A printed circuit board, a method for manufacturing a printed circuit board, and an electronic device.
By employing anti-plating and selective etching methods, zero-residue printed circuit boards were fabricated, solving the performance limitations of conventional printed circuit boards in high-signal-rate electronic devices and achieving high-density and high-signal-transmission effects.
Patent Information
- Application Number
- CN202110637081.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-06-08
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2041-06-08
AI Technical Summary
Conventional printed circuit board manufacturing methods are difficult to meet the needs of high signal rate electronic devices. Back drilling processes are prone to producing residual stubs, and a single lamination process can only produce a single-hole single-channel structure.
By employing anti-plating coating, one-time lamination technology, and selective etching, a suitable anti-plating coating is formed through a patterning process. Through-holes are then prepared and excess metal layers are removed, achieving a zero-residue pile and a multi-channel structure in a single hole.
This achieves zero-residue printed circuit boards, improving the performance and density of the boards and meeting the needs of high-signal-rate electronic devices.
Smart Images

Figure CN115460772B_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of electronic technology, and in particular to a printed circuit board, a method for manufacturing a printed circuit board, and an electronic device. Background Technology
[0002] Printed circuit boards (PCBs) are crucial components of electronic products. With the development of communication technology, the signal rates of electronic products such as bearer networks are constantly increasing. Conventional PCB fabrication methods are insufficient to meet the demands of these products' ever-increasing speeds. On one hand, PCB fabrication typically employs back-drilling, a process prone to producing residual spikes; on the other hand, conventional one-pass lamination PCB manufacturing processes can only produce single-channel structures with a single hole. Therefore, improvements to PCB performance are necessary. Summary of the Invention
[0003] This application provides a printed circuit board, a method for manufacturing the printed circuit board, and an electronic device to improve the performance of the circuit board and thus meet the needs of high signal rate electronic devices.
[0004] According to a first aspect of this application, a method for manufacturing a printed circuit board is provided, comprising the following steps:
[0005] A first anti-plating layer is prepared on the first core board;
[0006] A second anti-plating layer is formed on the first core board using a patterning process;
[0007] The second anti-plating layer is the patterned version of the first anti-plating layer;
[0008] The first core board and the second core board are stacked and pressed together;
[0009] Preparation of through holes;
[0010] The through hole passes through the second anti-plating layer and penetrates both the first core plate and the second core plate;
[0011] Remove the second anti-plating layer;
[0012] Preparation of metal layer;
[0013] The metal layer includes a first metal layer disposed in a first region of the inner wall of the through hole and a second metal layer disposed in a second region of the inner wall of the through hole;
[0014] Remove the second metal layer to expose the first metal layer.
[0015] According to a second aspect of this application, a method for manufacturing a printed circuit board is provided.
[0016] A first anti-plating layer is prepared on a first core board, a seventh anti-plating layer is prepared on a second core board, and a third anti-plating layer is prepared on a third core board.
[0017] A fourth anti-plating layer is formed on the first core board, a fifth anti-plating layer is formed on the second core board, and a sixth anti-plating layer is formed on the second core board using a patterning process.
[0018] The first core board, the second core board, the fourth core board and the third core board are stacked and pressed together in sequence;
[0019] Preparation of through holes;
[0020] The through hole passes through the fourth anti-plating layer, the fifth anti-plating layer and the sixth anti-plating layer, and penetrates the first core plate, the second core plate, the fourth core plate and the third core plate;
[0021] Remove the fourth, fifth, and sixth anti-plating layers;
[0022] Preparation of metal layer;
[0023] The metal layer includes a first metal layer disposed in a first region of the inner wall of the through hole, a fifth metal layer disposed in a second region of the inner wall of the through hole, a fourth metal layer disposed in a fourth region of the inner wall of the through hole, and a third metal layer disposed in a third region of the inner wall of the through hole.
[0024] Remove the fourth metal layer; expose the first metal layer, the fifth metal layer, and the third metal layer.
[0025] According to a third aspect of this application, a printed circuit board is provided, which is obtained by the above-described preparation method.
[0026] According to a third aspect of this application, an electronic device is provided, including the printed circuit board described above.
[0027] The technical solution provided in this application uses anti-plating layer, one-time lamination technology and selective etching to prepare a zero-residue circuit board, thereby improving the performance of the circuit board; at the same time, the technology provided in this application can also be used to prepare a one-hole multi-channel circuit board, increasing the circuit board density to meet the needs of high signal rate electronic devices. Attached Figure Description
[0028] Figure 1 This is a flowchart of a specific embodiment of the printed circuit board fabrication method in this application;
[0029] Figure 2 This is a flowchart illustrating the removal of the second metal layer in an embodiment of this application;
[0030] Figure 3This is a cross-sectional view of the first core board in an embodiment of this application;
[0031] Figure 4 This is a cross-sectional view of the first core board with an anti-plating layer in an embodiment of this application;
[0032] Figure 5 This is a partial cross-sectional view of the multilayer composite panel in the embodiments of this application;
[0033] Figure 6 This is a partial cross-sectional view of the multilayer composite panel in the embodiments of this application;
[0034] Figure 7 This is a cross-sectional view of the multilayer composite plate before drilling in an embodiment of this application;
[0035] Figure 8 This is a cross-sectional view of the multilayer composite panel after drilling in an embodiment of this application;
[0036] Figure 9 This is a cross-sectional view of the multilayer composite board during chemical copper plating in the embodiments of this application;
[0037] Figure 10 This is a cross-sectional view of the multilayer composite board after slight etching in an embodiment of this application;
[0038] Figure 11 This is a cross-sectional view of the multilayer composite board after copper plating in the embodiments of this application;
[0039] Figure 12 This is a cross-sectional view of an embodiment of this application after the second metal layer has been removed;
[0040] Figure 13 This is a cross-sectional view of the multilayer composite board formed by stacking the first core board, the second core board, the third core board and the fourth core board in the embodiments of this application;
[0041] Figure 14 yes Figure 13 Cross-sectional view of a multilayer composite board after copper plating;
[0042] Figure 15 yes Figure 14 Cross-sectional view after the second metal layer has been removed. Detailed Implementation
[0043] To make the objectives, technical solutions, and advantages of this application clearer, the following detailed description is provided in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the scope of this application. Unless otherwise specified, the embodiments and features described herein can be arbitrarily combined with each other.
[0044] The terms "first," "second," etc., used in the specification, claims, and accompanying drawings are used to distinguish similar objects and are not necessarily used to describe a specific order or sequence. It should be understood that if directional descriptions are involved, such as "up," "down," "front," "back," "left," "right," etc., indicating directions or positional relationships based on the directions or positional relationships shown in the accompanying drawings, this is only for the convenience of describing this application and simplifying the description, and does not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation; therefore, it should not be construed as a limitation of this application.
[0045] It should be noted that "several" means one or more, "multiple" means two or more, "greater than," "less than," and "exceeding" are understood to exclude the number itself, while "above," "below," and "within" are understood to include the number itself. If the terms "first" and "second" are used, they are only for distinguishing technical features and should not be construed as indicating or implying relative importance, or implicitly indicating the number of technical features indicated, or implicitly indicating the order of the technical features indicated.
[0046] In related technologies, stubs can cause signal reflection and resonance, leading to deterioration of insertion and return losses. As signal transmission speeds continue to increase, the length of stubs has an increasingly significant impact on signal transmission integrity. To reduce the length of stubs, backdrilling is typically used to remove them. Backdrilling reduces the length of the stub, shifting its resonant frequency to higher frequencies, thereby reducing its impact on the signal.
[0047] Back drilling utilizes the depth control function of a drilling rig to process blind holes. Its tolerances are primarily affected by the precision of the back drilling equipment and the thickness tolerance of the medium. In addition, its precision is easily influenced by external factors such as the resistance of the drill bit, the drill bit tip angle, the contact effect between the cover plate and the measuring unit, and the warpage of the plate. Furthermore, since the drill bit tip is generally V-shaped, during back drilling, in order to avoid the first metal layer, some residual piles may remain in the area between the first and second metal layers, affecting electrical conductivity and signal integrity, making it impossible to achieve the ideal situation of zero residual piles.
[0048] The following disclosure provides many different implementation methods or examples for different schemes of implementing this application.
[0049] Reference Figure 1 , Figures 3 to 12 The printed circuit board manufacturing method according to the first aspect of this application includes the following steps:
[0050] S101: Prepare a first anti-plating layer 220 on the first core board;
[0051] S102: Forming the second anti-plating layer 221 through a patterning process.
[0052] S103: The first core board 200 and the second core board 600 are stacked and pressed together;
[0053] S104: Prepare a through hole 400 that penetrates the first core plate 200 and the second core plate 600;
[0054] S105: Remove the second anti-plating layer 221;
[0055] S106: Prepare a metal layer, including a first metal layer 280 and a second metal layer 270;
[0056] S107: Remove the second metal layer 270 to expose the first metal layer 280.
[0057] In step S101, the boundary layer between the first metal layer 280 and the second metal layer 270, where metallization holes need to be processed, is pre-selected. Based on the location of the boundary layer, a first core board 200 is selected from the core boards of the printed circuit board 500 to be formed. In some embodiments, the first core board 200 has an inner copper foil 210 and an outer copper foil 240. The outer copper foil 240 can also be disposed on the first core board 200 using a prepreg 230. The inner copper foil 210 on the first core board 200 serves as the boundary layer. A first resist layer 220 is formed on the pre-drilled area of the inner copper foil 210. The material of the first resist layer 220 can be oil-based paint, ink, dry film, or wet film. The first resist layer 220 can be formed by screen printing, stencil printing, or exposure and development.
[0058] Reference Figures 3 to 5 After the first anti-plating layer 220 is fabricated in step S102, a patterning process is performed on the first core board 200. Through the patterning process, the first anti-plating layer 220 is fabricated into a suitable second anti-plating layer 221. Simultaneously, during the patterning process, an inner copper foil 210 is fabricated, partially retaining the inner copper foil 210 on the first core board 200. This ensures that the area of the inner copper foil 210 and the second anti-plating layer 221 are mutually compatible, with a preset drilling area located within this area, and this area should be larger than the preset drilling area. Specifically, the area of the second anti-plating layer 221 is smaller than the area of the retained inner copper foil 210, and the area difference between the two is between 1.5 mil and 2.5 mil, preferably 2 mil.
[0059] Reference Figures 5 to 7In step S103, a second core board 600 is provided below the first core board 200. The second core board 600 has the same structure as the first core board, and both have an inner copper foil 210 and an outer copper foil 240. The two can together form a multilayer composite board 300. Before forming the multilayer composite board 300, the first core board 200 and the second core board 600 are stacked in sequence, so that the second anti-plating layer 221 is located between the first core board 200 and the second core board 600. After stacking, the stacked structure is pressed by high temperature and high pressure, so that each part is fused into one, forming a multilayer composite board 300. The multilayer composite board 300 is the printed circuit board 500 to be drilled.
[0060] Reference Figure 5 as well as Figure 8 In step S104, any outer copper foil 240 on the laminated multilayer composite board 300 is used as the drilling surface. A hole is drilled in a predetermined drilling area on the drilling surface to form a through hole 400. The through hole 400 penetrates the entire multilayer composite board 300 from top to bottom, that is, it penetrates the first core board 200 and the second core board 600. At the same time, the through hole 400 passes through the second anti-plating layer 221.
[0061] Reference Figure 5 , Figures 8 to 10After step S104, the second anti-plating layer 221 located between the first core plate 200 and the second core plate 600 can be completely removed using conventional methods for removing the second anti-plating layer 221. For example, chemical solutions can be used to completely remove the second anti-plating layer 221. After removing the second anti-plating layer 221, a cavity is formed between the first core plate 200 and the second core plate 600, and the through hole 400 forms a discontinuity at the cavity. In some embodiments, the method for removing the second anti-plating layer 221 specifically involves: chemically depositing copper on the surface of the multilayer composite board 300, which is composed of the first core board 200 and the second core board 600 after lamination, and on the through-holes 400 inside, so that copper layers are attached to the second anti-plating layer 221 and the non-anti-plating layer areas on the board surface and in the through-holes 400. Because the copper absorption rates of the second anti-plating layer 221 and the non-anti-plating layer areas are different, the copper thickness on the second anti-plating layer 221 is less than the copper thickness in the non-anti-plating layer areas; specifically, the difference in copper thickness between the two is 22 μm. Next, a light etching process is used to remove the copper layer attached to the second anti-plating layer 221. Since the copper thickness in the non-anti-plating layer areas is greater than the copper thickness on the second anti-plating layer 221, after the light etching, only the copper layer on the second anti-plating layer 221 is completely removed, while some of the copper layer in the non-anti-plating layer areas remains, so that only the second anti-plating layer 220 is exposed to air inside the through-holes 400. Subsequently, the second anti-plating layer 220 located on the first core board 200 can be completely removed by the conventional method of removing the second anti-plating layer 221. At this time, the copper layer attached to the non-anti-plating layer area after chemical copper plating can protect the non-anti-plating layer area, so that only the second anti-plating layer 221 is removed during the use of chemical solutions.
[0062] Reference Figures 10 to 12 In step S106, an electroplated copper layer 260 is applied to the surface of the multilayer composite board 300, and copper is electroplated inside the through-hole 400. All non-anti-plating areas are re-plated with copper, while no copper layer is plated in the cavities. After the entire multilayer composite board 300 is electroplated, the inner wall of the through-hole 400 is divided into a first region and a second region by the unplated cavities. A first metal layer 280 is attached to the first region, and a second metal layer 270 is attached to the second region, making the through-hole 400 a discontinuous metallized hole. By forming a discontinuous metallized hole, the first metal layer 280 and the second metal layer 270 within the metallized hole can be separated. When the second metal layer 270 needs to be removed subsequently, whether by back drilling or other methods, the residual pile can be completely removed without touching the first metal layer 280, achieving zero residual pile.
[0063] In step S107, the second metal layer 270 is removed, leaving only the first metal layer 280, thereby enabling the printed circuit board 500 to achieve conductive connection within the area of the first metal layer 280. In some embodiments, the method for removing the second metal layer 270 is "applying a protective layer - three-stage wet etching," the steps of which include:
[0064] A first protective layer is prepared on the surface of the first metal layer 280, and a second protective layer is prepared on the surface of the second metal layer 270.
[0065] Wet etching removes the second protective layer;
[0066] Wet etching is used to remove the second metal layer;
[0067] Wet etching removes the first protective layer, exposing the first metal layer 280.
[0068] Specifically, a dry film (second protective layer) is applied to the area of the second metal layer 270, so that the area of the second metal layer 270 is completely covered by the dry film; further, the multilayer composite board 300 and the first metal layer 280 are protected by tin plating (first protective layer). After tin plating, the dry film (second protective layer) on the surface of the second metal layer 270 is removed by a first chemical etching (first wet etching). At this time, the first chemical etching only reacts chemically with the dry film and causes the dry film to peel off; then a second chemical etching is used to remove the dry film. The second metal layer 270 undergoes a second wet etching process. During this process, the second etching solution only reacts chemically with the second metal layer 270, completely removing the second metal layer 270 (i.e., the residual substrate). Further, a third wet etching process is performed on the area protected by tin plating (the first protective layer), namely the surface of the multilayer composite board 300 and the area of the first metal layer 280. This removes the tin plating layer covering the surface of the multilayer composite board 300 and the first metal layer 280, exposing the first metal layer 280. Removing the second metal layer 270 in this way reduces production costs, eliminates the need for back drilling, and ensures processing quality. The multilayer composite board 300 after removing the second metal layer 270 is thus a printed circuit board 500 with zero residual substrates.
[0069] Reference Figures 5 to 7In some embodiments, the first core board 200 and the second core board 600 can be stacked using a prepreg 230, with the stacking order being first core board 200 - prepreg 230 - second core board 600. This ensures that the second anti-plating layer 221 on the first core board 200 is in contact with the prepreg 230. After stacking, the layers are pressed together under high temperature and pressure. After removing the second anti-plating layer 221, a groove 250 is formed in the prepreg 230. After copper electroplating, the first metal layer 280 and the second metal layer 270 are respectively disposed on both sides of the groove 250 along the vertical direction. In some embodiments, to ensure a tighter bonding between the core layers and the first core 200, a groove 231 can be formed on the prepreg 230 at a position corresponding to the second resist layer 221. This allows the second resist layer 221 and the retained inner copper foil 210 to be accommodated within the groove 231 during bonding, thereby ensuring a tight fit between the prepreg 230 and the first core 200 in areas without the groove 231. To prevent the second resist layer 221 from entering the pattern during PCB misalignment, the diameter of the groove 231 is larger than the diameter of the through-hole; specifically, the diameter difference is between 5.5 mil and 6.5 mil, preferably 6 mil.
[0070] Reference Figures 13 to 15 The printed circuit board manufacturing method according to the second aspect of this application includes:
[0071] A first anti-plating layer 220 is prepared on the first core board 200, a seventh anti-plating layer 610 is prepared on the second core board 600, and a third anti-plating layer 710 is prepared on the third core board 700.
[0072] Through a patterning process, a fourth anti-plating layer 222 is formed on the first core board 200, a fifth anti-plating layer 611 is formed on the second core board 600, and a sixth anti-plating layer 711 is formed on the third core board 700.
[0073] The first core board 200, the second core board 600, the fourth core board 800 and the third core board 700 are stacked and pressed together in sequence;
[0074] Prepare a 400mm through-hole;
[0075] The through hole 400 passes through the fourth anti-plating layer 222, the fifth anti-plating layer 611 and the sixth anti-plating layer 711, and penetrates the first core plate 200, the second core plate 600, the fourth core plate 800 and the third core plate 700.
[0076] Remove the fourth anti-plating layer 222, the fifth anti-plating layer 611 and the sixth anti-plating layer 711;
[0077] Preparation of metal layer;
[0078] The metal layer includes a first metal layer 280 disposed in a first region of the inner wall of the through hole 400, a fifth metal layer 620 disposed in a second region of the inner wall of the through hole 400, a fourth metal layer 820 disposed in a fourth region of the inner wall of the through hole 400, and a third metal layer 720 disposed in a third region of the inner wall of the through hole 400.
[0079] Remove the fourth metal layer 820; expose the first metal layer 280, the fifth metal layer 620, and the third metal layer 720.
[0080] This method eliminates the need for copper layers in areas where electrical conduction and signal transmission are not required, resulting in a single-hole multi-channel zero-residue printed circuit board 500. This increases the circuit board density to meet the needs of high-signal-rate electronic devices.
[0081] Specifically, similar to the first aspect of the embodiment, a first anti-plating layer, a seventh anti-plating layer 610, and a third anti-plating layer 710 are respectively applied to the first core board 200, the second core board 600, and the third core board 700, all of which are applied to the three core boards as a whole. Furthermore, through a patterning process, the first anti-plating layer, the seventh anti-plating layer 610, and the third anti-plating layer 710 are respectively transformed into a fourth anti-plating layer 222, a fifth anti-plating layer 611, and a sixth anti-plating layer 711 with suitable shapes and sizes. During the patterning process, inner copper foil 210 is fabricated on the first core board 200, the second core board 600, and the third core board 700, and the inner copper foil 210 on each core board is partially retained, so that the area of the fourth anti-plating layer 222, the fifth anti-plating layer 611, and the sixth anti-plating layer 711 is adapted to the area of their respective inner copper foil 210. Next, a fourth core board 800 is added, and the above four core boards are stacked in the order of first core board 200-second core board 600-fourth core board 800-third core board 700, and then pressed together under high temperature and high pressure to form a multi-layer composite board. Starting from the outer copper foil of the first core board 200, holes are drilled from top to bottom in the preset drilling area to form through holes 400 in the multi-layer composite board 300 that penetrate the first core board 200, the second core board 600, the fourth core board 800 and the third core board 700. Next, the fourth resist layer 222, the fifth resist layer 611, and the sixth resist layer 711 are removed by chemical methods. Before removing the three resist layers, a chemical copper plating-light etching process can be used to protect the non-resist layer areas, so that only the fourth resist layer 222, the fifth resist layer 611, and the sixth resist layer 711 are removed. This creates cavities in the areas where the three resist layers have been removed. These cavities allow a single via 400 to form a multi-channel via 400. Next, copper is electroplated into the multi-channel via 400, so that all areas within the via 400 except for the cavities are covered with a metal layer (copper layer). The copper layers sequentially include: a first metal layer 280 (located in the first core board 200), a fifth metal layer 620 (located in the second core board 600), a fourth metal layer 820 (located in the fourth core board 800), and a third metal layer 720 (located in the third core board 700). Thus, the through-hole 400 has been formed as a multi-channel, discontinuous metallized via. Since the fourth metal layer 820, located in the middle of the laminated multilayer composite board 300, does not require electrical conduction or signal transmission, it is removed from the through-hole 400, leaving only the first metal layer 280, the fifth metal layer 620, and the third metal layer 720. The printed circuit board after removing the fourth metal layer 820 has no residual solder points and does not affect the integrity of signal transmission.
[0082] Reference Figure 2 as well as Figure 14In some embodiments, to completely remove the fourth metal layer 820, exposing the first metal layer 280, the fifth metal layer 620, and the third metal layer 720, and to reduce costs, a "protective layer application-three-stage wet etching" method can be used to remove the fourth metal layer 820. The steps include: preparing a dry film (second protective layer) in the area of the fourth metal layer 820, such that the area of the fourth metal layer 820 is completely covered by the dry film; further, tin plating (first protective layer) is applied to the first metal layer 280, the fifth metal layer 620, and the third metal layer 720 for protection; after tin plating, a single chemical etching (first wet etching) is performed to remove the dry film (second protective layer) from the surface of the fourth metal layer 820. The first etching solution reacts chemically only with the dry film, causing it to peel off. Then, a second etching solution is used to perform a second wet etching on the fourth metal layer 820 after the dry film has been removed. At this time, the second etching solution only reacts chemically with the fourth metal layer 820, that is, it completely removes the fourth metal layer 820 (i.e., the residual stump). Further, a third etching solution is used to perform a third wet etching on the area protected by tin plating (the first protective layer), that is, the area of the first metal layer 280, the fifth metal layer 620, and the third metal layer 720, so that the tin plating layer covering the first metal layer 280, the fifth metal layer 620, and the third metal layer 720 is removed, thereby exposing the first metal layer 280, the fifth metal layer 620, and the third metal layer 720.
[0083] Reference Figure 13In some embodiments, the step of removing the fourth anti-plating layer 222, the fifth anti-plating layer 611, and the sixth anti-plating layer 711 includes: chemically depositing copper on the through holes 400 of the first core board 200, the second core board 600, the fourth core board 800, and the third core board 700 after lamination, so that copper layers are attached to the fourth anti-plating layer 222, the fifth anti-plating layer 611, and the sixth anti-plating layer 711 in the through holes 400 as well as to the non-anti-plating layer areas. Since the copper absorption rates of the fourth anti-plating layer 222, the fifth anti-plating layer 611, and the sixth anti-plating layer 711 are different from those of the non-anti-plating layer areas, the copper thickness on the fourth anti-plating layer 222, the fifth anti-plating layer 611, and the sixth anti-plating layer 711 is less than the copper thickness in the non-anti-plating layer areas. A light etching process is then used to remove the copper layers attached to the fourth resist layer 222, the fifth resist layer 611, and the sixth resist layer 711. Since the copper thickness in the non-resistance areas is greater than that in the fourth resist layer 222, the fifth resist layer 611, and the sixth resist layer 711, only the copper layers on these layers are completely removed after the light etching. Part of the copper layer in the non-resistance areas remains, resulting in only the fourth resist layer 222, the fifth resist layer 611, and the sixth resist layer 711 being exposed to air inside the via 400. After chemical copper plating, the copper layer attached to the non-resistance areas provides protection for these areas. Then, a chemical solution is used to remove the fourth resist layer 222, the fifth resist layer 611, and the sixth resist layer 711.
[0084] Reference Figure 13 To ensure a tighter bonding between the first core board 200, the second core board 600, the fourth core board 800, and the third core board 700 during lamination, prepreg sheets 230 are inserted between each of them, and the first core board 200, the second core board 600, the fourth core board 800, and the third core board 700, along with their respective prepreg sheets 230, are stacked. The fourth anti-plating layer 222, the fifth anti-plating layer 611, and the sixth anti-plating layer 711 are respectively bonded to the prepreg sheets 230. During lamination, the fourth anti-plating layer 222, the fifth anti-plating layer 611, and the sixth anti-plating layer 711 can embed into their respective prepreg sheets 230. Therefore, after removing the fourth anti-plating layer 222, the fifth anti-plating layer 611, and the sixth anti-plating layer 711, grooves 250 are formed in the corresponding prepreg sheets 230.
[0085] Reference Figure 13In some embodiments, to provide a circuit board with one hole and multiple channels, a three-layer core board stacking and lamination method can be used. That is, the first core board 200, the second core board 600, and the third core board 700 are stacked and laminated in sequence. Using the above-described preparation method, an anti-plating layer is applied to the first core board 200 and the third core board 700 respectively. After drilling and removing the anti-plating layer, copper is plated in the through hole 400. Finally, the copper layer (residual stud) attached to the second core board 600 is removed by "applying a protective layer - three wet etching" to form a one-hole, three-channel printed circuit board. Similarly, a multi-layer core board stacking and lamination method can also be used, and the steps will not be described in detail here.
[0086] The printed circuit board 500 of the third aspect of this application is manufactured by the manufacturing method described above. The printed circuit board 500 manufactured by the above method achieves zero-residue printed circuit board performance by employing anti-plating layer, one-time lamination technology, and selective etching; simultaneously, the multi-channel printed circuit board with a single via can increase the circuit board density to meet the needs of high-signal-rate electronic devices.
[0087] The electronic device according to the fourth aspect of this application includes the printed circuit board 500 described above. Since the printed circuit board has the characteristic of zero residual points, it can improve the signal transmission performance and electrical conduction performance of the electronic device.
[0088] The above is a detailed description of the preferred embodiments of this application. However, this application is not limited to the above embodiments. Those skilled in the art can make various equivalent modifications or substitutions without departing from the spirit of this application. All such equivalent modifications or substitutions are included within the scope defined by the claims of this application.
Claims
1. A method of manufacturing a printed circuit board, characterized by, include: A first anti-plating layer is prepared on the first core board; A second anti-plating layer is formed on the first core board using a patterning process; The second anti-plating layer is the patterned version of the first anti-plating layer; The first core board and the second core board are stacked and pressed together; A through-hole is prepared, the through-hole passing through the second anti-plating layer and penetrating the first core plate and the second core plate; Remove the second anti-plating layer to form a groove; Preparation of metal layer; The metal layer includes a first metal layer disposed in a first region of the inner wall of the through hole and a second metal layer disposed in a second region of the inner wall of the through hole; the preparation of the metal layer includes: forming the first metal layer and the second metal layer in different regions separated by the groove by electroplating the whole plate; the first metal layer and the second metal layer are respectively disposed on both sides of the groove; Remove the second metal layer to expose the first metal layer.
2. The production method according to claim 1, characterized by, The removal of the second metal layer and exposure of the first metal layer includes: A first protective layer is prepared on the surface of the first metal layer, and a second protective layer is prepared on the surface of the second metal layer; Wet etching is used to remove the second protective layer; Wet etching is used to remove the second metal layer; Wet etching is used to remove the first protective layer and expose the first metal layer.
3. The method of claim 1, wherein: Removing the second anti-plating layer includes: Chemical copper plating is performed on the first and second core boards after lamination. Etching is performed on the first and second core boards after lamination; The second anti-plating layer is removed by chemical solutions.
4. The preparation method according to claim 1, characterized in that: The first core board and the second core board are laminated and pressed together by prepreg; After removing the second anti-plating layer, the groove is formed in the prepreg.
5. The method of claim 4, wherein: A groove is provided on the side of the semi-cured sheet near the second anti-plating layer, so that the second anti-plating layer is accommodated in the groove.
6. The preparation method according to claim 5, characterized in that: The diameter of the groove is larger than the diameter of the through hole, with a diameter difference of 5.5 mil to 6.5 mil.
7. The method of claim 1, wherein: The first core board includes an inner copper foil. When the second anti-plating layer is formed on the first core board through a patterning process, the inner copper foil is partially retained so that the area of the inner copper foil corresponds to the area of the second anti-plating layer.
8. The printed circuit board manufacturing method according to claim 7, characterized in that: The area difference between the second anti-plating layer and the inner copper foil is 1.5mil to 2.5mil.
9. A method of manufacturing a printed circuit board, characterized by, include: A first anti-plating layer is prepared on a first core board, a seventh anti-plating layer is prepared on a second core board, and a third anti-plating layer is prepared on a third core board. A fourth anti-plating layer is formed on the first core board, a fifth anti-plating layer is formed on the second core board, and a sixth anti-plating layer is formed on the third core board using a patterning process. The first core board, the second core board, the fourth core board and the third core board are stacked and pressed together in sequence; Preparation of through holes; The through hole passes through the fourth anti-plating layer, the fifth anti-plating layer and the sixth anti-plating layer, and penetrates the first core plate, the second core plate, the fourth core plate and the third core plate; Remove the fourth, fifth, and sixth anti-plating layers to form a groove; Preparation of metal layer; The metal layer includes a first metal layer disposed in a first region of the inner wall of the through hole, a fifth metal layer disposed in a second region of the inner wall of the through hole, a fourth metal layer disposed in a fourth region of the inner wall of the through hole, and a third metal layer disposed in a third region of the inner wall of the through hole. The preparation of the metal layer includes: forming the first metal layer, the fifth metal layer, the fourth metal layer and the third metal layer in different regions separated by the groove by whole-plate electroplating; The first metal layer and the fifth metal layer are respectively disposed on both sides of the groove formed by removing the fourth anti-plating layer; The fifth metal layer and the fourth metal layer are respectively disposed on both sides of the groove formed by removing the fifth anti-plating layer; The fourth metal layer and the third metal layer are respectively disposed on both sides of the groove formed by removing the sixth anti-plating layer; Remove the fourth metal layer; expose the first metal layer, the fifth metal layer, and the third metal layer.
10. The method of claim 9, wherein, The removal of the fourth metal layer and exposure of the first metal layer, the fifth metal layer, and the third metal layer includes: A first protective layer is prepared on the surface of the first, fifth, and third metal layers, and a second protective layer is prepared on the surface of the fourth metal layer; Wet etching is used to remove the second protective layer; The fourth metal layer is removed by wet etching. Wet etching is used to remove the first protective layer, exposing the first, fifth, and third metal layers.
11. The preparation method according to claim 9, characterized in that: Removing the fourth, fifth, and sixth anti-plating layers includes: Chemical copper plating is performed on the first core board, the second core board, the fourth core board, and the third core board after lamination. The first core board, the second core board, the fourth core board, and the third core board after lamination are etched. The fourth, fifth, and sixth anti-plating layers are removed by chemical solutions.
12. The preparation method according to claim 9, characterized in that: The first core board, the second core board, the fourth core board, and the third core board are stacked and pressed together using prepreg; After removing the fourth, fifth, and sixth anti-plating layers, the groove is formed in the corresponding prepreg.
13. A printed circuit board, characterized in that, The printed circuit board is obtained by the method according to any one of claims 1-12.
14. An electronic device, characterized in that, include: The printed circuit board as described in claim 13.
Citation Information
Patent Citations
Circuit board as well as selective plating process and manufacturing process thereof
CN108901146A