A casting method for a casting with a complex blind cavity structure
By combining the split wax mold with a process window in the wax mold production, the problem of insufficient connection strength at the bonding of the casting wax mold is solved, ensuring the quality and structural integrity of the casting.
Patent Information
- Application Number
- CN202211053391.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-31
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2042-08-31
AI Technical Summary
During the wax mold bonding process of castings, since the whole is in a fully enclosed form, the bonding strength is insufficient, and the problems of seams or misalignment are prone to occur, especially in the manufacturing of complex blind cavity structures, where ceramic cores are difficult to remove. Down.
By bonding and combining the split wax mold with a process window in the wax mold production step, the inner surface of the bonding is repaired using the process window to ensure that the connection strength meets the requirements and form a complete wax mold whole.
It effectively avoids insufficient connection strength at the overall bonding of the wax mold, prevents seams or misalignment, solves the problem that the fully enclosed wax mold cannot be repaired in the inner surface, and ensures the quality of the castings.
Smart Images

Figure CN115401167B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a casting method for a casting with a complex blind cavity structure, belonging to the technical field of casting. Background Art
[0002] For a casting 1 with a complex blind cavity structure 11 on its periphery, ceramic core molding can be used during investment casting production if the blind cavity structure is not complex (see Chinese Patent Publication No. CN107999706A, a casting method for a casting with an internal cavity). However, due to the complex blind cavity structure, the ceramic core is difficult to remove from the sand mold shell later using the ceramic core molding method. Therefore, it is necessary to consider the use of wax mold split bonding manufacturing.
[0003] In a method for manufacturing a closed impeller wax mold with Chinese patent publication number CN105344935B, the technology publicly adopted is: the closed impeller wax mold is divided into three parts for separate manufacturing, including a gate wax mold, an internal wax mold and an outer cover wax mold, and the gate wax mold and the outer cover wax mold are bonded to the inner wax mold to complete the manufacturing of the closed impeller wax mold; although the publicly used split wax mold bonding manufacturing does not have a ceramic core, avoiding the situation where the ceramic core is difficult to remove, but after the closed impeller wax mold is formed by bonding the gate wax mold, the internal wax mold and the outer cover wax mold, since the whole formed by the bonding of the wax mold is in a fully enclosed type, there is a problem that the inner surface of the bonding part cannot be repaired, which easily leads to insufficient connection strength at the wax mold bonding part and the occurrence of cracks or dislocations. Summary of the Invention
[0004] In order to solve the above technical problems, the present invention provides a casting method for a casting with a complex blind cavity structure.
[0005] The present invention is achieved through the following technical solutions.
[0006] The present invention provides a casting method for a casting with a complex blind cavity structure, comprising:
[0007] The wax mold assembly step is to repair the inner surface of the bonding part to meet the connection strength requirements to form a wax mold as a whole.
[0008] The wax model assembly steps are: bonding the split wax model and the main wax model together, repairing the inner surface of the bonding point between the split wax model and the main wax model through the process window, so that the connection strength between the split wax model and the main wax model meets the requirements to form a wax model as a whole.
[0009] Before the wax mold assembly step is performed, a wax mold making step is also included.
[0010] The wax model making steps are: using wax material to make a main wax model and a split wax model with a process window based on a casting with a complex blind cavity structure.
[0011] In the wax mold making step: blind cavity interface A, blind cavity interface B, blind cavity interface C, and blind cavity interface D are formed on the main wax mold.
[0012] In the wax model making step: the split wax model consists of four parts, namely, split wax model cover plate A, split wax model cover plate B, split wax model cover plate C, and split wax model cover plate D, all of which are provided with process windows.
[0013] In the wax mold making step: the split wax mold cover plate A, the split wax mold cover plate B, the split wax mold cover plate C, and the split wax mold cover plate D are all integrally fixed with positioning bosses.
[0014] In the wax model making step: the split wax model cover plate A is bonded to the main wax model at the blind cavity interface A through the positioning boss, and the bonding inner surface is repaired through the process window on the split wax model cover plate A;
[0015] The split wax mold cover plate B is bonded to the main wax mold at the blind cavity interface B through the positioning boss, and the inner surface of the bond is repaired through the process window on the split wax mold cover plate B;
[0016] The split wax mold cover plate C is bonded to the main wax mold at the blind cavity interface C through the positioning boss, and the inner surface of the bond is repaired through the process window on the split wax mold cover plate C;
[0017] The split wax mold cover plate D is bonded to the main wax mold at the blind cavity interface D through the positioning boss, and the inner surface of the bond is repaired through the process window on the split wax mold cover plate D. After the process window is assembled to form the overall wax mold, wax material is used to fill it into a solid body.
[0018] The casting comprises a casting having a stepped through hole in the middle and a stepped outer portion;
[0019] Complex blind cavity structures fixed to the outside of the casting.
[0020] The beneficial effect of the present invention is that: since the inner surface of the bonding point during the wax model assembly step can be repaired through the process window on the split wax model, the connection strength of the bonding point between the split wax model and the main wax model meets the requirements to form a wax model as a whole, avoiding the situation where the connection strength of the bonding point constituting the wax model as a whole is insufficient and cracks or misalignments appear, and solves the problem that the whole wax model is in a fully enclosed state and the inner surface of the bonding point cannot be repaired. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 It is a structural schematic diagram of the casting of the present invention;
[0022] Figure 2 This is a top view of the main wax model and the split wax model of the present invention before they are assembled;
[0023] Figure 3 1 is a schematic top view of the main wax model of the present invention;
[0024] Figure 4 1 is a top view of a split wax mold cover plate C in the split wax mold of the present invention;
[0025] Figure 5 1 is a top view schematic diagram of the split wax mold cover plate A, the split wax mold cover plate B, and the split wax mold cover plate D in the split wax mold of the present invention;
[0026] Figure 6 This is a schematic structural diagram of the main wax model and the split wax model of the present invention after being combined;
[0027] In the figure: 1-casting; 11-complex blind cavity structure;
[0028] 21-main wax mold; 221-blind cavity interface A; 212-blind cavity interface B; 213-blind cavity interface C; 214-blind cavity interface D;
[0029] 22-split wax mold; 221-split wax mold cover A; 222-split wax mold cover B; 223-split wax mold cover C; 224-split wax mold cover D;
[0030] 23-process window; 24-positioning boss. DETAILED DESCRIPTION
[0031] The technical solution of the present invention is further described below, but the scope of protection claimed is not limited to the description.
[0032] like Figures 1 to 6 shown.
[0033] The present invention provides a casting method for a casting with a complex blind cavity structure, comprising:
[0034] Step 1, wax mold making: use wax material to make the main wax mold 21 and the split wax mold 22 according to the casting 1 with a complex blind cavity structure 11, and form a blind cavity interface A211, a blind cavity interface B212, a blind cavity interface C213, and a blind cavity interface D214 on the main wax mold 21; a process window 23 is provided on the split wax mold 22, and the split wax mold 22 consists of four split wax mold cover plates A221, a split wax mold cover plate B222, a split wax mold cover plate C223, and a split wax mold cover plate D224, all of which are provided with a process window 23; the split wax mold cover plates A221, the split wax mold cover plates B222, the split wax mold cover plates C223, and the split wax mold cover plates D224 are all integrally fixed with positioning bosses 24.
[0035] Step 2: wax mold assembly: The split wax mold 22 is bonded to the main wax mold 21, and the inner surface of the bonding point between the split wax mold 22 and the main wax mold 21 is repaired through the process window 23, so that the connection strength between the split wax mold 22 and the main wax mold 21 meets the requirements to form a wax mold as a whole, avoiding the situation where the bonding strength of the wax mold as a whole is insufficient and cracks or dislocations occur, solving the problem that the wax mold as a whole is in a fully enclosed state and cannot be repaired on the inner surface of the bonding point;
[0036] Specifically, the split wax mold cover A221 is bonded to the main wax mold 21 at the blind cavity interface A211 through the positioning boss 24, and the inner surface of the bond is repaired through the process window 23 on the split wax mold cover A221;
[0037] The split wax mold cover plate B222 is bonded to the main wax mold 21 at the blind cavity interface B212 through the positioning boss 24, and the inner surface of the bond is repaired through the process window 23 on the split wax mold cover plate B222;
[0038] The split wax mold cover plate C223 is bonded to the main wax mold 21 at the blind cavity interface C213 through the positioning boss 24, and the inner surface of the bond is repaired through the process window 23 on the split wax mold cover plate C223;
[0039] The split wax mold cover plate D224 is bonded to the main wax mold 21 at the blind cavity interface D214 via the positioning boss 24, and the inner surface of the bond is repaired through the process window 23 on the split wax mold cover plate D224. The process window 23 is filled with wax to form a solid body after the whole wax mold is assembled.
[0040] After the wax mold assembly is completed, shell making, dewaxing, roasting, melting and pouring are carried out in sequence to form a casting 1 with a complex blind cavity structure 11. Since shell making, dewaxing, roasting, melting and pouring are existing technologies, they will not be repeated here.
[0041] The molded casting 1 includes a casting 1 with a stepped through hole in the middle and a stepped outer portion of the casting 1;
[0042] A complex blind cavity structure 11 is integrally formed and fixed to the outside of the casting 1 .
[0043] Since the inner surface of the bonding point during the wax model assembly step can be repaired through the process window 23 on the split wax model 22, the connection strength at the bonding point between the split wax model 22 and the main wax model 21 meets the requirements to form a wax model as a whole, avoiding the situation where the connection strength of the bonding point constituting the wax model as a whole is insufficient and cracks or misalignments occur, and solving the problem that the wax model as a whole is in a fully enclosed state and the inner surface of the bonding point cannot be repaired.
Claims
1. A casting method for a casting with a complex blind cavity structure, characterized in that: include: The wax model assembly step is to repair the inner surface of the bonding part to meet the connection strength requirements to form a wax model as a whole; The wax model assembly step comprises: bonding and assembling the split wax model (22) and the main wax model (21), repairing the inner surface of the bonding point between the split wax model (22) and the main wax model (21) through the process window (23), so that the connection strength of the bonding point between the split wax model (22) and the main wax model (21) meets the requirements to form a wax model as a whole; Before the wax model assembly step, the method further includes a wax model making step; The wax model making steps are: using wax material to make a main wax model (21) and a split wax model (22) provided with a process window (23) according to a casting (1) with a complex blind cavity structure (11); In the wax model making step: a blind cavity interface A (211), a blind cavity interface B (212), a blind cavity interface C (213), and a blind cavity interface D (214) are formed on the main wax model (21); In the wax model making step: the split wax model (22) is composed of four parts, namely, a split wax model cover plate A (221), a split wax model cover plate B (222), a split wax model cover plate C (223), and a split wax model cover plate D (224), all of which are provided with a process window (23); In the wax model making step: the split wax model cover plate A (221), the split wax model cover plate B (222), the split wax model cover plate C (223), and the split wax model cover plate D (224) are all integrally fixed with a positioning boss (24); In the wax model making step: the split wax model cover plate A (221) is bonded to the main wax model (21) at the blind cavity interface A (211) via the positioning boss (24), and the inner surface of the bonding is repaired via the process window (23) on the split wax model cover plate A (221); The split wax mold cover plate B (222) is bonded to the main wax mold (21) at the blind cavity interface B (212) via the positioning boss (24), and the inner surface of the bond is repaired via the process window (23) on the split wax mold cover plate B (222); The split wax mold cover plate C (223) is bonded to the main wax mold (21) at the blind cavity interface C (213) via the positioning boss (24), and the inner surface of the bond is repaired via the process window (23) on the split wax mold cover plate C (223); The split wax mold cover plate D (224) is bonded to the main wax mold (21) at the blind cavity interface D (214) through the positioning boss (24), and the inner surface of the bond is repaired through the process window (23) on the split wax mold cover plate D (224); The process window (23) is filled with wax material to form a solid body after the whole wax model is assembled; After the wax mold is assembled, shell making, dewaxing, roasting, smelting and pouring are performed in sequence to form a casting (1) with a complex blind cavity structure (11); The molded casting (1) has a stepped through hole in the middle and a stepped shape on the outside; The complex blind cavity structure (11) is fixed outside the casting (1).