Edge-corner-strengthened r-t-b rare earth permanent magnet and manufacturing method therefor

By coating diffusion sources of Zr, Ti, and Nb elements in the corner areas of NdFeB magnets and coating heavy rare earth element diffusion sources in non-corner areas, grain boundary diffusion technology is used to solve the problem of transportation and assembly of NdFeB magnets. The problem of missing edges and corners during the process improves the mechanical properties and coercive force of the edges and corners, and reduces the rate of missing edges and corners.

WO2024216705A1PCT designated stage expired Publication Date: 2024-10-24ZHEJIANG INNUOVO MAGNETICS

Patent Information

Application Number
PCT/CN2023/096223
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-21
Filing Date
2023-05-25
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

NdFeB magnets are prone to missing edges and corners during transportation and assembly, resulting in reduced product quality.

Method used

By coating the corner areas of the magnet with a diffusion source containing Zr, Ti, and Nb elements, and coating the non-corner areas with a heavy rare earth element diffusion source that does not contain these elements, grain boundary diffusion technology is used to strengthen the corner areas of the magnet. Mechanical properties, repair micro-cracks caused by machining, and improve the impact resistance of corners.

Benefits of technology

Significantly reduces the rate of missing edges and corners of magnets during transportation and assembly, improves the mechanical properties of NdFeB magnets, enhances the strength and coercive force of edges and corners, and improves the product qualification rate without affecting the quality of the magnets. Residual magnetic properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023096223_24102024_PF_FP_ABST
    Figure CN2023096223_24102024_PF_FP_ABST
Patent Text Reader

Abstract

Disclosed in the present invention are an edge-corner-strengthened R-T-B rare earth permanent magnet and a manufacturing method therefor. A magnet diffusion source coating surface is divided into an edge-corner area and a non-edge-corner area. The edge-corner area of a magnet is coated with a diffusion source containing a Zr, Ti or Nb element, while the non-edge-corner area of the magnet is coated with a diffusion source containing a heavy rare earth element other than said element. In a grain boundary diffusion process, the Zr, Ti or Nb element is diffused into the grain boundary R-rich phase of the magnet, and the grain boundary R-rich phase of the magnet is strengthened by means of a solid solution or generation of a second-phase precipitate, thereby improving the strength of the edges and corners of the magnet. The present invention improves the mechanical properties of the edge-corner area of the magnet by means of partition grain boundary diffusion without affecting the non-edge-corner area of the magnet, can remarkably reduce the edge missing and corner loss rate of the magnet in a transportation and assembly process without reducing the magnetic performance of the magnet, and has important significance for reducing the costs of a neodymium-ferrum-boron product.
Need to check novelty before this filing date? Find Prior Art

Description

A corner-reinforced RTB rare earth permanent magnet and its preparation method Technical Field

[0001] The invention relates to an edge-reinforced RTB rare earth permanent magnet and a preparation method thereof, belonging to the field of rare earth magnets. Background Art

[0002] Grain boundary diffusion is a new technology developed in recent years. It can significantly improve the coercive force of RTB rare earth permanent magnets while ensuring that the magnets have high remanence. It is a commonly used method for preparing high-performance RTB rare earth permanent magnets.

[0003] Grain boundary diffusion (GBD) treatment begins by coating the magnet surface with a diffusion source layer containing heavy rare earth elements. The magnet is then heated to a specified temperature and held there for a period of time. During this high-temperature period, the heavy rare earth elements in the diffusion source on the magnet surface diffuse into the magnet along the R-rich phase at the grain boundaries, forming a shell with a high anisotropy field on the surface of the magnet's main phase grains. Furthermore, the GBD process allows additional rare earth elements to infiltrate the magnet, increasing the magnet's total rare earth content and making the R-rich phase at the grain boundaries between the main phase grains more continuous, thereby achieving de-exchange coupling between the main phase grains. Therefore, GBD improves the magnet's coercivity by increasing the surface anisotropy field of the main phase grains and optimizing the distribution of the R-rich phase at the grain boundaries.

[0004] While RTB rare earth permanent magnets possess high magnetic properties, they are also quite brittle due to the material's intrinsic properties. During machining, stress from machining can cause numerous microcracks in the corners of the magnets. During subsequent transportation and assembly, even minor bumps can cause cracks in the corners, resulting in chipping and chipping.

[0005] Adding a certain amount of high-melting-point metallic elements like Zr, Ti, and Nb to a magnet can strengthen the magnet's grain boundary R-rich phase through solid solution or the formation of a secondary precipitate, thereby improving the magnet's mechanical properties. However, as the content of non-magnetic elements increases, the magnet's remanence decreases. Furthermore, during transportation and assembly, NdFeB magnets are prone to defects at their corners due to collisions, while other parts of the magnet rarely experience collision defects. This means that by ensuring that certain elements like Zr, Ti, and Nb are present in the corners of the magnet without affecting other areas of the magnet, the qualified rate of NdFeB magnets can be improved without affecting the magnet's magnetic properties. Technical issues

[0006] In view of the fact that NdFeB magnets are prone to edge and corner chipping during transportation and assembly, the present invention provides an RTB rare earth permanent magnet with reinforced edges and corners and a preparation method thereof. Technical Solutions

[0007] The technical solution adopted in the present invention is as follows:

[0008] A corner-reinforced RTB rare earth permanent magnet, comprising the following components in mass fractions:

[0009] R: 28.5~34.0wt.%, R consists of RL and RH, the RH content is 0.1wt.%~10.0wt.% of the magnet mass, RH is at least one of Dy, Tb, and Ho; the balance of R is RL, RL represents one or more elements selected from Nd, Pr, La, Ce, Er, Gd, Sm, Tm, Lu, and Y, containing at least light rare earth elements; the light rare earth elements are one or more of La, Ce, Pr, and Nd;

[0010] B: 0.85~1.1wt.%,

[0011] M: 0.01-8.0 wt.%, M represents a plurality of elements selected from Al, Cu, Ga, Ni, Zn, Sn, Mn, Cr, Zr, Ti, and Nb, containing at least M and X, X being one or more of Zr, Ti, and Nb; M being one or more of Al, Ga, and Cu;

[0012] The balance is T and other unavoidable impurities, T is Fe or Fe and Co;

[0013] The magnet has at least one surface A, and the light rare earth element content in the corner area of ​​the surface A is not lower than the average light rare earth content of the surface A; the light rare earth element is one or more of La, Ce, Pr, and Nd; and the corner area of ​​the surface A contains X, and X is one or more of Zr, Ti, and Nb.

[0014] Furthermore, the surface A is a coating surface of the magnet coated with a diffusion source.

[0015] Furthermore, preferably, in the RH, RH accounting for 0.05-2.5 wt.% of the mass of the magnet is obtained by grain boundary diffusion.

[0016] The M or X in the magnet can be obtained entirely or partially through grain boundary diffusion.

[0017] Preferably, in the magnet, more than 70% of RL is Nd;

[0018] Preferably, in the magnet, X is Zr;

[0019] Preferably, in the magnet, M is Ga and Cu.

[0020] Furthermore, within a depth range of 0.6 mm perpendicularly to the surface A of the magnet, the X content in the corner body region is 0.05-1.2 wt.%.

[0021] The average X content of the magnet is 0.05-0.8 wt.%.

[0022] The corner area refers to the surface area within the width range of 0~Kmm from the edge line, K is the width of the corner area, and the range of K is 0.2~0.6. The non-corner area refers to the surface area outside the width range of Kmm from the edge line.

[0023] The corner body region is a body region enclosed by the corner area and a depth of 0.6 mm perpendicular to the surface A. The non-corner body region is a magnetic region outside the corner body region.

[0024] The non-corner body region of the magnet does not contain X, or the X content in the non-corner body region is lower than the X content in the corner body region of the magnet.

[0025] The edge-reinforced RTB rare earth permanent magnet is preferably prepared according to the following method:

[0026] (1) Setting an H1 diffusion source coating area and an H2 diffusion source coating area on the diffusion surface of the RTB magnet substrate, and coating the diffusion sources in different areas. The H1 diffusion source coating area is coated with the diffusion source H1, and the H2 diffusion source coating area is coated with the diffusion source H2; the H1 diffusion source coating area is the corner area of ​​the diffusion surface, and the H2 diffusion source coating area is the non-corner area of ​​the diffusion surface;

[0027] The corner area refers to the surface area within the width range of 0~Kmm from the edge line, K is 0.2~0.6, and the non-corner area refers to the surface area outside the width range of Kmm from the edge line.

[0028] Schematic diagrams of the corner and non-corner areas of some commonly shaped magnets are shown in FIG1 .

[0029] The diffusion source H1 includes the following components by mass fraction:

[0030] R1: 50.0-80.0 wt.%, R1 includes RL1 and RH1, RH1 is one or more of Dy, Tb, and Ho, and accounts for 30.0-70.0 wt.% of the mass ratio of H1, and the balance of R1 is RL1, RL1 represents one or more elements selected from Nd, Pr, La, Ce, Er, Gd, Sm, Tm, Lu, and Y containing at least light rare earth elements; the light rare earth elements are one or more of La, Ce, Pr, and Nd; preferably, RL1 is Nd and Pr;

[0031] X1: 10-30 wt.%, X1 is one or more of Zr, Ti, and Nb; preferably Zr;

[0032] M1: 5.0-40.0 wt.%, M1 is one or more of Al, Ga, and Cu; preferably Ga;

[0033] The diffusion source H2 is a mixture of one or more pure metals, alloys, or compounds containing heavy rare earth elements, wherein the heavy rare earth element is at least one of Dy, Tb, and Ho. Preferably, the content of heavy rare earth elements in H2 is greater than 70%.

[0034] Furthermore, the content of heavy rare earth elements in the diffusion source H1 is lower than that in H2.

[0035] Preferably, H1 is composed of the following components: R1: 65-75%, X1: 15-25%, M1: 10-15%, more preferably R1: 70%, X1: 20%, M1: 10%.

[0036] The coating thickness of the diffusion source H1 and the coating thickness of the diffusion source H2 may be the same or different. Preferably, the coating thickness of the diffusion source H1 and the coating thickness of the diffusion source H2 are the same.

[0037] The coating amount of diffusion source H1 is generally 0.5~2.0% of the mass of the magnet; the coating amount of diffusion source H2 is generally 0.5~2.0% of the mass of the magnet.

[0038] (2) The magnet coated with the diffusion source is subjected to diffusion treatment at a diffusion temperature of 800°C to 1000°C for a holding time of 6 to 30 hours. After cooling, the magnet is subjected to tempering treatment to obtain the RTB rare earth permanent magnet.

[0039] The present invention also provides a method for preparing an edge-reinforced RTB rare earth permanent magnet, the method comprising the following steps:

[0040] (1) Setting an H1 diffusion source coating area and an H2 diffusion source coating area on the diffusion surface of the RTB magnet substrate, and coating the diffusion sources in different areas. The H1 diffusion source coating area is coated with the diffusion source H1, and the H2 diffusion source coating area is coated with the diffusion source H2; the H1 diffusion source coating area is the corner area of ​​the diffusion surface, and the H2 diffusion source coating area is the non-corner area of ​​the diffusion surface;

[0041] The corner area refers to the surface area within the width range of 0~Kmm from the edge line, K is the width of the corner area, and the range of K is 0.2~0.6. The non-corner area refers to the surface area outside the width range of Kmm from the edge line;

[0042] The diffusion source H1 includes the following components by mass fraction:

[0043] R1: 50.0-80.0 wt.%, R1 includes RL1 and RH1, RH1 is one or more of Dy, Tb, and Ho, and accounts for 30.0-70.0 wt.% of the mass ratio of H1, and the balance of R1 is RL1, RL1 represents one or more elements selected from Nd, Pr, La, Ce, Er, Gd, Sm, Tm, Lu, and Y containing at least light rare earth elements; the light rare earth elements are one or more of La, Ce, Pr, and Nd;

[0044] X1: 10-30wt.%, X1 is one or more of Zr, Ti, and Nb;

[0045] M1: 5.0~40.0wt.%, M1 is one or more of Al, Ga, and Cu;

[0046] The diffusion source H2 is one or more mixtures of pure metals, alloys or compounds containing heavy rare earth elements, and the heavy rare earth element is at least one of Dy, Tb and Ho;

[0047] The content of heavy rare earth elements in the diffusion source H1 is lower than that in H2;

[0048] (2) The magnet coated with the diffusion source is subjected to diffusion treatment at a diffusion temperature of 800°C to 1000°C for a holding time of 6 to 30 hours. After cooling, the magnet is subjected to tempering treatment to obtain the RTB rare earth permanent magnet.

[0049] In the step (1), the diffusion surface refers to the surface of the magnet coated with the diffusion source, which can generally be a magnet surface perpendicular to the magnet orientation direction, parallel to the magnet orientation direction, or at any angle to the magnet orientation direction.

[0050] The surface A is the diffusion surface.

[0051] Preferably, the diffusion surfaces are two surfaces perpendicular to the orientation direction of the magnet.

[0052] In step (1), the partitioned coating of the diffusion source can be achieved by the following methods:

[0053] Use shielding sheet 1 to cover the corners of the magnet, exposing the non-corner areas as H2 diffusion source coating areas, and apply diffusion source H2. Then use shielding sheet 2 to cover the non-corner areas of the magnet, exposing the corners as H1 diffusion source coating areas, and apply diffusion source H1. Alternatively, use shielding sheet 2 to cover the non-corner areas of the magnet, exposing the corners as H1 diffusion source coating areas, and apply diffusion source H1. Then use shielding sheet 1 to cover the corners of the magnet, exposing the non-corner areas as H2 diffusion source coating areas, and apply diffusion source H2. Exchanging the coating order of diffusion sources H1 and H2 will not affect the final effect.

[0054] The shielding sheet 1 is composed of a shielding area 1 and a hollow area 1. The shielding area 1 corresponds to the corner area of ​​the magnet, and the hollow area 1 corresponds to the non-corner area of ​​the magnet;

[0055] The shielding sheet 2 consists of a shielding area 2 and a hollow area 2. The shielding area 2 corresponds to the non-corner area of ​​the magnet, and the hollow area corresponds to the corner area of ​​the magnet.

[0056] The shielding piece 1 or the shielding piece 2 can be made of a polymer plastic material or a metal material such as stainless steel.

[0057] The diffusion source may be coated by PVD, spraying or printing.

[0058] When the diffusion source is coated by PVD, the diffusion source H1 is obtained by melting a large ingot; when the diffusion source is coated by spraying or printing, the diffusion source H1 is obtained as a powder by melting and throwing SC sheets, hydrogen crushing and air flow grinding.

[0059] When the diffusion source is coated by printing, the printed coating needs to be dried between two coatings.

[0060] Printing and coating the diffusion source has the advantage of simple operation and is very suitable for mass production of products. Therefore, in the present invention, screen printing is preferably used to coat the diffusion source:

[0061] Furthermore, the diffusion source is preferably coated in zones by screen printing, which specifically includes the following steps:

[0062] (a) Hollow areas with holes and shielding areas without holes are set on the screen, and the positions of the hollow areas and shielding areas of the printing screen are changed according to the size of the product and the size of the corner area. At least printing screen 1 and printing screen 2 should be included, wherein the hollow areas of printing screen 1 correspond to the non-corner areas of the magnet, and the shielding areas correspond to the corner areas of the magnet; the hollow areas of printing screen 2 correspond to the corner areas of the magnet, and the shielding areas correspond to the non-corner areas of the magnet; printing screen 1 and printing screen 2 can include multiple hollow areas or shielding areas, and multiple magnetic sheets can be printed at the same time;

[0063] (b) Align the shielded areas of printing screen 1 with the corners of the magnet and the hollowed areas with the non-corner areas to form the H2 diffusion source coating area. Print the diffusion source H2 and dry it. Then, align the shielded areas of printing screen 2 with the non-corner areas of the magnet and the hollowed areas with the corners of the magnet to form the H1 diffusion source coating area. Print the diffusion source H1 and dry it. Alternatively, perform zone coating in the reverse order.

[0064] The RTB magnet matrix of the present invention is obtained by processing a sintered bulk NdFeB magnet into a desired shape and size, and then cleaning and drying the magnet after surface treatment.

[0065] The surface treatment of the magnet is to remove oil stains and rust spots on the surface of the magnet by grinding, pickling or sandblasting.

[0066] In the step (2), the diffusion treatment is generally performed in a vacuum diffusion furnace.

[0067] In the tempering treatment, the tempering temperature is 400° C. to 600° C. (preferably 480° C. to 420° C.), and the tempering time is 2 h to 10 h (preferably 3 h to 5 h).

[0068] NdFeB magnets are quite brittle, making them susceptible to chipping and falling due to collisions during transportation and assembly. Furthermore, machining during NdFeB product preparation can cause microcracks in the corners of the magnets, making them more susceptible to falling off due to impact. Improving the mechanical properties of NdFeB magnets can reduce the chipping rate. Traditionally, this approach involves adding certain amounts of elements such as Zr, Ti, and Nb to the raw materials. These elements strengthen the R-rich phase at the magnet's grain boundaries through solid solution or the formation of second-phase precipitates, thereby improving the mechanical properties of the NdFeB magnets. However, as the content of non-magnetic elements increases, the remanence of the magnets gradually decreases. At the same time, defects in NdFeB magnets are primarily concentrated in the corners. Therefore, simply improving the mechanical properties of the corners can significantly reduce the chipping rate during transportation and assembly.

[0069] Based on the above reasons, the present invention provides an RTB rare earth permanent magnet with enhanced corners and a preparation method thereof. By analyzing the areas of the magnet that are prone to mechanical property defects, the magnet diffusion source coating surface is divided into corner areas and non-corner areas. The corner areas of the magnet are coated with diffusion sources containing Zr, Ti, and Nb elements, while the non-corner areas are coated with heavy rare earth element diffusion sources that do not contain these elements. During the grain boundary diffusion process, the Zr, Ti, and Nb elements diffuse into the grain boundary R-rich phase of the magnet, and Zr, Ti, and Nb are enriched only in the corner areas of the magnet. The grain boundary R-rich phase in the magnet corner areas is strengthened by solid solution or the formation of second-phase precipitates, thereby improving the strength and other mechanical properties of the magnet corner areas. In addition, the diffusion sources in the magnet corner areas contain a certain amount of light rare earth elements. During the grain boundary diffusion process, they can repair microcracks caused by machining, eliminate the deteriorating effects of machining on the mechanical properties of the magnet corners, further enhance the ability of the magnet corners to resist impact, and are of great significance for reducing the rate of product chipping and corner chipping.

[0070] This invention uses zoned grain boundary diffusion to improve the mechanical properties of magnet corners without affecting non-corner areas. This method significantly reduces the rate of edge and corner chipping during transportation and assembly without compromising magnetic properties, significantly reducing the cost of NdFeB products.

[0071] The diffusion source H1 of the present invention contains 10 to 30 wt.% of one or more of the elements Zr, Ti, and Nb. During grain boundary diffusion, these elements diffuse into the interior of the magnet along the grain boundary R-rich phase. The R-rich phase at the grain boundary of the magnet is strengthened by solid solution or by forming second-phase precipitates with other elements, thereby increasing the strength of the magnet's corners and enhancing their ability to resist impact. In the present invention, within a depth range of 0.6 mm vertically from the surface A, the X content in the corner body region is 0.05 to 1.2 wt.%.

[0072] In addition, the inclusion of a certain concentration of RL in the diffusion source H1 can repair microcrack defects caused by machining during the grain boundary diffusion process, further improving the mechanical properties of the corners of the magnet. During the machining process of the magnet, the impact force and processing stress of the machining will cause microcracks at the corners of the magnet. During the subsequent product transportation and assembly process, any slight bump between products may cause the cracks to expand and cause the magnet to have chipped edges and corners. The RL added in H1 will diffuse into the interior of the magnet through the grain boundaries during the grain boundary diffusion process, and the molten RL will repair the cracks located in the R-rich phase at the grain boundaries of the magnet, thereby eliminating the deterioration effect of machining defects on the mechanical properties of the corners of the magnet. In the present invention, the diffusion source H1 contains RL and the diffusion source H2 does not contain RL. Therefore, the light rare earth element RL content in the corner area of ​​the magnet surface A after the grain boundary diffusion source is not lower than the average light rare earth content of the surface A.

[0073] Diffusion source H1 also contains 30.0-70.0 wt.% RH. After grain boundary diffusion of RH, a shell rich in heavy rare earth elements RH is formed on the surface of the main phase grains of the magnet. Because this shell has a high anisotropy field, it can significantly improve the coercivity of the NdFeB magnet. The 5-40 wt.% M1 in diffusion source H1 can lower the melting point of the diffusion source and the melting point of the R-rich phase at the magnet grain boundaries during grain boundary diffusion. This increases the RH diffusion depth and enhances the RL's ability to repair microcracks.

[0074] The present invention coats the non-corner areas of the magnet with a diffusion source H2 that does not contain Zr, Ti, or Nb. The diffusion source H2 is a pure metal, alloy, or compound containing at least one of the heavy rare earth elements Dy, Tb, and Ho. Because the heavy rare earth element diffusion source also generates certain diffusion internal stresses, which can degrade the mechanical properties of the magnet's corners, the heavy rare earth element content of H1 is lower than that of H2 in the present invention.

[0075] In the present invention, the diffused source coating method can be PVD, spraying or printing.

[0076] In the present invention, the diffusion source H1 is prepared by smelting and mixing the ingredients according to the actual composition. When PVD coating is used, a large ingot can be directly prepared by smelting. When coating the diffusion source by coating or printing, a powdered diffusion source is prepared by melting SC sheets, hydrogen crushing, and jet milling.

[0077] The diffusion source H2 can directly adopt commercial pure metal, alloy or compound ingot or powder containing at least one of the heavy rare earth elements Dy, Tb and Ho. Beneficial effects

[0078] The beneficial effects of the present invention are embodied in that: by analyzing the areas of the magnet that are prone to mechanical property defects, the diffusion source coating surface of the magnet is divided into corner areas and non-corner areas. The corner areas of the magnet are coated with diffusion sources containing Zr, Ti, and Nb elements, while the non-corner areas of the magnet are coated with diffusion sources that do not contain the above elements. During the grain boundary diffusion process, the Zr, Ti, and Nb elements diffuse into the grain boundary R-rich phase of the magnet, and strengthen the grain boundary R-rich phase of the magnet by solid solution or the generation of second phase precipitates, thereby improving the strength of the magnet corners. The present invention improves the mechanical properties of the magnet corner areas by partitioning the grain boundary diffusion without affecting the non-corner areas of the magnet. The above method can significantly reduce the rate of missing edges and corners of the magnet during transportation and assembly without reducing the magnetic properties of the magnet, which is of great significance for reducing the cost of NdFeB products. BRIEF DESCRIPTION OF THE DRAWINGS

[0079] Figure 1 Schematic diagram of the corner and non-corner areas of commonly shaped magnets.

[0080] Figure 2 Schematic diagram of magnet-selected area printing in Experiment No. 2 and Experiment No. 4.

[0081] Figure 3: Cross-sectional view of the corner area of ​​the magnet in Experiment No. 2. Best Mode for Carrying Out the Invention

[0082] The sintered RTB magnet is prepared by melt-spinning SC sheets, hydrogen crushing, air flow grinding, orientation forming, isostatic pressing, vacuum sintering and aging. The bulk NdFeB magnet is processed into the required shape and size. After surface treatment, the magnet is cleaned and dried to obtain the RTB magnet matrix.

[0083] An H1 diffusion source coating area and an H2 diffusion source coating area are set on the diffusion surface of the RTB magnet substrate, and the diffusion sources are coated in different areas. The H1 diffusion source coating area is coated with the diffusion source H1, and the H2 diffusion source coating area is coated with the diffusion source H2; the H1 diffusion source coating area is the corner area of ​​the diffusion surface, and the H2 diffusion source coating area is the non-corner area of ​​the diffusion surface.

[0084] The corner area refers to the surface area within the width range of 0~Kmm from the edge line, K is 0.2~0.6, and the non-corner area refers to the surface area outside the width range of Kmm from the edge line.

[0085] Schematic diagrams of the corner and non-corner areas of some commonly shaped magnets are shown in FIG1 .

[0086] The magnet coated with diffusion sources in different areas is subjected to diffusion treatment at a diffusion temperature of 800° C. to 1000° C. for a holding time of 6 to 30 hours. After the diffusion treatment, the magnet is cooled to room temperature and then heated to 400 to 600° C. for a holding time of 2 to 10 hours to obtain the magnet.

[0087] The surface of the magnet after secondary aging was sandblasted to expose the fresh surface of the magnet. ICP was used to measure the magnet composition, and SEM and EPMA were used to analyze the magnet microstructure and micro-region composition. NIM equipment was used to measure the magnetic properties of the magnet. 11 samples were tested in each group of experiments, and the average value of the magnetic performance index was calculated. 200 products were selected for the drop test. The drop height was 1 meter and the number of drops was 1. There were particles larger than 0.3mm on the corners of the magnet. 2 Products in defective areas are considered unqualified products, and the qualified rate of products is calculated. Example

[0088] The sintered RTB magnet is prepared by melt-spinning SC sheets, hydrogen crushing, air flow milling, orientation molding, isostatic pressing, vacuum sintering and aging.

[0089] The sintered and aged magnets are machined into magnetic sheets with a length × width × height of 10 mm × 10 mm × 5 mm, where the height direction is the orientation direction of the magnet. The surface oil and rust of the magnets are cleaned by pickling, then rinsed with clean water and dried.

[0090] The powder of the diffusion source H1 is prepared by melt-spinning SC sheets, hydrogen crushing, and air flow milling. The powder particle size SMD is 1.5 μm. The composition of the heavy rare earth element powder of the diffusion source H1 is as follows:

[0091] R: 70wt.%, R includes RL and RH, RH is Tb and accounts for 60% of the mass ratio of H1, the balance of R is RL, RL is Pr and Nd, the ratio of Pr to Nd is 25:75 by mass,

[0092] Zr: 20wt.%,

[0093] Ga: 10wt.%,

[0094] The heavy rare earth element powder of the diffusion source H2 is commercial terbium hydride powder (Tb content 98.2 wt.%), and the powder particle size SMD is 1.5 μm.

[0095] The screen printing coating was prepared according to the following ratio: the mass ratio of heavy rare earth diffusion source powder, terpineol, polyvinyl butyral and aluminum oxide was 70:26:2:2, and the screen printing coating was obtained after mixing evenly.

[0096] Diffusion sources were printed on both surfaces of the magnet perpendicular to the orientation direction, with a diffusion source layer thickness of 15μm. In Experiment No. 1, diffusion source H2 was printed on both surfaces of the magnet. Experiment No. 2 employed zoned diffusion source coating, with diffusion source H1 applied to the corners of the magnet and diffusion source H2 applied to the non-corner areas. The corner areas were 0.4mm wide. Experiment No. 2 achieved zoned diffusion source coating by designing two printing screens of different sizes. A schematic diagram of the printing screen for Experiment No. 2 is shown in Figure 2. The printing screen in Figure 2 can simultaneously print three magnets of the same size.

[0097] The shielding area of ​​the printing screen on the left side of FIG2 is aligned with the corner area of ​​the magnet, and the hollow area is aligned with the non-corner area, as the H2 diffusion source coating area, and the diffusion source H2 is printed and dried. Then, the shielding area of ​​the printing screen on the right side of FIG2 is aligned with the non-corner area of ​​the magnet, and the hollow area is aligned with the corner area of ​​the magnet, as the H1 diffusion source coating area, and the diffusion source H1 is printed and dried.

[0098] After printing on one side of the magnet, it is dried in a drying tunnel at 50°C, and then printed on the second side and dried again.

[0099] The magnet was placed in a vacuum diffusion furnace and heated to 950° C., kept warm for 15 hours, cooled to room temperature, and then heated to 520° C., kept warm for 4 hours to obtain the magnet.

[0100] The surface of the magnet after secondary aging was sandblasted to expose the fresh surface of the magnet. ICP was used to measure the magnet composition, and SEM and EPMA were used to analyze the magnet microstructure and micro-region composition. NIM equipment was used to measure the magnetic properties of the magnet. 11 samples were tested in each group of experiments, and the average value of the magnetic performance index was calculated. 200 products were selected for the drop test. The drop height was 1 meter and the number of drops was 1. There were particles larger than 0.3mm on the corners of the magnet. 2 Products in defective areas are considered unqualified products, and the qualified rate of products is calculated.

[0101] The magnet matrix compositions of Experiment No. 1 and Experiment No. 2 are the same. The magnet matrix and magnet compositions after grain boundary diffusion are shown in Table 1:

[0102] Table 1

[0103] No.NdPrCoCuGaTbFeZrMatrix27.60.600.970.10.1 / Bal / 127.70.610.970.10.10.21Bal / 227.70.600.970.10.110.20Bal0.1

[0104] The magnetic properties and qualified rate of the magnets are shown in Table 2:

[0105] Table 2

[0106] Test No. Br (kGs) Hcj (kOe) Pass rate (%) 114.521.180% 214.521.096%

[0107] As can be seen from the data in Tables 1 and 2, the Tb content of the magnets in Experiment No. 1 and Experiment No. 2 after grain boundary diffusion is essentially the same. However, because the magnet in Experiment No. 2 uses a partitioned grain boundary diffusion method, i.e., the diffusion source in the coating area at the corners of the magnet contains a certain amount of Zr, the magnet contains 0.1 wt.% Zr after grain boundary diffusion. Simultaneously, as can be seen from the magnetic properties of the magnets in Table 2, the magnetic properties of Experiment No. 1 and Experiment No. 2 after grain boundary diffusion are essentially the same, but the qualified rate of the magnet in Experiment No. 2 is significantly higher than that in Experiment No. 1. This indicates that the partitioned grain boundary diffusion method provided by the present invention can effectively improve the mechanical properties of the corners of NdFeB magnets, thereby reducing the rate of edge and corner chipping in the product.

[0108] As shown in Figure 3, precision wire cutting was used to cut the corners of the magnet and test their composition. The results showed that the average Zr content at the corners of the magnet was 0.4wt.%, which was significantly higher than the average Zr content of the magnet. This indicates that after the surface of the corners of the magnet was coated with a Zr-containing diffusion source and grain boundary diffusion was performed, the Zr element would be enriched at the corners of the magnet. With the help of PEMA point scanning analysis, it was found that the Zr element was mainly distributed in the R-rich phase at the grain boundaries of the magnet. The Zr element can strengthen the R-rich phase at the grain boundaries of the magnet by solid solution or the formation of second-phase precipitates, thereby improving the mechanical properties of the corners of the magnet. In addition, since the Zr element-rich area is only concentrated at the corners of the magnet, it will not affect the magnetic properties of the magnet.

[0109] EPMA surface scanning was used to analyze the average light rare earth element content in the corner areas of the magnet surface A and the average light rare earth element content of the entire surface A. It was found that the light rare earth element content in the corner areas of the magnet surface A was not lower than the average light rare earth content of the surface A. In the present invention, the corner area diffusion source H1 uses a portion of the light rare earth element RL to replace RH. After grain boundary diffusion, RL is mainly concentrated in the grain boundary phase of the magnet, repairing microcracks at the corners of the magnet caused by machining, thereby enhancing the mechanical properties of the magnet corners. In addition, due to the high diffusion rate of RL, it will not be enriched only in the corner areas of the magnet. Therefore, the light rare earth element content in the corner areas of the magnet surface A is not lower than the average light rare earth content of the surface A. In addition, as can be seen from the data in Table 2, the magnetic properties of the magnet in Experiment No. 2 are not reduced compared with Experiment No. 1. Therefore, the use of a portion of the light rare earth element RL to replace RH in the diffusion source H1 of the present invention does not lead to a reduction in magnetic properties.

[0110] The present invention realizes the partitioned grain boundary diffusion of NdFeB magnet by adopting the method of partitioned coating diffusion source, by coating the diffusion source containing Zr, Ti and Nb elements in the corner area of ​​the magnet, while the non-corner area of ​​the magnet is coated with the diffusion source without the above elements. During the grain boundary diffusion process, Zr, Ti and Nb elements diffuse into the grain boundary R-rich phase of the magnet, and strengthen the grain boundary R-rich phase of the magnet by solid solution or generation of second phase precipitates, thereby improving the strength of the magnet corner. The present invention improves the mechanical properties of the magnet corner area by partitioned grain boundary diffusion without affecting the non-corner area of ​​the magnet. By the above method, the rate of missing edges and corners of the magnet during transportation and assembly can be significantly reduced without reducing the magnetic properties of the magnet, which is of great significance for reducing the cost of NdFeB products.

[0111] Example 2:

[0112] The sintered RTB magnet is prepared by melt-spinning SC sheets, hydrogen crushing, air flow milling, orientation molding, isostatic pressing, vacuum sintering and aging.

[0113] The sintered and aged magnets are machined into magnetic sheets with a length × width × height of 10 mm × 10 mm × 5 mm, where the height direction is the orientation direction of the magnet. The surface oil and rust of the magnets are cleaned by pickling, then rinsed with clean water and dried.

[0114] The powder of the diffusion source H1 is prepared by melt-spinning SC sheets, hydrogen crushing, and air flow milling. The powder particle size SMD is 1.5 μm. The composition of the heavy rare earth element powder of the diffusion source H1 is as follows:

[0115] R: 70wt.%, R includes RL and RH, RH is Tb and accounts for 60% of the mass ratio of H1, the balance of R is RL, RL is Pr and Nd, the ratio of Pr to Nd is 25:75 by mass,

[0116] Zr: 20wt.%,

[0117] Ga: 10wt.%,

[0118] The diffusion source H2 containing heavy rare earth element powder is commercial terbium hydride powder, and the powder particle size SMD is 1.5 μm.

[0119] The screen printing coating was prepared according to the following ratio: the mass ratio of heavy rare earth diffusion source powder, terpineol, polyvinyl butyral and aluminum oxide was 70:26:2:2, and the screen printing coating was obtained after mixing evenly.

[0120] Diffusion sources were printed on both surfaces of the magnet perpendicular to the orientation direction, with a diffusion source layer thickness of 20 μm. Experiment No. 3 had diffusion source H2 printed on both surfaces of the magnet. Experiment No. 4 employed zoned diffusion source coating, with diffusion source H1 applied to the corners of the magnet and diffusion source H2 applied to the non-corner areas. The corner areas were 0.4 mm wide. The diffusion source was applied by printing, and after printing on one side of the magnet, it was dried in a drying tunnel at 50°C. The second side was then printed and dried again.

[0121] The magnet was placed in a vacuum diffusion furnace and heated to 950° C., kept warm for 15 hours, cooled to room temperature, and then heated to 520° C., kept warm for 4 hours to obtain the magnet.

[0122] The surface of the magnet after secondary aging was sandblasted to expose the fresh surface of the magnet. ICP was used to measure the magnet composition, and SEM and EPMA were used to analyze the magnet microstructure and micro-region composition. NIM equipment was used to measure the magnetic properties of the magnet. 11 samples were tested in each group of experiments, and the average value of the magnetic performance index was calculated. 200 products were selected for the drop test. The drop height was 1 meter and the number of drops was 1. There were particles larger than 0.3mm on the corners of the magnet. 2 Products in defective areas are considered unqualified products, and the qualified rate of products is calculated.

[0123] The magnet matrix compositions of Experiment No. 3 and Experiment No. 4 are the same. The magnet matrix and magnet compositions after grain boundary diffusion are shown in Table 3:

[0124] Table 3

[0125] No.NdPrCoCuGaTbFeZrMatrix27.60.600.970.10.1 / Bal0.1327.80.610.970.10.10.22Bal0.1427.80.600.970.10.120.22Bal0.16

[0126] The magnetic properties and qualified rate of the magnets are shown in Table 4:

[0127] Table 4

[0128] Test No.Br (kGs)Hcj (kOe)Quality rate (%)314.4522.085%414.4522.098%

[0129] As shown in Table 3 and Table 4, the Tb content of Experiment No.3 and Experiment No.4 magnets is substantially the same after grain boundary diffusion. Simultaneously, due to the fact that the magnet matrix contains 0.1wt.% Zr in the present embodiment, the Zr content in Experiment No.3 magnet is identical with the matrix after grain boundary diffusion, while the Zr content in Experiment No.4 magnet is significantly increased compared with Experiment No.1. Simultaneously, as shown in the magnetic properties of the magnet, due to the addition of a certain amount of Zr in the matrix, the remanence of Experiment No.3 and Experiment No.4 magnets is reduced, but the magnetic properties of Experiment No.3 and Experiment No.4 magnets are substantially the same from the experimental results. As can be seen from the qualified rate of the magnet, due to the addition of 0.1wt.% Zr in the magnet matrix, the final qualified rate of Experiment No.3 magnet increases, but is still lower than Experiment No.4, indicating that when containing a certain Zr element in the magnet matrix, the mechanical properties of the magnet corners can be significantly improved using method provided by the present invention, thereby reducing the edge and corner loss rate of the product.

[0130] Precision wire cutting was used to cut the corner area of ​​the magnet as shown in Figure 3. The Zr element content in the corner area of ​​the magnets of Experiment No. 3 and Experiment No. 4 was measured. The results are shown in Table 5:

[0131] Table 5

[0132] Experiment No. Zr content in the corner area wt.% 30.140.52

[0133] The results show that the average Zr content in the corners of the magnet in Experiment No. 4 is significantly higher than in the non-corner areas, indicating that Zr is enriched in these corners after coating the magnet's corners with a Zr-containing diffusion source and undergoing grain boundary diffusion. PEMA point scanning analysis revealed that Zr is primarily distributed in the R-rich phase at the magnet's grain boundaries. Zr can strengthen the R-rich phase at the magnet's grain boundaries through solid solution or the formation of second-phase precipitates, thereby improving the mechanical properties of the magnet's corners. Furthermore, since the Zr-rich regions are concentrated only at the magnet's corners, they do not affect the magnet's magnetic properties.

[0134] EPMA surface scanning was used to analyze the average light rare earth element content in the corner areas of the magnet surface A and the average light rare earth element content of the entire surface A. It was found that the light rare earth element content in the corner areas of the magnet surface A was not lower than the average light rare earth content of the surface A. In the present invention, the corner area diffusion source H1 uses a portion of the light rare earth element RL to replace RH. After grain boundary diffusion, RL is mainly concentrated in the grain boundary phase of the magnet, repairing microcracks at the corners of the magnet caused by machining, thereby enhancing the mechanical properties of the magnet corners. In addition, due to the high diffusion rate of RL, it will not be enriched only in the corner areas of the magnet. Therefore, the light rare earth element content in the corner areas of the magnet surface A is not lower than the average light rare earth content of the surface A. In addition, as can be seen from the data in Table 4, the magnetic properties of the magnet in Experiment No. 4 are not reduced compared with Experiment No. 3. Therefore, the use of a portion of the light rare earth element RL to replace RH in the diffusion source H1 of the present invention does not lead to a reduction in magnetic properties.

[0135] The present invention realizes the partitioned grain boundary diffusion of NdFeB magnet by adopting the method of partitioned coating diffusion source, by coating the diffusion source containing Zr, Ti and Nb elements in the corner area of ​​the magnet, while the non-corner area of ​​the magnet is coated with the diffusion source without the above elements. During the grain boundary diffusion process, Zr, Ti and Nb elements diffuse into the grain boundary R-rich phase of the magnet, and strengthen the grain boundary R-rich phase of the magnet by solid solution or generation of second phase precipitates, thereby improving the strength of the magnet corner. The present invention improves the mechanical properties of the magnet corner area by partitioned grain boundary diffusion without affecting the non-corner area of ​​the magnet. By the above method, the rate of missing edges and corners of the magnet during transportation and assembly can be significantly reduced without reducing the magnetic properties of the magnet, which is of great significance for reducing the cost of NdFeB products.

[0136] Example 3:

[0137] The sintered RTB magnet is prepared by melt-spinning SC sheets, hydrogen crushing, air flow milling, orientation molding, isostatic pressing, vacuum sintering and aging.

[0138] The sintered and aged magnets are machined into magnetic sheets with a length × width × height of 10 mm × 10 mm × 5 mm, where the height direction is the orientation direction of the magnet. The surface oil and rust of the magnets are cleaned by pickling, then rinsed with clean water and dried.

[0139] The powder of the diffusion source H1 is prepared by melt-spinning SC sheets, hydrogen crushing, and air flow milling. The powder particle size SMD is 1.5 μm. The composition of the heavy rare earth element powder of the diffusion source H1 is as follows:

[0140] R: 70wt.%, R includes RL and RH, RH is Tb and accounts for 60% of the mass ratio of H1, the balance of R is RL, RL is Pr and Nd, the ratio of Pr to Nd is 25:75 by mass,

[0141] Zr: 20wt.%,

[0142] Ga: 10wt.%,

[0143] The diffusion source H2 containing heavy rare earth element powder is commercial terbium hydride powder, and the powder particle size SMD is 1.5 μm.

[0144] The screen printing coating was prepared according to the following ratio: the mass ratio of heavy rare earth diffusion source powder, terpineol, polyvinyl butyral and aluminum oxide was 70:26:2:2, and the screen printing coating was obtained after mixing evenly.

[0145] Diffusion sources were printed on both surfaces of the magnet perpendicular to the orientation direction, with a diffusion source layer thickness of 20 μm. Experiments No. 5 to No. 7 all used zoned diffusion source coating, with diffusion source H1 applied to the corners of the magnets and diffusion source H2 applied to the non-corner areas. The corner area width of the magnet in Experiment No. 5 was 0.1 mm, the corner area width of the magnet in Experiment No. 6 was 0.4 mm, and the corner area width of the magnet in Experiment No. 7 was 1.0 mm. The diffusion source was applied by printing. After printing on one side of the magnet, it was dried in a drying tunnel at 50°C, and then printed on the second side, followed by drying again.

[0146] The magnet was placed in a vacuum diffusion furnace and heated to 950° C., kept warm for 15 hours, cooled to room temperature, and then heated to 520° C., kept warm for 4 hours to obtain the magnet.

[0147] The surface of the magnet after secondary aging was sandblasted to expose the fresh surface of the magnet. ICP was used to measure the magnet composition, and SEM and EPMA were used to analyze the magnet microstructure and micro-region composition. NIM equipment was used to measure the magnetic properties of the magnet. 11 samples were tested in each group of experiments, and the average value of the magnetic performance index was calculated. 200 products were selected for the drop test. The drop height was 1 meter and the number of drops was 1. There were particles larger than 0.3mm on the corners of the magnet. 2 Products in defective areas are considered unqualified products, and the qualified rate of products is calculated.

[0148] The magnet matrix compositions of Experiment No. 5 to Experiment No. 7 are the same. The magnet matrix and magnet compositions after grain boundary diffusion are shown in Table 6:

[0149] Table 6

[0150] No.NdPrCoCuGaTbFeZrMatrix27.60.600.970.10.1 / Bal0.1527.80.600.970.10.110.22Bal0.13627.80.600.970.10.110.22Bal0.16727.80.600.970.10.110.22Bal0.20

[0151] The magnetic properties and qualified rate of the magnets are shown in Table 7:

[0152] Table 7

[0153] Experiment No. Br (kGs) Hcj (kOe) Pass rate (%) 514.45 22.087% 614.45 22.098% 714.38 21.999%

[0154] From the data in Tables 6 and 7, it can be seen that the Tb content of the magnets of Experiment No. 5 to Experiment No. 7 is basically the same after grain boundary diffusion, and the Zr content of the magnets increases significantly after grain boundary diffusion.

[0155] However, the sizes of the corner areas of the magnets in different experimental groups are different. The width of the corner area of ​​Experiment No. 5 is 0.1 mm. Although the mechanical properties of the corners are enhanced after the grain boundary partitioning and grain boundary diffusion, the corner areas are narrow and the volume of the corner strengthening area is small, so the improvement of the mechanical properties of the magnet corners is limited. When the magnet corner range is within the scope of the present invention (Experiment No. 6), the mechanical properties of the magnet corner areas can be effectively improved by partitioning grain boundary diffusion, thereby improving the qualified rate of the product. However, when the corner area size of the magnet is too large (Experiment No. 7), the volume of the strengthened corner area increases. As can be seen from Table 7, although the qualified rate of the magnet can also be improved, the remanence of the magnet is significantly reduced due to the large volume fraction of the Zr-rich area. Therefore, it is necessary to reasonably control the size of the corner area. In the present invention, the corner area size is between 0.2 and 0.6 mm.

[0156] Example 4:

[0157] The sintered RTB magnet is prepared by melt-spinning SC sheets, hydrogen crushing, air flow milling, orientation molding, isostatic pressing, vacuum sintering and aging.

[0158] The sintered and aged magnets are machined into magnetic sheets with a length × width × height of 10 mm × 10 mm × 5 mm, where the height direction is the orientation direction of the magnet. The surface oil and rust of the magnets are cleaned by pickling, then rinsed with clean water and dried.

[0159] The powder of diffusion source H1 was prepared by melt-spinning SC sheets, hydrogen crushing, and air flow milling. The powder particle size SMD was 1.5 μm. The composition of the heavy rare earth element powder of diffusion source H1 in Experiment No. 8 was as follows:

[0160] R: 70wt.%, R includes RL and RH, RH is Tb and accounts for 60% of the mass ratio of H1, the balance of R is RL, RL is Pr and Nd, the ratio of Pr to Nd is 25:75 by mass,

[0161] Zr: 20wt.%,

[0162] Ga: 10wt.%,

[0163] The composition of the heavy rare earth element powder in Experiment No. 9 Energy H1 is as follows:

[0164] R: 70wt.%, R includes RL and RH, RH is Tb and accounts for 60% of the mass ratio of H1, the balance of R is RL, RL is Pr and Nd, the ratio of Pr to Nd is 25:75 by mass,

[0165] Zr: 30wt.%,

[0166] The diffusion source H2 containing heavy rare earth element powder is commercial terbium hydride powder, and the powder particle size SMD is 1.5 μm.

[0167] The screen printing coating was prepared according to the following ratio: the mass ratio of heavy rare earth diffusion source powder, terpineol, polyvinyl butyral and aluminum oxide was 70:26:2:2, and the screen printing coating was obtained after mixing evenly.

[0168] Diffusion sources were printed on both surfaces of the magnet perpendicular to the orientation direction, with a thickness of 20 μm. Experiments No. 8 and No. 9 both employed zoned diffusion source coating: diffusion source H1 was applied to the corners of the magnet, and diffusion source H2 was applied to the non-corner areas. The corner coating area was 0.4 mm thick. The diffusion sources were applied by printing. After printing on one side of the magnet, the magnet was dried in a drying oven at 50°C. Printing was then performed on the second side, followed by drying again.

[0169] The magnet was placed in a vacuum diffusion furnace and heated to 950° C., kept warm for 15 hours, cooled to room temperature, and then heated to 520° C., kept warm for 4 hours to obtain the magnet.

[0170] The surface of the magnet after secondary aging was sandblasted to expose the fresh surface of the magnet. ICP was used to measure the magnet composition, and SEM and EPMA were used to analyze the magnet microstructure and micro-region composition. NIM equipment was used to measure the magnetic properties of the magnet. 11 samples were tested in each group of experiments, and the average value of the magnetic performance index was calculated. 200 products were selected for the drop test. The drop height was 1 meter and the number of drops was 1. There were particles larger than 0.3mm on the corners of the magnet. 2 Products in defective areas are considered unqualified products, and the qualified rate of products is calculated.

[0171] The magnet matrix compositions of Experiment No. 8 and Experiment No. 9 are the same. The magnet matrix and magnet compositions after grain boundary diffusion are shown in Table 8:

[0172] Table 8

[0173] No.NdPrCoCuGaTbFeZrMatrix27.60.600.970.10.1 / Bal0.1827.80.600.970.10.110.22Bal0.16927.80.600.970.10.1022Bal0.13

[0174] The magnetic properties and qualified rates of the magnets are shown in Table 9:

[0175] Table 9

[0176] Test No.Br (kGs)Hcj (kOe)Quality rate (%)814.4522.098%914.4522.091%

[0177] In this example, the composition of diffusion source H1 in Experiment No. 8 falls within the recommended range of the present invention, but the diffusion source H1 in Experiment No. 9 does not contain the M1 element. Table 8 shows that even though the Zr content in diffusion source H1 in Experiment No. 9 is higher than that in the magnets of Experiment No. 8, the average Zr content in the magnets of Experiment No. 9 after grain boundary diffusion is lower than that of Experiment No. 8. Consequently, the qualified rate of the magnets of Experiment No. 9 is lower than that of Experiment No. 8.

[0178] This is because Zr has a high melting point. To accelerate the grain boundary diffusion rate of diffusion source H1, its melting point needs to be lowered. Therefore, in the present invention, a certain amount of M1 (Al, Ga, Cu) is added to diffusion source H1 to lower its melting point and increase its diffusion efficiency. Therefore, although the Zr content in diffusion source H1 in Experiment No. 9 is higher than in Experiment No. 8, its higher melting point and slower grain boundary diffusion rate weaken the corner strengthening effect of the magnet in Experiment No. 9, resulting in a lower pass rate. Therefore, in the present invention, diffusion source H1 within the recommended composition range is preferred.

[0179] Embodiment 5:

[0180] The sintered RTB magnet is prepared by melt-spinning SC sheets, hydrogen crushing, air flow milling, orientation molding, isostatic pressing, vacuum sintering and aging.

[0181] The sintered and aged magnets are machined into magnetic sheets with a length × width × height of 10 mm × 10 mm × 5 mm, where the height direction is the orientation direction of the magnet. The surface oil and rust of the magnets are cleaned by pickling, then rinsed with clean water and dried.

[0182] The powder of diffusion source H1 was prepared by melt-spinning SC sheets, hydrogen crushing, and air flow milling. The powder particle size SMD was 1.5 μm. The composition of the heavy rare earth element powder of diffusion source H1 in Experiment No. 10 was as follows:

[0183] R: 75wt.%, R includes RL and RH, RH is Tb and accounts for 60% of the mass ratio of H1, the balance of R is RL, RL is Pr and Nd, the ratio of Pr to Nd is 25:75 by mass,

[0184] Ti: 15wt.%,

[0185] Cu: 15wt.%,

[0186] The diffusion source H2 containing heavy rare earth element powder is commercial terbium hydride powder, and the powder particle size SMD is 1.5 μm.

[0187] The composition of the heavy rare earth element powder of the diffusion source H1 in Experiment No. 11 is as follows:

[0188] R: 65wt.%, R includes RL and RH, RH is Tb and accounts for 55% of the mass ratio of H1, the balance of R is RL, RL is Pr and Nd, the ratio of Pr to Nd is 25:75 by mass,

[0189] Nb: 25wt.%,

[0190] Al: 10wt.%,

[0191] The diffusion source H2 containing heavy rare earth element powder is commercial terbium hydride powder, and the powder particle size SMD is 1.5 μm.

[0192] The screen printing coating was prepared according to the following ratio: the mass ratio of heavy rare earth diffusion source powder, terpineol, polyvinyl butyral and aluminum oxide was 70:26:2:2, and the screen printing coating was obtained after mixing evenly.

[0193] Diffusion sources are printed on two surfaces of the magnet perpendicular to the orientation direction, and the thickness of the diffusion source layer is 20 μm.

[0194] The magnet matrix composition of Experiment No. 10 and Experiment No. 11 is the same. Experiment No. 10 and Experiment No. 11 adopt zoned coating of diffusion source, with diffusion source H1 coated on the corner area of ​​the magnet and diffusion source H2 coated on the non-corner area. The width of the corner area is 0.6 mm.

[0195] The diffusion source is applied by printing. After printing on one side of the magnet, it is dried in a drying tunnel at 50°C, and then the second side is printed and dried again.

[0196] The magnet was placed in a vacuum diffusion furnace and heated to 950° C., kept warm for 15 hours, cooled to room temperature, and then heated to 520° C., kept warm for 4 hours to obtain the magnet.

[0197] The surface of the magnet after secondary aging was sandblasted to expose the fresh surface of the magnet. ICP was used to measure the magnet composition, and SEM and EPMA were used to analyze the magnet microstructure and micro-region composition. NIM equipment was used to measure the magnetic properties of the magnet. 11 samples were tested in each group of experiments, and the average value of the magnetic performance index was calculated. 200 products were selected for the drop test. The drop height was 1 meter and the number of drops was 1. There were particles larger than 0.3mm on the corners of the magnet. 2 Products in defective areas are considered unqualified products, and the qualified rate of products is calculated.

[0198] The magnet matrix compositions of Experiment No. 10 and Experiment No. 11 are the same. The magnet matrix and magnet compositions after grain boundary diffusion are shown in Table 10:

[0199] Table 10

[0200] No.NdPrCoCuGaTbFeZrTiNbAl Matrix 27.60.600.970.10.1 / Bal0.1 / / / 1027.80.600.970.110.10.22Bal0.10.08 / / 1127.80.600.970.10.1022Bal0.1 / 0.10.02

[0201] The magnetic properties and qualified rates of the magnets are shown in Table 11:

[0202] Table 11

[0203] Test No. Br (kGs) Hcj (kOe) Pass rate (%) 1014.4522.097% 1114.4522.097%

[0204] As can be seen from the data in Tables 10 and 11, the Tb content of the magnets of Experiment No. 10 and Experiment No. 11 is basically the same after grain boundary diffusion, and the magnetic properties are also basically the same. The qualified rate after partition diffusion is higher. Within the scope of the present invention, changing the ratio of the diffusion source H1, or replacing the elements of X1 or M1, does not affect the technical effect of the present invention. The H1 diffusion source within the protection scope of the present invention, after partition coating, can effectively improve the mechanical properties of the corners of the NdFeB magnet, reduce the edge and corner missing rate of the product, and has no effect on the magnet performance.

Claims

1. An edge-reinforced RTB rare earth permanent magnet, characterized in that The magnet comprises the following components in mass fractions: R: 28.5~34.0wt.%, R is composed of RL and RH, the content of RH is 0.1wt.%~10.0wt.% of the mass of the magnet, RH is at least one of Dy, Tb, Ho; the remainder of R is RL, RL represents one or more elements selected from Nd, Pr, La, Ce, Er, Gd, Sm, Tm, Lu, Y containing at least light rare earth elements; the light rare earth elements are one or more of La, Ce, Pr, Nd; B: 0.85~1.1wt.%, M: 0.01-8.0wt.%, M represents a plurality of elements selected from Al, Cu, Ga, Ni, Zn, Sn, Mn, Cr, Zr, Ti, and Nb, containing at least M and X, X is one or more of Zr, Ti, and Nb; M is one or more of Al, Ga, and Cu; The balance is T and other unavoidable impurities, T is Fe or Fe and Co; The magnet has at least one surface A, and the light rare earth element content in the corner area of ​​the surface A is not lower than the average light rare earth content of the surface A; the light rare earth element is one or more of La, Ce, Pr, and Nd; and the corner area of ​​the surface A contains X, and X is one or more of Zr, Ti, and Nb.

2. The edge-strengthened RTB rare earth permanent magnet according to claim 1, characterized in that Within the depth range of 0.6 mm vertically from the surface A of the magnet, the X content in the corner area is 0.05-1.2 wt.%; the average X content of the magnet is 0.05-0.8 wt.%.

3. The edge-strengthened RTB rare earth permanent magnet according to claim 1, characterized in that The corner area refers to the surface area within the width range of 0~Kmm from the edge line of the magnet, K is the width of the corner area, and the range of K is 0.2~0.

6. The non-corner area refers to the surface area outside the width range of Kmm from the edge line.

4. The edge-strengthened RTB rare earth permanent magnet according to claim 2, characterized in that The corner body region is a body region enclosed by the corner area and a depth of 0.6 mm vertically away from the surface A; the non-corner body region of the magnet does not contain X, or the X content in the non-corner body region is lower than the X content in the corner body region of the magnet; the non-corner body region is a magnet region outside the corner body region.

5. The edge-strengthened RTB rare earth permanent magnet according to any one of claims 1 to 4, characterized in that The edge-strengthened RTB rare earth permanent magnet is prepared according to the following method: (1) An H1 diffusion source coating area and an H2 diffusion source coating area are set on the diffusion surface of the RTB magnet substrate, and the diffusion sources are coated in different areas. The H1 diffusion source coating area is coated with the diffusion source H1, and the H2 diffusion source coating area is coated with the diffusion source H2; the H1 diffusion source coating area is the corner area of ​​the diffusion surface, and the H2 diffusion source coating area is the non-corner area of ​​the diffusion surface; The diffusion source H1 includes the following components in mass fraction: R1: 50.0~80.0wt.%, R1 includes RL1 and RH1, RH1 is one or more of Dy, Tb, Ho, and accounts for 30.0~70.0wt.% of the mass ratio of H1, and the balance of R1 is RL1, RL1 represents one or more elements selected from Nd, Pr, La, Ce, Er, Gd, Sm, Tm, Lu, Y containing at least light rare earth elements; the light rare earth elements are one or more of La, Ce, Pr, Nd; X1: 10-30wt.%, X1 is one or more of Zr, Ti, and Nb; M1: 5.0~40.0wt.%, M1 is one or more of Al, Ga, and Cu; The diffusion source H2 is one or more mixtures of pure metals, alloys or compounds containing heavy rare earth elements, and the heavy rare earth element is at least one of Dy, Tb and Ho; And the content of heavy rare earth elements in the diffusion source H1 is lower than that in H2; (2) The magnet coated with the diffusion source is subjected to diffusion treatment at a diffusion temperature of 800°C to 1000°C for a holding time of 6 to 30 hours, and then subjected to tempering treatment after cooling to obtain the RTB rare earth permanent magnet.

6. A method for preparing an edge-reinforced RTB rare earth permanent magnet, characterized in that The method comprises the following steps: (1) An H1 diffusion source coating area and an H2 diffusion source coating area are set on the diffusion surface of the RTB magnet substrate, and the diffusion sources are coated in different areas. The H1 diffusion source coating area is coated with the diffusion source H1, and the H2 diffusion source coating area is coated with the diffusion source H2; the H1 diffusion source coating area is the corner area of ​​the diffusion surface, and the H2 diffusion source coating area is the non-corner area of ​​the diffusion surface; The corner area refers to the surface area within the range of 0~Kmm width from the edge line, K is the width of the corner area, and the range of K is 0.2~0.

6. The non-corner area refers to the surface area outside the range of Kmm width from the edge line; The diffusion source H1 includes the following components in mass fraction: R1: 50.0~80.0wt.%, R1 includes RL1 and RH1, RH1 is one or more of Dy, Tb, Ho, and accounts for 30.0~70.0wt.% of the mass ratio of H1, and the balance of R1 is RL1, RL1 represents one or more elements selected from Nd, Pr, La, Ce, Er, Gd, Sm, Tm, Lu, Y containing at least light rare earth elements; the light rare earth elements are one or more of La, Ce, Pr, Nd; X1: 10-30wt.%, X1 is one or more of Zr, Ti, and Nb; M1: 5.0~40.0wt.%, M1 is one or more of Al, Ga, and Cu; The diffusion source H2 is one or more mixtures of pure metals, alloys or compounds containing heavy rare earth elements, and the heavy rare earth element is at least one of Dy, Tb and Ho; And the content of heavy rare earth elements in the diffusion source H1 is lower than that in H2; (2) The magnet coated with the diffusion source is subjected to diffusion treatment at a diffusion temperature of 800°C to 1000°C for a holding time of 6 to 30 hours, and then subjected to tempering treatment after cooling to obtain the RTB rare earth permanent magnet.

7. The method according to claim 6, characterized in that The coating amount of the diffusion source H1 is 0.5~2.0% of the mass of the magnet; the coating amount of the diffusion source H2 is 0.5~2.0% of the mass of the magnet.

8. The method according to claim 6, characterized in that In the step (1), the partition coating diffusion source is achieved by the following method: Use shielding sheet 1 to cover the corner area of ​​the magnet to expose the non-corner area as the H2 diffusion source coating area, and coat the diffusion source H2. Then use shielding sheet 2 to cover the non-corner area of ​​the magnet to expose the corner area of ​​the magnet as the H1 diffusion source coating area, and coat the diffusion source H1; or first use shielding sheet 2 to cover the non-corner area of ​​the magnet to expose the corner area of ​​the magnet as the H1 diffusion source coating area, and coat the diffusion source H1. Then use shielding sheet 1 to cover the corner area of ​​the magnet to expose the non-corner area as the H2 diffusion source coating area, and coat the diffusion source H2.

9. The method according to claim 6, characterized in that When the diffusion source is coated in different areas, the diffusion source is coated by PVD, spraying or printing.

10. The method according to claim 9, characterized in that The partition coating diffusion source adopts screen printing to partition coating diffusion source, which includes the following steps: (a) A hollow area with holes and a shielding area without holes are set on the screen, and the positions of the hollow area and the shielding area of ​​the printing screen are changed according to the product size and the size of the corner area. At least printing screen 1 and printing screen 2 should be included, wherein the hollow area of ​​printing screen 1 corresponds to the non-corner area of ​​the magnet, and the shielding area corresponds to the corner area of ​​the magnet; the hollow area of ​​printing screen 2 corresponds to the corner area of ​​the magnet, and the shielding area corresponds to the non-corner area of ​​the magnet; (b) Align the shielding area of ​​printing screen 1 with the corner area of ​​the magnet, align the hollow area with the non-corner area, as the H2 diffusion source coating area, print the diffusion source H2, and dry it. Then align the shielding area of ​​printing screen 2 with the non-corner area of ​​the magnet, align the hollow area with the corner area of ​​the magnet, as the H1 diffusion source coating area, print the diffusion source H1, and dry it; or use the opposite order to perform zone coating.

Citation Information

Patent Citations

  • R-T-B series permanent magnet material and preparation method and application thereof

    CN110853855A

  • Method for improving coercive force of neodymium-iron-boron magnet through efficient diffusion

    CN113506665A

  • Surface-strengthened R-T-B rare earth permanent magnet based on high-melting-point element grain boundary diffusion and preparation method of surface-strengthened R-T-B rare earth permanent magnet

    CN115732153A

  • Rare earth magnet and method for manufacturing the same

    US20220203440A1

Cited By

  • Sintered neodymium-iron-boron magnet with optimized grain boundary structure and preparation method and application of sintered neodymium-iron-boron magnet

    CN121617763A

  • Neodymium-iron-boron magnet and preparation method thereof

    CN121983424A

  • Sintered neodymium iron boron grain boundary diffusion process and system based on AI vision and multi-material gradient dispensing