Leather and method for manufacturing the same

Through the combined structure of the polyester base material, the adhesive layer and the surface layer, the leather is manufactured using melt-blown and thermal pressing processes, which solves the problems of environmental pollution and difficulty in recycling materials in the existing technology, and achieves environmental benefits and manufacturing cost savings. , while improving product performance.

CN115538177BActive Publication Date: 2024-10-22SAN FANG CHEM IND
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111150238.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-06-30
Filing Date
2021-09-29
Publication Date
2024-10-22
Estimated Expiration
2041-09-29

AI Technical Summary

Technical Problem

Most of the existing artificial leather manufacturing methods involve complicated processes, use of solvents leads to environmental pollution, and the materials are difficult to recycle, violating environmental protection requirements.

Method used

It adopts a combined structure of polyester base material, polyester bonding layer and polyester surface layer, and manufactures leather through melt-blown and thermal pressing processes. All materials are made of a single polyester material and can be recycled, granulated and reused.

Benefits of technology

It achieves environmental benefits and manufacturing cost savings, improves the product's temperature resistance, mechanical strength and lightweight properties, making it suitable for long-term wear.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115538177B_ABST
    Figure CN115538177B_ABST
Patent Text Reader

Abstract

The present invention relates to a leather and a manufacturing method thereof. The leather is recyclable and comprises: a polyester substrate, a polyester adhesive layer and a polyester surface layer. The polyester adhesive layer is arranged on the polyester substrate. The polyester surface layer is arranged on the polyester adhesive layer. All materials of the leather of the present invention are made of the same polyester material. The leather of the present invention can be recycled and granulated after use, which has environmental benefits.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to leather and a method for making the same. Background Art

[0002] Conventional methods for making artificial leather generally use a variety of complicated processes, and some processes require the use of solvents, which are harmful to the environment and do not meet environmental protection requirements. In addition, conventional materials for making artificial leather require the use of raw materials of different materials, so that conventional artificial leather cannot be recycled after use.

[0003] Therefore, it is necessary to provide an innovative and progressive leather and a method for manufacturing the same to solve the above-mentioned conventional deficiencies. Summary of the invention

[0004] The present invention relates to a leather. In one embodiment, the leather comprises: a polyester substrate, a polyester adhesive layer and a polyester surface layer. The polyester adhesive layer is disposed on the polyester substrate. The polyester surface layer is disposed on the polyester adhesive layer.

[0005] The present invention relates to a method for manufacturing leather. In one embodiment, the method comprises the following steps: providing a polyester substrate; melt-blowing a polyester adhesive layer onto the polyester substrate; melt-blowing a polyester surface layer onto the polyester adhesive layer; and heat-pressing the polyester substrate, the polyester adhesive layer, and the polyester surface layer. BRIEF DESCRIPTION OF THE DRAWINGS

[0006] Figure 1 A schematic diagram showing the structure of leather according to an embodiment of the present invention.

[0007] Figure 2 A schematic diagram showing a process flow of a method for manufacturing leather according to an embodiment of the present invention.

[0008] 10: Leather

[0009] Description of reference numerals:

[0010] 11: Polyester base material

[0011] 12: Polyester adhesive layer

[0012] 13: Polyester surface layer

[0013] 111: First surface

[0014] 112: Second surface

[0015] S21~S24: Steps DETAILED DESCRIPTION

[0016] See also Figure 1, which is a schematic diagram showing the structure of a leather according to an embodiment of the present invention. In one embodiment, the leather 10 of the present invention comprises: a polyester substrate 11 , a polyester adhesive layer 12 and a polyester surface layer 13 .

[0017] In one embodiment, the polyester substrate 11 has a first surface 111 and a second surface 112, and the second surface 112 is opposite to the first surface 111. In one embodiment, the polyester substrate 11 is made of PET (Polyethylene Terephthalate), which is an engineering plastic. The polyester substrate 11 can be 100% PET recycled cotton or 60% PET recycled cotton mixed with 40% PET cotton, and entangled to form a non-woven fabric using a needle-pressing method; or 100% recycled PET fiber or general PET fiber is woven into a woven fabric. Therefore, the polyester substrate 11 is completely made of polyester material. In one embodiment, the polyester substrate 11 can be TPEE (Thermoplastic Polyether Elastomer) material or PBT (Polybutylene Terephthalate) material.

[0018] In one embodiment, the polyester adhesive layer 12 is disposed on the first surface 111 of the polyester substrate 11. The polyester adhesive layer 12 may be made of TPEE (Thermoplastic Polyether Elastomer), which is an engineering plastic with elastomer properties, or PBT (Polybutylene Terephthalate), which is a thermoplastic engineering polymer. The weight of the polyester adhesive layer 12 is 50-400 g / m 2 , density is 0.2-0.8g / cm 3 The polyester adhesive layer 12 has thermoplasticity. In one embodiment, the polyester adhesive layer 12 can be made of PET.

[0019] In one embodiment, the polyester surface layer 13 is disposed on the polyester adhesive layer 12. The polyester surface layer 13 can be made of PET, TPEE or PBT. The weight of the polyester surface layer 13 is 50-400 g / m 2 , density is 0.5-0.9g / cm 3 The polyester surface layer 13 has thermoplasticity.

[0020] In one embodiment, the leather 10 of the present invention comprises: the polyester substrate 11, the polyester adhesive layer 12 and the polyester surface layer 13, wherein the polyester substrate 11, the polyester adhesive layer 12 and the polyester surface layer 13 are made of a single polyester material and do not have other materials. Therefore, all materials of the leather 10 of the present invention are made of the same polyester material, and the leather 10 of the present invention can be recycled and granulated after use, which has environmental benefits. In addition, the recycled thermoplastic polyester particles obtained by recycling and granulation can be added to the manufacturing process of the leather 10 of the present invention to further enhance the environmental benefits and save manufacturing costs.

[0021] In one embodiment, since the leather 10 of the present invention is made of a single polyester material, and since the polyester material has a higher glass transition temperature and melting point than the polyester material, when the leather 10 of the present invention is applied to a product, the product can have higher temperature resistance and thermal stability. In addition, since the polyester material has a better mechanical strength than the polyester material, when the leather 10 of the present invention is applied to a product, the mechanical strength of the product can be improved, such as the tensile strength and tear strength of the shoe material, which can improve the usability of the product. Furthermore, since the polyester material has a lower density than the polyester material, when the leather 10 of the present invention is applied to a product, the overall weight of the product can be reduced to make the product lighter, making the product more suitable for long-term wear.

[0022] In one embodiment, as described above, the recycled thermoplastic polyester particles obtained by recycling and granulation can be added to the manufacturing process of the leather 10 of the present invention. The polyester surface layer 13 includes a thermoplastic polyester material and a thermoplastic polyester recycled material, and the mixing weight ratio of the thermoplastic polyester material to the thermoplastic polyester recycled material ranges from 75%:25% to 100%:0%.

[0023] Figure 2 A schematic diagram showing a process flow of a leather manufacturing method according to an embodiment of the present invention is shown. Figure 1 and Figure 2 First, referring to step S21, a polyester substrate 11 is provided, wherein the polyester substrate 11 has a first surface 111 and a second surface 112, and the second surface 112 is opposite to the first surface 111. In one embodiment, the polyester substrate 11 is made of PET (Polyethylene Terphthalates). The polyester substrate 11 can be 100% PET recycled cotton or 60% PET recycled cotton mixed with 40% PET cotton, and needle-punched to form a non-woven fabric; or 100% recycled PET fiber or general PET fiber is used to weave into a woven fabric. Therefore, the polyester substrate 11 is made entirely of polyester material.

[0024] Referring to step S22, a polyester adhesive layer 12 is melt-sprayed onto the first surface 111 of the polyester substrate 11. In one embodiment, in the step of melt-spraying the polyester adhesive layer 12, first thermoplastic polyester particles (not shown) are further used, and the melting point thereof is 120-150°C. The first thermoplastic polyester particles may be PBT particles or TPEE particles. In one embodiment, in the step of melt-spraying the polyester adhesive layer 12, the melt-spraying distance thereof is 250-350 mm.

[0025] Referring to step S23, a thermoplastic polyester surface layer 13 is melt-sprayed onto the thermoplastic polyester adhesive layer 12. In one embodiment, in the step of melt-spraying the polyester surface layer 13, a second thermoplastic polyester particle (not shown) is further used, and the melting point thereof is 130-170°C. The second thermoplastic polyester particle may be a TPEE particle. In one embodiment, in the step of melt-spraying the polyester surface layer 13, the melt-spraying distance thereof is 150-250 mm.

[0026] In one embodiment, the step of melt-blowing the polyester surface layer further comprises using recycled thermoplastic polyester particles, wherein the weight ratio of the second thermoplastic polyester particles to the recycled thermoplastic polyester particles is in the range of 75%:25% to 100%:0%. The recycled thermoplastic polyester particles may be the recycled thermoplastic polyester particles obtained by recycling and granulating the leather after use according to the present invention.

[0027] Referring to step S24, the polyester substrate 11, the polyester adhesive layer 12 and the polyester surface layer 13 are subjected to heat pressing. In one embodiment, the temperature during the heat pressing step is 140° C. to 160° C. During the heat pressing step, since the temperature is higher than the melting point of the first thermoplastic polyester particles, the polyester adhesive layer 12 can be melted to be combined with the polyester substrate 11 and the polyester surface layer 13.

[0028] In one embodiment, after the heat pressing step, the leather of the present invention may be subjected to surface thermoplastic processing, such as thermoplastic embossing process, to have different surface textures.

[0029] Therefore, using the manufacturing method of the leather of the present invention, the polyester substrate 11, the polyester adhesive layer 12 and the polyester surface layer 13 are made of a single polyester material, and thus are produced with a single raw material, which can simplify the manufacturing process and material preparation of the leather of the present invention, improve manufacturing efficiency, and reduce manufacturing costs. In addition, the leather 10 of the present invention can be recycled and granulated after use, which has environmental benefits. Moreover, the recycled thermoplastic polyester particles obtained by recycling and granulation can be added to the manufacturing process of the leather 10 of the present invention to further improve environmental benefits and save manufacturing costs.

[0030] [Invention Example 1]

[0031] 100% recycled PET cotton or 60% recycled PET cotton mixed with 40% normal PET cotton is used to form a non-woven fabric as the polyester substrate 11 by needle-pressing.

[0032] TPEE particles with a Shore hardness of 80A and a melting point of 145°C were used, dried at a set drying temperature of 70°C for 4 hours, and the moisture content was measured to be less than 200ppm. The TPEE particles were then melted using a first extruder, and the temperatures from the feed port to the outlet were 170°C, 190°C, 210°C, 230°C, and 250°C in sequence, the head temperature was 250°C, the die temperature was 255°C, the hot air temperature at the spinning port was 275°C, the spinneret pressure was controlled at 1.0-3.0MPa, the melt-blowing distance from the die to the mesh curtain was 300mm, and the melt-blown polyester adhesive layer 12 was stacked in a fibrous manner on the non-woven polyester substrate 11, and its stacking density was 0.6-0.8g / cm 3 , fiber fineness is 3-50 microns, stacking weight is 200g / m 2 .

[0033] TPEE particles with a hardness of 80A and a melting point of 160°C were used, dried at a set drying temperature of 80°C for 4 hours, and the moisture content was measured to be less than 200ppm. The TPEE particles were then melted using a second extruder, and the temperatures from the feed port to the outlet were 220°C, 240°C, 260°C, 280°C, and 290°C in sequence, the head temperature was 290°C, the die temperature was 300°C, the hot air temperature at the spinning port was 320°C, the spinneret pressure was controlled at 1.0-3.0MPa, the melt-blowing distance from the die to the mesh curtain was 250mm, and the melt-blown polyester surface layer 13 was stacked in a fibrous manner on the polyester adhesive layer 12, and its stacking density was 0.6-0.8g / cm 3 , fiber fineness is 3-50 microns, stacking weight is 250g / m 2 .

[0034] The three-layer structure (the polyester substrate 11, the polyester adhesive layer 12 and the polyester surface layer 13) formed by meltblowing stacking is composite-molded by a track hot pressing method. The track heating temperature is set at 150°C, the pressure is 2-5Kg, and the vehicle speed is 3m / min to obtain a composite structure.

[0035] By using a thermoplastic embossing process to create a surface texture, a fully polyester system that is recyclable and environmentally friendly synthetic leather can be produced.

[0036] [Invention Example 2]

[0037] 100% recycled PET cotton or 60% recycled PET cotton mixed with 40% normal PET cotton is used to form a non-woven fabric as the polyester substrate 11 by needle-pressing.

[0038] PBT particles with a melting point of 145°C were used, and dried at a set drying temperature of 75°C for 4 hours, and the moisture content was measured to be less than 200ppm. The PBT particles were then melted by the first extruder, and the temperatures from the feed port to the outlet were 170°C, 185°C, 205°C, 225°C, and 245°C in sequence, the head temperature was 255°C, the die temperature was 255°C, the hot air temperature at the spinning port was 280°C, the spinneret pressure was controlled at 1.0-3.0MPa, the melt-blowing distance from the die to the mesh curtain was 300mm, and the melt-blown polyester adhesive layer 12 was stacked in a fibrous manner on the non-woven polyester substrate 11, and its stacking density was 0.2-0.4g / cm 3 , fiber fineness is 3-50 microns, stacking weight is 150g / m 2 .

[0039] TPEE particles with a hardness of 80A and a melting point of 165°C were used, dried at a set drying temperature of 80°C for 4 hours, and the moisture content was measured to be less than 200ppm. The TPEE particles were then melted using a second extruder, and the temperatures from the feed port to the outlet were 220°C, 240°C, 260°C, 280°C, and 290°C in sequence, the head temperature was 290°C, the die temperature was 300°C, the hot air temperature at the spinning port was 320°C, the spinneret pressure was controlled at 1.0-3.0MPa, the melt-blowing distance from the die to the mesh curtain was 200mm, and the melt-blown polyester surface layer 13 was stacked in a fibrous manner on the polyester adhesive layer 12, and its stacking density was 0.6-0.8g / cm 3 , fiber fineness is 3-50 microns, stacking weight is 200g / m 2 .

[0040] The three-layer structure (the polyester substrate 11, the polyester adhesive layer 12 and the polyester surface layer 13) formed by meltblowing stacking is composite-molded by a track hot pressing method. The track heating temperature is set at 155°C, the pressure is 2-5Kg, and the vehicle speed is 3m / min to obtain a composite structure.

[0041] By using a thermoplastic embossing process to create a surface texture, a fully polyester system that is recyclable and environmentally friendly synthetic leather can be produced.

[0042] [Invention Example 3]

[0043] The polyester base material 11 is made of 100% recycled PET fibers or woven fabric made of general PET fibers.

[0044] TPEE particles with a Shore hardness of 80A and a melting point of 130°C were used, dried at a set drying temperature of 70°C for 4 hours, and the moisture content was measured to be less than 200ppm. The TPEE particles were then melted using a first extruder, and the temperatures from the feed port to the outlet were 170°C, 190°C, 210°C, 230°C, and 250°C in sequence, the head temperature was 250°C, the die temperature was 255°C, the hot air temperature at the spinning port was 275°C, the spinneret pressure was controlled at 1.0-3.0MPa, the melt-blowing distance from the die to the mesh curtain was 300mm, and the melt-blown polyester adhesive layer 12 was stacked in a fibrous manner on the non-woven polyester substrate 11, and its stacking density was 0.6-0.8g / cm 3 , fiber fineness is 3-50 microns, stacking weight is 150g / m 2 .

[0045] TPEE particles with a hardness of 80A and a melting point of 150°C were used, dried at a set drying temperature of 75°C for 4 hours, and the moisture content was measured to be less than 200ppm. The TPEE particles were then melted using a second extruder, and the temperatures from the feed port to the outlet were 220°C, 240°C, 260°C, 280°C, and 290°C in sequence, the head temperature was 290°C, the die temperature was 300°C, the hot air temperature at the spinning port was 320°C, the spinneret pressure was controlled at 1.0-3.0MPa, the melt-blowing distance from the die to the mesh curtain was 250mm, and the melt-blown polyester surface layer 13 was stacked in a fibrous manner on the polyester adhesive layer 12, and its stacking density was 0.6-0.8g / cm 3 , fiber fineness is 3-50 microns, stacking weight is 200g / m 2 .

[0046] The three-layer structure (the polyester substrate 11, the polyester adhesive layer 12 and the polyester surface layer 13) formed by meltblowing stacking is composite-molded by a track hot pressing method. The track heating temperature is set at 140°C, the pressure is 2-5Kg, and the vehicle speed is 3m / min to obtain a composite structure.

[0047] By using a thermoplastic embossing process to create a surface texture, a fully polyester system that is recyclable and environmentally friendly synthetic leather can be produced.

[0048] [Invention Example 4]

[0049] The substrate 11 is made of 100% recycled PET fiber or woven fabric made of general PET fiber.

[0050] PBT particles with a melting point of 145°C were used, and dried at a set drying temperature of 75°C for 4 hours, and the moisture content was measured to be less than 200ppm. The PBT particles were then melted by the first extruder, and the temperatures from the feed port to the outlet were 170°C, 185°C, 205°C, 225°C, and 245°C in sequence, the head temperature was 255°C, the die temperature was 255°C, the hot air temperature at the spinning port was 280°C, the spinneret pressure was controlled at 1.0-3.0MPa, the melt-blowing distance from the die to the mesh curtain was 300mm, and the melt-blown polyester adhesive layer 12 was stacked in a fibrous manner on the non-woven polyester substrate 11, and its stacking density was 0.2-0.4g / cm 3 , fiber fineness is 3-50 microns, stacking weight is 150g / m 2 .

[0051] TPEE particles with a hardness of 80A and a melting point of 155°C were used, dried at a set drying temperature of 80°C for 4 hours, and the moisture content was measured to be less than 200ppm. The TPEE particles were then melted using a second extruder, and the temperatures from the feed port to the outlet were 220°C, 240°C, 260°C, 280°C, and 290°C in sequence, the head temperature was 290°C, the die temperature was 300°C, the hot air temperature at the spinning port was 320°C, the spinneret pressure was controlled at 1.0-3.0MPa, the melt-blowing distance from the die to the mesh curtain was 250mm, and the melt-blown polyester surface layer 13 was stacked in a fibrous manner on the polyester adhesive layer 12, and its stacking density was 0.6-0.8g / cm 3 , fiber fineness is 3-50 microns, stacking weight is 200g / m 2 .

[0052] The three-layer structure (the polyester substrate 11, the polyester adhesive layer 12 and the polyester surface layer 13) formed by meltblowing stacking is composite-molded by a track hot pressing method. The track heating temperature is set at 150°C, the pressure is 2-5Kg, and the vehicle speed is 3m / min to obtain a composite structure.

[0053] By using a thermoplastic embossing process to create a surface texture, a fully polyester system that is recyclable and environmentally friendly synthetic leather can be produced.

[0054] [Invention Example 5]

[0055] The leather products of the present invention in the above-mentioned Invention Examples 1 to 4 are crushed as a whole, and then melt-granulated to form thermoplastic polyester recycled particles.

[0056] 100% recycled PET cotton or 60% recycled PET cotton mixed with 40% normal PET cotton is used to form a non-woven fabric as the polyester substrate 11 by needle-pressing.

[0057] TPEE particles with a Shore hardness of 80A and a melting point of 125°C were used, dried at a set drying temperature of 70°C for 4 hours, and the moisture content was measured to be less than 200ppm. The TPEE particles were then melted using a first extruder, and the temperatures from the feed port to the outlet were 170°C, 190°C, 210°C, 230°C, and 250°C in sequence, the head temperature was 250°C, the die temperature was 255°C, the hot air temperature at the spinning port was 275°C, the spinneret pressure was controlled at 1.0-3.0MPa, the melt-blowing distance from the die to the mesh curtain was 300mm, and the melt-blown polyester adhesive layer 12 was stacked in a fibrous manner on the non-woven polyester substrate 11, and its stacking density was 0.6-0.8g / cm 3 , fiber fineness is 3-50 microns, stacking weight is 200g / m 2 .

[0058] TPEE particles with a hardness of 80A and a melting point of 140°C were mixed with the above-mentioned thermoplastic polyester recycled particles, dried at a set drying temperature of 70°C for 4 hours, and the moisture content was measured to be less than 200ppm. Thermoplastic polyester recycled particles were added to TPEE particles in a mixed manner, and the mixing weight ratio of the TPEE particles and the thermoplastic polyester recycled particles was 85%:15%. The TPEE particles and thermoplastic polyester recycled particles were melt-mixed by a second extruder, and the temperatures from the feed port to the outlet were 220°C, 240°C, 260°C, 280°C, and 290°C in sequence, the head temperature was 290°C, the die temperature was 300°C, the hot air temperature at the spinning mouth was 320°C, the spinneret pressure was controlled at 1.0-3.0MPa, the melt-blown distance from the die to the mesh curtain was 250mm, and the melt-blown polyester surface layer 13 was stacked in a fibrous manner on the polyester adhesive layer 12, and its stacking density was 0.6-0.8g / cm 3 , fiber fineness is 3-50 microns, stacking weight is 200g / m 2 .

[0059] The three-layer structure (the polyester substrate 11, the polyester adhesive layer 12 and the polyester surface layer 13) formed by meltblowing stacking is composite-molded by a track hot pressing method. The track heating temperature is set at 130°C, the pressure is 2-5Kg, and the vehicle speed is 3m / min to obtain a composite structure.

[0060] By using a thermoplastic embossing process to create a surface texture, a fully polyester system that is recyclable and environmentally friendly synthetic leather can be produced.

[0061] [Invention Example 6]

[0062] The leather products of the present invention in the above-mentioned Invention Examples 1 to 4 are crushed as a whole, and then melt-granulated to form thermoplastic polyester recycled particles.

[0063] The substrate 11 is made of 100% recycled PET fiber or woven fabric made of general PET fiber.

[0064] TPEE particles with a Shore hardness of 80A and a melting point of 130°C were used, dried at a set drying temperature of 70°C for 4 hours, and the moisture content was measured to be less than 200ppm. The TPEE particles were then melted using a first extruder, and the temperatures from the feed port to the outlet were 170°C, 190°C, 210°C, 230°C, and 250°C in sequence, the head temperature was 250°C, the die temperature was 255°C, the hot air temperature at the spinning port was 275°C, the spinneret pressure was controlled at 1.0-3.0MPa, the melt-blowing distance from the die to the mesh curtain was 300mm, and the melt-blown polyester adhesive layer 12 was stacked in a fibrous manner on the non-woven polyester substrate 11, and its stacking density was 0.6-0.8g / cm 3 , fiber fineness is 3-50 microns, stacking weight is 150g / m 2 .

[0065] TPEE particles with a hardness of 80A and a melting point of 150°C were mixed with the above-mentioned thermoplastic polyester recycled particles, dried at a set drying temperature of 75°C for 4 hours, and the moisture content was measured to be less than 200ppm. Thermoplastic polyester recycled particles were added to TPEE particles in a mixed manner, and the mixing weight ratio of the TPEE particles and the thermoplastic polyester recycled particles was 75%:25%. The TPEE particles and thermoplastic polyester recycled particles were melt-mixed by a second extruder, and the temperatures from the feed port to the outlet were 220°C, 240°C, 260°C, 280°C, and 290°C in sequence, the head temperature was 290°C, the die temperature was 300°C, the hot air temperature at the spinning mouth was 320°C, the spinneret pressure was controlled at 1.0-3.0MPa, the melt-blown distance from the die to the mesh curtain was 150mm, and the melt-blown polyester surface layer 13 was stacked in a fibrous manner on the polyester adhesive layer 12, and its stacking density was 0.6-0.8g / cm 3 , fiber fineness is 3-50 microns, stacking weight is 200g / m 2 .

[0066] The three-layer structure (the polyester substrate 11, the polyester adhesive layer 12 and the polyester surface layer 13) formed by meltblowing stacking is composite-molded by a track hot pressing method. The track heating temperature is set at 140°C, the pressure is 2-5Kg, and the vehicle speed is 3m / min to obtain a composite structure.

[0067] By using a thermoplastic embossing process to create a surface texture, a fully polyester system that is recyclable and environmentally friendly synthetic leather can be produced.

[0068] The above embodiments are only for explaining the principle and efficacy of the present invention, but not for limiting the present invention. The modifications and changes made by those skilled in the art to the above embodiments still do not violate the spirit of the present invention. The scope of rights of the present invention shall be as listed in the claims.

Claims

1. A leather comprising: A polyester substrate; A polyester adhesive layer is disposed on the polyester substrate by melt-blowing; and A polyester surface layer is disposed on the polyester adhesive layer by meltblowing, and the polyester surface layer includes a thermoplastic polyester material and a thermoplastic polyester recycled material, and the mixing weight ratio of the thermoplastic polyester material to the thermoplastic polyester recycled material ranges from 75%:25% to 85%:15%; The polyester adhesive layer and the polyester surface layer are fiber mesh structures; The density of the polyester adhesive layer is 0.2-0.8 g / cm 3 ; The density of the polyester surface layer is 0.5-0.9 g / cm 3 ; The polyester adhesive layer includes first thermoplastic polyester particles having a melting point of 120 to 150° C.; The melting point of the thermoplastic polyester material in the polyester surface layer is 130-170°C.

2. The leather as claimed in claim 1, wherein the polyester substrate is made of polyethylene terephthalate, thermoplastic polyether ester elastomer or polybutylene terephthalate.

3. The leather as claimed in claim 1, wherein the polyester adhesive layer is made of polyethylene terephthalate, thermoplastic polyether ester elastomer or polybutylene terephthalate.

4. The leather as claimed in claim 3, wherein the weight of the polyester adhesive layer is 50-400 g / m 2 .

5. The leather as claimed in claim 1, wherein the polyester surface layer is made of polyethylene terephthalate, thermoplastic polyether ester elastomer or polybutylene terephthalate.

6. The leather as claimed in claim 5, wherein the weight of the polyester surface layer is 50-400 g / m 2 .

7. A method for manufacturing leather, comprising the following steps: Providing a polyester substrate; A melt-blown polyester adhesive layer is stacked in a fibrous manner into a web on the polyester substrate, and the density of the polyester adhesive layer is 0.2-0.8 g / cm 3 ; The melt-blown polyester surface layer is stacked in a fibrous manner into a web on the polyester adhesive layer, and the density of the polyester surface layer is 0.5-0.9 g / cm 3 ;and Thermally pressing the polyester substrate, the polyester adhesive layer and the polyester surface layer; The step of melt-blowing the polyester adhesive layer further comprises using first thermoplastic polyester particles having a melting point of 120 to 150° C.; The step of melt-blowing the polyester surface layer further includes utilizing second thermoplastic polyester particles and thermoplastic polyester recycled particles, wherein the melting point of the second thermoplastic polyester particles is 130-170° C., and the mixing weight ratio of the second thermoplastic polyester particles and the thermoplastic polyester recycled particles ranges from 75%:25% to 85%:15%. 8 . The method for producing leather according to claim 7 , wherein the first thermoplastic polyester particles are PBT particles or TPEE particles. 9 . The method for producing leather according to claim 7 , wherein the second thermoplastic polyester particles are TPEE particles.

10. The method for producing leather according to claim 7, wherein in the heat pressing step, the temperature is 140°C to 160°C.

11. The method for manufacturing leather according to claim 7, wherein in the step of melt-blowing the polyester adhesive layer, the melt-blowing distance is 250-350 mm.

12. The method for manufacturing leather according to claim 7, wherein in the step of melt-blowing the polyester surface layer, the melt-blowing distance is 150-250 mm.