A porous Ti-Zr-Nb-Ta high entropy alloy and a preparation method thereof
Through mechanical alloying method and discharge plasma sintering technology, porous Ti-Zr-Nb-Ta high-entropy alloy is prepared, and MgO is used to regulate Young's modulus and strength, which solves the problem of high Young's modulus of biomedical materials and achieves The strength and biocompatibility match human bone, reducing preparation costs and energy consumption.
Patent Information
- Application Number
- CN202211163480.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-23
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2042-09-23
AI Technical Summary
The Young's modulus of existing biomedical metal materials is higher than that of human bones, resulting in a 'stress shielding effect' after implantation. Moreover, the pore-forming agents commonly used in the preparation process of porous materials are easy to volatilize at high temperatures, affecting the mechanical properties of the materials.
The Ti-Zr-Nb-Ta high-entropy alloy was prepared using a mechanical alloying method, using MgO as a pore-forming agent, and adjusting the MgO volume fraction and sintering conditions through discharge plasma sintering technology to obtain porous Ti-Zr-Nb-Ta high-entropy alloys. Entropy alloy meets the Young's modulus and strength requirements of human bone.
A porous Ti-Zr-Nb-Ta high-entropy alloy with high strength and low Young's modulus has been realized, which has good biocompatibility and mechanical properties. It solves the problem of mismatch between the material and human bone modulus and reduces the preparation time. Process energy consumption and costs.
Smart Images

Figure CN115533100B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of alloy materials, and in particular relates to a porous Ti-Zr-Nb-Ta high entropy alloy and a preparation method thereof. Background Art
[0002] At present, the biomedical metal materials widely used in clinical practice mainly include stainless steel, titanium and titanium alloys, cobalt-based alloys, and biodegradable magnesium alloys. However, the above materials have some disadvantages to a greater or lesser extent: (1) Poor biocompatibility. The common Ti alloy (Ti-6Al-4V) will cause cytotoxicity and allergies due to the release of Al and V metal ions during its long-term service, and is not suitable for long-term use in the human body. The release of Ni ions and Cr ions in stainless steel and Co ions and Cr ions in cobalt-chromium alloys will also cause cytotoxicity and metal allergic reactions to the human body, ultimately leading to implant failure; (2) High specific gravity and high elastic modulus. Compared with the Young's modulus of natural human bone (10-30 GPa), metal biomedical materials exhibit a higher Young's modulus. For example: the Young's modulus of Ti-6Al-4V is 110 GPa, the Young's modulus of 316L ss is 210 GPa, and the Young's modulus of CoCrMo alloy is 230 GPa. The Young's modulus of the above alloys is much higher than that of natural human bone. After implantation, they are likely to cause the "stress shielding effect" of human bones, thereby inducing the fragility of normal tissues around the implants; (3) Biological inertness. Therefore, it is particularly urgent to develop a biomedical orthopedic material that matches the Young's modulus of human bones and has good biocompatibility.
[0003] Many scientific researchers have done a lot of research to solve the problem of the mismatch between the Young's modulus of metal implant materials and human bones. In recent decades, there are two main research works: (1) Research and development of the third-generation new β-type (including full β-type, metastable β-type, near β-type or α+β-rich) medical titanium alloys that are free of toxic elements, high strength, and low Young's modulus. The currently developed β-type titanium alloys still have many problems, such as the high melting point of the alloy, the Young's modulus still cannot meet the matching of human bones, and biological inertness. (2) Porous materials. By adding pore-forming agents, a porous structure similar to human bones is formed to achieve the matching of the Young's modulus of human bones and materials. However, the introduction of porous structures will cause serious damage to the mechanical properties of the materials, so there are certain requirements for the mechanical properties of the materials. Moreover, the common pore-forming agents in the preparation of porous materials are NH 4 HCO 3 , NaCl, CaCl 2 , carbodiamide, etc. These pore-forming agents are volatile and meltable at high temperatures and cannot be used for materials prepared under high temperature and loaded pressure calcination conditions.
[0004] Since the concept of high entropy alloy was proposed, it has been favored by many scientific researchers. This is because it has excellent properties that traditional alloys cannot match, such as high strength, high hardness, wear and corrosion resistance, oxidation resistance, and good biocompatibility. In addition, it can also be given certain antibacterial properties by adding silver and copper. According to previous reports, the concept of high entropy is combined with the design of biomedical metal materials to prepare many high entropy alloy systems, such as TiZrNbTa, TiZrNbTaMo, TiZrNbTaHf, TiZrNbTaFe, etc. However, these studies have not solved the problem of mismatch between Young's modulus and human bone, and there is still a gap with the requirements of actual clinical applications. At present, many scientific researchers choose vacuum arc melting in the preparation process, and the melting point of metal materials with good biocompatibility is high, and the requirements for equipment become higher accordingly. At the same time, this process often leads to coarsening of material grains and uneven composition, which ultimately leads to a decrease in the mechanical properties of the material, making it more difficult to control the subsequent Young's modulus. Summary of the invention
[0005] In view of the above technical problems, the present invention discloses a porous Ti-Zr-Nb-Ta high entropy alloy and a preparation method thereof. The Young's modulus of the obtained high entropy alloy matches that of human bones, and it has high strength and good biocompatibility.
[0006] To this end, the technical solution adopted by the present invention is:
[0007] A method for preparing a porous Ti-Zr-Nb-Ta high entropy alloy comprises the following steps:
[0008] Step S1, preparing Ti-Zr-Nb-Ta alloy powder;
[0009] Step S2, mechanically mixing MgO and Ti-Zr-Nb-Ta alloy powder to obtain a mixed powder, wherein the volume percentage of MgO is 30%-50%;
[0010] Step S3, sintering the mixed powder by discharge plasma to obtain a block sample, the sintering temperature is 900-1100° C., and the loading pressure is 0-40 MPa;
[0011] Step S4: the bulk sample is placed in HNO 3 The pore former is removed from the solution to obtain a porous Ti-Zr-Nb-Ta high entropy alloy.
[0012] This technical solution uses Ti, ZrH with good biocompatibility 2, Nb, and Ta as raw materials, Ti-Zr-Nb-Ta alloy powder is obtained by mechanical alloying, and MgO with a high melting point and rough surface is used as a pore-forming agent. Combined with spark plasma sintering technology, the porous Ti-Zr-Nb-Ta high entropy alloy obtained has good biocompatibility, and there is no need to worry about cell death due to residues. By adjusting the volume fraction of MgO, a porous Ti-Zr-Nb-Ta high entropy alloy with low Young's modulus and high strength is prepared, which can meet the Young's modulus and higher strength that match human bones, solving the problem of mismatch between implant materials and human bones' Young's modulus.
[0013] In this technical solution, the use of MgO as a pore-forming agent has the basic characteristics of low cost, easy removal, controllable morphology and size. The melting point of MgO is as high as 2800°C. The high melting point allows MgO to be sintered at high temperature and with a certain loading pressure, so that the matrix material is sintered more tightly to improve the mechanical properties of the material. In addition, as an element with good biocompatibility, there is no need to worry about its residue being harmful to the human body when used as a pore-forming agent. The most critical thing is that no intermetallic compounds will be generated between Mg and a variety of elements, such as Ti, Zr, Nb, Ta, Hf, Mo, Fe, V, Cr and Mn, which is more reliable.
[0014] As a further improvement of the present invention, the volume percentage of MgO is 40%-50%.
[0015] As a further improvement of the present invention, in step S1, the prepared Ti-Zr-Nb-Ta alloy powder has a nano-scale grain size, uniform composition and a wide particle size distribution.
[0016] As a further improvement of the present invention, in step S3, the sintering temperature is 1000° C. and the loading pressure is 30 MPa.
[0017] As a further improvement of the present invention, in step S4, the reaction temperature is 40-60°C.
[0018] As a further improvement of the present invention, in step S4, HNO 3 The concentration of the solution is 2~3 mol / L, and further HNO 3 The concentration of the solution is 2.5 mol / L.
[0019] As a further improvement of the present invention, in step S2, MgO and Ti-Zr-Nb-Ta alloy powders are mechanically mixed and then passed through a 200-mesh sieve to obtain a mixed powder.
[0020] As a further improvement of the present invention, in step S2, the mechanical mixing is performed using a desktop double-motion mixer.
[0021] As a further improvement of the present invention, the particle size of the MgO is micrometer-level or nanometer-level.
[0022] As a further improvement of the present invention, step S1 comprises: Ti, ZrH 2 The raw metal powders of Zr, Nb and Ta are added into a stainless steel ball mill in an equiatomic ratio for alloying to prepare a Ti-Zr-Nb-Ta alloy powder with a nano-scale grain size. Furthermore, during the ball milling, the powder dispersing time interval is 1-5 h; during the ball milling in step S1, the ball-to-material ratio is 10-20:1; further, during the ball milling, the mass of the small stainless steel balls accounts for 40-65% of the total mass of the grinding balls. Further, the particle size distribution of the obtained Ti-Zr-Nb-Ta alloy powder is 1-400 μm.
[0023] The present invention also discloses a porous Ti-Zr-Nb-Ta high entropy alloy, which is prepared by using any one of the above methods for preparing the porous Ti-Zr-Nb-Ta high entropy alloy.
[0024] Compared with the prior art, the present invention has the following beneficial effects:
[0025] First, the technical solution of the present invention selects Ti, ZrH with good biocompatibility. 2 , Nb, and Ta metals as raw materials, and mechanical alloying combined with discharge plasma process were used to prepare large-block samples of Ti-Zr-Nb-Ta high-entropy alloy with added MgO. After removing the MgO pore-forming agent, the obtained porous Ti-Zr-Nb-Ta high-entropy alloy can meet the strength requirements of human bones of more than 100 MPa and a Young's modulus of 10-30 GPa, and also has good biocompatibility.
[0026] Furthermore, the compression performance and Young's modulus of the porous Ti-Zr-Nb-Ta high entropy alloy were tested and it was found that when the MgO addition was 40 vol.%, the strength and Young's modulus of the porous Ti-Zr-Nb-Ta high entropy alloy were 297.0 ± 12.1 MPa and 30.5 GPa, respectively. When the MgO addition was 45 vol.%, the strength and Young's modulus of the porous Ti-Zr-Nb-Ta high entropy alloy were 206.4 ± 5.3 MPa and 18.1 GPa, respectively. When the MgO addition was 50 vol.%, the strength and Young's modulus of the porous Ti-Zr-Nb-Ta high entropy alloy were 113.8 ± 3.9 MPa and 10.6 GPa, respectively.
[0027] Second, the technical solution of the present invention uses MgO as a pore-forming agent, which is low in cost, easy to remove, and has controllable morphology and size. Moreover, the melting point of MgO is as high as 2800°C. The higher melting point allows MgO to be sintered at high temperature and with a certain loading pressure, so that the matrix material is sintered more tightly, which is beneficial to improving the mechanical properties of the material. In addition, Mg is an element with good biocompatibility, so there is no need to worry about its residue being harmful to the human body when used as a pore-forming agent. The most critical thing is that no intermetallic compounds are generated between Mg and various elements, such as Ti, Zr, Nb, Ta, Hf, Mo, Fe, V, Cr and Mn. Therefore, it can be used in alloy systems containing the above elements. The rough surface of the MgO particles will serve as a template to regulate the microstructure in the pores. After being removed, the pores of the matrix material will become rough, which is beneficial to the attachment, proliferation and differentiation of cells.
[0028] Third, the technical solution of the present invention adopts a mechanical alloying method in the preparation process of the alloy, which can effectively reduce the alloying temperature and eliminate the input of other heat sources, effectively reduce energy consumption, save costs, and solve the problem of inevitable microstructural defects such as uneven material composition, segregation and grain coarsening caused by the arc melting process. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 3 are SEM images of MgO powder and Ti-Zr-Nb-Ta alloy powder of Example 1 of the present invention, wherein a) and b) are SEM images of MgO powder at different magnifications, and c) and d) are SEM images of Ti-Zr-Nb-Ta alloy powder at different magnifications.
[0030] Figure 2 1 and 2 are particle size distribution diagrams of MgO and Ti-Zr-Nb-Ta alloy powders of Example 1 of the present invention, wherein a) is the particle size distribution diagram of MgO, and b) is the particle size distribution diagram of Ti-Zr-Nb-Ta alloy powder.
[0031] Figure 3 It is the XRD comparison diagram of MgO and Ti-Zr-Nb-Ta in Example 1 of the present invention.
[0032] Figure 4 These are SEM images of the embodiments of the present invention when MgO pore formers with different volume fractions are not removed after sintering; a) is 30%, b) is 35%, c) and d) are SEM images of 40% at different magnifications, e) is 45%, and f) is 50%.
[0033] Figure 51 and 2 are SEM images of MgO pore formers with different volume fractions after removal according to the embodiments of the present invention; a) is 30%, b) is 35%, c) and d) are SEM images of 40% at different magnifications, e) is 45%, and f) is 50%.
[0034] Figure 6 1 and 2 are SEM images of the internal cross-sections of the embodiments of the present invention after removing the MgO pore formers with different volume fractions; a) is 30%, b) is 35%, c) is 40%, d) is 45%, and e) is 50%.
[0035] Figure 7 1 is an XRD diagram of a Ti-Zr-Nb-Ta high entropy alloy before and after the removal of MgO pore formers with different volume fractions in an embodiment of the present invention; wherein a) is when the MgO pore former is not removed, and b) is after the pore former is removed.
[0036] Figure 8 These are the SEM images, corresponding element distribution diagrams, and EDS results of the Ti-Zr-Nb-Ta high entropy alloy added with 40 vol.% MgO pore former in the embodiment of the present invention, wherein a) is the SEM image of the Ti-Zr-Nb-Ta high entropy alloy, b) is the EDS result, and a1) to a6) are the corresponding element distribution diagrams.
[0037] Fig. 9 EBSD images and grain size distribution images of the Ti-Zr-Nb-Ta high entropy alloy added with 40 vol.% MgO pore former according to an embodiment of the present invention; wherein a) and b) are EBSD images at different magnifications, and c) is a grain size distribution image.
[0038] Fig.10 It is a stress-strain curve diagram of the porous Ti-Zr-Nb-Ta high entropy alloy obtained after removing the MgO pore former in the embodiment of the present invention.
[0039] Fig.11 This is a columnar comparison chart of the Young's modulus of the porous Ti-Zr-Nb-Ta high entropy alloy obtained in the embodiment of the present invention and other biomedical materials.
[0040] Fig.12 The SEM images of the comparative examples of the present invention after sintering with different pore-forming agents, after removing the pore-forming agents, and their cross-sections; wherein a) is the SEM image of comparative example 1 sintered with pore-forming agent Si, and b) is the SEM image of comparative example 2 sintered with pore-forming agent Si / SiO 2 Sintered SEM image, c) is the comparative example 3 using pore-forming agent SiO 2 SEM images of sintering, a1) is the SEM image of comparative example 1 after removing the pore-forming agent Si, b1) is the SEM image of comparative example 2 after removing the pore-forming agent Si / SiO 2SEM image of the comparative example 3 where the pore-forming agent SiO is removed. 2 a2) is the SEM image of the cross section of the comparative example 1 after the pore-forming agent Si is removed, and b2) is the SEM image of the cross section of the comparative example 2 after the pore-forming agent Si / SiO is removed. 2 The cross-sectional SEM image of the sample c2) is the comparative example 3 in which the pore-forming agent SiO is removed. 2 SEM image of the cross section. DETAILED DESCRIPTION
[0041] The preferred embodiments of the present invention are described in further detail below.
[0042] Example 1
[0043] Ti, ZrH 2 The raw metal powders of Zr, Nb and Ta are added into a stainless steel ball mill in equal atomic ratios for mechanical alloying to prepare Ti-Zr-Nb-Ta alloy powder with nano-scale grain size, uniform composition and wide particle size distribution. The particle size distribution of Ti-Zr-Nb-Ta alloy powder is 1-400 μm, with an average particle size of 57 μm. In order to ensure that no other impurities are introduced, no process control agent is added. The specific ball milling process is:
[0044] The powder dispersing time interval is 1-5 h, and the ball-to-material ratio is 10-20:1. In the ball mill, the mass of the small stainless steel balls accounts for 40-65% of the total mass of the grinding balls. The small stainless steel balls are small stainless steel balls in the ball mill of the prior art, the powder dispersing time interval is 1 h, and the ball-to-material ratio is 15:1. In the ball mill, the mass of the small stainless steel balls accounts for 64% of the total mass of the grinding balls.
[0045] MgO was selected as a pore-forming agent, and the alloy powder after mechanical alloying was sieved through a 200-mesh stainless steel sieve. Under mechanical mixing conditions, MgO and Ti-Zr-Nb-Ta alloy powder were mixed for 999 min, and the volume fraction of MgO was 30%.
[0046] The mixed powder was sintered by spark plasma to obtain a bulk sample at a sintering temperature of 1000°C and a loading pressure of 30 MPa. 3 The pore former is removed by reaction in the solution to obtain a porous Ti-Zr-Nb-Ta high entropy alloy.
[0047] Example 2
[0048] Based on Example 1, in this example, the volume fraction of MgO is 35%. Other details are the same as in Example 1.
[0049] Example 3
[0050] Based on Example 1, in this example, the volume fraction of MgO is 40%. Other aspects are the same as in Example 1.
[0051] Example 4
[0052] Based on Example 1, in this example, the volume fraction of MgO is 45%. Other aspects are the same as in Example 1.
[0053] Example 5
[0054] On the basis of Example 1, in this example, the volume fraction of MgO is 50%, and the rest is the same as Example 1.
[0055] In Example 1, the SEM images of MgO powder and Ti-Zr-Nb-Ta alloy powder are as follows: Figure 1 As shown, the particle size distribution of MgO and Ti-Zr-Nb-Ta alloy powders is shown in Figure 2 As shown, the XRD pattern is Figure 3 As shown, the average particle size of the Ti-Zr-Nb-Ta high entropy alloy powder is about 31 μm, which is close to the average particle size of the pore-forming agent MgO (33 μm).
[0056] The microscopic morphology of the MgO pore-forming agent without removing the pore-forming agent after sintering in Examples 1 to 5 is as follows: Figure 4 As shown in FIG. 1 , as the volume percentage of MgO increases, MgO is evenly distributed in the block sample obtained after sintering. The microscopic morphology and cross-sectional diagram of the removal of MgO pore-forming agent with different volume fractions in Example 1 to Example 5 are shown in FIG. Figure 5 and Figure 6 As shown in the figure, it can be seen that when the volume fraction of the pore former is 30%, there are still pore formers inside the matrix that have not been removed, and no interconnected pores are formed. As the volume fraction of the pore former increases to 35%-50%, most of the interconnected pores are formed, and the MgO pore former is completely removed. It can be seen that the pore size of the implant material can be controlled according to the particle size of the pore former. The choice of the particle size of the pore former is diverse, and pore formers of different particle sizes can be selected.
[0057] The XRD patterns of Ti-Zr-Nb-Ta high entropy alloys before and after sintering without removing the MgO pore former are shown in Figure 2. Figure 7 As shown in the figure, by comparison, it is found that the MgO pore former does not generate other compounds with other elements in the matrix material. Among them, the SEM image of the Ti-Zr-Nb-Ta high entropy alloy with 40 vol.% MgO pore former added, its corresponding element distribution map and EDS results are shown in the figure. Figure 8 The EBSD map and grain size distribution of Ti-Zr-Nb-Ta high entropy alloy with 40 vol.% MgO pore former added are shown in Fig. 9As shown in the figure, the average grain size of the bulk Ti-Zr-Nb-Ta high entropy alloy was found to be 237.1 ± 12.0 nm. According to the Hall-Petch formula, the nanoscale grain size will give the material high strength. Due to the sintering conditions of 1000°C high temperature and 30 MPa loading pressure, and the relatively rough surface of MgO, this rough surface acts as a template to make the Ti-Zr-Nb-Ta high entropy alloy have protrusions in the pores and become rough after removing MgO. This rough pore environment will be conducive to the proliferation, attachment and differentiation of osteoblasts. At the same time, under the condition of adding more than 35 vol.% MgO, the Ti-Zr-Nb-Ta high entropy alloy becomes a three-dimensional interconnected pore structure. This structure is conducive to allowing cells to enter its interior to promote bone regeneration and vascularization, promote the absorption of osteoinductive proteins, and ion exchange (Ca 2+ / PO 4 3- ) and apatite (bone mineral phase). The porous Ti-Zr-Nb-Ta high entropy alloy without the pore-forming agent was compressed and tested for Young's modulus, and finally a Ti-Zr-Nb-Ta high entropy alloy with high strength, low Young's modulus and great application potential was successfully produced.
[0058] The stress-strain curves of the porous Ti-Zr-Nb-Ta high entropy alloys obtained after removing the MgO pore-forming agent in Examples 1 to 5 are shown in FIG. Fig.10 As shown, the Young's modulus comparison of the porous Ti-Zr-Nb-Ta high entropy alloy obtained in Examples 1 to 5 and other existing biomedical materials is shown in FIG. Fig.11 As shown, it can be seen that when the MgO addition is 40 vol.%, the strength and Young's modulus of the porous Ti-Zr-Nb-Ta high entropy alloy are 297.0 ± 12.1 MPa and 30.5 GPa, respectively. When the MgO addition is 45 vol.%, the strength and Young's modulus of the porous Ti-Zr-Nb-Ta high entropy alloy are 206.4 ± 5.3 MPa and 18.1 GPa, respectively. When the MgO addition is 50 vol.%, the strength and Young's modulus of the porous Ti-Zr-Nb-Ta high entropy alloy are 113.8 ± 3.9 MPa and 10.6 GPa, respectively. It meets the requirements of human bones for strength of more than 100 MPa and Young's modulus of 10-30GPa. At the same time, it also lays the foundation for the preparation of porous materials under high temperature and loading pressure preparation conditions.
[0059] From the experiment, when the volume percentage of MgO added is less than 30%, the volume fraction of the pore former is too low, resulting in the inability to form interconnected pores, which is not conducive to the transmission of nutrients after implantation. When the volume percentage of MgO added exceeds 50% and reaches 55%, the experiment shows that the compressive strength is lower than 100 MPa, which cannot meet the requirement of human bone strength of 100 MPa. That is, when the volume fraction of the pore former is too large, the mechanical properties of the matrix material will be greatly damaged, making it impossible for the matrix material to meet the mechanical properties requirements of the implant material. Therefore, in combination with the mechanical properties, a volume fraction of the pore former of 40%-50% is very appropriate. It meets the requirements of human bone strength of 100 MPa and Young's modulus of 10-30 GPa.
[0060] Moreover, human bones present a multi-gradient pore structure, ranging from micrometers to nanometers. Therefore, the pore size of the implant material can be controlled according to the particle size of the pore-forming agent. The choice of the particle size of the pore-forming agent is diverse, and pore-forming agents of different particle sizes can be selected.
[0061] Comparative Example 1
[0062] On the basis of Example 1, in the process of exploring suitable pore-forming agents, this comparative example 1 uses spherical Si as a pore-forming agent, the volume fraction of the pore-forming agent is 50%, and the spark plasma sintering process (SPS) is used under the conditions of sintering pressure of 1000°C and 30 MPa. It is found that the spherical Si of the pore-forming agent forms an obvious diffusion layer with the matrix Ti-Zr-Nb-Ta high entropy alloy, such as Fig.12 After 72 h of removing the pore former in 5 mol / L NaOH solution at 50°C, it was found that the Ti-Zr-Nb-Ta matrix was corroded and produced a large number of cracks, and there was still pore former inside the matrix that was not successfully removed, as shown in Fig.12 a1) and Fig.12 a2).
[0063] Comparative Example 2
[0064] Based on Example 1, this comparative example 2 uses spherical silicon to be heat-treated and oxidized in oxygen to form a core-shell structure Si / SiO 2 (Heat treatment conditions: 300 ° C, 40 h) as a pore-forming agent. Under the conditions of pore-forming agent volume fraction of 50%, sintering pressure of 1000 ° C, 30 MPa, spark plasma sintering (SPS) was used to sinter. It was found that the pore-forming agent core-shell structure Si / SiO 2 It forms an obvious diffusion layer with the matrix Ti-Zr-Nb-Ta high entropy alloy, such as Fig.12b). After 72 h of removing the pore former in 50°C and 5 mol / L NaOH solution, it was found that the Ti-Zr-Nb-Ta matrix was corroded and produced a large number of cracks, and there was still pore former inside the matrix that was not successfully removed, as shown in Fig.12 b1) and Fig.12 b2).
[0065] Comparative Example 3
[0066] Based on Example 1, this comparative example 3 uses commercial SiO 2 As a pore-forming agent, the spark plasma sintering process (SPS) was used under the conditions of 50% pore-forming agent volume fraction, 1000 ° C, and 30 MPa. It was found that the core-shell structure Si / SiO 2 It forms an obvious diffusion layer with the matrix Ti-Zr-Nb-Ta high entropy alloy, such as Fig.12 c). After 72 h of removing the pore former in 5 mol / L NaOH solution at 50°C, it was found that the Ti-Zr-Nb-Ta matrix was corroded and produced a large number of cracks, and there was still pore former inside the matrix that was not successfully removed, as shown in Fig.12 c1) and Fig.12 c2).
[0067] By comparing Examples 1 to 5 and Comparative Examples 1 to 3, it can be seen that the technical solution of the embodiment of the present invention, that is, using MgO as a pore-forming agent with a volume fraction of 30%-50%, can significantly reduce the Young's modulus, which can meet the requirement of 10-30 GPa of the Young's modulus of human bone, and is close to the strength of human bone 100 MPa. As an implant material, it can match the Young's modulus of human bone and meet the requirements of subsequent clinical applications. At the same time, it also lays a foundation for the preparation of porous materials under high temperature and loading pressure preparation conditions.
[0068] The above contents are further detailed descriptions of the present invention in combination with specific preferred embodiments, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. For ordinary technicians in the technical field to which the present invention belongs, several simple deductions or substitutions can be made without departing from the concept of the present invention, which should be regarded as falling within the scope of protection of the present invention.
Claims
1. A method for preparing a porous Ti-Zr-Nb-Ta high entropy alloy, characterized in that: The steps include: Step S1, preparing Ti-Zr-Nb-Ta alloy powder, comprising: adding Ti, ZrH2, Nb, and Ta metal raw powders in an equal atomic ratio into a stainless steel ball mill for alloying to obtain Ti-Zr-Nb-Ta alloy powder with nano-scale grain size; Step S2, mechanically mixing MgO and Ti-Zr-Nb-Ta alloy powder to obtain mixed powder, wherein the volume percentage of MgO is 40%-50%; the particle size of the MgO is micron-level and the surface is rough; Step S3, sintering the mixed powder by discharge plasma to obtain a block sample, the sintering temperature is 900-1100° C., and the loading pressure is 30 MPa; Step S4, removing the pore former from the bulk sample in a HNO3 solution to obtain a porous Ti-Zr-Nb-Ta high entropy alloy.
2. The method for preparing a porous Ti-Zr-Nb-Ta high entropy alloy according to claim 1, characterized in that: In step S3, the sintering temperature is 1000°C.
3. The method for preparing the porous Ti-Zr-Nb-Ta high entropy alloy according to claim 1, characterized in that: In step S4, the reaction temperature is 40-60°C, and the concentration of the HNO3 solution is 2.5 mol / L.
4. The method for preparing the porous Ti-Zr-Nb-Ta high entropy alloy according to claim 1, characterized in that: In step S2, MgO and Ti-Zr-Nb-Ta alloy powders are mechanically mixed and then passed through a 200-mesh sieve to obtain a mixed powder.
5. The method for preparing the porous Ti-Zr-Nb-Ta high entropy alloy according to claim 4, characterized in that: In step S2, the mechanical mixing is performed using a desktop double-motion mixer.
6. The method for preparing the porous Ti-Zr-Nb-Ta high entropy alloy according to claim 1, characterized in that: In the ball milling, the powder dispersing time interval is 1-5 h; in the ball milling of step S1, the ball-to-material ratio is 10-20:
1.
7. The method for preparing the porous Ti-Zr-Nb-Ta high entropy alloy according to claim 6, characterized in that: In ball milling, the mass of small stainless steel balls accounts for 40~65% of the total mass of the grinding balls.
8. The method for preparing the porous Ti-Zr-Nb-Ta high entropy alloy according to claim 7, characterized in that: The particle size distribution of the obtained Ti-Zr-Nb-Ta alloy powder is 1-400 μm.
9. A porous Ti-Zr-Nb-Ta high entropy alloy, characterized in that: The porous Ti-Zr-Nb-Ta high entropy alloy is prepared by the preparation method of any one of claims 1 to 8.