Preparation and application of a ferroferric oxide nanofluid modified microbubble cleaning fluid
Through the modified microbubble cleaning liquid of iron tetraoxide nanofluid, the cleaning problem of high viscosity oil-containing sludge is solved, low-cost and efficient oil material peeling and recycling is achieved, environmental pollution is avoided, and environmental protection and safety is demonstrated. Processing effect.
Patent Information
- Application Number
- CN202211356871.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-01
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2042-11-01
AI Technical Summary
The existing oil-containing sludge treatment technology has problems such as transfer of oily substances to the environment, incineration produces toxic substances, pyrolysis of residual oils, high extraction costs and secondary pollution, especially the poor cleaning effect of high-viscosity oil-containing sludge.
The nanomaterials are prepared by co-precipitation method by using iron tetraoxide nanofluid modified microbubble cleaning solution. After vacuum freeze-drying, the surfactant is dispersed under ultrasonic stirring to form uniform nanofluid modified microbubble, combined with magnetic field recovery , reduce oil viscosity and improve the peeling efficiency of oil substances.
It realizes low-cost and efficient oil-wet sludge cleaning, reduces the amount of surfactant, avoids secondary pollution, and is both biodegradable and environmentally friendly.
Smart Images

Figure CN115536239B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of solid waste treatment and disposal, and specifically relates to the preparation and application of a ferroferric oxide nanofluid modified microbubble cleaning liquid, which is suitable for cleaning oil-containing solid phases, especially for cleaning high-viscosity oily sludge. Background Art
[0002] Oily sludge is a hazardous solid waste generated during oil extraction and wastewater treatment. The oil in oily sludge consists of four types of substances: saturated fraction, aromatic fraction, colloid, and asphaltene. Oily sludge has the characteristics of high yield, complex nature, and high pollution. If it is not effectively treated, it will inevitably pose a serious threat to humans and the environment.
[0003] Existing technologies for treating oily sludge include solidification, landfill, incineration, pyrolysis, extraction, etc. These technologies all have certain defects. Solidification and landfill may transfer oil substances into the environment, posing the risk of polluting soil and groundwater; incineration produces toxic organic dioxins, which pollute the environment and the oil substances are not recovered; oil substances still remain on the sludge after pyrolysis and cannot be harmlessly treated; extraction has problems such as high processing costs and secondary pollution caused by residual extraction agents.
[0004] Patent document CN 114956491 A discloses a chemical cleaning agent and its preparation method and application. The chemical cleaning agent includes a first cleaning agent and a second cleaning agent. The first cleaning agent includes sodium carbonate, sodium bicarbonate and sodium hydroxide to emulsify oil substances on sludge. The second cleaning agent includes various surfactants to separate the emulsified oil from the sludge, and the dry oil content is reduced to less than 2wt%. However, the surfactant dosage of this method is as high as 3wt% to 20wt%, which is costly and can easily cause secondary pollution if the cleaning liquid is improperly handled. This method produces a large amount of emulsified oil when cleaning sludge, and it is difficult to demulsify. In view of this, the present invention provides an environmentally friendly, safe and efficient Fe3O4 nanofluid modified microbubble cleaning liquid preparation method. Summary of the invention
[0005] To solve the above problems, the present invention provides a preparation and application of a ferroferric oxide nanofluid modified microbubble cleaning liquid. The cleaning liquid is prepared by a two-step method. First, a coprecipitation method is used to prepare ferroferric oxide nanomaterials. After the nanomaterials are dialyzed, the nanomaterials are vacuum freeze-dried by controlling the thickness, drying time and temperature of the nanomaterials to volatilize the water between the nanomaterials without destroying the original structure of the materials, thereby ensuring that the prepared nanomaterials do not agglomerate. Then, under ultrasonic stirring conditions, the nanomaterials are dispersed with a pressurized surfactant solution to prepare a uniform nanofluid and generate modified microbubbles at the same time. The nanomaterials are adsorbed on the microbubbles or the surfactant molecules are adsorbed on the surface, and no agglomeration occurs. The particle size of the modified microbubbles reaches the micrometer level, and it is easy to combine with oil substances. The cleaning liquid of the present invention is applied to the cleaning of oily sludge under gradient magnetic field conditions, and is particularly suitable for oil-wet solid phase cleaning. The Fe3O4 magnetic nanomaterials are recovered using a magnetic field.
[0006] The Fe3O4 magnetic nanofluid in the cleaning liquid of the present invention has the functions of reducing oil viscosity, changing the wettability of the solid phase surface, etc., can strengthen the stripping of oil from the solid phase, has a good cleaning effect on oil-wet sludge, and the Fe3O4 magnetic nanofluid can be recovered by a magnetic field, and the cleaning cost is low; the modified microbubbles generated by the cleaning liquid of the present invention through self-assembly can reduce the critical micelle concentration of the surfactant, the amount of the surfactant is reduced to 1wt% at least, and the emulsification amount of oil substances can be ensured to be small, which is convenient for recycling; in addition, the Fe3O4 nanomaterial of the present invention is recovered by a magnetic field, and the surfactants used in the present invention include sodium fatty alcohol polyoxyethylene ether carboxylate and sophora biosurfactant, have a biodegradability of 100%, do not generate secondary pollution, and are environmentally friendly.
[0007] Technical Difficulties
[0008] The technical difficulties of the present invention are:
[0009] (1) Fe3O4 nanoparticles have a large specific surface area and high surface activity. They are prone to agglomeration during the preparation of magnetic nanomaterials and magnetic nanofluids, thus losing their nanofluid function.
[0010] (2) The oil-wet solid surface has a strong adsorption strength for oil substances, the sludge has high viscosity and poor fluidity, and conventional chemical cleaning agents have poor cleaning effects on oil-wet sludge.
[0011] (3) The cleaning fluid contains a large amount of surfactants, which can easily cause secondary pollution if not handled properly.
[0012] Technical Solution
[0013] The technical scheme for preparing and applying the ferroferric oxide nanofluid-modified microbubble cleaning liquid of the present invention is as follows:
[0014] (1) Fe3O4 nanomaterials with a particle size of 5 to 60 nm and no agglomeration were prepared by co-precipitation, dialysis and vacuum freeze drying.
[0015] (2) A surfactant solution of sodium polyoxyethylene fatty alcohol carboxylate and sophorolipids was pressurized to disperse Fe3O4 nanoparticles under ultrasonic and stirring conditions to prepare a Fe3O4 nanofluid modified microbubble cleaning liquid with good dispersion, high gas content, no agglomeration and good stability.
[0016] (3) The prepared Fe3O4 nanofluid modified microbubble cleaning fluid is applied to the cleaning of oily sludge, the parameters affecting the cleaning process are controlled, and efficient cleaning of the oil-wet solid phase is achieved.
[0017] (4) After cleaning, the Fe3O4 nanoparticles are recovered by a magnetic field, and the recovered petroleum is recycled.
[0018] The significant innovation of the present invention lies in that a Fe3O4 nanomaterial with uniform particle size and dispersion is prepared by a pressurized composite surfactant solution, a dispersion coprecipitation, a dialysis, and a vacuum freeze-drying method at normal pressure, and a Fe3O4 nanofluid modified microbubble cleaning solution with good stability and high gas content is simultaneously prepared. The magnetic nanofluid solid phase wetting reversal, anti-oil droplet aggregation, and increased separation pressure in the cleaning solution of the present invention synergize the modified microbubbles to reduce interfacial tension and solubilize, prevent oil droplets from aggregating into large particles on the oil sludge, promote the curling of oil substances on the surface of the oil sludge, and accelerate the peeling of oil substances from the solid phase. The oil removal rate of the oil-wet solid phase is high. Combined with the implementation steps of the present invention, its innovation and beneficial effects are as follows:
[0019] A method for preparing a Fe3O4 nanofluid modified microbubble cleaning liquid comprises the following steps:
[0020] (1) Add distilled water to the reactor, raise the temperature to 80-90°C under nitrogen and stirring conditions, add iron precursor solution, the weight ratio of iron precursor solution to distilled water is 1:100-1:15, and quickly add 25wt% ammonia water after adding the precursor solution. Raise the temperature to 100°C, react for 1-3h, stop heating, cool to room temperature under anaerobic conditions, and dialyze the mixed solution with a 8000-12000kDa dialysis bag for 3-5d.
[0021] In the step (1), the nitrogen flow rate is 30-60 mL / min, the stirring speed is 50-200 r / min; the addition ratio of ammonia water (25 wt%) is 1:10-2:5, and the addition rate is 100-400 g / (L·min); the iron precursor solution solvent is concentrated sulfuric acid or concentrated nitric acid, the solute concentration is 0.5-1 mol FeCl3·6H2O / L, 0.25-0.5 mol FeSO4·7H2O / L, and the molar ratio of Fe 3+ :Fe 2+ =2:1.
[0022] (2) The dialyzed material is vacuum freeze-dried with a vacuum degree of 20 to 80 Pa.
[0023] In the step (2), the pre-freezing temperature of the vacuum freeze drying is -40°C to -50°C, and the pre-freezing treatment is 6 to 10 hours. The thickness of the vacuum freeze drying material is 3 to 6 mm. If the material is too thick, the dehydration effect is poor, and if the material is too thin, the drying efficiency is low. The vacuum freeze drying has three stages: freezing at -15°C to -10°C for 0.8h to 1h, freezing at 0°C to 5°C for 0.8h to 1h, and freezing at 10°C to 25°C for 0.5 to 1h. The heating rate between the two drying stages is 0.5 to 2°C / min. The drying process can remove 99% of the moisture and ensure that the nanomaterial does not agglomerate. The particle size of the black Fe3O4 nanomaterial obtained by vacuum freeze drying is 5 to 60nm.
[0024] (3) Compounding surfactant solution, the compounding ratio of fatty alcohol polyoxyethylene ether carboxylate sodium (AEC-9Na): sophorolipid (SL) = 5:6 to 5:1, and the total surfactant concentration is 1 to 3 wt%.
[0025] In the step (3), the sodium fatty alcohol polyoxyethylene ether carboxylate (AEC-9Na) and the sophorolipid (SL) are anionic surfactants and nonionic surfactants, respectively. The compounding can reduce the electrostatic repulsion on the outer shell of the modified microbubbles, and more surfactant molecules can be arranged on the outer shell, thereby enhancing the ability of the modified microbubbles to bind to the oil. The total concentration of the surfactant is 1 to 3 wt %. At a higher concentration, the excess surfactant binds to the Fe3O4 nanoparticles to prevent them from agglomerating in the solution.
[0026] (4) Pressurizing the surfactant solution to dissolve air, and releasing it into a container containing the Fe3O4 nanomaterial prepared in step (1) at normal pressure, wherein the concentration of the Fe3O4 nanomaterial is 0.2-0.8 wt %. Stirring and contacting in an ultrasonic field for 3-7 min, a Fe3O4 nanofluid-modified microbubble cleaning solution is obtained.
[0027] In the step (4), the pressure is 0.2-1.5 MPa; the ultrasonic condition frequency is 20000-30000 Hz and the intensity is 20-400 W / L, so that the system is fully mixed to form modified microbubbles, disperse the nanomaterials, and make some nanomaterials adsorbed on the microbubbles; the stirring rate is 10-90 r / min, and the nanomaterials are dispersed by hydraulic shear.
[0028] (5) treating the oily sludge with the Fe3O4 nanofluid modified microbubble cleaning solution prepared in step (4), and recovering the Fe3O4 nanoparticles with a magnetic field after the cleaning is completed.
[0029] In the step (5), the cleaning liquid-solid ratio is 3:1-7:1, the initial cleaning temperature is 10-20°C, the temperature is programmed to rise by 4-10°C / min, and the temperature is raised to 60-90°C; the mixed liquid circulates up and down in the container, the magnetic field direction is 90° to the flow direction, the magnetic field intensity Hmax=500-2000Gs, the magnetic field gradient dH / dx=0.01-10T / m, the stirring intensity is 200-1500r / min, and the cleaning is carried out for 10-30min; the magnetic nanofluid is recovered by a magnetic field, and the magnetic field intensity H=2300-3000Gs.
[0030] (6) After the magnetic nanofluid is recovered, the cleaning system is allowed to stand for 5 to 10 minutes before solid-liquid separation; the rotation speed is 500 to 1500 r / min, and the liquid phase is centrifuged for 3 to 6 minutes before oil-water separation, and the oil material is recycled.
[0031] The beneficial effects of the present invention are as follows:
[0032] 1. The nanomaterial prepared by the present invention has uniform particle size, the particle size is between 5 and 60 nm, and the specific surface area is large; the nanomaterial after dialyzation is treated by vacuum freeze drying to ensure that the nanomaterial does not agglomerate before use, and the surface activity of the nanomaterial is retained to the maximum extent.
[0033] 2. A pressurized surfactant solution is used as a base liquid to disperse Fe3O4 nanomaterials, and modified microbubbles are generated at the same time, and Fe3O4 nanofluid modified microbubble solution is prepared synchronously. The process is simple, the nanomaterials in the Fe3O4 nanofluid modified microbubble cleaning liquid have good dispersion and no agglomeration, and the cleaning liquid is stable. The magnetic nanofluid enhances heat transfer, improves thermal efficiency, increases separation pressure, and changes the wettability of the solid surface. The modified microbubbles are combined with solubilization, reduce oil-water interfacial tension, peel, and prevent oil aggregation and precipitation, thereby enhancing the separation of oil and oil-wet sludge, accelerating the rate of oil transfer to the liquid phase, and improving the oil removal rate.
[0034] 3. After cleaning, the Fe3O4 nanomaterials are recovered by magnetic field, ultrasonically dispersed and then vacuum freeze-dried for reuse; the surfactants fatty alcohol polyoxyethylene ether carboxylate sodium and sophorolipids are non-toxic and harmless, 100% biodegradable, and green and environmentally friendly. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 It is a flowchart of the steps of preparing the cleaning solution in the present invention.
[0036] Figure 2 This is a diagram of the cleaning mechanism of Fe3O4 nanofluid modified microbubbles in the present invention. DETAILED DESCRIPTION
[0037] The present invention will be further described below in conjunction with embodiments and drawings, but the present invention is not limited by the following embodiments.
[0038] Example 1
[0039] This example is about a preparation method of Fe3O4 nanofluid modified microbubble cleaning fluid and its application in chemical cleaning of oil sludge in a refinery tank. The four components of crude oil (measured with reference to SH / T0509-92 (98)) are saturated 29.84%, aromatic 38.77%, colloid 15.89%, asphalt 15.50%, and the three-phase composition of oily sludge is water content 49.36%, solid content 39.72%, and oil content 10.92%.
[0040] The processing steps are as follows:
[0041] (1) Add distilled water to the reactor, and heat it to 80°C under nitrogen and stirring conditions; add an iron precursor solution with a concentration of 0.25 molFe / LHCl, the iron precursor solution: distilled water = 1:15 by weight, and the addition ratio of ammonia water (25wt%), ammonia water: distilled water = 1:10, and the addition rate is 100 g / (L·min); heat to 100°C, react for 1 hour, stop heating, cool to room temperature under anaerobic conditions, and dialyze the mixed solution with a 8000-12000 kDa dialysis bag for 3 days.
[0042] (2) The dialyzed material was vacuum freeze-dried at a vacuum degree of 50 Pa. The pre-freezing temperature was -40°C and the pre-freezing treatment was 6 hours. The material thickness was 3 mm and the vacuum degree was 60 Pa. The vacuum freeze-drying temperature and time were controlled, freezing at -15°C for 0.8 hours, freezing at 0°C for 0.8 hours, freezing at 10°C for 0.5 hours, and the heating rate between the two drying stages was 0.5°C / min, and black Fe3O4 nanopowder with a particle size of 5 to 60 nm was obtained.
[0043] (3) Compounding surfactant solution, the compounding ratio of fatty alcohol polyoxyethylene ether carboxylate sodium (AEC-9Na): sophorolipid (SL) = 5:6, the total surfactant concentration is 1.5wt%.
[0044] (4) Pressurizing the surfactant solution: In step (4), the air is pressurized to 0.2 MPa and released into a container containing the Fe3O4 nanomaterial prepared in step (1) at normal pressure. The concentration of the Fe3O4 nanomaterial is 0.2 wt %, the ultrasonic field frequency is 20000, the sound intensity is 20 W / L, the stirring rate is 10 r / min, and the contact time is 3 min to obtain the Fe3O4 nanofluid modified microbubble cleaning solution.
[0045] (5) Fe3O4 nanofluid modified microbubble cleaning liquid and oily sludge were added to the cleaning device, with a liquid-to-solid ratio of 3:1, an initial temperature of 20°C, a programmed temperature increase of 4°C / min, and a temperature increase to 60°C; the mixed liquid circulated up and down in the container, the magnetic field direction was 90° to the flow direction, the magnetic field intensity Hmax = 500 Gs, the magnetic field gradient dH / dx = 0.01 T / m, the stirring intensity was 200 r / min, and the cleaning was carried out for 10 min.
[0046] (6) Magnetic field strength H = 2300Gs to recover Fe3O4 nanoparticles.
[0047] (7) After the magnetic nanofluid is recovered, the cleaning system is allowed to stand for 5 minutes before solid-liquid separation. The rotation speed is 500 r / min, and the liquid phase is centrifuged for 3 minutes before oil-water separation, and the oil material is recycled.
[0048] The results are shown in Table 1.
[0049] Table 1 Cleaning effect of different cleaning fluids on oily sludge
[0050] Cleaning fluid Residual oil rate, % Oil removal rate, % Cleaning liquid of the present invention 6.3 93.7 Distilled water 90.2 9.8 <![CDATA[Fe3O4 nanofluid]]> 73.7 26.3 AEC-9Na solution 31.5 68.5 SL solution 19.4 80.6
[0051] Example 2
[0052] This example is about a preparation method of Fe3O4 nanofluid modified microbubble cleaning fluid and its application in chemical cleaning of oil sludge in an oil field in Xinjiang. The four components of crude oil (measured with reference to SH / T0509-92 (98)) are saturated 31.63%, aromatic 31.58%, colloid 17.45%, asphalt 19.34%, and the three-phase composition of oily sludge is water content 25.67%, solid content 48.96%, and oil content 25.37%.
[0053] The processing steps are as follows
[0054] (1) Add distilled water to the reactor, and heat it to 90°C under nitrogen and stirring conditions; add 0.5 molFe / LH2SO4 iron precursor solution, the weight ratio of iron precursor solution: distilled water = 1:100, the addition ratio of ammonia water (25wt%), ammonia water: distilled water = 2:5, and the addition rate is 400 g / (L·min); heat to 100°C, react for 3 hours, stop heating, cool to room temperature under anaerobic conditions, and dialyze the mixed solution with a 8000-12000 kDa dialysis bag for 5 days.
[0055] (2) The dialyzed material was vacuum freeze-dried with a vacuum degree of 80 Pa. The pre-freezing temperature was -50 °C and the pre-freezing treatment was 10 hours. The material thickness was 6 mm and the vacuum degree was 80 Pa. The vacuum freeze-drying temperature and time were controlled, freezing at -10 °C for 1 hour, freezing at 5 °C for 1 hour, and freezing at 25 °C for 1 hour. The heating rate between the two drying stages was 2 °C / min, and black Fe3O4 nanopowder with a particle size of 5 to 60 nm was obtained.
[0056] (3) Compounding surfactant solution, the compounding ratio of fatty alcohol polyoxyethylene ether carboxylate sodium (AEC-9Na): sophorolipid (SL) = 5:1, the total surfactant concentration is 3wt%.
[0057] (4) The surfactant solution is pressurized to 1.5 MPa to dissolve air, and then released into a container containing the Fe3O4 nanomaterial prepared in step (1) at normal pressure. The concentration of the Fe3O4 nanomaterial is 0.8 wt %, the ultrasonic field frequency is 30000 Hz, the intensity is 400 W / L, the stirring rate is 90 r / min, and the contact time is 7 min to obtain the Fe3O4 nanofluid modified microbubble cleaning solution.
[0058] (5) Fe3O4 nanofluid modified microbubble cleaning liquid and oily sludge were added to the cleaning device, with a liquid-to-solid ratio of 7:1, an initial temperature of 20°C, a programmed temperature increase of 10°C / min, and a temperature increase to 90°C; the mixed liquid circulated up and down in the container, the magnetic field direction was 90° to the flow direction, the magnetic field intensity Hmax = 2000Gs, the magnetic field gradient dH / dx = 10T / m, the stirring intensity was 1500r / min, and the cleaning was carried out for 30min.
[0059] (6) Magnetic field strength H = 3000Gs to recover Fe3O4 nanoparticles.
[0060] (7) After the magnetic nanofluid is recovered, the cleaning system is left to stand for 10 minutes before solid-liquid separation. The rotation speed is 1500 r / min, and the liquid phase is centrifuged for 6 minutes before oil-water separation, and the oil material is recycled.
[0061] The results are shown in Table 2.
[0062] Table 2 Cleaning effect of different cleaning fluids on oily sludge
[0063] Cleaning fluid Residual oil rate, % Oil removal rate, % Cleaning liquid of the present invention 5.7 94.3 Distilled water 96.8 5.2 <![CDATA[Fe3O4 nanofluid]]> 79.7 20.3 AEC-9Na solution 38.8 61.2 SL solution 36.2 63.8
[0064] Example 3
[0065] This example is about a preparation method of Fe3O4 nanofluid modified microbubble cleaning fluid and its application in chemical cleaning of oil sludge in an oil field in Xinjiang. The four components of crude oil (measured with reference to SH / T0509-92 (98)) are saturated 31.63%, aromatic 31.58%, colloid 17.45%, asphalt 19.34%, and the three-phase composition of oily sludge is water content 25.67%, solid content 48.96%, and oil content 25.37%.
[0066] The processing steps are as follows
[0067] (1) Add distilled water to the reactor, and heat it to 90°C under nitrogen and stirring conditions; add iron precursor solution, the weight ratio of iron precursor solution: distilled water = 1:50, ammonia water (25wt%) addition ratio, ammonia water: distilled water = 1:5, and the addition rate is 200g / (L·min); heat to 100°C, react for 2.5h, stop heating, cool to room temperature under anaerobic conditions, and dialyze the mixed solution with a 8000-12000kDa dialysis bag for 3d.
[0068] (2) The dialyzed material was vacuum freeze-dried with a vacuum degree of 50 Pa. The pre-freezing temperature was -40°C and the pre-freezing treatment was 6 hours. The material thickness was 5 mm and the vacuum degree was 60 Pa. The vacuum freeze-drying temperature and time were controlled, freezing at -12°C for 0.9 hours, freezing at 3°C for 0.9 hours, and freezing at 20°C for 0.8 hours. The heating rate between the two drying stages was 1°C / min, and black Fe3O4 nanopowder with a particle size of 5 to 60 nm was obtained.
[0069] (3) Compounding surfactant solution, the compounding ratio of fatty alcohol polyoxyethylene ether carboxylate sodium (AEC-9Na): sophorolipid (SL) = 1:1, the total surfactant concentration is 1.8wt%.
[0070] (4) The surfactant solution is pressurized to 0.7 MPa to dissolve air, and then released into a container containing the Fe3O4 nanomaterial prepared in step (1) at normal pressure. The concentration of the Fe3O4 nanomaterial is 0.5 wt %, the ultrasonic field frequency is 30000 Hz, the intensity is 300 W / L, the stirring rate is 90 r / min, and the contact time is 6 min to obtain the Fe3O4 nanofluid modified microbubble cleaning solution.
[0071] (5) Fe3O4 nanofluid modified microbubble cleaning liquid and oily sludge were added to the cleaning device, with a liquid-to-solid ratio of 5:1, an initial temperature of 20°C, a programmed temperature increase of 10°C / min, and a temperature increase to 60°C; the mixed liquid circulated up and down in the container, the magnetic field direction was 90° to the flow direction, the magnetic field intensity Hmax = 2000Gs, the magnetic field gradient dH / dx = 5T / m, the stirring intensity was 200r / min, and the cleaning was carried out for 30min.
[0072] (6) Magnetic field strength H = 2500Gs to recover Fe3O4 nanoparticles.
[0073] (7) After the magnetic nanofluid is recovered, the cleaning system is allowed to stand for 7 minutes before solid-liquid separation. The rotation speed is 1000 r / min, and the oil and water are separated after centrifugation for 5 minutes, and the oil substances are recycled.
[0074] The results are shown in Table 3.
[0075] Table 3 Cleaning effect of different cleaning fluids on oily sludge
[0076] Cleaning fluid Residual oil rate, % Oil removal rate, % Cleaning liquid of the present invention 10.7 89.3 Distilled water 94.9 5.1 <![CDATA[Fe3O4 nanofluid]]> 92.2 17.8 AEC-9Na microbubble solution 36.5 73.5 SL Microbubble Solution 24.8 75.2
Claims
1. An application of Fe3O4 nanofluid modified microbubble cleaning fluid, comprising the following steps: (1) Add distilled water to the reactor, raise the temperature to 80-90° C. under nitrogen and stirring conditions, add the iron precursor solution, and add the iron precursor solution: distilled water = 1:100-1:
15. After adding the iron precursor solution, quickly add 25wt% ammonia water, raise the temperature to 100° C., react for 1-3 hours, stop heating, cool to room temperature under anaerobic conditions, and dialyze the mixed solution with a 8000-12000 kDa dialysis bag for 3-5 days; (2) vacuum freeze-drying the dialyzed material to obtain Fe3O4 nanomaterials; (3) preparing a surfactant solution, wherein the ratio of fatty alcohol polyoxyethylene ether carboxylate sodium (AEC-9Na) to sophorolipid (SL) is 5:6 to 5:1, and the total surfactant concentration is 1 to 3 wt%; (4) pressurizing the composite surfactant solution in step (3) to dissolve air, and releasing it into a container containing the Fe3O4 nanomaterial prepared in step (2) at normal pressure, wherein the concentration of the Fe3O4 nanomaterial is 0.2-0.8 wt %, and the solution is stirred and contacted in an ultrasonic field for 3-7 min to obtain a Fe3O4 nanofluid modified microbubble cleaning solution; (5) treating the oily sludge with the Fe3O4 nanofluid modified microbubble cleaning fluid prepared in step (4); (6) After the cleaning is completed, the Fe3O4 nanoparticles are recovered by a magnetic field; (7) After the magnetic nanofluid is recovered, the cleaning system is allowed to stand for 5 to 10 minutes before solid-liquid separation. The rotation speed is set at 500 to 1500 r / min, and the liquid phase is centrifuged for 3 to 6 minutes before oil-water separation. The oil is then recycled.
2. The use of a Fe3O4 nanofluid modified microbubble cleaning liquid according to claim 1, characterized in that: In the step (1), the nitrogen flow rate is 30-60 mL / min, and the stirring speed is 50-200 r / min.
3. The use of a Fe3O4 nanofluid modified microbubble cleaning fluid according to claim 1, characterized in that: The solvent of the iron precursor solution in step (1) is concentrated sulfuric acid or concentrated nitric acid, with a molar ratio of Fe 3+ :Fe 2+ =2:1,Fe 2+ Concentration: 0.25~0.5mmoL / L.
4. The use of a Fe3O4 nanofluid modified microbubble cleaning fluid according to claim 1, characterized in that: In the step (1), the ratio of ammonia water to distilled water is 1:10 to 2:5, and the addition rate is 100 to 400 g / (L·min).
5. The use of a Fe3O4 nanofluid modified microbubble cleaning fluid according to claim 1, characterized in that: The vacuum degree of step (2) is 20 to 80 Pa, the pre-freezing temperature of vacuum freeze drying is -40°C to -50°C, and the pre-freezing treatment is 6 to 10 hours; the thickness of the vacuum freeze-dried material is 3 to 6 mm, and the vacuum freeze drying has three stages: freezing at -15°C to -10°C for 0.8h to 1h, freezing at 0°C to 5°C for 0.8h to 1h, and freezing at 10°C to 25°C for 0.5 to 1h, and the heating rate between the two drying stages is 0.5 to 2°C / min.
6. The use of a Fe3O4 nanofluid modified microbubble cleaning liquid according to claim 1, characterized in that: The particle size of the Fe3O4 nanomaterial in step (2) is 5 to 60 nm.
7. The use of a Fe3O4 nanofluid modified microbubble cleaning fluid according to claim 1, characterized in that: In the step (4), the dissolved gas pressurization pressure is 0.2-1.5 MPa, the ultrasonic frequency is 20000-30000 Hz, the ultrasonic power density is 20-400 W / L, and the stirring rate is 10-90 r / min.
8. The use of a Fe3O4 nanofluid modified microbubble cleaning fluid according to claim 1, characterized in that: In the step (5), the application conditions of the Fe3O4 nanofluid modified microbubble cleaning liquid are as follows: a liquid-to-solid ratio of 3:1 to 7:1, an initial cleaning temperature of 10 to 20°C, a programmed temperature increase of 4 to 10°C / min, and a temperature increase to 60 to 90°C; the mixed liquid circulates up and down in the container, the magnetic field direction is 90° to the liquid flow direction, the magnetic field intensity Hmax = 500 to 2000 Gs, the magnetic field gradient dH / dx = 0.01 to 10 T / m, the stirring intensity is 200 to 1500 r / min, and the cleaning time is 10 to 30 min.
9. The use of a Fe3O4 nanofluid modified microbubble cleaning fluid according to claim 1, characterized in that: In the step (6), the magnetic field strength for recovering Fe3O4 nanoparticles is H=2300-3000GS.