

6. The automotive adhesive composition according to claim 1 or 2, wherein: At least one of the latent curing agents (C) comprises a latent curing agent satisfying formula (1), [Chemical formula 1] (1) In formula (1), n=10-23.

7. The automotive adhesive composition according to claim 1 or 2, wherein: At least one of the latent curing agents (C) comprises dodecanedioic acid dihydrazide.

8. An adhesive for use in a process for manufacturing a vehicle body, wherein: A vehicle adhesive composition comprising the adhesive composition according to any one of claims 1 to 7.