Superatomic materials, sols, preparation methods and applications thereof

By doping superatomic materials on inorganic carriers, the problems of high mobility and poor thermal stability of traditional antibacterial materials are solved, the service life is extended, the antibacterial effect is enhanced, and environmental pollution and safety risks are reduced.

CN115397585BActive Publication Date: 2024-10-22刘峰
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080098915.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-07-21
Publication Date
2024-10-22
Estimated Expiration
2040-07-21

AI Technical Summary

Technical Problem

Existing antibacterial materials have high silver ion mobility and poor thermal stability, which leads to environmental pollution and shortened antibacterial life. Moreover, traditional antibacterial materials may cause harm to the skin.

Method used

Superatomic materials are used, including carriers and doped silver, copper, and zinc superatoms, and the sol is prepared through a hydrothermal method. The superatomic scale is 100pm to 3000pm, and is fixed on an inorganic carrier to reduce mobility and improve antibacterial properties.

Benefits of technology

It extends the service life of antibacterial materials, reduces the risk of environmental pollution, enhances antimicrobial and antiviral effects, and because superatoms cannot easily enter the skin, it improves safety and environmental effects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115397585B_ABST
    Figure CN115397585B_ABST
Patent Text Reader

Abstract

Provided are a super-atom material, a sol, a preparation method and an application thereof. The super-atom material comprises a carrier and a super-atom doped in the carrier, wherein the super-atom is one or more of silver, copper, zinc super-atom and rare earth element super-atom, and the scale of the super-atom is 100 pm to 3000 pm; the carrier is an inorganic carrier. The super-atom material and the sol have excellent anti-microbial and anti-viral properties, and have a long service life and are green and environmentally friendly.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of antibacterial materials, and in particular to super-atomic materials, sols, and preparation methods and applications thereof. Background Art

[0002] As people's quality of life improves, the demand for antibacterial materials is gradually increasing. At present, antibacterial materials mainly include two types, one is inorganic antibacterial materials represented by silver, titanium oxide, zinc oxide, etc., and the other is organic antibacterial materials represented by quaternary ammonium salts, chitosan and its derivatives. Among them, inorganic antibacterial materials have excellent antibacterial effects and are widely used. In particular, silver-containing antibacterial materials, such as Ag / TiO2 composite powder materials, in which silver usually exists in the form of ions or complexes, which can destroy bacterial cell membranes and enter bacterial cells, and interact with bacterial DNA, resulting in high concentration of DNA and loss of replication ability. Silver can also combine with the thiol group of protein to make the protein inactive; titanium oxide has photocatalytic properties, which can cause microorganisms to die in a short time, thereby further improving the antibacterial effect of such materials. However, the silver ions in such materials have a high mobility and poor thermal stability, and are also easy to migrate to the environment, causing environmental damage. At the same time, the migration of metal ions will greatly shorten the antibacterial life of the product. Summary of the invention

[0003] Based on this, it is necessary to provide a super-atom material, a sol, and a preparation method and application thereof. The super-atom material and the sol have a long service life and are green and environmentally friendly.

[0004] A superatom material comprises a carrier and superatoms doped in the carrier, wherein the superatoms are one or more of silver, copper, zinc superatoms and rare earth element superatoms, and the scale of the superatoms is 100pm to 3000pm; and the carrier is an inorganic carrier.

[0005] A sol comprising the above-mentioned super-atom material.

[0006] A method for preparing a sol comprises the following steps:

[0007] mixing a metal salt, a carrier precursor and water to obtain a mixed solution;

[0008] The mixed solution is treated by the following method to obtain a sol:

[0009] Heating: raising the temperature of the mixed solution to 120° C. to 250° C. and the pressure to 15 bar to 60 bar within 200 seconds;

[0010] Keep warm: reduce the pressure to 10 bar to 40 bar and control the temperature at 130°C to 200°C for 270s to 330s;

[0011] Cooling: lower the temperature to 5℃~50℃ within 60s;

[0012] Wherein, the metal salt is an organic salt or an inorganic salt containing silver, copper, zinc or a rare earth element;

[0013] The carrier precursor is an inorganic acid or an inorganic acid complex which can generate an inorganic carrier through hydrothermal treatment.

[0014] An antimicrobial and antiviral coating comprising the above-mentioned super-atom material.

[0015] An antimicrobial and antiviral coating is mainly prepared from the above sol or the sol prepared by the above preparation method.

[0016] Application of the super-atom material, the sol, and the sol prepared by the preparation method in the preparation of daily necessities, cosmetics, coatings or sealants.

[0017] An antimicrobial and antiviral product comprises a substrate and a super-atom material loaded on the substrate, wherein the super-atom material is the above-mentioned super-atom material or a super-atom material prepared from a sol, and the sol is the above-mentioned sol or a sol prepared by the above-mentioned preparation method.

[0018] The above-mentioned super-atom material effectively improves the antimicrobial and antiviral effects of the super-atom material by using an inorganic carrier to dope super-atoms of a specific particle size range, and the super-atom material has a broad spectrum and can resist a variety of microorganisms and viruses, which can effectively increase the scope of application. In addition, the above-mentioned super-atom material can reduce the content of metal elements in the super-atom material, thereby achieving the purpose of reducing the toxicity of the super-atom material itself, and can effectively expand the scope of application. And because super-atoms are not easy to migrate to the environment, the environmental pollution caused by the super-atom material can be effectively avoided, and the service life of the super-atom material can be increased. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 A schematic diagram of forming an antimicrobial and antiviral coating by a sol and antimicrobial and antiviral powder according to an embodiment of the present invention;

[0020] Figure 2 is the XPS graph of the sol of Example 2;

[0021] Figure 3 The XPS spectrum of the sol of Example 6

[0022] Figure 4 is a (high resolution) electron microscope image of the sol of Example 2;

[0023] Figure 5is a (high resolution) electron microscope image of the sol of Example 2;

[0024] Figure 6 is a (high resolution) electron microscope image of the sol of Example 2;

[0025] Figure 7 is a (high resolution) electron microscope image of the sol of Example 4;

[0026] Figure 8 is a (high resolution) electron microscope image of the sol of Example 5;

[0027] Fig. 9 A (high resolution) electron microscope high angle annular dark field image of the sol of Example 6;

[0028] Fig.10 The yellow leaf disease virus infection titer of the sol of Example 2 under different light intensities;

[0029] Fig.11 is the molecular correlation spectrum of the sol of Example 1;

[0030] Fig.12 is the XRD pattern of the sol of Example 1;

[0031] Fig.13 is the surface charge value of the superatom material in the sol of Example 1. DETAILED DESCRIPTION

[0032] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively below, and preferred embodiments of the present invention are provided. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive.

[0033] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.

[0034] The superatom material of one embodiment of the present invention includes a carrier and superatoms doped in the carrier, the superatoms are one or more of silver, copper, zinc superatoms and rare earth element superatoms, and the scale of the superatoms is 100pm to 3000pm; the carrier is an inorganic carrier.

[0035] In the present invention, "superatom" refers to an atomic cluster composed of more than two atoms, a critical structure between nanoparticles and single atoms. Superatoms are not ions and have their own unique properties. Compared with ions or complexes containing the ions, superatoms have lower mobility and are not easy to enter the environment. Moreover, since the superatoms of the superatomic material of the present invention are doped in a carrier, the superatoms are fixed on a carrier with a larger size and therefore will not enter the skin barrier. The surface-doped superatoms (clusters) can provide extremely high activity, so that the superatomic material combination can take into account both safety and high performance. Compared with traditional antibacterial materials, it not only has better antimicrobial and antiviral properties, but also has higher environmental effects and safety, and can effectively avoid environmental pollution caused by the entry of metal elements into the natural environment. Taking the 2nm silver-containing complex material with better performance in traditional products as an example, it can invade the skin system for several mm and may bring unknown hazards.

[0036] Furthermore, the nano-size effect of the superatom is stronger. From the perspective of specific surface area alone, the theoretical equivalent specific surface area of ​​a 2nm silver superatom is 286m 2 / g, while the equivalent specific surface area of ​​15nm nanosilver commonly seen on the market is 38m 2 / g, which will bring about a huge difference in performance; and because the superatoms of the above-mentioned superatomic materials are not easy to enter the environment, the service life of the superatomic materials can also be effectively extended. Compared with traditional antibacterial materials (generally 1-2 years), the life can be extended to more than 5 years.

[0037] In addition, since the metal elements in the above-mentioned super-atom materials exist in the form of super-atoms, they have a better sterilization effect, and the amount of doped metal required is lower, which makes the super-atom materials themselves less toxic, and can effectively expand the scope of application, for example, they can be used in the preparation of daily necessities, cosmetics, etc. And the above-mentioned super-atom materials have strong dispersibility and can be evenly dispersed in solvents such as water and alcohol without agglomeration, thereby improving the processing performance of the materials.

[0038] Further, the scale of the super-atom is 100pm to 2500pm; further, the scale of the super-atom is 100pm to 2300pm; further, the scale of the super-atom is 100pm to 2200pm; further, the scale of the super-atom is 100pm to 2100pm; further, the scale of the super-atom is 100pm to 2000pm; further, the scale of the super-atom is less than 2000pm and greater than or equal to 100pm; further, the scale of the super-atom is 100pm to 1500pm; further, The scale of superatoms is 100pm to 1200pm; further, the scale of superatoms is 100pm to 1000pm; further, the scale of superatoms is less than 1000pm and greater than or equal to 100pm; further, the scale of superatoms is less than or equal to 1000pm and greater than 100pm; further, the scale of superatoms is less than 1000pm and greater than 100pm; further, the scale of superatoms is 200pm to 800pm; further, the scale of superatoms is 300pm to 500pm.

[0039] Furthermore, the above-mentioned carrier is a quantum size carrier; further, the particle size of the above-mentioned carrier is less than 10nm; further, the particle size of the above-mentioned carrier is 1-10nm.

[0040] Further, the carrier is doped with at least silver superatoms;

[0041] Further, the carrier is doped with at least copper superatoms;

[0042] Furthermore, the carrier contains silicon;

[0043] Furthermore, the carrier is a carrier modified by a silicon-based substance to modify the surface of the carrier and improve the surface adhesion of the carrier, which is conducive to forming a product with small and uniform particle size, further extending the service life of the superatomic material and avoiding environmental pollution.

[0044] Furthermore, the carrier is doped with a substance generated by a hydrothermal reaction of a silicon-based substance.

[0045] It is understandable that the "silicon-based material" in the present invention refers to silicon-containing materials that are acceptable in the art for carrier surface modification, including but not limited to: silicon oxide and materials that can be hydrolyzed into silicon oxide such as alkoxysilane; further, the carrier is preferably doped with one or more of tetramethoxysilane, tetraethoxysilane, γ-glycidyloxypropyltrimethoxysilane, γ-methacryloxypropyltrimethoxysilane, γ-aminopropyltriethoxysilane or trimethoxysilane. This type of material has a better surface modification effect, can further improve adhesion, optimize the size of the super-atomic material and improve the uniformity of the product particle size.

[0046] The "carrier" in the present invention refers to an inorganic substance used to dope superatoms. The specific type is not particularly limited, and acceptable carrier materials in the art can be used. Furthermore, it is preferred that the carrier is a titanium-containing carrier to further improve the antimicrobial and antiviral properties of the superatomic material; further, the carrier is one or more of titanium oxide, titanium nitride and titanium peroxide. Further, the carrier is a material with photocatalytic properties; further, the carrier is anatase titanium dioxide nanocrystal. Under the action of light, a large amount of ·OH and ·O can be produced on the surface of titanium oxide, which can cause the death of microorganisms in a short time after contact with microorganisms, and there is a synergistic effect between the superatoms and the carrier, which can improve the bactericidal efficiency and bactericidal effect of the superatoms by synergizing with the superatoms.

[0047] Furthermore, the superatom is a silver superatom, and the carrier is anatase titanium dioxide nanocrystal. By utilizing the characteristics of light-excited electron-hole separation, hole injection can excite the silver atoms in the superatom cluster to become in-situ transient high-valent silver ions, thereby having stronger antimicrobial and antiviral properties, while not generating silver ions, which are easily soluble in water and enter the environment and human body, causing high risks.

[0048] Furthermore, the carrier is nitrogen interstitially doped titanium oxide; further, the superatom is a silver superatom, and the carrier is nitrogen interstitially doped titanium oxide to form an Ag / N / TiO2 composite doped superatom material. Nitrogen interstitial doping improves the efficiency of generating electron-hole pairs after TiO2 is photoactivated, and the photogenerated holes can be injected into Ag superatoms to form in-situ transient high-valent silver ions, bringing further performance improvement.

[0049] Further, at least one crystal plane width of the carrier is less than 10 nm. Further, the two-dimensional projection shape of the carrier is a quadrilateral, a spindle or a circle.

[0050] Furthermore, the carrier surface carries an electric charge (positive charge or negative charge); further, the absolute value of the electric charge is greater than or equal to 15 mV; by charging the surface of the carrier, agglomeration can be avoided, and the dispersibility of the super-atomic material can be further improved.

[0051] The above-mentioned super-atom material effectively improves the antimicrobial and antiviral effects of the super-atom material by using an inorganic carrier to dope super-atoms of a specific particle size range, and can reduce the content of metal elements in the super-atom material, thereby achieving the purpose of reducing the toxicity of the super-atom material itself, and can effectively expand the scope of application. And because super-atoms are not easy to migrate into the environment, it can effectively avoid environmental pollution caused by super-atom materials, and at the same time can increase the service life of super-atom materials.

[0052] The present invention also provides a sol, including the above-mentioned super-atom material. Since the above-mentioned super-atom material adopts the form of carrier-doped super-atoms, it has better dispersion performance than traditional antibacterial materials, and can use solvents as dispersants, which in turn avoids the agglomeration of super-atom materials and further improves the uniformity of the sol. In addition, since the super-atoms of the above-mentioned super-atom material are not easy to fall off or migrate into the solvent, the formed sol has high stability.

[0053] Furthermore, the super-atomic material in the above sol is in a monodisperse state; further, the ratio of DLS average particle size / XRD average particle size of the super-atomic material is less than 4, further, less than 3, and further, less than 2.

[0054] Figure 1 Schematic diagram of coating formed by antimicrobial and antiviral materials with different properties. Figure 1 Where a is a coating formed by the sol of the present invention, Figure 1 b and c are antimicrobial and antiviral powders prepared by traditional preparation methods. Figure 1 As shown in a, since the super-atom material of the present invention can be uniformly dispersed in the solvent to form a monodisperse sol, and since the super-atom material of the present invention has excellent adsorption, it can be directly coated without the need for additional adhesives, etc. After the coating is dried, the super-atom material is uniformly arranged to form a relatively dense and regular network structure, thereby making the entire coating have strong strength and toughness, and since there is no coating of other agents such as adhesives, more super-atom materials are exposed, thereby improving the antimicrobial and antiviral effects of the coating; and as shown in FIG. Figure 1 As shown in Fig. 2(b) and (c), conventional powdered materials (i.e., antimicrobial and antiviral powders) need to be used in combination with adhesives and other reagents to form a coating, and if the amount of adhesive is too small, the powdered materials are easy to fall off (e.g., Figure 1 A large amount of adhesive wrapping the powdered material will affect the antimicrobial and antiviral properties of the coating to a certain extent (as shown in b). Figure 1 (as shown in c).

[0055] It is understandable that the solvent in the above sol can be selected according to the actual situation of the application field, and is not particularly limited here and should not be understood as limiting the present invention. Further, the solvent is water or ethanol; further, in the sol, the mass percentage of the solvent is not less than 90%.

[0056] Furthermore, additives acceptable in the art may be added to the sol to further improve the dispersibility of the superatomic material. Some functional additives may also be added, which are not particularly limited here and should be understood to be within the scope of protection of the present invention.

[0057] The present invention also provides a method for preparing the above sol, comprising the following steps:

[0058] S101: mixing a metal salt, a carrier precursor and water to obtain a mixed solution;

[0059] The carrier precursor is an inorganic acid or an inorganic acid complex that can generate an inorganic carrier through a hydrothermal reaction, and the specific type of the carrier precursor can be selected according to the type of the selected carrier. In one embodiment, the carrier precursor is a titanium-containing inorganic acid or a titanium-containing inorganic acid complex; further, the carrier precursor is selected from: one or more of peroxytitanic acid, orthotitanic acid, peroxytitanic acid complex and orthotitanic acid complex; further, the carrier precursor contains at least one of peroxytitanic acid complex and orthotitanic acid complex, and by introducing a complexing agent into the mixed solution, a sol with better physical properties can be formed.

[0060] Wherein, the inorganic acid complex can be prepared by commercially available raw materials or by existing methods, specifically by mixing an inorganic acid, a complexing agent and a solvent, and stirring and reacting for a predetermined time. It should be noted that the prepared inorganic acid complex can be separated and used for the preparation of sol, or the reaction solution can be directly used for the preparation of sol without separation. In addition, a sol mixed solution can be prepared while preparing the inorganic acid complex, that is, a metal salt, an inorganic acid, a complexing agent and water are mixed to prepare a mixed solution, which should be understood to be within the scope of protection of the present invention.

[0061] Further, the complexing agent is one or more of peroxide (such as hydrogen peroxide), tartaric acid, malic acid and citric acid. In the above mixed liquid system, the use of the complexing agent can promote the formation of sol with excellent physical properties, so as to facilitate subsequent processing and application.

[0062] In the present invention, "metal salt" refers to a salt containing a desired metal element, specifically an organic or inorganic salt containing silver, copper, zinc or a rare earth element; further, the metal salt is selected from one or more of silver acetate, silver nitrate, silver sulfate, copper nitrate, zinc nitrate, zinc sulfate and copper sulfate; further, the metal salt is silver acetate or silver nitrate;

[0063] Furthermore, step S101 also includes the step of adding a silicon-based substance; further, the silicon-based substance is one or more of tetramethoxysilane, tetraethoxysilane, γ-glycidyloxypropyltrimethoxysilane, γ-methacryloxypropyltrimethoxysilane, γ-aminopropyltriethoxysilane or trimethoxysilane to modify the surface of the carrier and further improve the surface adhesion of the carrier.

[0064] Furthermore, step S101 also includes the step of adding ammonia water, triethylamine or ammonium salt; further, the amount of ammonia water or ammonium salt added is a trace amount, and further, the amount of ammonia water or ammonium salt is 4%-6% of the oxygen content in the carrier, so as to facilitate the preparation of nitrogen-doped superatomic materials.

[0065] Furthermore, step S101 includes the following steps:

[0066] S1011: mixing a metal salt and water to obtain a first solution;

[0067] Further, in step S1011, the mixture is mixed at a temperature of 25°C-35°C to fully dissolve the metal salt; further, the water is preferably heated to 25°C-35°C before adding the metal salt;

[0068] Furthermore, in the first solution, the concentration of the metal element is 10ppm-1000ppm; further, the concentration of the metal element is 100ppm-800ppm; further, the concentration of the metal element is 300ppm-600ppm.

[0069] S1012: mixing the carrier precursor with water to obtain a second solution;

[0070] Furthermore, in step S1012, the mixture is mixed at a temperature of 15°C-25°C to fully dissolve the carrier precursor; further, the water is preferably heated to 15°C-25°C before adding the carrier precursor;

[0071] It is understandable that there is no order between step S1011 and step S1012. Step S1011 may be performed first and then step S1012, or step S1012 may be performed first and then step S1011.

[0072] Furthermore, the concentration of the carrier precursor is 1%-30%.

[0073] S1013: dripping the first solution into the second solution at a speed of 100 mL / min to 200 mL / min, stirring, and obtaining a mixed solution.

[0074] By dripping the first solution into the second solution at a fixed speed, the metal ions can be uniformly dispersed in the solution, avoiding the coating of inorganic acid or inorganic acid complex, improving the uniformity of the mixed solution, and facilitating the subsequent steps.

[0075] S102: Treat the mixed solution by the following method to obtain a sol:

[0076] Heating: raise the temperature of the mixed liquid to 120°C to 250°C and the pressure to 15 bar to 60 bar within 200 seconds;

[0077] Keep warm: reduce the pressure to 10 bar to 40 bar and control the temperature at 130°C to 200°C for 270s to 330s;

[0078] Cooling: lower the temperature to 5℃~50℃ within 60s;

[0079] By adopting a critical hydrothermal heating process of rapid heating-avalanche cooling, super atoms with a size between nanoparticles and ions can be generated, and the carrier can be rapidly crystallized, so that the carrier crystals can be kept with strong uniformity, not easy to agglomerate, and small size, so that the obtained sol has strong antimicrobial, antiviral and long service life. Hydrothermal can form crystals such as titanium oxide, and can also reduce precursors such as silver and copper into single substances. However, the traditional hydrothermal process is long, resulting in a wide range of crystallization particle sizes and large particles. The inventors have found through research that high temperature is the key to completing crystallization, and a slower heating process will cause the particles to become larger. Therefore, by adopting a method of rapid heating and rapid cooling, the size of super atoms can be controlled to the maximum extent on the basis of completing crystallization and super atom synthesis. If the traditional method is adopted, 1) it is difficult to obtain quantum-sized nano titanium oxide carriers, and agglomeration and precipitation will occur; 2) super atoms will also grow into nano metal particles without special properties; 3) super atoms will separate and precipitate from titanium oxide, and super atom materials doped with super atoms in the carrier cannot be formed.

[0080] In addition, through the above method, the surface of the super-atomic material dispersed in the sol can be made to carry a charge of no less than 15 mV, which can effectively avoid the occurrence of agglomeration and improve the stability of the sol.

[0081] In addition, the above-mentioned critical hydrothermal heating process of rapid heating and avalanche cooling takes a short time, and the whole process does not exceed 10 minutes, which can greatly improve the production efficiency. Compared with the traditional high-temperature calcination method, the temperature is lower, which can avoid high temperature from destroying the activity of superatoms, and can also avoid the condensation of superatoms into nanoparticles, and avoid the growth of quantum dot crystals into agglomerated nanoparticles. At the same time, it can reduce energy consumption and is suitable for industrial production applications.

[0082] Existing instruments and equipment may be used for heating, heat preservation and cooling, and are not particularly limited here.

[0083] Further, in the temperature increasing step, the temperature and pressure are increased to the target value in 200s; further, the temperature and pressure are increased to the target value in 195s; further, the temperature and pressure are increased to the target value in 190s; further, the temperature and pressure are increased to the target value in 188s; further, the temperature and pressure are increased to the target value in 185s; further, the temperature and pressure are increased to the target value in 180s; further, the temperature and pressure are increased to the target value in 170s;

[0084] Further, in the temperature raising step, the target temperature is 130°C to 220°C; further, the target temperature is 140°C to 210°C; further, the target temperature is 145°C to 200°C; further, the target temperature is 150°C to 180°C; further, the target temperature is 155°C to 175°C; further, the target temperature is 157°C to 170°C; further, the target temperature is 155°C to 168°C; further, the target temperature is 156°C to 167°C; further, the target temperature is 157°C to 166°C; further, the target temperature is 158°C to 165°C; further, the target temperature is 159°C to 164°C; further, the target temperature is 162°C;

[0085] Further, in the temperature raising step, the target pressure is 12 bar to 60 bar; further, the target pressure is 15 bar to 50 bar; further, the target pressure is 15 bar to 40 bar; further, the target pressure is 15 bar to 30 bar; further, the target pressure is 16 bar to 29 bar; further, the target pressure is 17 bar to 25 bar; further, the target pressure is 18 bar to 24 bar; further, the target pressure is 19 bar to 22 bar;

[0086] Further, in the heating step, the temperature of the mixed solution is raised to 130°C-220°C and the pressure is raised to 12bar-50bar within 200s; further, in the heating step, the temperature of the mixed solution is raised to 135°C-210°C and the pressure is raised to 15bar-40bar within 200s; further, in the heating step, the temperature of the mixed solution is raised to 150°C-200°C and the pressure is raised to 18bar-22bar within 200s; further, in the heating step, the temperature of the mixed solution is raised to 150°C-200°C and the pressure is raised to 18bar-22bar within 180s; further, the temperature of the mixed solution is raised to 150°C-180°C and the pressure is raised to 18bar-22bar within 180s.

[0087] Further, in the heating step, the heating rate is 50 degrees / min to 51 degrees / min; further, the heating rate is 50.1 degrees / min to 50.9 degrees / min; further, the heating rate is 50.2 degrees / min to 50.8 degrees / min; further, the heating rate is 50.3 degrees / min to 50.7 degrees / min;

[0088] Further, in the heat preservation step, the pressure is 10 bar to 40 bar; further, the pressure is 10 bar to 30 bar; further, the target pressure is 10 bar to 20 bar; further, the target pressure is 12 bar to 18 bar; further, the target pressure is 13 bar to 17 bar; further, the target pressure is 14 bar to 16 bar;

[0089] Further, in the heat preservation step, the temperature is 150°C to 180°C; further, the temperature is 155°C to 170°C; further, the temperature is 155°C to 166°C; further, the temperature is 156°C to 165°C; further, the temperature is 157°C to 164°C; further, the temperature is 158°C to 162°C; further, the temperature is 160;

[0090] Further, in the heat preservation step, the heat preservation time is 270s to 330s; further, the heat preservation time is 280s to 320s; further, the heat preservation time is 290s to 310s; further, the heat preservation time is 292s to 308s;

[0091] Further, in the heat preservation step, the pressure is reduced to 10 bar to 40 bar, and the temperature is controlled at 150°C to 180°C for 270s to 330s; further, in the heat preservation step, the pressure is reduced to 15 bar to 30 bar, and the temperature is controlled at 150°C to 170°C for 270s to 330s. Further, in the heat preservation step, the pressure is reduced to 15 bar to 21 bar, and the temperature is controlled at 150°C to 160°C for 300s to 320s.

[0092] Further, in the cooling step, the temperature is lowered to 5°C to 50°C within 65 seconds; further, in the cooling step, the temperature is lowered to 5°C to 50°C within 60 seconds; further, in the cooling step, the temperature is lowered to 5°C to 40°C within 60 seconds. Further, in the cooling step, the temperature is lowered to 10°C to 30°C within 60 seconds.

[0093] Further, in the cooling step, the cooling rate is 120 degrees / min to 140 degrees / min; further, the cooling rate is 122 degrees / min to 138 degrees / min; further, the cooling rate is 123 degrees / min to 137 degrees / min; further, the cooling rate is 124 degrees / min to 136 degrees / min; further, the cooling rate is 125 degrees / min to 135 degrees / min;

[0094] Furthermore, in the heating step, the heating rate is 50 degrees / min to 51 degrees / min; in the insulation step, the pressure is 15 bar to 21 bar, the temperature is 154°C to 160°C, and the time is 300s to 312s; in the cooling step, the cooling rate is 125 degrees / min to 135 degrees / min.

[0095] The preparation method of the above sol can form a monodisperse sol through the rapid crystallization technology directly synthesized in liquid, so that the surface of the sol is stabilized by the double electric layer without the need for a surfactant. In this way, after the above sol is coated on the surface of the object, the evaporation of water will cause the double electric layer to disappear, and the first contact between the particles will occur. Because the carrier nanoparticles are less than 10nm, they have a very strong surface effect, and there are a large number of active-broken chemical bonds on the surface, so chemical bridging will occur between the particles to form an inorganic mineral film, and the whole process does not require a film-forming substance, so it will not wrap the active substance and affect the performance (such as Figure 1 (shown in a).

[0096] The present invention also provides an antimicrobial and antiviral powder, comprising the above-mentioned super-atom material.

[0097] The present invention also provides a method for preparing the antimicrobial and antiviral powder, comprising the following steps: drying and grinding the sol to obtain the antimicrobial and antiviral powder. The method for preparing the sol is as described in S101 to S102 or S201 to S203, which will not be described in detail here.

[0098] Furthermore, the method for preparing the antimicrobial and antiviral powder comprises the following steps:

[0099] S301: mixing a metal salt, a carrier precursor and water to obtain a mixed solution;

[0100] The carrier precursor is an inorganic acid which can generate an inorganic carrier through hydrothermal treatment.

[0101] Step S301 is the same as step S101 except that there is no complexing agent in the mixed liquid system, and will not be described again here.

[0102] S302: Treat the mixed solution by the following method to obtain a suspension:

[0103] Heating: raise the temperature of the mixed liquid to 120°C to 250°C and the pressure to 15 bar to 60 bar within 200 seconds;

[0104] Keep warm: reduce the pressure to 10 bar to 40 bar and control the temperature at 130°C to 200°C for 270s to 330s;

[0105] Cool down and reduce the temperature to 5℃~50℃ within 60s.

[0106] Step S302 is the same as step S102 and will not be described again here.

[0107] S303: Drying the suspension to obtain.

[0108] Existing methods can be used for drying, such as vacuum drying, spray drying or freeze drying, which can be selected according to actual needs.

[0109] The present invention also provides an antimicrobial and antiviral coating, comprising the above-mentioned super-atom material, wherein the super-atom material is as described above and will not be described in detail here.

[0110] The present invention also provides another antimicrobial and antiviral coating, which is mainly prepared from the above sol or the sol prepared by the above preparation method.

[0111] It is understandable that the above sol can be applied to the target area and then dried. Since the above sol has excellent adhesion and the super-atom material can form a regularly arranged mesh structure after coating, the use of adhesives and other reagents can be avoided, effectively improving the antimicrobial and antiviral properties of the antimicrobial and antiviral coating.

[0112] The application fields of the above antimicrobial and antiviral coatings are not particularly limited, for example, they can be applied on indoor wall decoration, glass, fibers, etc.

[0113] The present invention also provides the use of the above-mentioned super-atom material, sol, and the sol prepared by the above-mentioned preparation method in the preparation of daily necessities, coatings or sealants. Since the above-mentioned super-atom material has excellent antimicrobial and antiviral properties and is not easy to migrate into the environment, it has high safety and environmental protection effects and is suitable for use in daily necessities, cosmetics, coatings or sealants.

[0114] The present invention also provides antimicrobial and antiviral products, including a substrate and a superatomic material loaded on the substrate, the superatomic material is the above-mentioned superatomic material or a superatomic material prepared from a sol, and the sol is the above-mentioned sol or a sol prepared by the above-mentioned preparation method.

[0115] Furthermore, the matrix is ​​a zeolite, a molecular sieve, an inorganic oxide or a fiber with a particle size of 0.1-2 μm, a molecular sieve of 0.1-2 μm, an inorganic oxide of 0.1-2 μm, or a hollow fiber.

[0116] It should be noted that the preparation method of the above antimicrobial and antiviral products is not particularly limited, and the substrate can be immersed in a solution or sol containing the superatom material and then dried.

[0117] Specific embodiments are listed below to illustrate the present invention.

[0118] Example 1

[0119] (1) adding 2 g of silver acetate to 500 ml of water and stirring, heating to 40° C. and stirring for about 1 hour to fully dissolve, then cooling to room temperature and filtering to obtain a first solution;

[0120] (2) taking 5 kg (2% wt) of an aqueous solution of an orthotitanic acid complex (citric acid), diluting it to 10 kg (1% wt) with water to obtain a second solution;

[0121] (3) dropping the first solution into the second solution at a rate of 150 ml / min and stirring thoroughly to obtain a mixed solution;

[0122] (4) The mixed solution was treated in the following manner using a nano supercritical segmented programmable hydrothermal reactor with an avalanche cooling module (commercial model NanoHydrosynthesis SH5UC): the pressure was increased to 20 bar (heating rate 50.6°C / min), the maximum temperature was 162°C, after reaching the maximum temperature, the pressure was reduced to 15 bar and the temperature was maintained at 160°C for 300 seconds, then the pressure was increased to 12 bar to enter the avalanche cooling program and the solution temperature was reduced to 30°C within 60 seconds (programmed cooling rate 130 degrees / min) to obtain the desired nano titanium dioxide doped silver superatomic sol.

[0123] Example 2

[0124] (1) adding 2 g of silver sulfate to 500 ml of water and stirring, heating to 40° C. and stirring for about 1 hour to fully dissolve, then cooling to room temperature and filtering to obtain a first solution;

[0125] (2) taking 5 kg (2% wt) of an aqueous solution of peroxytitanic acid, diluting it to 10 kg (1% wt) with water to obtain a second solution;

[0126] (3) dropping the first solution into the second solution at a rate of 150 ml / min and stirring thoroughly to obtain a mixed solution;

[0127] (4) Add 0.05 ml of ammonia water (30%) to the mixture;

[0128] (5) The mixed solution was treated in the following manner using a nano supercritical segmented programmable hydrothermal reactor with an avalanche cooling module (commercial model NanoHydrosynthesis SH5UC): the pressure was increased to 20 bar (heating rate 50.6 °C / min), the maximum temperature was 162 °C, and the maximum temperature was reached after about 192 seconds. The pressure was then reduced to 15 bar and the temperature was maintained at 160 °C for 300 seconds. The pressure was then increased to 12 bar to enter the avalanche cooling program and the solution temperature was reduced to 30 °C within 60 seconds (programmed cooling rate 130 °C / min) to obtain the desired Ag / N / TiO2 composite doped sol.

[0129] Example 3

[0130] (1) adding 2 g of silver nitrate to 500 ml of water and stirring, heating to 40° C. and stirring for about 1 hour to fully dissolve, then cooling to room temperature and filtering to obtain a first solution;

[0131] (2) taking 5 kg (2% wt) of an aqueous solution of peroxytitanic acid, diluting it to 10 kg (1% wt) with water to obtain a second solution;

[0132] (3) dropping the first solution into the second solution at a rate of 150 ml / min and stirring thoroughly to obtain a mixed solution;

[0133] (4) Add 0.05 ml of ammonia water (30%) to the mixture;

[0134] (5) The mixed solution was treated in the following manner using a nano supercritical segmented programmable hydrothermal reactor with an avalanche cooling module (commercial model NanoHydrosynthesis SH5UC): the pressure was increased to 20 bar (heating rate 50.8 degrees / min), the maximum temperature was 165°C, after reaching the maximum temperature, the pressure was reduced to 15 bar and the temperature was maintained at 160 degrees for 308 seconds, and then the pressure was increased to 12 bar to enter the avalanche cooling program to reduce the solution temperature to 30°C within 60 seconds (programmed cooling rate 130°C / min) to obtain the desired Ag / N / TiO2 composite doped sol.

[0135] Example 4

[0136] (1) adding 2 g of silver nitrate to 500 ml of water and stirring, heating to 40° C. and stirring for about 1 hour to fully dissolve, then cooling to room temperature and filtering to obtain a first solution;

[0137] (2) taking 5 kg (2% wt) of an aqueous solution of peroxytitanic acid, diluting it to 10 kg (1% wt) with water to obtain a second solution;

[0138] (3) dropping the first solution into the second solution at a rate of 150 ml / min and stirring thoroughly to obtain a mixed solution;

[0139] (4) Add 0.05 ml of ammonia water (30%) to the mixture;

[0140] (5) The mixed solution was treated in the following manner using a nano supercritical segmented programmable hydrothermal reactor with an avalanche cooling module (commercial model NanoHydrosynthesis SH5UC): the pressure was increased to 20 bar (heating rate 50.6 degrees / min), the maximum temperature was 162°C, after reaching the maximum temperature, the pressure was reduced to 15 bar and the temperature was maintained at 160°C for 300 seconds, and then the pressure was increased to 12 bar to enter the avalanche cooling program to reduce the solution temperature to 30°C within 60 seconds (programmed cooling rate 132°C / min) to obtain the desired Ag / N / TiO2 composite doped sol.

[0141] Example 5

[0142] (1) adding 2 g of silver acetate to 500 ml of water and stirring, heating to 40° C. and stirring for about 1 hour to fully dissolve, then cooling to room temperature and filtering to obtain a first solution;

[0143] (2) taking 5 kg (2% wt) of an aqueous solution of peroxytitanic acid, diluting it to 10 kg (1% wt) with water to obtain a second solution;

[0144] (3) dropping the first solution into the second solution at a rate of 150 ml / min and stirring thoroughly to obtain a mixed solution;

[0145] (4) Take 10 g of tetramethoxysilane and slowly drop it into the above mixed solution and stir for 30 minutes.

[0146] (5) The mixed solution was treated in the following manner using a nano supercritical segmented programmable hydrothermal reactor with an avalanche cooling module (commercial model NanoHydrosynthesis SH5UC): the pressure was increased to 20 bar (heating rate 50.6°C / min), the maximum temperature was 162°C, and the maximum temperature was reached after about 192 seconds. The pressure was then reduced to 15 bar and the temperature was maintained at 160°C for 300 seconds. The pressure was then increased to 12 bar to enter the avalanche cooling program and the solution temperature was reduced to 30°C within 60 seconds (programmed cooling rate 130°C / min) to obtain the desired silicon surface modified nano titanium dioxide doped silver superatomic sol.

[0147] Example 6

[0148] (1) adding 2 g of copper sulfate to 500 ml of water and stirring, heating to 40° C. and stirring for about 1 hour to fully dissolve, then cooling to room temperature and filtering to obtain a first solution;

[0149] (2) taking 5 kg (2% wt) of an aqueous solution of an orthotitanic acid complex (citric acid), diluting it to 10 kg (1% wt) with water to obtain a second solution;

[0150] (3) dropping the first solution into the second solution at a rate of 150 ml / min and stirring thoroughly to obtain a mixed solution;

[0151] (4) The mixed solution was treated in the following manner using a nano supercritical segmented programmable hydrothermal reactor with an avalanche cooling module (commercial model NanoHydrosynthesis SH5UC): the pressure was increased to 20 bar (heating rate 50.6 degrees / min), the maximum temperature was 162°C, and the maximum temperature was reached after about 192 seconds. The pressure was then reduced to 15 bar and the temperature was maintained at 160°C for 300 seconds. The pressure was then increased to 12 bar to enter the avalanche cooling program and the solution temperature was reduced to 30°C within 60 seconds (programmed cooling rate 130°C / min) to obtain the desired nano titanium dioxide doped copper superatomic sol.

[0152] Example 7

[0153] (1) adding 2 g of zinc nitrate to 500 ml of water and stirring, heating to 40° C. and stirring for about 1 hour to fully dissolve, then cooling to room temperature and filtering to obtain a first solution;

[0154] (2) taking 5 kg (2% wt) of an aqueous solution of orthotitanate complex (malic acid), diluting it to 10 kg (1% wt) with water to obtain a second solution;

[0155] (3) dropping the first solution into the second solution at a rate of 150 ml / min and stirring thoroughly to obtain a mixed solution;

[0156] (4) Add 0.05 ml of triethylamine to the mixed solution;

[0157] (5) The mixed solution was treated in the following manner using a nano supercritical segmented programmable hydrothermal reactor with an avalanche cooling module (commercial model NanoHydrosynthesis SH5UC): the pressure was increased to 20 bar (heating rate 50.6 °C / min), the maximum temperature was 162 °C, and the maximum temperature was reached after about 192 seconds. The pressure was then reduced to 15 bar and the temperature was maintained at 160 °C for 300 seconds. The pressure was then increased to 12 bar to enter the avalanche cooling program and the solution temperature was reduced to 30 °C within 60 seconds (programmed cooling rate 130 °C / min) to obtain the desired Zn / N / TiO2 composite doped sol.

[0158] Effect verification experiment

[0159] 1. Experiment to verify the existence of superatoms

[0160] A.XPS research

[0161] (1) XPS study of the Ag / N / TiO2 composite doped sol of Example 2, its XPS spectrum is as follows Figure 2 As shown, the specific data is as follows Table 1:

[0162] Table 1

[0163] sample track Peak position Peak area Silver superatom sample Ag 3d5 / 2 368.000 857 Ag 3d3 / 2 373.950 590 Silver Ag 3d5 / 2 368 Ag 3d3 / 2 374

[0164] Among them, the silver element data sample comes from the PE company Handbook of X-ray Photoelectron Spectroscopy. By comparison, it can be seen that the silver superatom has the same valence state as the silver element, proving that the superatom does not exist in an ionic state.

[0165] (2) XPS study of the nano-titanium dioxide doped copper superatom sol of Example 6, the spectrum is as follows Figure 3 As shown, the specific data is as follows Table 2:

[0166] Table 2

[0167] sample track Peak position Peak area Copper superatom sample Cu2p(1) 932.870 1850 Cu2p(2) 952.893 2440 Copper Cu2p(1) 933 Cu2p(2) 953

[0168] Among them, the silver element data sample comes from the PE company Handbook of X-ray Photoelectron Spectroscopy. By comparison, it can be seen that the copper superatom has the same valence state as the silver element, proving that the superatom does not exist in an ionic state.

[0169] B. Ultrafiltration and nanofiltration experiments:

[0170] Experimental method and principle: The Ag / N / TiO2 composite doped sol of Example 2 was subjected to ultrafiltration (cross-flow filtration) with an interception pore of 10-200 nm. The separated permeate was subjected to ICP-AES and ICP-MS analysis, and no silver and titanium elements were detected. Because ultrafiltration can intercept nano-titanium oxide carriers, silver superatoms are loaded on the carrier and therefore cannot pass through the ultrafiltration membrane. If silver ions, free silver superatoms or complex ultra-small nano-silver exist, silver elements can be detected in the permeate through ultrafiltration.

[0171] C. (High resolution) electron microscopy EDX research

[0172] The Ag / N / TiO2 composite doped sols of Examples 2 to 5 were tested using a (high resolution) electron microscope. The test spectrum of Example 2 is as follows: Figure 4-Figure 6 As shown, the test spectrum of Example 4 is as follows Figure 7 As shown, the test spectrum of Example 5 is as follows Figure 8 As shown (Example 3 is basically the same as Example 2, so it is not shown);

[0173] from Figure 4 It can be seen that Ti and O elements are evenly distributed to form a TiO2 carrier, and Ag elements are formed on the surface of the TiO2 carrier in the form of atomic clusters and embedded; Figure 5 It can be seen that Ag superatoms (clusters) are formed and embedded on the surface of the TiO2 carrier in the form of atomic clusters, and their size is about 1000-2000pm (1-2nm); Figure 6 It can be seen that Ti and O elements are evenly distributed to form a TiO2 carrier, N element is evenly distributed in the TiO2 structure to form a doping structure, Ag element is formed on the surface of the TiO2 carrier in the form of atomic clusters and embedded, Ag superatoms (clusters) are formed on the surface of the TiO2 carrier in the form of atomic clusters and embedded, and their size is approximately between 1000-2000pm (1-2nm).

[0174] Figure 7 A represents the distribution of Ti, B represents the distribution of O, C represents the distribution of Ag, D represents the spectrum analysis of a random 2nm range, and E represents its XPS spectrum. Figure 8 It can be seen that in the crystal transmission electron microscopy EESL mapping of Example 4, the Ti and O elements are evenly distributed to form a TiO2 carrier, the Ag element is formed in the form of smaller atomic clusters and embedded on the surface of the TiO2 carrier, and the Ag superatom (cluster) is formed in the form of atomic clusters and embedded on the surface of the TiO2 carrier, and its size is about 100-500pm (0.1-0.5nm). EELS spectrum analysis can find that there is an obvious silver signal in the 2×2nm random area. According to the XPS conclusion, silver belongs to a single substance. Based on this, silver exists here in an atomic cluster smaller than the system resolution. According to the EELS surface scanning data, the Ag signal is basically a group of 1×1-2×2 pixels with a scattered distribution, and the scale size is 5 pixels = 2nm. Based on this, it is estimated that its size is 0.4-0.8nm (400-800pm), and the maximum does not exceed 3×3 pixels. It is estimated that the super atom is 1.2nm (1200pm);

[0175] from Figure 8It can be seen that the Ti and O elements are evenly distributed to form a TiO2 carrier, and the TiO2 lattice fringes formed can be clearly seen. In this case, the Ag element is formed and embedded on the surface of the TiO2 carrier in the form of smaller atomic clusters. It can be seen that Ag superatoms (clusters) are formed and embedded on the surface of the TiO2 carrier in the form of atomic clusters, and their size is about 100-500pm (0.1-0.5nm).

[0176] D. (High resolution) electron microscope high angle annular dark field imaging study

[0177] The nano-titanium dioxide doped copper superatomic sol of Example 6 was subjected to (high resolution) electron microscope high-angle annular dark field imaging study (in the high-angle annular dark field image, the heavier the element, the brighter the color, so it can be used to distinguish the TiO2 carrier and the Cu atomic cluster), and the test spectrum is as follows Fig. 9 As shown;

[0178] from Fig. 9 It can be seen that copper atom clusters (highlight spots) with a size of 0.5-2 nm are doped into the TiO2 carrier.

[0179] 2. Antimicrobial and antiviral performance testing experiments

[0180] A. Study on the infection titer of yellow leaf disease virus

[0181] The antibacterial properties of the Ag / N / TiO2 composite doped sol (i.e., silver superatom interstitial nitrogen doped titanium oxide) of Example 2 and the Zn / N / TiO2 composite doped sol (i.e., zinc superatom interstitial nitrogen doped titanium oxide) of Example 7 were tested under different light intensities. The test results are as follows: Fig.10 As shown, the virus infection titer after 15 minutes is shown in Table 3, and the virus reduction performance value (log) / % after 15 minutes is shown in Table 4;

[0182] Among them, the interstitial nitrogen-doped titanium oxide manufacturer is Green Earth Nano Science in Canada;

[0183] Nanosilver (20nm) is synthesized by a patented strain (CTCCM2012524). The main process is: culture the strain in PDA medium, collect the mycelium, add deionized water at 10mL / g, place at 37℃ for 24h, filter to remove the mycelium, filter the filtrate through a 0.22μm filter membrane, add 1μg / mL silver nitrate, and react at 37℃ for 48h. Wash the synthesized nanosilver with deionized water three times, centrifuge at 12000r / min, 30min.

[0184] Table 3. Virus infection titer after 15 minutes

[0185] Light intensity 30000 LUX 1200 LUX 300 LUX No light Interstitial nitrogen-doped titanium oxide 3.5 7.0 7.0 6.9 <![CDATA[Ag / N / TiO2 composite doped sol]]> 0 3.1 3.8 6.5 <![CDATA[Zn / N / TiO2 composite doped sol]]> 0.5 5.1 6.1 6.9 Nanosilver (20NM) 6.4 7.2 7.0 6.9

[0186] Table 4. Virus reduction performance value (log) / % after 15 minutes (compared with nanosilver)

[0187]

[0188] It can be seen from Tables 3 and 4 above that the antiviral effect of the superatom material of the present invention, i.e., superatom-doped titanium oxide, is significantly better than that of a single carrier (interstitial nitrogen-doped titanium oxide) or a single nanosilver, and the silver superatom interstitial nitrogen-doped titanium oxide (i.e., Ag / N / TiO2 composite-doped sol) still has certain bactericidal properties under conditions without light.

[0189] B. Study on the antibacterial activity of silver superatom titanium oxide against bacteria

[0190] The antibacterial activity of the nano-titanium dioxide doped silver superatom sol of Example 1 against different bacterial species is shown in Table 5:

[0191] Table 5

[0192]

[0193]

[0194] #The strain still did not grow at the lowest test concentration, but grew well in the control sample

[0195] As can be seen from Table 5, the compound has excellent antibacterial effect on various bacterial species, and the antibacterial concentration is low, which is both effective and safe.

[0196] C. Study on the antibacterial activity of silver superatomic titanium oxide coating on stainless steel (method JIS2801)

[0197] The sols of the test sample and the control sample were respectively coated on stainless steel to form a coating, and the antibacterial activity against bacteria was detected. The test results are shown in Table 6, wherein the test sample is the nano-titanium dioxide doped silver superatom sol of Example 1, and the blank sample is stainless steel without sol coating;

[0198] Table 6

[0199]

[0200]

[0201] #All bacteria in the test sample were killed below the detection limit.

[0202] It can be seen from Table 6 that the coating formed by the sol of Example 1 has a good antibacterial effect on various bacterial species, which is significantly better than the blank stainless steel without antibacterial coating, and the antibacterial concentration is low, which has both effectiveness and safety.

[0203] D. Study on the antibacterial activity of silver superatom titanium oxide coating on textiles (method ISO20743)

[0204] The nano-titanium dioxide doped silver superatom sol of Example 1 was applied on textiles to form a coating, and its antibacterial activity against bacteria was tested. The test results are shown in Table 7;

[0205] Table 7

[0206]

[0207]

[0208] It can be seen from Table 7 that the coating formed by the nano-titanium dioxide doped silver superatom sol of Example 1 has a relatively good antibacterial effect on various bacterial species.

[0209] E. Study on the antiviral activity of silver superatomic titanium oxide coating on glass (method ISO21702)

[0210] The sols of the test sample and the control sample were coated on glass to form a coating, and their antiviral activity against bacteria was tested. The test results are shown in Table 8, wherein the control sample was a commercially available silver ion superatom material (Fujifilm, Japan), and the test sample was the nano-titanium dioxide-doped silver superatom sol of Example 1.

[0211] Table 8

[0212]

[0213] It can be seen from Table 8 that the antiviral activity of the nano-titanium dioxide doped silver superatom sol of Example 1 is significantly better than that of the control sample.

[0214] F. Study on the antiviral activity of copper superatom titanium oxide coating on glass (method ISO21702)

[0215] The nano-titanium dioxide doped copper superatom sol of Example 6 was applied on textiles to form a coating. The coating was measured twice each time and the average value was recorded to detect its antiviral activity against viruses. The test results are shown in Table 9.

[0216] Table 9

[0217]

[0218]

[0219] It can be seen from Table 9 that the coating formed by the nano-titanium dioxide doped copper superatom sol of Example 6 has a relatively good antiviral effect on various viruses.

[0220] G. Study on the antibacterial activity of copper superatom titanium oxide coating on glass (method ISO22196)

[0221] The nano-titanium dioxide doped copper super-atom sol of Example 6 was applied on textiles to form a coating, and its antibacterial activity against bacteria was tested. The test results are shown in Table 10;

[0222] Table 10

[0223]

[0224] It can be seen from Table 10 that the coating formed by the nano-titanium dioxide doped copper superatom sol of Example 6 has a relatively good antibacterial effect on various bacterial species.

[0225] H. Silver superatomic titanium oxide liquid state directly mixed with virus for 60 minutes (method EN14476)

[0226] The antiviral ability of the nano-titanium dioxide doped silver superatom sol of Example 1 was tested, and the test results are shown in Tables 11 and 12:

[0227] Table 11

[0228]

[0229] Table 12

[0230]

[0231] It can be seen from Tables 11 and 12 that the nano-titanium dioxide doped silver superatom sol of Example 1 has a better antiviral effect.

[0232] 3. Monodispersity study

[0233] The DLS / PCS (molecular correlation spectroscopy) of the sol of Example 1 is as follows: Fig.11 As shown, from Fig.11 It can be seen that the DLS / PCS (molecular correlation spectroscopy) results show that the average kinetic diameter (secondary particle size) of the particles in the sol is 7.838nm; the XRD results are as follows Fig.12 As shown, from Fig.12 It can be seen that the XRD results show that the crystal grain size (primary particle size) is 5.4 nm according to the Scherrer formula, and the main crystal plane size is 5.8 / 6.9 / 5.7 nm. Based on this, the agglomeration index is 7.838 / 5.4=1.45<2, which is close to a monodisperse state.

[0234] 4. Surface charge study

[0235] The surface potential of the sol of Example 1 is detected as follows Fig.13 As shown, from Fig.13 It can be seen that the absolute value of the surface charge of the super-atom material in the nano-titanium dioxide-doped silver super-atom sol of Example 1 is greater than or equal to 15 mV, which can effectively avoid agglomeration and enhance dispersibility.

[0236] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0237] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A superatomic material, characterized in that: The invention comprises a carrier and a super atom doped in the carrier, wherein the super atom is one or more of silver, copper and zinc super atoms, and the scale of the super atom is 100 pm to 2500 pm; the carrier is anatase titanium dioxide nanocrystal; and the particle size of the carrier is 1 nm to 10 nm; The two-dimensional projection shape of the carrier is a quadrilateral, a spindle or a circle; The carrier surface carries an electric charge, and the absolute value of the electric charge is greater than or equal to 15 mV.

2. The superatomic material according to claim 1, characterized in that: The chemical valence state of the superatom is 0.

3. The superatomic material according to claim 1, characterized in that: The carrier is nitrogen interstitially doped titanium oxide.

4. The superatomic material according to claim 1, characterized in that: The superatom is a silver superatom, and the XPS spectrum of the superatom material has peaks at 368.000±0.200 and 374.000±0.200; or The super atom is a copper super atom, and the XPS spectrum of the super atom material has peaks at 933±0.200 and 953±0.

200.

5. The superatomic material according to claim 1, characterized in that: The carrier surface has a negative charge.

6. A sol, characterized in that: The super-atomic material comprises the super-atomic material according to any one of claims 1 to 5.

7. The sol according to claim 6, characterized in that The ratio of the DLS average particle size to the XRD average particle size of the super-atom material is less than 4.

8. A method for preparing a sol, characterized in that: The following steps are involved: mixing a metal salt, a carrier precursor and water to obtain a mixed solution; The mixed solution is treated by the following method to obtain a sol: Heating: raising the temperature of the mixed solution to 120° C. to 250° C. and the pressure to 15 bar to 60 bar within 200 seconds; Keep warm: reduce the pressure to 10 bar to 40 bar and control the temperature at 130°C to 200°C for 270s to 330s; Cooling: lower the temperature to 5℃~50℃ within 65s; Wherein, the metal salt is an organic or inorganic salt containing silver, copper or zinc; The carrier precursor contains at least one of a peroxotitanic acid complex and an orthotitanic acid complex.

9. The preparation method according to claim 8, characterized in that: In the temperature raising step, the temperature of the mixed solution is raised to 150° C. to 200° C. and the pressure is raised to 15 bar to 60 bar within 200 seconds; In the heat preservation step, the pressure is reduced to 10 bar to 40 bar, and the temperature is controlled at 150° C. to 180° C. for 270 seconds to 330 seconds; In the cooling step, the temperature is lowered to 5°C to 50°C within 60s.

10. The preparation method according to claim 9, characterized in that: In the heating step, the heating rate is 50°C / min to 51°C / min; and / or In the insulation step, the pressure is 15 bar to 21 bar, the temperature is 154° C. to 160° C., and the time is 300 s to 312 s; and / or In the cooling step, the cooling rate is 125°C / min to 135°C / min.

11. The preparation method according to any one of claims 8 to 10, characterized in that: The step of mixing the metal salt, the carrier precursor and water to obtain a mixed solution comprises the following steps: mixing a metal salt and water to obtain a first solution; mixing the support precursor with water to obtain a second solution; The first solution is dropped into the second solution at a speed of 100 mL / min to 200 mL / min, and stirred to obtain a mixed solution.

12. The preparation method according to claim 11, characterized in that: The metal salt is selected from: one or more of silver acetate, silver nitrate, silver sulfate, copper nitrate, zinc nitrate, zinc sulfate and copper sulfate; and / or In the first solution, the concentration of the metal element is 10ppm-1000ppm; and / or In the second solution, the concentration of the carrier precursor is 1%-30%.

13. The preparation method according to any one of claims 8 to 10, characterized in that: The step of mixing the metal salt, the carrier precursor and water further comprises the step of adding a silicon-based substance; and / or The step of mixing the metal salt, the carrier precursor and water further includes the step of adding ammonia water, triethylamine or ammonium salt.

14. An antimicrobial and antiviral coating, characterized in that: The super-atomic material comprises the super-atomic material according to any one of claims 1 to 5.

15. An antimicrobial and antiviral coating, characterized in that: The sol is mainly prepared by the sol described in any one of claims 6 to 7, or the sol prepared by the preparation method described in any one of claims 8 to 13.

16. Use of the superatomic material according to any one of claims 1 to 5, the sol according to any one of claims 6 to 7, or the sol prepared by the preparation method according to any one of claims 8 to 13 in the preparation of daily necessities, cosmetics, coatings or sealants.

17. An antimicrobial and antiviral product, characterized in that: It includes a substrate and a super-atomic material loaded on the substrate, wherein the super-atomic material is the super-atomic material described in any one of claims 1-5 or a super-atomic material prepared from a sol, and the sol is the sol described in any one of claims 6-7 or a sol prepared by the preparation method described in any one of claims 8-13.

18. The antimicrobial and antiviral product according to claim 17, characterized in that: The matrix is ​​a zeolite with a particle size of 0.1-2 μm, a molecular sieve with a particle size of 0.1-2 μm, an inorganic oxide with a particle size of 0.1-2 μm, or a hollow fiber.