Preparation of phosphorus-sulfur alloy micro-nano particles and their application in electrocatalysis
Using laser liquid phase ablation technology, phosphorus-sulfur series materials are mixed with precious metals to form phosphorus-sulfur series alloy micro-nano particles, which solves the problems of high cost of platinum-based materials and insufficient research on phosphorus-sulfur series catalysts, and realizes the application in the field of electrocatalysis Performance comparable to platinum-based catalysts.
Patent Information
- Application Number
- CN202211021234.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-24
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2042-08-24
AI Technical Summary
The existing problems of high cost and low reserves of platinum-based materials in the field of electrocatalysis, and the lack of research on phosphorus-sulfur series composite metal catalytic materials, lead to the lack of non-noble metal catalysts with excellent performance.
Laser liquid phase ablation technology is used to mix phosphorus-sulfur series two-dimensional compounds such as copper indium phosphorus sulfur, silver indium phosphorus sulfur, and copper vanadium phosphorus sulfur with precious metals (such as palladium, platinum, ruthenium, and iridium) to form a phosphorus-sulfur series alloy microstructure. Nanoparticles break chemical bonds and embed precious metal atoms through laser ablation to form a multifunctional catalyst.
Significantly improve the conductivity and number of active sites of phosphorus-sulfur alloy micro-nano particles, making the electrocatalytic performance under acidic and alkaline conditions close to that of platinum-based catalysts, solving the problem of high cost of platinum-based materials, and in It exhibits excellent performance in the fields of electrochemistry and photoelectrocatalysis.
Smart Images

Figure CN115449836B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of electrochemical technology, and in particular relates to the preparation of phosphorus-sulfur alloy micro-nano particles and their application in the field of electrocatalysis. Background Art
[0002] In the field of electrocatalysis, the best catalytic materials that can be commercially applied are platinum metal or platinum-based materials. Platinum metal or platinum-based catalytic materials can greatly reduce the overpotential of the catalytic reaction and increase the energy conversion efficiency in the catalytic process. However, platinum-based materials have long been limited by the high price and low reserves of platinum resources. Therefore, most researchers now increase the specific surface area of platinum-based materials or disperse platinum-based precious metals as much as possible on non-precious metal materials (such as carbon-based materials) carriers to increase the activity of precious metal catalytic sites in catalytic materials, thereby reducing the use of platinum-based precious metals in catalytic materials.
[0003] In addition, some researchers are committed to finding non-precious metal-based catalysts with excellent performance, or alloying precious metals with other transition metals or metal compounds to make them cheap substitutes for platinum-based materials. Phosphorus and sulfur-based materials are inexpensive and have certain electrocatalytic activity, which has become a very important exploration direction in the current field of catalytic research. In theory, phosphorus-based or sulfur-based materials may have relatively good catalytic performance. However, there are few reports on phosphorus-based or sulfur-based composite metal catalytic materials. Therefore, the development of a phosphorus-based or sulfur-based alloy catalyst material with excellent performance has a good application prospect. Summary of the invention
[0004] In order to overcome the shortcomings of the above-mentioned prior art, the present invention proposes a method for preparing phosphorus-sulfur alloy micro-nano particles. The prepared phosphorus-sulfur alloy micro-nano particles are a type of catalytic material with excellent performance, which has good electrocatalytic performance under alkaline and acidic conditions and is expected to be used in the fields of electrochemistry and photoelectrocatalysis.
[0005] In order to achieve the above object, the technical solution adopted by the present invention is:
[0006] The present invention provides a method for preparing phosphorus-sulfur alloy micro-nano particles, specifically: using any one or more phosphorus-sulfur two-dimensional compound crystal materials of copper indium phosphorus-sulfur (CuInP2S6), silver indium phosphorus-sulfur (AgInP2S6), copper vanadium phosphorus-sulfur (CuVP2S6) and silver vanadium phosphorus-sulfur (AgVP2S6) as a matrix material, mixing them with precious metals and then performing laser ablation treatment using laser liquid phase ablation technology, so that the mixed material is alloyed under the action of laser liquid phase ablation and forms a micro-nano spherical structure, that is, preparing phosphorus-sulfur alloy micro-nano particles, wherein the precious metals include at least two of palladium, platinum, ruthenium and iridium.
[0007] As a preferred embodiment of the present invention, the above-mentioned method for preparing phosphorus-sulfur alloy micro-nano particles comprises the following steps:
[0008] S1. adding a precious metal to a mixed solution of an organic solvent and water, mixing the mixture, and irradiating the mixed solution with a pulsed laser for laser treatment, so that the precious metal powder is pre-alloyed in the mixed solution by laser liquid phase ablation;
[0009] S2. Add the matrix material powder to the pre-alloyed mixed solution, mix well, and then irradiate the mixed solution with a pulsed laser again for laser treatment, and prepare phosphorus-sulfur alloy micro-nano particles after forming a micro-nano spherical structure through laser liquid phase ablation. The matrix material is any one or more of copper-indium-phosphorus-sulfur, silver-indium-phosphorus-sulfur, copper-vanadium-phosphorus-sulfur and silver-vanadium-phosphorus-sulfur.
[0010] Preferably, the noble metal is a mixture of palladium and any one of platinum, ruthenium and iridium. More preferably, the mass ratio of palladium to another noble metal is 9:1.
[0011] Preferably, the matrix material is a combination of any one or more of copper indium phosphide (CuInP2S6), silver indium phosphide (AgInP2S6), copper vanadium phosphide (CuVP2S6) and silver vanadium phosphide (AgVP2S6).
[0012] The original phosphorus-sulfur crystal powder [copper indium phosphorus-sulfur (CuInP2S6) or silver indium phosphorus-sulfur (AgInP2S6) or copper vanadium phosphorus-sulfur (CuVP2S6) or silver vanadium phosphorus-sulfur (AgVP2S6)] almost has no electrocatalytic performance, because of its poor conductivity and very few active sites. The present invention prepares unique micro-nano spherical particles by laser liquid phase ablation, and uses the strong effect of laser to break the weaker chemical bonds in the original phosphorus-sulfur crystal material (copper indium phosphorus-sulfur (CuInP2S6) or silver indium phosphorus-sulfur (AgInP2S6) or copper vanadium phosphorus-sulfur (CuVP2S6) or silver vanadium phosphorus-sulfur (AgVP2S6)), and the noble metal atoms in the molten state under the laser liquid phase ablation state are embedded into the parent phosphorus-sulfur crystal with broken chemical bonds by the action of the laser, and form phosphorus-sulfur alloy micro-nano particles through alloying. The embedding of precious metal atoms and the change of the original crystal chemical bonds will significantly enhance the conductivity of the phosphorus-sulfur alloy micro-nano particle materials, and the embedding of precious metal atoms will also greatly increase the number of active sites in the micro-nano particles, greatly improving their catalytic performance; and the laser liquid phase ablation itself will also improve the performance of the catalyst and can be reused repeatedly, maximizing the effectiveness of the catalytic material and achieving environmentally friendly catalytic reaction behavior.
[0013] The present invention uses copper indium phosphosulfide (CuInP2S6) or silver indium phosphosulfide (AgInP2S6) or copper vanadium phosphosulfide (CuVP2S6) or silver vanadium phosphosulfide (AgVP2S6), as well as precious metals such as palladium, platinum, ruthenium, iridium, and rhodium as materials, and adopts laser liquid phase ablation technology to perform laser ablation treatment in liquid to form a nanosphere structure to prepare a phosphorus-sulfur alloy micro-nano granular material. The prepared phosphorus-sulfur alloy micro-nano granular material is a polycrystalline or amorphous micro-nano sphere structure, which is a bifunctional catalyst, has a good catalytic overpotential in both HER and ORR catalysis fields, and has photoelectrocatalytic performance comparable to that of platinum-based catalysts, and is expected to be used in the field of electrochemistry.
[0014] Preferably, when pulse laser irradiation is performed in steps S1 and S2, the energy of the pulse laser is 100-500 mJ, the frequency is 1-50 Hz, and the action time is 1-10 h.
[0015] Preferably, when performing pulsed laser irradiation in steps S1 and S2, a 532 nm YAG laser and a 532 nm total reflection mirror or a 355 nm YAG laser and a 355 nm total reflection mirror are used.
[0016] Preferably, the mass ratio of the matrix material to the precious metal is 1:1.
[0017] Preferably, the organic solvent is ethanol or ascorbic acid, and the volume ratio of the organic solvent to water is (2-4): 1. More preferably, the volume ratio of the organic solvent to water is 3:1.
[0018] The present invention provides phosphorus-sulfur alloy micro-nano particles prepared by the above-mentioned preparation method.
[0019] The phosphorus-sulfur alloy micro-nano particle material prepared by the present invention is a kind of multifunctional electrocatalyst with excellent electrochemical performance under acidic and alkaline conditions, which is very close to the performance of platinum catalysts reported in the literature (H. Xie, S. Chen, J. Liang, T. Wang, Z. Hou, H. Wang, G. Chai, Q. Li, Weakening Intermediate Bindings on CuPd / Pd Core / shell Nanoparticles to Achieve Pt-Like Bifunctional Activity for Hydrogen Evolution and Oxygen Reduction Reactions. Adv Funct Materials. 31, 2100883 (2021).), and the Tafel slope has surpassed that reported in the literature (C. Li, L. Zhang, Y. Zhang, Y. Zhou, J. Sun, X. Ouyang, X. Wang, J. Zhu, Y. Fu, PtRu alloy nanoparticles embedded on C2N nanosheets for efficient hydrogen evolution reaction in both acidic and alkaline solutions.Chemical Engineering Journal.428,131085(2022).) The Tafel slope (1-2) of publicly reported platinum catalysts.
[0020] The present invention provides the application of the above-mentioned phosphorus-sulfur alloy micro-nano particles in the field of electrochemistry.
[0021] The phosphorus-sulfur alloy micro-nano particle material prepared by the method of the present invention is a multifunctional electrocatalyst, which has a good overpotential under acidic and alkaline conditions, and has the same characteristics as those in the literature (A.Shan, X.Teng, Y.Zhang, P.Zhang, Y.Xu, C.Liu, H.Li, H.Ye, R.Wang, Interfacial electronic structure modulation of Pt-MoS2heterostructure for enhancing electrocatalytic hydrogenevolution reaction.Nano Energy.94,106913(2022); HCFu, XHWang, XHChen, Q.Zhang, NBLi, HQLuo, Interfacial engineering of Ni(OH)2on W2C for remarkable alkaline hydrogen production.Applied Catalysis B: Environmental. 301, 120818 (2022).) The photoelectrocatalytic performance is comparable to that of publicly reported platinum-based catalysts (3–4), while solving the cost problem of platinum-based catalysts. It can be used to prepare materials with catalytic effects, and can even be combined with conductive hydrogels and aerogels for the catalytic decomposition of gases such as CH4, which has a wide range of application value.
[0022] Preferably, the electrochemical field is the field of electrochemical hydrogen evolution or the field of electrochemical oxygen reduction.
[0023] It should be noted that the phosphorus-sulfur alloy micro-nano particles of the present invention can also be synthesized by other means, such as hydrothermal method, and obtained by changing the compounds used, such as other sulfides, phosphides or nitrides. In addition, the phosphorus-sulfur alloy micro-nano particles of the present invention can also be obtained by means such as chemical vapor deposition.
[0024] Compared with the prior art, the present invention has the following beneficial effects:
[0025] In order to develop a class of phosphorus-sulfur catalyst materials with excellent performance, the present invention discloses a method for preparing a phosphorus-sulfur alloy micro-nano granular material, using any one or more phosphorus-sulfur two-dimensional compound crystal materials such as copper indium phosphorus-sulfur (CuInP2S6) or silver indium phosphorus-sulfur (AgInP2S6) or copper vanadium phosphorus-sulfur (CuVP2S6) or silver vanadium phosphorus-sulfur (AgVP2S6) as a matrix material, mixing it with precious metal powder (palladium, platinum, ruthenium, iridium, etc.), laser treatment by laser liquid phase ablation technology, forming a micro-nano spherical structure to prepare a phosphorus-sulfur alloy micro-nano granular material. The prepared phosphorus-sulfur alloy micro-nano granular material is a micro-nano spherical structure of a mixed state of polycrystalline micro-nano particles and amorphous micro-nano particles, belonging to a class of multifunctional catalysts, having good overpotentials under both alkaline and acidic conditions, having catalytic performance comparable to that of platinum-based catalysts, and can be applied in the field of electrochemistry or photoelectrocatalysis. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 This is a TEM image of spherical micro-nanoparticles obtained by copper indium phosphosulfide (CuInP2S6) loaded with palladium platinum under the action of 355nm laser;
[0027] Figure 2 This is a TEM image of the spherical micro-nanostructure obtained by loading palladium ruthenium on silver indium phosphosulfide (AgInP2S6) under 355nm laser.
[0028] Figure 3 This is a TEM image of spherical micro-nanoparticles obtained by loading ruthenium platinum on copper vanadium phosphorus sulfur (CuVP2S6) under 355nm laser irradiation;
[0029] Figure 4 This is a TEM image of spherical micro-nanoparticles obtained by loading palladium iridium on silver vanadium phosphorus sulfur (AgVP2S6) under 355nm laser action;
[0030] Figure 5 This is a TEM image of spherical micro-nanoparticles obtained by copper indium phosphosulfide (CuInP2S6) loaded with palladium platinum under the action of 532nm laser;
[0031] Figure 6 This is the electrochemical hydrogen evolution performance diagram of spherical micro-nano particles obtained by loading palladium and platinum on copper indium phosphide (CuInP2S6);
[0032] Figure 6 In the figure, CIPS@PdPt is a phosphorus-sulfur alloy micro-nano particle obtained by laser processing copper indium phosphorus-sulfur loaded with palladium-platinum.
[0033] Figure 7 The electrochemical hydrogen evolution performance diagram of spherical micro-nano particles obtained by loading palladium and ruthenium on silver indium phosphosulfide (AgInP2S6);
[0034] Figure 7 AIPS@PdRu is a phosphorus-sulfur alloy micro-nano particle obtained by laser processing silver-indium-phosphorus-sulfur loaded palladium-ruthenium.
[0035] Figure 8 This is the electrochemical hydrogen evolution performance diagram of spherical micro-nanoparticles obtained by loading ruthenium and platinum on copper vanadium phosphorus sulfur (CuVP2S6);
[0036] Figure 8 In the figure, CVPS@RuPt is a phosphorus-sulfur alloy micro-nano particle obtained by laser processing copper-vanadium-phosphorus-sulfur loaded ruthenium-platinum.
[0037] Fig. 9 This is the electrochemical hydrogen evolution performance diagram of spherical micro-nanoparticles obtained by loading palladium and iridium on silver vanadium phosphorus sulfur (AgVP2S6);
[0038] Fig. 9 AVPS@PdIr is a phosphorus-sulfur alloy micro-nano particle obtained by laser processing silver-vanadium-phosphorus-sulfur loaded with palladium-iridium.
[0039] Fig.10 The electrochemical oxygen reduction performance diagram of spherical micro-nanoparticles obtained by loading palladium and platinum on copper indium phosphide (CuInP2S6);
[0040] Fig.10 In the figure, CIPS@PdPt is a phosphorus-sulfur alloy micro-nano particle obtained by laser processing copper indium phosphorus-sulfur loaded with palladium-platinum.
[0041] Fig.11 This is the electrochemical hydrogen evolution performance diagram of spherical micro-nano particles obtained after copper indium phosphide (CuInP2S6) is exposed to laser.
[0042] Fig.11 In the figure, CIPS is a spherical micro-nanoparticle obtained by laser processing copper indium phosphide (CuInP2S6).
[0043] Fig.12 This is the electrochemical hydrogen evolution performance diagram of spherical micro-nanoparticles obtained by loading palladium on copper indium phosphide (CuInP2S6).
[0044] Fig.12 In the figure, CIPS@Pd is a spherical micro-nanoparticle obtained by laser processing copper indium phosphide (CuInP2S6) loaded with palladium. DETAILED DESCRIPTION
[0045] The specific embodiments of the present invention are further described below. It should be noted that the description of these embodiments is used to help understand the present invention, but does not constitute a limitation of the present invention. In addition, the technical features involved in each embodiment of the present invention described below can be combined with each other as long as they do not conflict with each other.
[0046] The experimental methods in the following examples are conventional methods unless otherwise specified, and the experimental materials used in the following examples are commercially available unless otherwise specified.
[0047] The laser irradiation treatment in the following embodiments is performed using a laser liquid phase ablation device, namely a YAG laser.
[0048] Example 1 Preparation of Phosphorus-Sulfur Alloy Micro-Nano Particles
[0049] (1) 10 mg of palladium and platinum precious metal powders were mixed in a weight ratio of 9:1 and dispersed into a mixed solution of anhydrous ethanol and water in a volume ratio of 3:1, with a total volume of 50 mL. The dispersed mixed solution was placed in a glass bottle and uniformly dispersed by ultrasonication at room temperature. The glass bottle was then fixed on a magnetic stirrer, and the magnetic stirrer was kept running continuously (the speed could be set at 100-800 rpm). A 355 nm YAG laser and a 355 nm total reflection mirror were used to irradiate the mixed solution at the bottle mouth with a pulsed laser. The energy of the pulsed laser was 100 mJ, the frequency was 50 Hz, and the irradiation time was 1 h, thereby completing pre-alloying.
[0050] (2) 10 mg of copper indium phosphorus-sulfur matrix material (for the specific preparation method, refer to the Chinese invention patent "CN112195024B Preparation of High-yield CuInP2S6 Quantum Dots") is added to the pre-alloyed mixed solution, and a 355 nm YAG laser and a 355 nm total reflection mirror are used to irradiate the mixed solution at the bottle mouth with a pulse laser for 1 hour to obtain phosphorus-sulfur alloy micro-nano particles. The energy of the pulse laser is 100 mJ and the frequency is 50 Hz.
[0051] Example 2 Preparation of Phosphorus-Sulfur Alloy Micro-Nano Particles
[0052] (1) 10 mg of palladium and ruthenium precious metal powders were mixed in a weight ratio of 9:1 and dispersed into a mixed solution of anhydrous ethanol and water in a volume ratio of 3:1, with a total volume of 50 mL. The dispersed mixed solution was placed in a glass bottle and uniformly dispersed by ultrasonication at room temperature. The glass bottle was then fixed on a magnetic stirrer, and the magnetic stirrer was kept running continuously. A 355 nm YAG laser and a 355 nm total reflection mirror were used to irradiate the mixed solution at the bottle mouth with a pulse laser. The energy of the pulse laser was 200 mJ, the frequency was 40 Hz, and the irradiation time was 1 h, thereby completing pre-alloying.
[0053] (2) 10 mg of silver indium phosphorus-sulfur matrix material (for the specific preparation method, refer to the Chinese invention patent "CN112195024B Preparation of High-yield CuInP2S6 Quantum Dots") was added to the pre-alloyed mixed solution, and a 355 nm YAG laser and a 355 nm total reflection mirror were used to irradiate the mixed solution at the bottle mouth with a pulsed laser for 1 h to obtain phosphorus-sulfur alloy micro-nano particles. The energy of the pulsed laser was 200 mJ and the frequency was 40 Hz.
[0054] Example 3 Preparation of Phosphorus-Sulfur Alloy Micro-Nano Particles
[0055] (1) 10 mg of ruthenium and platinum precious metal powders were mixed in a weight ratio of 9:1 and dispersed into a mixed solution of anhydrous ethanol and water in a volume ratio of 3:1, with a total volume of 50 mL. The dispersed mixed solution was placed in a glass bottle and uniformly dispersed by ultrasonication at room temperature. The glass bottle was then fixed on a magnetic stirrer, and the magnetic stirrer was kept running continuously. A 355 nm YAG laser and a 355 nm total reflection mirror were used to irradiate the mixed solution at the bottle mouth with a pulse laser. The energy of the pulse laser was 300 mJ, the frequency was 25 Hz, and the irradiation time was 1 h, thereby completing pre-alloying.
[0056] (2) 10 mg of copper vanadium phosphorus sulfur matrix material (for the specific preparation method, refer to the Chinese invention patent "CN112195024B Preparation of High-yield CuInP2S6 Quantum Dots") was added to the pre-alloyed mixed solution, and a 355 nm YAG laser and a 355 nm total reflection mirror were used to irradiate the mixed solution at the bottle mouth with a pulsed laser for 1 h to obtain phosphorus sulfur alloy micro-nano particles. The energy of the pulsed laser was 300 mJ and the frequency was 25 Hz.
[0057] Example 4 Preparation of Phosphorus-Sulfur Alloy Micro-Nano Particles
[0058] (1) 10 mg of palladium and iridium precious metal powders were mixed in a weight ratio of 9:1 and dispersed into a mixed solution of ascorbic acid and water in a volume ratio of 3:1, with a total volume of 50 mL. The dispersed mixed solution was placed in a glass bottle and uniformly dispersed by ultrasonication at room temperature. The glass bottle was then fixed on a magnetic stirrer, and the magnetic stirrer was kept running continuously. A 355 nm YAG laser and a 355 nm total reflection mirror were used to irradiate the mixed solution at the bottle mouth with a pulse laser. The energy of the pulse laser was 400 mJ, the frequency was 20 Hz, and the irradiation time was 1 h to complete pre-alloying.
[0059] (2) 10 mg of silver vanadium phosphorus-sulfur matrix material (for the specific preparation method, refer to the Chinese invention patent "CN112195024B Preparation of High-yield CuInP2S6 Quantum Dots") was added to the pre-alloyed mixed solution, and a 355 nm YAG laser and a 355 nm total reflection mirror were used to irradiate the mixed solution at the bottle mouth with a pulsed laser for 1 h to obtain phosphorus-sulfur alloy micro-nano particles. The energy of the pulsed laser was 400 mJ and the frequency was 20 Hz.
[0060] Example 5 Preparation of Phosphorus-Sulfur Alloy Micro-Nano Particles
[0061] (1) 10 mg of palladium and platinum precious metal powders were mixed in a ratio of 9:1 and dispersed into a mixed solution of ascorbic acid and water in a volume ratio of 3:1. The total volume of the solution was 50 mL. The dispersed mixed solution was placed in a glass bottle and uniformly dispersed by ultrasonication at room temperature. The glass bottle was then fixed on a magnetic stirrer, and the magnetic stirrer was kept running continuously. A 532 nm YAG laser and a 532 nm total reflection mirror were used to irradiate the mixed solution at the bottle mouth with a pulse laser. The energy of the pulse laser was 500 mJ, the frequency was 10 Hz, and the irradiation time was 5 h. The pre-alloying was completed.
[0062] (2) 10 mg of silver vanadium phosphorus-sulfur matrix material (for the specific preparation method, refer to the Chinese invention patent "CN112195024B Preparation of High-yield CuInP2S6 Quantum Dots") was added to the pre-alloyed mixed solution, and a 532 nm YAG laser and a 532 nm total reflection mirror were used to irradiate the mixed solution at the bottle mouth with a pulsed laser for 5 h to obtain phosphorus-sulfur alloy micro-nano particles. The energy of the pulsed laser was 500 mJ and the frequency was 10 Hz.
[0063] Comparative Example 1 Preparation of Phosphorus-Sulfur Micro-Nano Particles
[0064] 10 mg of copper indium phosphorus-sulfur matrix material was dispersed in a mixed solution of anhydrous ethanol and water in a volume ratio of 3:1. The total volume of the solution was 50 mL. The dispersed mixed solution was placed in a glass bottle and evenly dispersed by ultrasonication at room temperature. The glass bottle was then fixed on a magnetic stirrer, and the magnetic stirrer was kept running continuously. A 355 nm YAG laser and a 355 nm total reflection mirror were used to irradiate the mixed solution at the bottle mouth with a pulsed laser. The pulsed laser action time was 1 hour to obtain phosphorus-sulfur micro-nano particles. The energy of the pulsed laser was 100 mJ and the frequency was 50 Hz.
[0065] Comparative Example 2 Preparation of a Phosphorus-Sulfur Alloy Micro-Nano Particle
[0066] First, 10 mg of palladium powder was dispersed in a mixed solution of anhydrous ethanol and water in a volume ratio of 3:1. The total volume of the solution was 50 mL. The dispersed mixed solution was placed in a glass bottle and evenly dispersed by ultrasonication at room temperature. Then, 10 mg of copper indium phosphorus-sulfur matrix material was added to the mixed solution. The glass bottle was fixed on a magnetic stirrer, and the magnetic stirrer was kept running continuously. A 355 nm YAG laser and a 355 nm total reflection mirror were used to irradiate the mixed solution at the bottle mouth with a pulsed laser for 1 h to obtain phosphorus-sulfur alloy micro-nano particles. The energy of the pulsed laser was 100 mJ and the frequency was 50 Hz.
[0067] Experimental Example 1 Characteristics and Performance Analysis of Phosphorus-Sulfur Alloy Micro-Nano Particles
[0068] (1) Transmission electron microscopy (TEM) analysis
[0069] The phosphorus-sulfur alloy micro-nano particles prepared in Examples 1-5 were used as test samples and subjected to TEM analysis using a 300 kV transmission electron microscope (FEITecnai G2 F30, FEI Company, USA). The obtained TEM images are shown in FIG. Figure 1-5 As shown, it can be seen from the TEM image that the prepared phosphorus-sulfur alloy micro-nano particles are spherical micro-nano particles with uniform size distribution.
[0070] (2) Electrochemical performance test
[0071] All electrocatalytic performance tests were conducted using a three-electrode system. The working electrode in the test was a glassy carbon electrode loaded with phosphorus-sulfur alloy micro-nano particle catalysts, the counter electrode was a graphite rod electrode, the reference electrode was a silver / silver chloride electrode under acidic conditions, and a mercury / mercuric oxide electrode under alkaline conditions, and the electrolyte was a 0.5M sulfuric acid solution and a 0.1M or 1M potassium hydroxide solution. The preparation method of the working electrode is as follows:
[0072] Weigh 5 mg of the phosphorus-sulfur alloy micro-nano particles obtained in Example 1-5, add 975 μL of deionized water, then add 5 μL of 5wt% Nafion dispersion, and after ultrasonic dispersion, take 5 μL of the prepared catalyst ink and drop it on the polished glassy carbon electrode surface, dry it naturally at room temperature, and obtain a working electrode.
[0073] The electrocatalytic hydrogen evolution performance under acidic conditions was tested in 0.5M sulfuric acid. The test results are shown in Figure 6-7 , as shown in 11 and 12. The scanning rate of the linear sweep voltammetry is 5 mV / s.
[0074] Depend on Figure 6 The electrochemical performance diagram shows that under acidic conditions, the copper indium phosphide sulfur supported palladium platinum (CIPS@PdPt) micro-nano particles have a high conductivity at 10 mA cm -2The corresponding overpotential at the current density is -64mV. Figure 7 The electrochemical performance diagram shows that under acidic conditions, the micro-nanoparticles of silver indium phosphosulfide supported palladium ruthenium (AIPS@PdRu) have a high conductivity at 10 mA cm -2 The corresponding overpotential at the current density is -80mV. Fig.11 The electrochemical performance diagram shows that under acidic conditions, the micro-nano particles obtained after laser treatment of copper indium phosphide have an electrochemical performance of 10 mA cm -2 The corresponding overpotential at the current density is only -649mV, indicating that the micro-nano particles obtained after laser treatment of copper indium phosphorus sulfur show poor electrocatalytic hydrogen evolution performance. Fig.12 The electrochemical performance diagram shows that under acidic conditions, the micro-nano particles obtained by copper indium phosphorus sulfur loading palladium have an electrochemical performance of 10 mA cm -2 The corresponding overpotential at the current density is only -178mV. Although its electrocatalytic performance is greatly improved compared with that of laser-treated copper indium phosphide, it is still far inferior to the micro-nanoparticles obtained by laser loading precious metal alloys (i.e., alloyed micro-nanoparticles). This shows that the phosphorus-sulfur alloy spherical micro-nanoparticles obtained by laser loading double precious metal alloys exhibit the most outstanding electrocatalytic hydrogen evolution performance.
[0075] The electrocatalytic hydrogen evolution performance under alkaline conditions was tested in 1M potassium hydroxide. The test results are shown in Figure 8 , 9 The scanning rate of the linear sweep voltammetry is 5 mV / s.
[0076] Depend on Figure 8 The electrochemical performance diagram shows that under alkaline conditions, the copper vanadium phosphorus sulfur supported ruthenium platinum (CVPS@RuPt) micro-nano particles have a high conductivity at 10 mA cm -2 The corresponding overpotential at the current density is -63mV. Fig. 9 The electrochemical performance diagram shows that under alkaline conditions, the micro-nano particles of silver vanadium phosphorus sulfur supported palladium iridium (AVPS@PdIr) have a high conductivity at 10 mA cm -2 The corresponding overpotential at the current density is -73mV.
[0077] The electrocatalytic oxygen reduction performance under alkaline conditions was tested in 0.1 M potassium hydroxide. Fig.10 As shown in FIG. 1 , the scanning rate of the linear sweep voltammetry is 10 mV / s.
[0078] Depend on Fig.10 The electrochemical performance diagram shows that under alkaline conditions, the half-wave potential of copper indium phosphorus sulfur supported palladium platinum (CIPS@PdPt) micro-nanoparticles is 0.81 V and the limiting current density is -4.95 mA cm -2This electrocatalytic performance is comparable to that of existing commercial Pt / C catalysts and has reached the level of commercial catalysts.
[0079] In summary, the phosphorus-sulfur alloy micro-nano particles prepared by the method of the present invention are a multifunctional catalyst having excellent electrochemical hydrogen evolution or electrochemical oxygen reduction performance under both acidic and alkaline conditions.
[0080] The embodiments of the present invention are described in detail above, but the present invention is not limited to the described embodiments. For those skilled in the art, various changes, modifications, substitutions and variations of these embodiments are made without departing from the principles and spirit of the present invention, and still fall within the protection scope of the present invention.
Claims
1. A method for preparing phosphorus-sulfur alloy micro-nano particles, It is characterized in that The following steps are involved: S1. Adding precious metal powder to a mixed solution of an organic solvent and water, mixing well, irradiating the obtained mixed solution with a pulsed laser for laser treatment, and pre-alloying the precious metal powder in the mixed solution by laser liquid phase ablation; the precious metal is at least two of palladium, platinum, ruthenium, and iridium; the organic solvent is ethanol or ascorbic acid; and the volume ratio of the organic solvent to water is 2-4:1; S2, adding a powder of a phosphorus-sulfur crystal matrix material to a pre-alloyed mixed solution, wherein the mass ratio of the matrix material to the precious metal is 1:1, and after mixing, irradiating the obtained mixed solution with a pulsed laser again for laser treatment, and forming a micro-nano spherical structure through laser liquid phase ablation to obtain phosphorus-sulfur alloy micro-nano particles, wherein the matrix material is any one or more of copper-indium-phosphorus-sulfur, silver-indium-phosphorus-sulfur, copper-vanadium-phosphorus-sulfur and silver-vanadium-phosphorus-sulfur; When performing pulse laser irradiation in steps S1 and S2, a 532nm YAG laser and a 532nm total reflection mirror or a 355nm YAG laser and a 355nm total reflection mirror are used; the energy of the pulse laser is 100-500 mJ, the frequency is 1-50 Hz, and the action time is 1-10 h.
2. The method for preparing phosphorus-sulfur alloy micro-nano particles according to claim 1, It is characterized in that The noble metal is a mixture of palladium and any one or more of platinum, ruthenium and iridium.
3. The method for preparing phosphorus-sulfur alloy micro-nano particles according to claim 1, It is characterized in that The volume ratio of the organic solvent to water in S1 is 3:
1.
4. Phosphorus-sulfur alloy micro-nano particles prepared by the preparation method according to any one of claims 1 to 3.
5. Application of the phosphorus-sulfur alloy micro-nano particles according to claim 4 in the field of electrochemistry.
Citation Information
Patent Citations
Preparation of CuInP2S6 quantum dots in high yield
CN112195024B
Method for regioselective synthesis of 1-alkyl-3-haloalkyl-1-pyrazol-4-carbonic acid derivatives
EP2100883A1
Method for preparing micro-nano medium-entropy and high-entropy materials through laser ablation
CN112643040A
Preparation of palladium-phosphorus-sulfur two-dimensional polycrystalline material and application thereof in electrochemical field
CN112742423A
Two-dimensional ferroelectric monatomic Ag loaded electrocatalyst
CN116516394A