A method for manufacturing a seamless steel pipe by continuously casting round billets of high carbon chromium bearing steel
Through the segmented heating and annealing process of continuous casting round billets, high carbon chromium bearing steel seamless steel pipes are directly produced, which solves the problems of complex traditional processes and low yield rate, and achieves performance standards and cost reduction.
Patent Information
- Application Number
- CN202211037974.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-26
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-08-26
AI Technical Summary
The production process of high-carbon chromium bearing steel is complex, the yield is low, and it is difficult to meet the liquid separation, micropore and other indicators of the YB/T 4146-2016 standard, resulting in high production costs and long production cycles.
The manufacturing method uses continuous-cast round billets for segmented heating, perforation, pipe rolling, diameter reduction, cooling and spheroidizing annealing, omitting the high-temperature diffusion process and directly producing standard seamless steel pipes.
The process flow is simplified, the yield rate is increased, and the production cost is reduced. The liquid separation, microstructure and other properties of the steel pipe comply with the YB/T 4146-2016 standard, and the delivery time is shortened.
Smart Images

Figure CN115415325B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metal pressure processing, and specifically relates to a method for manufacturing a seamless steel pipe by continuously casting round billets of high-carbon chromium bearing steel. Background Art
[0002] Direct hot rolling of continuous casting round billets into tubes has the advantages of high yield rate, low production cost and short production cycle. At present, ordinary carbon structural steel and alloy structural steel have achieved direct hot rolling of seamless steel tubes from "continuous casting round billets", while high carbon chromium bearing steel can only use "rolled round billets" and "forged round billets" as tube billets to roll seamless steel tubes.
[0003] High carbon chromium bearing steel is a hypereutectoid steel due to its special chemical composition. Its smelting and heating processes are different from those of conventional steel products. When continuous casting round billets are used to directly produce seamless steel pipes for high carbon chromium bearings, the liquid analysis, micropores and other indicators of the steel pipes are difficult to meet the requirements of the YB / T 4146-2016 standard.
[0004] The traditional production process of high carbon chromium bearing tubes is to produce round tube billets from continuous casting billets in electric furnaces or converters through forging or rolling mills. The intermediate billets need to undergo long-term high-temperature diffusion. In addition, the rolled and forged billets need to be softened and annealed to facilitate the sawing of the tube billets. Therefore, the traditional production process of high carbon chromium bearing tubes is complicated, the production cycle is long, and the comprehensive yield rate of the steel tubes is low.
[0005] Therefore, it is urgent to develop a method for manufacturing high-carbon chromium bearing tubes with simple process and high yield. Summary of the invention
[0006] In view of the shortcomings of the prior art, the present application provides a method for manufacturing seamless steel pipes from continuously cast round billets of high carbon chromium bearing steel, so as to solve the problems of low yield and high production cost in producing steel pipes from rolled and forged round billets of high carbon chromium bearing steel.
[0007] To achieve the above object, the present invention adopts the following technical solutions:
[0008] A method for manufacturing a seamless steel pipe made of high carbon chromium bearing steel continuous casting round billet, using a solid continuous casting round billet as a billet, and directly hot-rolling a seamless steel pipe using a continuous casting round billet, the manufacturing method comprises the following steps: billet heating, perforation, tube rolling, diameter reduction, cooling and heat treatment; wherein,
[0009] In the billet heating process, a segmented heating method is adopted to heat the solid continuous casting round tube billet, and the set heating temperature of the billet heating is 750-1230°C; the billet heating includes a preheating section, a heating section, a heating section, a heating section, a heating section, a heating section and a soaking section; the heating rate of the heating section is 80-150°C / h; the heating rate of the heating section is 80-150°C / h.
[0010] In the above manufacturing method, as a preferred embodiment, in the billet heating process, the set temperature of the preheating section is ≤750℃ (for example, 500℃, 550℃, 600℃, 650℃, 700℃, 740℃), and the heating rate is 300-600℃ / h (for example, 350℃ / h, 400℃ / h, 450℃ / h, 500℃ / h, 550℃ / h, 580℃ / h), that is, the furnace temperature is raised to the preheating temperature at a rate of 300-600℃ / h; preferably, the set temperature of the preheating section is 650℃-750℃ (for example, 660℃, 680℃, 700℃, 720℃, 730℃, 740℃).
[0011] In the above manufacturing method, as a preferred embodiment, in the billet heating process, the set temperature of the heating section is 800-890°C (for example, 810°C, 830°C, 850°C, 870°C, 880°C), and the heating rate is 80-150°C / h (for example, 90°C / h, 100°C / h, 110°C / h, 120°C / h, 130°C / h, 140°C / h), that is, the furnace temperature is raised to the set temperature of the heating section at a rate of 80-150°C / h.
[0012] In the above manufacturing method, as a preferred embodiment, in the billet heating process, the set temperature of the second heating stage is 910-1000°C (for example, 910°C, 930°C, 950°C, 970°C, 980°C), and the heating rate is 80-150°C / h (for example, 90°C / h, 100°C / h, 110°C / h, 120°C / h, 130°C / h, 140°C / h), that is, the furnace temperature is raised to the set temperature of the second heating stage at a rate of 80-150°C / h.
[0013] In the above manufacturing method, as a preferred embodiment, in the billet heating process, the set temperature of the three heating stages is 1070-1160°C (for example, 1080°C, 1100°C, 1120°C, 1130°C, 1150°C), and the heating rate is 130-200°C / h (for example, 140°C / h, 150°C / h, 160°C / h, 170°C / h, 180°C / h, 190°C / h), that is, the furnace temperature is raised to the set temperature of the three heating stages at a rate of 130-200°C / h.
[0014] In the above manufacturing method, as a preferred embodiment, in the billet heating process, the set temperature of the four heating stages is 1161-1230°C (for example, 1170°C, 1180°C, 1190°C, 1200°C, 1210°C, 1220°C), and the heating rate is 130-200°C / h (for example, 140°C / h, 150°C / h, 160°C / h, 170°C / h, 180°C / h, 190°C / h), that is, the furnace temperature is raised to the set temperature of the four heating stages at a rate of 130-200°C / h.
[0015] In the above manufacturing method, as a preferred embodiment, in the billet heating process, the insulation temperature of the equalizing section is 1161-1230°C (for example, 1170°C, 1180°C, 1190°C, 1200°C, 1210°C, 1220°C), and the insulation time is ≥220min.
[0016] In the present invention, in the billet heating process, the heating rate of the low temperature section (i.e., heating section one and heating section two) is gradually slowed down, which is beneficial to the uniformity of billet heating. At the same time, the uniformity of billet temperature is beneficial to the high temperature (heating section four and equalizing section) diffusion of high carbon chromium bearing steel, that is, it ensures that the temperature of high carbon chromium bearing steel diffuses uniformly from the surface to the inside when heated or equalized at high temperature, thereby improving the microscopic pores and liquid separation of the steel.
[0017] In the above manufacturing method, as a preferred embodiment, the diameter of the blank is It is preferably greater than 300 mm and less than or equal to 360 mm.
[0018] In the above manufacturing method, as a preferred embodiment, the specification of the seamless steel pipe prepared by the method is an outer diameter of Wall thickness: 16~70mm.
[0019] In the above manufacturing method, as a preferred embodiment, the total heating time of each segment and the total heating time of the soaking section in the billet heating process are determined according to the billet diameter range.
[0020] In the above manufacturing method, as a preferred embodiment, in the blank heating step, the blank diameter is The total heating time from the time the billet enters the preheating section to the time the billet leaves the preheating section is ≥30min (for example, 40min, 50min, 60min, 70min, 80min), the total heating time from the time the billet enters the heating section to the time the billet leaves the heating section is ≥110min (for example, 130min, 140min, 160min, 170min, 180min), and the total heating time from the time the billet enters the equalizing section to the time the billet leaves the equalizing section is ≥220min (for example, 230min, 250min, 280min, 300min); the total time of the billet heating process is 360-560min (for example, 380min, 400min, 420min, 450min, 480min, 500min).
[0021] In the above manufacturing method, as a preferred embodiment, in the billet heating process, when the billet diameter is greater than 300 mm and less than or equal to 360 mm, the total heating time from the billet entering the preheating section to the billet leaving the preheating section is ≥40 min (for example, 50 min, 60 min, 70 min, 80 min, 90 min, 100 min), the total heating time from the billet entering the heating section to the billet leaving the heating section is ≥120 min (for example, 130 min, 140 min, 160 min, 180 min, 200 min), and the total heating time from the billet entering the equalizing section to the billet leaving the equalizing section is ≥240 min (for example, 250 min, 280 min, 300 min, 320 min); the total time of the billet heating process is 400-600 min (for example, 430 min, 450 min, 500 min, 550 min, 580 min).
[0022] In the above manufacturing method, as a preferred embodiment, in the billet heating process, when the billet diameter is greater than 360 mm and less than or equal to 430 mm, the total heating time from the billet entering the preheating section to the billet leaving the preheating section is ≥60 min (for example, 70 min, 80 min, 90 min, 100 min, 110 min, 120 min), the total heating time from the billet entering the heating section to the billet leaving the heating section is ≥160 min (for example, 170 min, 180 min, 200 min, 220 min, 240 min), and the total heating time from the billet entering the equalizing section to the billet leaving the equalizing section is ≥260 min (for example, 210 min, 220 min, 240 min, 260 min, 280 min); the total time of the billet heating process is 480 to 720 min (for example, 500 min, 550 min, 580 min, 600 min, 650 min, 700 min).
[0023] In the above manufacturing method, as a preferred embodiment, in the billet heating process, when the billet diameter is greater than 430 mm and less than or equal to 480 mm, the total heating time from the billet entering the preheating section to the billet leaving the preheating section is ≥ 75 min (for example, 90 min, 100 min, 110 min, 120 min, 130 min, 140 min), and the total heating time from the billet entering the heating section to the billet leaving the heating section is ≥ 190 min (for example, 200 min, 220 min, 240 min). in, 260min, 270min), the total heating time from the billet entering the soaking section to the billet leaving the soaking section is ≥280min (for example, 300min, 320min, 340min, 360min, 380min, 400min, 420min); the total time of the billet heating process is 545~840min (for example, 560min, 580min, 600min, 650min, 700min, 750min, 800min, 820min).
[0024] In the above manufacturing method, as a preferred embodiment, in the billet heating process, when the billet diameter is greater than 480 mm and less than or equal to 520 mm, the total heating time from the billet entering the preheating section to the billet leaving the preheating section is ≥ 90 min (for example, 100 min, 110 min, 120 min, 130 min, 140 min, 150 min), and the total heating time from the billet entering the first heating section to the billet leaving the fourth heating section is ≥ 250 min (for example, 260 min, 270 min, 280 min, 290 min, 300 min, 310 min, 320 min, 330 min, 340 min, 350 min, 360 min, 370 min, 380 min, 390 min, 400 min, 410 min, 420 min, 430 min, 440 min, 450 min, 460 min, 470 min, 480 min, 490 min, 500 min, 510 min, 520 min, 530 min, 540 min, 550 min, 560 min, 570 min, 580 min, 590 min, 600 min, 610 min, 620 min, 630 min, 640 min, 650 min, 660 min, 670 min, 680 min, 690 min, 700 min, 710 min, 720 min, 730 min, 740 min, 750 min, 760 min, 770 min, 780 min, 790 min, 800 min, 810 min, 820 min, 830 min, 840 min, 850 min, 8 The total heating time from the time the billet enters the soaking section to the time the billet leaves the soaking section is ≥300min (for example, 350min, 380min, 400min, 420min, 440min, 460min, 480min); the total time of the billet heating process is 640-960min (for example, 660min, 700min, 750min, 800min, 850min, 900min, 950min).
[0025] Compared with the process of "continuously casting square billets and then forging or rolling them into round tube billets", the performance of the continuously cast round billets obtained by the billet heating process of the present invention can achieve the performance achieved by the intermediate billets in the traditional process after a long period of high-temperature diffusion. Therefore, by adopting the billet heating process of the present invention, the forging process before the traditional high carbon chromium bearing steel rolling can be omitted.
[0026] In the above-mentioned manufacturing method, as a preferred embodiment, in the punching process, the heated continuous cast round tube billet is punched through a two-roller puncher to obtain a rough tube, and the size of the rough tube (i.e., outer diameter * wall thickness) is (250~565) mm*(20~80) mm; preferably, in the punching process, the feed angle of the puncher is 8°~12°, the roller pitch is 220~480 mm, the lead distance is 232~510 mm, the plug diameter is φ120~440 mm, the plug length is 300~900 mm, and the top extension is 0~340 mm.
[0027] In the above manufacturing method, as a preferred embodiment, in the tube rolling process, the rough tube obtained in the perforation process is rolled by an ASSEL tube rolling mill to obtain a rough tube, and the size of the rough tube (i.e., outer diameter*wall thickness) is (φ230~560)mm*(16~75)mm.
[0028] In the above manufacturing method, as a preferred embodiment, in the tube rolling process, the mandrel diameter of the tube rolling mill is φ110~440mm, the throat diameter is φ142~540mm, the feed angle is 4°~9°, and the rolling angle is 3°~6°.
[0029] In the above manufacturing method, as a preferred embodiment, in the diameter reducing step, the rough pipe obtained in the pipe rolling step is reduced in diameter by a diameter reducing mill to obtain a seamless steel pipe with an outer diameter of φ219 to 530 mm and a wall thickness of 16 to 70 mm.
[0030] In the above manufacturing method, as a preferred embodiment, in the cooling process, the seamless steel pipe obtained after the diameter reduction is transferred to a cooling bed, and the cooling bed is continuously rotated and air-cooled to prevent the steel pipe from being severely bent during the cooling process.
[0031] In the above manufacturing method, as a preferred embodiment, in the heat treatment process, the cooled steel pipe is subjected to spheroidizing annealing in a heat treatment furnace, so that the structure and performance of the steel pipe after spheroidizing annealing meet the technical requirements of YB / T 4146-2016 standard.
[0032] In the above manufacturing method, as a preferred embodiment, in the heat treatment process, the specific steps of the spheroidizing annealing treatment are as follows:
[0033] First, heat the steel pipe to 790-810°C (i.e., 800±10°C) for insulation. After the insulation, cool it to 750-770°C (i.e., 760±10°C) at a cooling rate greater than 10°C / h and less than or equal to 20°C / h (e.g., 12°C / h, 15°C / h, 18°C / h), and then cool it to 710-730°C (i.e., 720±10°C) at a cooling rate ≤10°C / h, and keep it for a period of time; then cool it to 680-700 (i.e., 690±10°C) at a cooling rate ≤10°C / h, and then quickly cool it to below 600°C at a cooling rate greater than 10°C / h and less than or equal to 20°C / h before taking it out of the furnace.
[0034] In the present invention, under the condition that they do not conflict with each other, the above technical features can be freely combined to form a new technical solution.
[0035] The processes not specifically described in the present invention may adopt conventional processes in the art.
[0036] Compared with the prior art, the beneficial effects of the present invention are:
[0037] 1. The present invention can replace the high-temperature diffusion process before rolling of high-carbon chromium bearing steel in the existing process by controlling the tube billet heating process of the continuous casting round billet of bearing steel, that is, replace the "continuous casting square billet forging round tube billet" process.
[0038] 2. After the high carbon chromium bearing of the present invention is rolled into a steel pipe and subjected to spheroidizing annealing, the liquid separation, low magnification and other properties of the steel pipe meet the requirements of YB / T 4146-2016 "Seamless Steel Pipe for High Carbon Chromium Bearing Steel", and the quality of the microstructure, liquid separation, carbide network and other indicators of the continuous casting forging billet pipe is equivalent.
[0039] 3. The operation of the present invention is simple and easy. In the manufacturing process of high carbon chromium bearing steel seamless steel pipe, no additional process is required. Continuous casting round billets can be used instead of rolling / forging round billets, which greatly reduces the production cost of the bearing pipe and improves the product quality.
[0040] 4. The method of rolling seamless steel pipes from continuously cast round billets of high carbon chromium bearing steel of the present invention directly forms pipes from continuously cast round billets, and its comprehensive yield rate is increased by more than 8% compared with that of continuously cast forged billets. For steel pipes with an outer diameter ≥ 219 mm, forged round steel is usually used to produce pipe billets, while the continuous casting of round billets of the present invention can reduce the process cost by about 2,000 yuan / ton. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] Figure 1 This is a microstructure diagram of the seamless steel pipe produced in Example 1 of the present invention after spheroidizing annealing.
[0042] Figure 2 This is a carbide network diagram of the seamless steel pipe produced in Example 1 of the present invention after spheroidizing annealing.
[0043] Figure 3 This is the liquid chromatography diagram of the seamless steel pipe produced in Example 1 of the present invention after spheroidizing annealing.
[0044] Figure 4 This is a microstructure diagram of the seamless steel pipe produced in Comparative Example 1 of the present invention after spheroidizing annealing.
[0045] Figure 5 This is a carbide network diagram of the seamless steel pipe produced in Comparative Example 1 of the present invention after spheroidizing annealing. DETAILED DESCRIPTION
[0046] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0047] A method for manufacturing a seamless steel pipe made of high carbon chromium bearing steel continuous casting round billet, using a solid continuous casting round billet as a billet, and directly hot-rolling a seamless steel pipe using a continuous casting round billet, the manufacturing method comprises the following steps: billet heating, perforation, tube rolling, diameter reduction, cooling and heat treatment; wherein,
[0048] In the billet heating process, the solid continuous casting round tube billet is heated by a segmented heating method, and the billet heating includes a preheating section, a first heating section, a second heating section, a third heating section and a soaking section; specifically,
[0049] The set temperature of the preheating section is 660-750°C, and the heating rate is 300-600°C / h.
[0050] The set temperature of the heating stage is 800-890°C, and the furnace temperature is raised to the set temperature of the heating stage at a heating rate of 80-150°C / h;
[0051] The set temperature of the second heating stage is 910-1000°C, and the furnace temperature is raised to the set temperature of the second heating stage at a heating rate of 80-150°C / h;
[0052] The set temperature of the third heating stage is 1070-1160°C, and the furnace temperature is raised to the set temperature of the third heating stage at a heating rate of 130-200°C / h;
[0053] The set temperature of the fourth heating stage is 1161-1230°C, and the furnace temperature is raised to the set temperature of the fourth heating stage at a heating rate of 130-200°C / h;
[0054] The insulation temperature of the equalizing section is 1161~1230℃, and the insulation time is ≥220min.
[0055] By adopting the technical solution of the present invention, the comprehensive yield rate of the high-carbon chromium bearing steel seamless steel pipe produced is above 90.8%, and the delivery period of the steel pipe is 45 days.
[0056] Example 1
[0057] The manufacturing method of high carbon chromium bearing steel continuous casting round billet rolling seamless steel pipe provided in this embodiment adopts continuous casting round billet direct hot rolling seamless steel pipe, and the manufacturing method includes the following processes: solid continuous casting round billet heating, perforation, tube rolling, diameter reduction, cooling and heat treatment. Specifically, the process steps of producing high carbon chromium bearing steel seamless steel pipe are as follows:
[0058] (1) Billet heating
[0059] Obtained from converter smelting After continuous casting of round billets, the surface quality is checked and then cut off. Then the billets are placed in a ring furnace and heated and kept warm according to the specified heating system using a segmented heating method. Among them, the segmented heating includes preheating, heating one, heating two, heating three and soaking heating. The specific billet heating process parameters are shown in Table 1. Among them,
[0060] The total heating time of the preheating section is: the total heating time from the time the billet enters the preheating section to the time the billet leaves the preheating section;
[0061] The total heating time of the heating section is: the total heating time from the time when the blank enters the heating section to the time when the blank leaves the heating section;
[0062] The total heating time of the second heating stage is: the total heating time from the blank entering the second heating stage to the blank leaving the second heating stage;
[0063] The total heating time of the three heating stages is: the total heating time from the time the blank enters the three heating stages to the time the blank leaves the three heating stages;
[0064] The total heating time of the four heating stages is: the total heating time from the time the blank enters the four heating stages to the time the blank leaves the four heating stages;
[0065] The total heating time of the soaking zone is: the total heating time from the time the billet enters the soaking zone to the time the billet leaves the soaking zone.
[0066] Table 1 Process parameters of each stage in the blank heating in Examples 1-3
[0067]
[0068]
[0069] (2) Perforation
[0070] The continuous casting round billet after being taken out of the furnace is punched by a two-roller puncher to obtain a steel pipe billet, i.e., a rough pipe, with a size of 385mm*31mm; the punching process parameters are shown in Table 2.
[0071] Table 2 Process parameters of the punching machine in Example 1
[0072]
[0073] (3) Tube rolling:
[0074] The perforated steel tube billet is rolled by the ASSEL tube rolling mill to obtain a rough tube with a size of 359 mm*28 mm. The tube rolling process parameters are shown in Table 3.
[0075] Table 3 Process parameters of the tube rolling mill in Example 1
[0076]
[0077] (4) Reduction
[0078] The rolled pipe is reduced in diameter by a reducing mill to obtain a seamless steel pipe with a size of φ335mm*28mm.
[0079] (5) Cooling
[0080] The steel pipe after diameter reduction is transferred to the cooling bed and continuously rotated on the cooling bed for air cooling to prevent the steel pipe from being severely bent during the cooling process.
[0081] (6) Heat treatment
[0082] The cooled steel pipe is subjected to spheroidizing annealing in a heat treatment furnace so that the structure and performance of the steel pipe after spheroidizing annealing meet the technical requirements of the YB / T 4146-2016 standard. The specific steps of spheroidizing annealing are as follows:
[0083] First, heat the steel pipe to 800±10℃ for insulation. After the insulation, cool it to 760±10℃ at a cooling rate of ≤20℃ / h, and then cool it to 720±10℃ at a cooling rate of ≤10℃ / h, and keep it for a while; then cool it to 680-700 (i.e., 690±10℃) at a cooling rate of ≤10℃ / h, and then quickly cool it to 600℃ at a cooling rate greater than 10℃ / h and less than or equal to 20℃ / h before taking it out of the furnace.
[0084] By adopting the technical solution of this embodiment, the comprehensive yield rate of directly forming pipes from continuous casting round billets is 91.5%, and the delivery period of steel pipes is 43 days.
[0085] Example 2
[0086] This embodiment provides a method for manufacturing a seamless steel pipe by rolling a high carbon chromium bearing steel continuous casting round billet, except that the process parameters in the billet heating process are different from those in Example 1, the other processes are the same as those in Example 1. The process parameters in the billet heating process are shown in Table 1.
[0087] By adopting the technical solution of this embodiment, the comprehensive yield rate of directly forming pipes from continuous casting round billets is 92.1%, and the delivery period of steel pipes is 42 days.
[0088] Example 3
[0089] This embodiment provides a method for manufacturing a seamless steel pipe by rolling a high carbon chromium bearing steel continuous casting round billet, except that the process parameters in the billet heating process are different from those in Example 1, the other processes are the same as those in Example 1. The process parameters in the billet heating process are shown in Table 1.
[0090] By adopting the technical solution of this embodiment, the comprehensive yield rate of directly forming pipes from continuous casting round billets is 90.8%, and the delivery period of steel pipes is 45 days.
[0091] Performance testing:
[0092] The hardness, microstructure, and carbide inhomogeneity of the seamless steel pipes obtained after annealing in Examples 1-3 were tested. Table 4 lists the hardness, microstructure, and carbide inhomogeneity of the steel pipes prepared in Examples 1-3. Specifically,
[0093] According to the experimental method in GB / T 231.1, the hardness of the seamless steel pipe obtained after annealing in Examples 1-3 was tested, and the Brinell hardness of the steel pipe was 185-195 HBW, meeting the hardness requirement in the YB / T 4146-2016 standard.
[0094] According to the standard of Section 7.9 of GB / T 18254-2016, the microstructure of the steel tube obtained by spheroidizing annealing is inspected. Figure 1 The microstructure of the steel pipe after spheroidizing annealing in this embodiment is shown in FIG. Figure 1 It can be seen that the microstructure of the steel pipe is fine-grained pearlite, which meets the Grade 2 standard in the 5th rating diagram in Appendix A of GB / T 18254-2016 and meets the microstructure performance requirements in the YB / T 4146-2016 standard.
[0095] Table 4 Hardness, microstructure and carbide inhomogeneity of the steel pipes prepared in Examples 1-3
[0096]
[0097] According to the standard of Section 7.10 of GB / T 18254-2016, the steel pipe obtained by spheroidizing annealing is tested for carbide inhomogeneity. In this embodiment, the carbide network of the steel pipe after spheroidizing annealing meets the level 2 standard in the 6th rating diagram in Appendix A of GB / T18254-2016, the carbide band meets the level 2 standard in the 8th rating diagram in Appendix A of GB / T18254-2016, and the carbide liquid separation meets the level 0 standard in the 9th rating diagram in Appendix A of GB / T18254-2016, meeting the performance requirements of carbide inhomogeneity in the YB / T 4146-2016 standard. Figure 2-3 The carbide network diagram and liquid analysis diagram of the steel pipe after spheroidizing annealing in this embodiment are shown respectively.
[0098] In addition, the steel pipes obtained by spheroidizing annealing were tested for non-metallic inclusions, decarburized layer, micropores, etc. The properties of the steel pipes such as non-metallic inclusions, decarburized layer, micropores, etc. all met the technical requirements of the YB / T 4146-2016 standard.
[0099] By adopting the manufacturing method of producing seamless steel pipes by directly hot rolling the continuously cast round billets provided by the present invention, the comprehensive yield rate of directly forming pipes from the continuously cast round billets is not less than 90.8%, and the delivery period of the steel pipes is 45 days.
[0100] Comparative Example 1
[0101] This comparative example uses high carbon chromium bearing steel continuous casting forging billet to produce seamless steel pipes, and the process flow is as follows:
[0102] Converter / electric furnace + refining outside the furnace + vacuum treatment → continuous casting billet → continuous casting billet inspection → billet heating → forging round tube billet → cooling → finishing → forging round tube billet billet inspection → cutting → billet heating → piercing → tube rolling → diameter reduction → cooling → spheroidizing annealing → finishing → storage. The specific billet heating process is as follows:
[0103] Use forged After continuous casting forging (round) billets, the surface quality is checked and then cut off. Then the billets are placed in a ring furnace and heated and kept warm according to the specified heating system using a segmented heating method. Among them, the segmented heating includes preheating, heating one, heating two, heating three and soaking heating. The specific billet heating process parameters are shown in Table 5. Among them,
[0104] The total heating time of the preheating section is: the total heating time from the time the billet enters the preheating section to the time the billet leaves the preheating section;
[0105] The total heating time of the heating section is: the total heating time from the time when the blank enters the heating section to the time when the blank leaves the heating section;
[0106] The total heating time of the second heating stage is: the total heating time from the blank entering the second heating stage to the blank leaving the second heating stage;
[0107] The total heating time of the three heating stages is: the total heating time from the time the blank enters the three heating stages to the time the blank leaves the three heating stages;
[0108] The total heating time of the four heating stages is: the total heating time from the time the blank enters the four heating stages to the time the blank leaves the four heating stages;
[0109] The total heating time of the soaking zone is: the total heating time from the time the billet enters the soaking zone to the time the billet leaves the soaking zone.
[0110] Table 5 Process parameters of each section in the blank heating in Comparative Examples 1-3
[0111]
[0112]
[0113] The average comprehensive yield rate of seamless steel pipes produced by the conventional process in this comparative example is 81% (i.e., 90%*90%=81%, wherein the first 90% is the yield rate of the process of “continuous casting square billet→forging round tube billet→cooling→finishing”, and the second 90% is the yield rate of the process of “forging round tube billet billet inspection→cutting→billet heating→piercing→tube rolling→diameter reduction→cooling→spheroidizing annealing→finishing”), and the delivery time of the steel pipe is 60 days.
[0114] Performance Testing:
[0115] The seamless steel pipe obtained by spheroidizing annealing in this comparative example was tested for microstructure and carbide inhomogeneity by the same method as the performance test in Example 1. The microstructure of the seamless steel pipe after spheroidizing annealing in this comparative example is fine-grained pearlite, which meets the Grade 2 standard in the 5th rating diagram in Appendix A of GB / T 18254-2016 and meets the microstructure performance requirements in the YB / T 4146-2016 standard. Figure 4 The microstructure of the seamless steel pipe after spheroidizing annealing in this comparative example is shown.
[0116] The carbide inhomogeneity test results show that the carbide network of the steel pipe after spheroidizing annealing in this comparative example meets the 2.5 level standard in the 6th rating diagram in Appendix A of GB / T 18254-2016, the banded structure of the carbide meets the 2 level standard in the 8th rating diagram, and the liquid segregation of the carbide meets the 0 level standard in the 9th rating diagram, meeting the performance requirements for carbide segregation in the YB / T 4146-2016 standard. Figure 5 The carbide network diagram of the steel pipe after spheroidizing annealing in this comparative example is shown.
[0117] A comparative analysis of the above-mentioned specific implementation methods shows that, compared with the conventional process of producing high carbon chromium bearing steel seamless pipes using continuous casting forging billets, the technical solution provided by the present invention, i.e., directly hot rolling continuous casting round billets to produce high carbon chromium bearing steel seamless pipes, can omit the "continuous casting square billet inspection → billet heating → forging round tube billet → cooling → finishing" process, save about 15 days of production cycle, save about 2,000 yuan / ton of processing costs, and increase the comprehensive yield rate by more than 8%.
[0118] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Technical engineers in the art may make changes and modifications to these embodiments without violating the spirit and scope of the present invention. Therefore, all equivalent modifications or changes made by those with ordinary knowledge in the art without departing from the spirit and technical ideas disclosed by the present invention should still be covered by the claims of the present invention.
Claims
1. A method for manufacturing a seamless steel pipe by continuously casting round billets of high carbon chromium bearing steel, characterized in that: A solid continuous casting round tube billet is used as a billet to directly hot-roll a seamless steel pipe. The manufacturing method comprises the following steps: billet heating, perforation, tube rolling, diameter reduction, cooling and heat treatment; wherein: In the billet heating process, the solid continuous casting round tube billet is heated by a segmented heating method, and the set heating temperature of the billet heating is 750-1230°C; the billet heating includes a preheating section, a heating section, a heating section, a heating section, a heating section, a heating section, a heating section and a soaking section; wherein, The set temperature of the heating stage is 800-890°C, and the heating rate is 80-150°C / h; The set temperature of the second heating stage is 910-1000°C, and the heating rate is 80-150°C / h; The set temperature of the three heating stages is 1070-1160°C, and the heating rate is 130-200°C / h; The set temperature of the fourth heating stage is 1161-1230°C, and the heating rate is 130-200°C / h; The holding temperature of the soaking section is 1161-1230°C, and the holding time is ≥220min; The diameter of the blank is φ250-520 mm; The total heating time of each segment and the total heating time of the soaking section in the billet heating process are determined according to the billet diameter range; In the billet heating process, when the billet diameter is 250 mm to 300 mm, the total heating time from the billet entering the preheating section to the billet leaving the preheating section is ≥30 min, the total heating time from the billet entering the heating section to the billet leaving the heating section is ≥110 min, and the total heating time from the billet entering the soaking section to the billet leaving the soaking section is ≥220 min; the total time of the billet heating process is 360 to 560 min; In the billet heating process, when the billet diameter is greater than 300 mm and less than or equal to 360 mm, the total heating time from the billet entering the preheating section to the billet leaving the preheating section is ≥40 min, the total heating time from the billet entering the heating section to the billet leaving the heating section is ≥120 min, and the total heating time from the billet entering the soaking section to the billet leaving the soaking section is ≥240 min; the total time of the billet heating process is 400 to 600 min; In the billet heating process, when the billet diameter is greater than 360 mm and less than or equal to 430 mm, the total heating time from the billet entering the preheating section to the billet leaving the preheating section is ≥60 min, the total heating time from the billet entering the heating section to the billet leaving the heating section is ≥160 min, and the total heating time from the billet entering the soaking section to the billet leaving the soaking section is ≥260 min; the total time of the billet heating process is 480 to 720 min; In the billet heating process, when the billet diameter is greater than 430 mm and less than or equal to 480 mm, the total heating time from the billet entering the preheating section to the billet leaving the preheating section is ≥75 min, the total heating time from the billet entering the heating section to the billet leaving the heating section is ≥190 min, and the total heating time from the billet entering the soaking section to the billet leaving the soaking section is ≥280 min; the total time of the billet heating process is 545 to 840 min; In the billet heating process, when the billet diameter is greater than 480 mm and less than or equal to 520 mm, the total heating time from the billet entering the preheating section to the billet leaving the preheating section is ≥90 min, the total heating time from the billet entering the heating section to the billet leaving the heating section is ≥250 min, and the total heating time from the billet entering the equalizing section to the billet leaving the equalizing section is ≥300 min; the total time of the billet heating process is 640 to 960 min.
2. The manufacturing method according to claim 1, characterized in that: In the blank heating process, the set temperature of the preheating section is ≤750°C, and the heating rate is 300-600°C / h.
3. The manufacturing method according to claim 2, characterized in that: The set temperature of the preheating section is 650-750°C.
4. The manufacturing method according to claim 1, characterized in that: In the perforation process, the heated continuous casting round tube billet is perforated by a two-roll perforator to obtain a rough tube, and the size of the rough tube (ie, outer diameter*wall thickness) is (φ250-565) mm*(20-80) mm.
5. The manufacturing method according to claim 1, characterized in that: In the perforating process, the feed angle of the perforator is 8° to 12°, the roller pitch is 220 to 480 mm, the guide distance is 232 to 510 mm, the plug diameter is φ120 to 440 mm, the plug length is 300 to 900 mm, and the top extension is 0 to 340 mm.
6. The manufacturing method according to claim 1, characterized in that: In the tube rolling process, the rough tube obtained in the perforation process is rolled by an ASSEL tube rolling mill to obtain a rough tube, and the outer diameter*wall thickness of the rough tube is (φ230~560)mm*(16~75)mm.
7. The manufacturing method according to claim 6, characterized in that: In the tube rolling process, the mandrel diameter of the tube rolling mill is 110-440 mm, the throat diameter is 142-540 mm, the feed angle is 4°-9°, and the rolling angle is 3°-6°.
8. The manufacturing method according to claim 1, characterized in that: In the cooling process, the seamless steel pipe obtained after the diameter reduction is transferred to a cooling bed, and the cooling bed is continuously rotated for air cooling to prevent the steel pipe from being severely bent during the cooling process.
9. The manufacturing method according to claim 1, characterized in that: In the heat treatment process, the cooled steel pipe is subjected to spheroidizing annealing in a heat treatment furnace. The specific steps of the spheroidizing annealing are as follows: First, heat the steel pipe to 790-810℃ for insulation. After the insulation, cool it to 750-770℃ at a cooling rate greater than 10℃ / h and less than or equal to 20℃ / h, and then cool it to 710-730℃ at a cooling rate ≤10℃ / h, and keep it for a while; then cool it to 680-700℃ at a cooling rate ≤10℃ / h, and then quickly cool it to 600℃ at a cooling rate greater than 10℃ / h and less than or equal to 20℃ / h before taking it out of the furnace.
10. The manufacturing method according to claim 1, characterized in that: The specifications of the seamless steel pipe prepared by the manufacturing method are: outer diameter φ219-530mm, wall thickness 16-70mm.
Citation Information
Patent Citations
Manufacturing method for pipe die by using steel ingot great-reducing-forming blank
CN102962293A
On-line tube-expanding production process of large-diameter seamless steel tubes
CN105234200A
Seamless tube rolling method of ultrahigh-strength alloy
CN110280592A