A high thermal conductivity plastic thermal conductive mud and preparation method thereof

Through the combination of high-mass ratio alumina and volatile carriers, high thermal conductivity and easy-to-shape thermal conductive mud is prepared, which solves the problems of low thermal conductivity and poor stability, achieving significant improvement in thermal conductivity and efficient heat dissipation of electronic devices.

CN115404051BActive Publication Date: 2024-10-08NINGBO JULI NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211168657.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-24
Publication Date
2024-10-08
Estimated Expiration
2042-09-24

AI Technical Summary

Technical Problem

The thermal conductivity of existing thermal mud is low and cannot meet the higher thermal conductivity requirements of electronic devices in the 5G era. Moreover, thermal conductive materials on the market have problems with poor storage stability and poor processing plasticity.

Method used

Alumina with a high mass ratio is used as a combination of thermally conductive filler and carrier silicone oil. Volatile carriers such as dimethyl carbonate, 3# white mineral oil and octamethylcyclotetrasiloxane are added to improve the thermal conductivity network through modification and dispersion technology. Density and stability, high thermal conductivity and easy molding of thermal mud are prepared.

Benefits of technology

It significantly increases the thermal conductivity of thermal mud to above 10W/m.K, solves the problems of low thermal conductivity and poor stability, and improves the heat dissipation effect and storage stability of electronic devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003862580150000061
    Figure BDA0003862580150000061
Patent Text Reader

Abstract

The invention discloses a high thermal conductivity plastic thermal conductive mud and a preparation method thereof. The high thermal conductivity plastic thermal conductive mud comprises a carrier silicone oil and a thermal conductive filler, wherein the thermal conductive filler comprises at least alumina, and the mass ratio of the carrier silicone oil to the alumina is 1: (60-100). The preparation method is as follows: the carrier silicone oil, the volatile carrier, the alkoxy silicone oil and the hexamethyldisilazane are evenly dispersed, and then the alumina is added, stirred evenly, kept warm at 60-90°C for 30-90min, and then the temperature is increased and heated to a volatile content of less than 1%, and the high thermal conductivity plastic thermal conductive mud is obtained by refining after cooling. The present application performs a large amount of alumina filling by a specific method, so that the thermal conductivity effect of the established thermal conductive network is improved, thereby breaking through the limitation of the low thermal conductivity coefficient of the original thermal conductive mud, and the thermal conductivity coefficient of the thermal conductive mud is increased to more than 10 W / mK.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of thermal conductive materials, and in particular to a high thermal conductive and easily plastic thermal conductive mud and a preparation method thereof. Background Art

[0002] The power loss during the operation of electronic devices is mainly converted into heat energy, which causes the temperature of electronic equipment to rise and the thermal stress to increase, which has a serious impact on the reliability and service life of electronic devices. Therefore, this excess heat needs to be dissipated as quickly as possible.

[0003] Thermal interface materials can fill the micro gaps created by the contact between electronic devices and heat sinks, reducing the thermal resistance of heat transfer, and are widely used in heat dissipation of electronic devices.

[0004] With the advent of the 5G era, the power consumption of various electronic devices has increased significantly, and the heat generated has also increased significantly, which has put higher requirements and challenges on the thermal conductivity of thermal interface materials.

[0005] Common thermal interface materials on the market include thermal grease, thermal gaskets, and thermal mud. Among them, thermal grease has poor storage stability and is prone to oil-powder separation until the heat dissipation effect is lost. Thermal gaskets need to be pre-cut into the required size, and a lot of scraps are produced, resulting in a high waste rate. In order to improve the thermal conductivity, it is necessary to solve the problem of high filling amount of fillers. When less thermal conductive fillers are added, there is less contact between the thermal conductive fillers, the thermal conductive network is sparse and the thermal conductivity is not high. When the thermal conductive fillers are added beyond the thermal conductivity threshold, the thermal conductive fillers are in close contact, the thermal conductive network is complete and the thermal conductivity is high. Thermal mud has the advantages of on-site molding and easy assembly, and is a highly competitive thermal interface material. However, the thermal conductivity of the thermal conductive mud on the market is currently low, so it is urgent to break through the limitation of the low thermal conductivity of the thermal conductive mud and develop a thermal conductive mud with a higher thermal conductivity. Summary of the invention

[0006] In order to provide a thermal conductive mud with a high thermal conductivity coefficient, the present application provides a highly plastic thermal conductive mud and a preparation method thereof.

[0007] In the first aspect, the present application provides a high thermal conductivity and easy-to-plastic thermal conductive mud, which adopts the following technical solution:

[0008] A high thermal conductivity and easy-to-plastic thermal conductive mud comprises carrier silicone oil and a thermal conductive filler, wherein the thermal conductive filler contains at least aluminum oxide, and the mass ratio of the carrier silicone oil to the aluminum oxide is 1:(60-100).

[0009] The high thermal conductivity and easy-to-plastic thermal conductive mud prepared in the present application uses alumina as a thermal conductive filler, and the mass ratio of alumina to the carrier silicone oil is as high as 60-100:1. The thermal conductivity effect of the established thermal conductive network is improved by filling a large amount of alumina, thereby breaking through the limitation of the low thermal conductivity coefficient of the original thermal conductive mud, and the thermal conductivity coefficient of the thermal conductive mud is increased to above 10W / mK. Therefore, the high thermal conductivity and easy-to-plastic thermal conductive mud prepared in the present application can better adapt to the use requirements of electronic devices with higher thermal conductivity requirements.

[0010] Preferably, during the preparation of the highly thermally conductive and easily plastic thermally conductive mud, a volatile carrier is added, and the mass ratio of the volatile carrier to alumina is 1:(60-100).

[0011] The thermal conductive mud prepared in the present application is filled with a large amount of alumina filler, but as the filler increases, the product processing plasticity is poor and difficult to fill, and the unstable situation of oil-powder separation is prone to occur.

[0012] The volatile carrier is mainly used to improve the contact efficiency of the stabilizer with alumina and improve the modification effect. It ensures the plasticity of the thermal conductive mud. At the later stage, the volatile carrier can be removed by increasing the temperature and vacuum degree to increase the filling rate of the thermal conductive filler to achieve the purpose of high thermal conductivity.

[0013] By adding one or more of volatile dimethyl carbonate, 3# white mineral oil, and octamethylcyclotetrasiloxane as carriers and in combination with carrier silicone oil, the alumina content in the product can be greatly increased, and the processing process is less likely to have poor plasticity and difficulty in filling.

[0014] Preferably, the volatile carrier has a boiling point greater than 90°C.

[0015] Preferably, it is a combination of one or more of dimethyl carbonate, 3# white mineral oil and octamethylcyclotetrasiloxane.

[0016] Dimethyl carbonate, 3# white mineral oil, octamethylcyclotetrasiloxane and other volatile components can increase the filling of alumina, helping to overcome the problems of poor processing plasticity and difficulty in filling after adding a large amount of alumina. At the same time, the boiling points of dimethyl carbonate, 3# white mineral oil and octamethylcyclotetrasiloxane are greater than 90°C, ensuring that the alumina is stably dispersed based on the presence of the volatile carrier before the alumina is heated to the temperature required for modification. The storage stability of the alumina is improved after modification, thereby reducing the occurrence of oil-powder separation. The temperature is then raised to volatilize the volatile carrier, which can further increase the filling ratio of alumina.

[0017] Preferably, the thermally conductive filler may also include one or more of zinc oxide, boron nitride and aluminum nitride.

[0018] Thermally conductive fillers such as zinc oxide, boron nitride, and aluminum nitride can be added without affecting product performance.

[0019] Preferably, the alumina is spherical alumina.

[0020] Compared with other thermally conductive fillers, after the addition of dimethyl carbonate, 3# white mineral oil and octamethylcyclotetrasiloxane, spherical alumina can be filled at a high density as a thermally conductive material. By filling a large amount of spherical alumina, a rich thermally conductive network structure is constructed, breaking through the limitation of the low thermal conductivity of the original thermal conductive mud.

[0021] Preferably, during the preparation of the high thermal conductivity and easy-to-plastic thermal conductive mud, a stabilizing agent is also added. The stabilizing agent is compounded with carrier silicone oil, alkoxy silicone oil and hexamethylsilazane. The mass ratio of the alkoxy silicone oil to alumina is 10-20:1000, and the mass ratio of the hexamethylsilazane to alumina is 1-6:2000.

[0022] The presence of the volatile carrier increases the contact probability of the stabilizing agent with the thermal conductive powder, improves the surface modification ability of the thermal conductive powder, and improves the plasticity and stability of the thermal conductive mud.

[0023] Preferably, the viscosity of the alkoxy silicone oil is 10-300 mPa.s (25° C.), preferably 10-100 mPa.s (25° C.).

[0024] By selecting alkoxy silicone oil with lower viscosity, the reactivity of alumina with other components can be improved, thereby facilitating the surface modification reaction of alumina and improving the storage stability of alumina.

[0025] Preferably, the alkoxy silicone oil is one of methoxy silicone oil and ethoxy silicone oil, or a combination of the two.

[0026] A method for preparing a high thermal conductivity plastic thermal conductive mud comprises the following steps:

[0027] The carrier silicone oil, volatile carrier, alkoxy silicone oil and hexamethyldisilazane are mixed and dispersed evenly, then alumina is added, stirred evenly, kept warm at 60-90°C for 30-90 minutes, then the temperature is increased and heated to less than 1% of the volatile matter, cooled and then refined to obtain a high thermal conductivity and easy-to-shape thermal conductive mud.

[0028] After the components are evenly mixed, they are kept warm at 60-90°C for 30-90 minutes. The alkoxy silicone oil absorbs moisture on the surface of the filler and in the air and hydrolyzes to form hydroxyl silicone oil and small molecule alcohol. The hexamethylsilazane absorbs moisture on the surface of the filler and in the air and partially hydrolyzes to form silicon hydroxyl compounds. The hydrolysis products of the alkoxy silicone oil, the hydrolysis products of the hexamethylsilazane, and the hydroxyl groups on the surface of alumina condense with some hydroxyl groups of the carrier silicone oil, thereby improving the surface of the powder, increasing the storage stability between the oil and powder, and effectively preventing the oil and powder separation that is prone to occur when alumina is filled with more alumina, thereby improving the thermal conductivity of the product. The temperature is further increased and heated to a volatile content of less than 1%, and the by-products and volatile carriers are removed to increase the overall filler ratio, thereby improving the thermal conductivity of the product.

[0029] There is no special requirement for the mixing equipment, as long as it can meet the heating and vacuuming capabilities. Planetary dispersers, high-speed mixers and other equipment can be selected.

[0030] Preferably, the alumina is added in three times, 50-60wt% in the first time, 25-35wt% in the second time, and 10-25%wt% in the third time.

[0031] Adding alumina in batches is beneficial to improving the full dispersion of alumina and improving the dispersion efficiency of alumina.

[0032] In summary, this application has the following beneficial effects:

[0033] 1. The high thermal conductivity and easy-to-plastic thermal conductive mud prepared in this application uses alumina as a thermal conductive filler, and its mass ratio to the carrier silicone oil is as high as 60-100:1, which is conducive to breaking through the limitation of the low thermal conductivity of the original thermal conductive mud and increasing the thermal conductivity of the thermal conductive mud to more than 10W / mK.

[0034] 2. Compared with other filling materials, after the addition of dimethyl carbonate, 3# white mineral oil and octamethylcyclotetrasiloxane, spherical alumina can be filled at a high density as a thermal conductive material. By filling a large amount of spherical alumina to construct a rich thermal conductive network structure, the limitation of the low thermal conductivity of the original thermal conductive mud can be broken through.

[0035] 3. Dimethyl carbonate, 3# white mineral oil, octamethylcyclotetrasiloxane and other volatile components can increase the filling of alumina, helping to overcome the problems of poor processing plasticity and difficulty in filling after adding a large amount of alumina. At the same time, the boiling points of dimethyl carbonate, 3# white mineral oil and octamethylcyclotetrasiloxane are greater than 90°C, ensuring that the alumina is stably dispersed based on the presence of the volatile carrier before being heated to the temperature required for modification. The storage stability of alumina is improved after modification, thereby reducing the occurrence of oil-powder separation. The temperature is then raised to volatilize the volatile carrier, which can further increase the filling ratio of alumina. DETAILED DESCRIPTION

[0036] Experiment 1

[0037] A method for preparing a high thermal conductivity plastic thermal conductive mud is as follows:

[0038] 20g MDT silicone oil, 20g 3# white mineral oil, 10g ethoxy silicone oil and 1g hexamethyldisilazane were put into a dynamic mixer and dispersed for 10 minutes. The dispersion was uniform. Then 1200g spherical alumina was added in three steps, 60wt% for the first time, 30wt% for the second time, and 10wt% for the third time. After stirring evenly, the mixture was kept warm at 90°C for 30 minutes, and then the temperature was raised to 177°C, -0.098MPa, and vacuum heated until the volatile matter was less than 1%. After cooling, the mixture was refined on an open mill to obtain a high thermal conductivity and easy-to-plastic thermal conductive mud.

[0039] Experiment 2

[0040] A method for preparing a high thermal conductivity plastic thermal conductive mud is as follows:

[0041] 20g MDT silicone oil, 20g dimethyl carbonate, 30g ethoxy silicone oil and 3g hexamethyldisilazane were put into a dynamic mixer and dispersed for 10 minutes. The dispersion was uniform. Then 2000g spherical alumina was added in three steps, 60wt% for the first time, 30wt% for the second time and 10wt% for the third time. After stirring evenly, the mixture was kept warm at 60°C for 90min, then heated to 150°C, heated at -0.098MPa and vacuum heated until the volatile matter was less than 1%. After cooling, the mixture was refined on an open mill to obtain a highly thermally conductive and easily plastic thermal conductive mud.

[0042] Example 3

[0043] A method for preparing a high thermal conductivity plastic thermal conductive mud is as follows:

[0044] 20g MDT silicone oil, 20g octamethylcyclotetrasiloxane, 28g ethoxy silicone oil and 3g hexamethyldisilazane were put into a dynamic mixer and dispersed for 10 minutes. The dispersion was uniform. Then 1400g spherical alumina was added in three steps, 60wt% for the first time, 30wt% for the second time, and 10wt% for the third time. After stirring evenly, the mixture was kept warm at 80°C for 60min, then heated to 150°C, heated at -0.098MPa and vacuum heated until the volatile matter was less than 1%. After cooling, the mixture was refined on an open mill to obtain a highly thermally conductive and easily plastic thermal conductive mud.

[0045] Example 4

[0046] A method for preparing a high thermal conductivity plastic thermal conductive mud is as follows:

[0047] 20g MDT silicone oil, 20g octamethylcyclotetrasiloxane, 32g ethoxy silicone oil and 3g hexamethyldisilazane were put into a dynamic mixer and dispersed for 10 minutes. The dispersion was uniform. Then 1600g spherical alumina was added in three steps, 60wt% for the first time, 30wt% for the second time, and 10wt% for the third time. After stirring evenly, the mixture was kept warm at 80°C for 60min, then heated to 150°C, heated to a volatile matter of less than 1%, cooled and then refined on an open mill to obtain a high thermal conductivity and easy-to-plastic thermal conductive mud.

[0048] Example 5

[0049] A method for preparing a high thermal conductivity plastic thermal conductive mud is as follows:

[0050] 20g of the intermediate of the partial cross-linking reaction of vinyl silicone oil and hydrogen-containing silicone oil, 20g of octamethylcyclotetrasiloxane, 30g of ethoxy silicone oil and 3g of hexamethyldisilazane were put into a dynamic mixer and dispersed for 10 minutes. The dispersion was uniform. Then, 1600g of spherical alumina was added in three steps, 60wt% for the first time, 30wt% for the second time, and 10wt% for the third time. After stirring evenly, 200g of aluminum nitride was added. The mixture was kept warm at 80°C for 60 minutes, and then the temperature was raised to 150°C and heated until the volatile matter was less than 1% to obtain a high thermal conductivity and easy-to-plastic thermal conductive mud.

[0051] Comparative Example 1

[0052] A method for preparing a high thermal conductivity plastic thermal conductive mud is as follows:

[0053] 20g of MDT silicone oil, 28g of ethoxy silicone oil and 3g of hexamethyldisilazane were put into a dynamic mixer and dispersed for 10 minutes. Then 840g of spherical alumina was put into the mixer. Since no volatile carrier was added, the dynamic mixer of the equipment was overloaded and could not operate normally.

[0054] Comparative Example 2

[0055] A method for preparing a high thermal conductivity plastic thermal conductive mud is as follows:

[0056] 40g MDT silicone oil, 32g ethoxy silicone oil and 3g hexamethyldisilazane were put into a dynamic mixer and dispersed for 10 minutes. The dispersion was uniform. Then 1600g spherical alumina was added in three steps, 60wt% for the first time, 30wt% for the second time and 10wt% for the third time. After stirring evenly, the mixture was kept warm at 80°C for 60 minutes, then heated to 150°C, heated to a volatile matter of less than 1%, cooled and then refined on an open mill to obtain a highly thermally conductive and easily plastic thermal conductive mud.

[0057] Comparative Example 3

[0058] A method for preparing a high thermal conductivity plastic thermal conductive mud is as follows:

[0059] 20g MDT silicone oil, 20g octamethylcyclotetrasiloxane, 5g ethoxy silicone oil and 26g hexamethyldisilazane were put into a dynamic mixer and dispersed for 10 minutes. The dispersion was uniform. Then 1400g spherical alumina was added in three steps, 60wt% for the first time, 30wt% for the second time, and 10wt% for the third time. After stirring evenly, the mixture was kept warm at 80°C for 60min, then heated to 150°C, heated at -0.098MPa and vacuum heated until the volatile matter was less than 1%. After cooling, the mixture was refined on an open mill to obtain a high thermal conductivity and easy-to-plastic thermal conductive mud.

[0060] Comparative Example 4

[0061] A method for preparing a high thermal conductivity plastic thermal conductive mud is as follows:

[0062] 20g MDT silicone oil, 20g octamethylcyclotetrasiloxane and 31g ethoxy silicone oil were put into a dynamic mixer and dispersed for 10 minutes. Then, 1400g spherical alumina was added in three steps, 60wt% for the first time, 30wt% for the second time and 10wt% for the third time. After stirring evenly, the mixture was kept warm at 80°C for 60min, then heated to 150°C and kept warm for 2h. After cooling, the mixture was refined on an open mill to obtain a highly thermally conductive and easily plastic thermal conductive mud.

[0063] experiment

[0064] The performance of the highly thermally conductive and easily plastic thermally conductive mud prepared in the above embodiments and comparative examples was tested.

[0065] Thermal conductivity: The test method is carried out in accordance with ASTM D5470. The thermal conductive paste is applied on the test table of the Hotdisk tester by screen printing. The thickness is controlled at 0.075mm for thermal conductivity test.

[0066] Breakdown voltage: The test method is carried out according to ASTM D149 to test the breakdown voltage of the thermal conductive mud prepared in the above embodiments and comparative examples.

[0067] Storage stability evaluation: The thermal conductive pastes prepared in the above embodiments and comparative examples were stored at 50° C. for 30 days, and the appearance of the thermal conductive pastes was observed.

[0068] Evaluation of stability and adaptability in extreme environments: The thermal conductive mud prepared in the above embodiments and comparative examples was cycled 1000 times at -40°C for 30 min and 125°C for 30 min, and the appearance of the thermal conductive mud was observed.

[0069] The test results are shown in Table 1.

[0070] Table 1

[0071]

[0072] From the comparison of the data of Example 3 and Comparative Example 2 in Table 1, it can be seen that by adding MDT silicone oil instead of octamethylcyclotetrasiloxane, the thermal conductivity of the thermal conductive mud prepared in Comparative Example 2 is significantly lower than that of Example 3, which proves that after octamethylcyclotetrasiloxane is heated and volatilized, it is beneficial to improve the thermal conductivity of the thermal conductive mud.

[0073] From the data comparison of Example 3 with Comparative Examples 3 and 4 in Table 1, it can be obtained that the stabilizing agent of Example 3 is composed of 28g ethoxy silicone oil and 3g hexamethyldisilazane, the stabilizing agent of Comparative Example 3 is composed of 10g ethoxy silicone oil and 21g hexamethyldisilazane, and the stabilizing agent of Comparative Example 4 is 31g ethoxy silicone oil. The thermal conductive mud prepared in Example 3 has stable storage and good adaptability to extreme environments. After testing, it was found that oil-powder separation is not easy to occur. The thermal conductive muds prepared in Comparative Examples 3 and Comparative Examples 4 have poor stability and are very prone to oil-powder separation. It is proved that the combination of ethoxy silicone oil and hexamethyldisilazane in a specific ratio has a very outstanding effect on improving the stability of the thermal conductive mud.

[0074] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A high thermal conductivity plastic thermal conductive mud, characterized by: It includes carrier silicone oil and thermal conductive filler, wherein the thermal conductive filler contains at least alumina, and the mass ratio of the carrier silicone oil to the alumina is 1:(60-100); During the preparation of the highly thermally conductive and easily plastic thermal conductive mud, a stabilizing agent is also added. The stabilizing agent is compounded from alkoxy silicone oil and hexamethylsilazane. The mass ratio of the alkoxy silicone oil to alumina is 10-20:1000, and the mass ratio of the hexamethylsilazane to alumina is 1-6:2000.

2. The high thermal conductivity plastic thermal conductive mud according to claim 1, characterized in that: During the preparation of the highly thermally conductive and easily plastic thermally conductive mud, a volatile carrier is added, and the mass ratio of the volatile carrier to alumina is 1: (60-100).

3. The high thermal conductivity plastic thermal conductive mud according to claim 2, characterized in that: The volatile carrier has a boiling point greater than 90°C.

4. A high thermal conductivity plastic thermal conductive mud according to claim 2 or 3, characterized in that: The volatile carrier is one or a combination of dimethyl carbonate, 3# white mineral oil, and octamethylcyclotetrasiloxane.

5. The high thermal conductivity plastic thermal conductive mud according to claim 1, characterized in that: The aluminum oxide is spherical aluminum oxide.

6. The high thermal conductivity plastic thermal conductive mud according to claim 1, characterized in that: The thermal conductive filler may also include one or more of zinc oxide, boron nitride, and aluminum nitride.

7. A method for preparing a highly thermally conductive and plastic thermally conductive mud according to claim 1, characterized in that: The viscosity of the alkoxy silicone oil at 25° C. is 10-300 mPa.s.

8. The method for preparing a highly thermally conductive and plastic thermally conductive mud according to claim 1, characterized in that: The alkoxy silicone oil is one of methoxy silicone oil and ethoxy silicone oil, or a combination of the two.

9. A method for preparing a highly thermally conductive and easily plastic thermally conductive mud according to any one of claims 1 to 8, characterized in that: The carrier silicone oil, volatile carrier, alkoxy silicone oil and hexamethyldisilazane are mixed and dispersed evenly, and then alumina is added and stirred evenly. The mixture is kept at 60-90°C for 30-90 minutes, and then the temperature is increased and heated until the volatile matter is less than 1%. After cooling, the mixture is kneaded and mixed to obtain a high thermal conductivity and easy-to-shape thermal conductive mud.