A treatment method for improving the performance of high manganese steel by composite precipitation phase

Through solid solution aging treatment and second phase strengthening technology, the problems of deformation and insufficient wear resistance of high manganese steel are solved, its strength and wear resistance are significantly improved, the service life is extended, and the performance of high manganese steel under different conditions is achieved. excellent performance.

CN115572800BActive Publication Date: 2024-10-22KUNMING UNIV OF SCI & TECH
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
CN202211343000.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-31
Publication Date
2024-10-22
Estimated Expiration
2042-10-31

AI Technical Summary

Technical Problem

During the use of high manganese steel, due to uneven microstructure and uneven distribution of eutectic carbides, severe deformation, cracking and reduced wear resistance are caused, causing economic losses. Its mechanical properties and wear resistance need to be improved to extend its service life.

Method used

Through the solid solution aging treatment method, the number, size and distribution of the composite sub-micron precipitated phases in the high manganese steel matrix are changed, and the second phase strengthening effect of the (Ti, Nb, V) (C, N) precipitated phase is used, combined with the solid Solution strengthening, fine grain strengthening and dislocation strengthening improve the strength and wear resistance of high manganese steel.

Benefits of technology

Significantly improve the strength and wear resistance of high manganese steel, extend the service life, control the number and distribution of precipitated phases through reasonable aging treatment, enhance the hardness and work hardening ability of the matrix, reduce wear, and improve the performance in different services performance under conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115572800B_ABST
    Figure CN115572800B_ABST
Patent Text Reader

Abstract

The invention discloses a method for improving the performance of high manganese steel by composite precipitation phase, which belongs to the technical field of metal materials. The chemical composition mass percentage of the high manganese steel is: C: 0.85-0.95, N: 0.17-0.18, Mn: 18.0-19.0, Si: 0.8-1.0, Cr: 1.8-1.9, Ti: 0.08-0.1, V: 0.35-0.4, Nb: 0.1-0.12, Mo: 0.4-0.5, Ni: 0.2-0.3, Cu: 0.4-0.6, P: <0.02, S: <0.02, and the rest is Fe and unavoidable trace impurities. The treatment process includes: In summary: the chemical composition is used for batching, metal is smelted in a medium frequency induction furnace and cast into a steel ingot; the ingot is subjected to solid solution treatment and aging treatment in sequence, wherein the solid solution treatment is heat preservation at 1050-1150°C for 1h-2h and water quenching, and then aging treatment at 350-450°C for 48-96h and air cooling, through which a large number of composite submicron precipitated phases (Ti, Nb, V) (C, N) can be precipitated in the austenite matrix, so that the high manganese steel has the advantages of composite precipitation strengthening, high tensile strength and high wear resistance, and the performance of the high manganese steel is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metal materials, and specifically provides a processing method for improving the performance of high manganese steel by using a composite precipitated phase. Background Art

[0002] High manganese steel is widely used in large equipment required in the fields of machinery, mining, metallurgy, electricity, coal, chemical industry and railway. Most of its accessories are large, weighing several tons to more than ten tons, and the service conditions are harsh. Most of the cast high manganese steels have uneven structure and large eutectic carbides distributed at the grain boundaries. High manganese steels are severely deformed and cracked during use, and their wear resistance is reduced, causing huge economic losses. Therefore, it is urgent to improve the mechanical properties and wear resistance of high manganese steel, extend the service life of the workpiece, and reduce production costs.

[0003] Second phase strengthening is one of the important methods to improve the strength and wear resistance of high manganese steel. If a certain amount of high-hardness second phase can be dispersed in the austenite matrix of high manganese steel, it can hinder the slip of dislocations during deformation, strengthen the matrix, improve the work hardening ability, and effectively prevent grain coarsening during heat treatment. Solution treatment can dissolve most of the carbonitrides on the grain boundaries of cast high manganese steel and diffuse the alloy elements into the grains; aging treatment affects the precipitation evolution law of the second phase in the matrix. A reasonable aging treatment system can regulate the number and distribution of submicron precipitation phases in the high manganese steel matrix, improve the strength and wear resistance of high manganese steel, meet the use requirements of high manganese steel under different service conditions, and extend the service life of high manganese steel.

[0004] The present invention adopts a suitable processing method to obtain a composite submicron precipitate phase, fully exerts the role of alloy elements in improving the strength of steel, and utilizes the comprehensive strengthening effects of several strengthening mechanisms such as solid solution strengthening, fine grain strengthening, dislocation strengthening, and second phase strengthening to obtain high manganese steel with higher toughness and wear resistance. Summary of the invention

[0005] The invention aims to improve the strength and wear resistance of high manganese steel and solve the problems of deformation, cracking and severe wear of high manganese steel during use. A processing method for improving the performance of high manganese steel by using a composite precipitate phase is disclosed, which changes the number, size and distribution of the composite submicron precipitate phase in the high manganese steel matrix, improves the mechanical properties of the high manganese steel and increases the service life.

[0006] According to claim 1, a method for improving the performance of high manganese steel by using a composite precipitate phase, the cast structure of the obtained high manganese steel is an austenite matrix and micron-sized eutectic carbides precipitated along the grain boundaries at room temperature, and a large number of composite submicron-sized precipitates can be precipitated by solution aging treatment, wherein the composite submicron-sized precipitates are (Ti, Nb, V) (C, N), and the size of the precipitates is not more than 300 nm, comprising the following steps:

[0007] (1) Solution treatment: Heat the cast alloyed high manganese steel to 1050-1150℃, keep it warm for 1-2h and then quench it in water; the time from opening the furnace door to the high manganese steel entering the water is ≤60s; the water temperature before the high manganese steel enters the water is ≤30℃; the water temperature after entering the water is ≤50℃; the cooling time is ≥90min; the mass ratio of the casting to water is not greater than 1:10.

[0008] (2) Aging treatment: The alloyed high manganese steel obtained in step 1 is heated to 350°C to 450°C, kept at this temperature for 48 to 96 hours, and then air-cooled to room temperature to allow the alloyed high manganese steel to fully precipitate submicron carbides.

[0009] Furthermore, the chemical composition and mass percentage of the cast alloyed high manganese steel of the present invention are: C: 0.85-0.95, N: 0.17-0.18, Mn: 18.0-19.0, Si: 0.8-1.0, Cr: 1.8-1.9, Ti: 0.08-0.1, V: 0.35-0.4, Nb: 0.1-0.12, Mo: 0.4-0.5, Ni: 0.2-0.3, Cu: 0.4-0.6, P: <0.02, S: <0.02, and the rest are Fe and inevitable trace impurities.

[0010] Furthermore, the heating device described in the present invention is a box-type resistance furnace.

[0011] Furthermore, the heating rate in the solution treatment in step (1) of the present invention is not greater than 10°C / min.

[0012] Furthermore, in the aging treatment of step (2) of the present invention, the heating rate is controlled at 0.2-0.3°C / s, and the holding time is 48-96h.

[0013] Furthermore, in the air cooling process of step (2) of the present invention, the mixture is immediately placed in the air to cool after heat preservation.

[0014] Beneficial effects of the present invention:

[0015] (1) The selection of heat treatment temperature and time fully considers the comprehensive strengthening effects of solid solution strengthening, grain refinement strengthening, dislocation strengthening, and second phase strengthening. The most important of these is the second phase strengthening effect of the composite submicron precipitate phase.

[0016] (2) Metal smelting and casting are carried out in a medium frequency induction furnace to obtain a formed nitrogen microalloyed ultra-high manganese steel ingot, and the preparation process is simple; through solid solution treatment at 1050-1150°C (depending on the fineness or coarseness of the carbides in the steel), the large-sized MC-type and MN-type eutectic carbides at the grain boundaries are dissolved in the matrix, reducing the impact on the toughness of the high manganese steel; small-sized submicron-level precipitates are distributed in the austenite matrix, which can enhance the microhardness of the matrix and improve the wear resistance of the steel under the condition of impact abrasive wear.

[0017] (3) After being kept at 400℃ for different time periods of 48 to 96h, the composite submicron precipitate phase (Ti, Nb, V) (C, N) has a slow coarsening rate and a long holding time, which allows it to be fully precipitated, increasing the amount of (Ti, Nb, V) (C, N) precipitation and enhancing the matrix hardness. When a large number of submicron particles interact with dislocations, they hinder the movement of dislocations, causing dislocations to pile up and increase the strength of the steel. If the holding time is short, the number of precipitated particles is small and the strengthening effect is not obvious.

[0018] (4) The addition of other alloying elements such as Cr, Mo, Ni, and Cu further strengthens the austenite matrix, which can quickly produce a wear-resistant hardened layer under the action of external force, thereby improving the work hardening ability of high manganese steel and making high manganese steel exhibit good wear resistance under large impact load conditions. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 It is a schematic diagram of the heat treatment process of the alloyed high manganese steel of the present invention.

[0020] Figure 2 This is a SEM image of the submicron precipitate phase in the alloyed high manganese steel casting after solution aging treatment in Example 2 of the present invention.

[0021] Figure 3 This is an EDS image of the submicron precipitate phase in the alloyed high manganese steel casting after solution aging treatment in Example 2 of the present invention.

[0022] Figure 4 This is a SEM image of the wear morphology of the alloyed high manganese steel after solution treatment in the comparative example of the present invention and after 5 hours of impact wear.

[0023] Figure 5 This is a SEM image of the wear morphology of the alloyed high manganese steel after solution aging treatment and 5 hours of impact wear in Example 2 of the present invention. DETAILED DESCRIPTION

[0024] The present invention is further described in detail below in conjunction with specific embodiments, but the implementation manner of the present invention is not limited to the described contents.

[0025] Example 1

[0026] A method for improving the performance of high manganese steel by composite precipitation phase, specifically comprising the following steps:

[0027] In the present invention, the chemical composition (wt%) of the cast high manganese steel is: C: 0.90, Mn: 18.5, Cr: 1.85, Mo: 0.43, V: 0.37, Si: 0.91, Ni: 0.26, Nb: 0.12, Cu: 0.5, N: 0.17, P: 0.014, Ti: 0.094, S: 0.012, and the rest is Fe and inevitable impurities for smelting and casting to cast a high manganese steel casting with a size of 200mm×60mm×60mm.

[0028] Solution treatment: heat the cast alloyed high manganese steel to 1050℃ and keep it in temperature for 60min. The heating rate in this stage is 9℃ / min. Water quenching is carried out after the insulation. The time from opening the furnace door to the high manganese steel entering the water is ≤60s. The water temperature before the high manganese steel enters the water is ≤30℃, and the water temperature after entering the water is ≤50℃. The cooling time is ≥90min, and the mass ratio of the casting to water is not more than 1:10.

[0029] Isothermal aging treatment: The alloyed high manganese steel after the solution treatment in step 2 is heated to 400°C. The heating rate in this stage is 0.3°C / s. After keeping the temperature for 60 hours, it is air-cooled to room temperature.

[0030] Example 2

[0031] A method for improving the performance of high manganese steel by composite precipitation phase, specifically comprising the following steps:

[0032] In the present invention, the chemical composition (wt%) of the cast high manganese steel is: C: 0.94, Mn: 18.1, Cr: 1.89, Mo: 0.41, V: 0.4, Si: 0.98, Ni: 0.21, Nb: 0.11, Cu: 0.56, N: 0.18, P: 0.004, Ti: 0.09, S: 0.016, and the rest is Fe and inevitable impurities for smelting and casting to cast a high manganese steel casting with a size of 200mm×60mm×60mm.

[0033] Solution treatment: heat the cast alloyed high manganese steel to 1150℃ and keep it in water for 120min. The heating rate in this stage is 8℃ / min. Water quenching is carried out after the insulation. The time from opening the furnace door to the high manganese steel entering the water is ≤60s. The water temperature before the high manganese steel enters the water is ≤30℃, and the water temperature after entering the water is ≤50℃. The cooling time is ≥90min, and the mass ratio of the casting to water is not more than 1:10.

[0034] Aging treatment: Heat the alloyed high manganese steel after the solution treatment in step 2 to 450°C. The heating rate in this stage is 0.25°C / s. After keeping the temperature for 72 hours, air cool it to room temperature.

[0035] Example 3

[0036] A method for improving the performance of high manganese steel by composite precipitation phase, specifically comprising the following steps:

[0037] In the present invention, the chemical composition (wt%) of the cast high manganese steel is: C: 0.95, Mn: 18.7, Cr: 1.84, Mo: 0.49, V: 0.35, Si: 0.96, Ni: 0.28, Nb: 0.1, Cu: 0.45, N: 0.175, P: 0.019, Ti: 0.099, S: 0.011, and the rest is Fe and inevitable impurities for smelting and casting to cast a high manganese steel casting with a size of 200mm×60mm×60mm.

[0038] Solution treatment: heat the cast alloyed high manganese steel to 1100℃ and keep it in temperature for 90min. The heating rate in this stage is 7℃ / min. Water quenching is carried out after the insulation. The time from opening the furnace door to the high manganese steel entering the water is ≤60s. The water temperature before the high manganese steel enters the water is ≤30℃, and the water temperature after entering the water is ≤50℃. The cooling time is ≥90min, and the mass ratio of the casting to water is not more than 1:10.

[0039] Aging treatment: The alloyed high manganese steel after the solution treatment in step 2 is heated to 350°C. The heating rate in this stage is 0.2°C / s. After keeping the temperature for 84 hours, it is air-cooled to room temperature.

[0040] Comparative Example

[0041] The difference from Examples 1 to 3 is that the heat treatment process only performs solution treatment without aging treatment.

[0042] Microstructure characterization

[0043] The microstructure of the cast alloyed high manganese steel of Example 2 was observed. Figure 2 and Figure 3 They are respectively the SEM image and EDS image of the submicron precipitate phase in the alloyed high manganese steel casting after solution aging treatment; Figure 2 It can be seen that the alloyed high manganese steel austenite matrix prepared in Example 2 is distributed with submicron precipitates of size not greater than 300nm, the size of the submicron precipitates is between 100nm and 300nm, the number is large, the distribution is relatively uniform, and the shape is mainly irregular square. Figure 3From the EDS, it can be seen that the submicron precipitate phase is mainly composed of Ti, V, Nb, C and N elements, forming a composite (Ti, Nb, V) (C, N) precipitate phase. The submicron precipitate phase can hinder the movement of dislocations, induce the accumulation of dislocations, play a role in dislocation strengthening, and thus improve the strength of high manganese steel.

[0044] Mechanical properties test

[0045] The alloyed high manganese steel of Examples 1 to 3 and the comparative example was subjected to an impact abrasive wear test under the same environment, with an impact energy of 2 J, an abrasive particle size of 40 to 70 meshes, and an impact time of 5 hours. The impact wear specimens of Examples 1 to 3 and the comparative example were prepared by wire cutting, and the sample size was 10 mm × 10 mm × 30 mm.

[0046] The hourly wear amount and total wear amount of Examples 1 to 3 are shown in Table 1.

[0047]

[0048] The alloyed high manganese steels of Examples 1 to 3 and the comparative example were subjected to tensile tests and microhardness tests under the same environment to test their mechanical properties.

[0049] The yield strength, tensile strength, elongation and Vickers hardness of Examples 1 to 3 and the comparative example are shown in Table 2.

[0050]

[0051] Results and Analysis

[0052] It can be concluded from Tables 1 and 2 above that with the extension of aging time, the comprehensive mechanical properties of alloyed high manganese steel show a trend of first increasing and then decreasing. When kept at 450°C for 72 hours, the strength, hardness and wear resistance of high manganese steel all reach the peak value, and the work hardening ability is good; while the control sample without aging treatment has lower strength and more wear. Under the condition of impact wear, it cannot be fully work hardened and has poor wear resistance.

[0053] The results show that the strength, hardness and wear resistance of alloyed high manganese steel show different trends under different aging treatments; when the aging and heat preservation time is 60h and 72h, the strength and hardness continue to increase, which is due to the continuous precipitation of submicron precipitates (Ti, Nb, V) (C, N) with the extension of aging time. The number of precipitates continues to increase and is dispersed in the matrix, which enhances the work hardening ability of high manganese steel. It reaches a peak aging state at 72h. At this time, the precipitation strengthening effect of submicron precipitates is much greater than the softening effect caused by the recovery of the matrix; after the peak aging period, with the extension of aging time, the submicron precipitates (Ti, Nb, V) (C, N) undergo a certain degree of coarsening and the recovery softening of the matrix causes the strength and hardness values ​​of the alloyed high manganese steel to gradually decrease, showing an over-aging period.

[0054] Figure 4 and Figure 5 The wear morphology SEM images of alloyed high manganese steel after solution treatment and solution aging treatment after 5h impact wear are respectively Figure 4 It can be seen that many spalling pits appeared on the wear surface of the high manganese steel sample that had only been solution treated. At the same time, there were many furrows on the wear surface caused by the extrusion of abrasive particles, and the furrow area was large, and some furrows were deep, indicating that the wear was serious, which was consistent with the mass loss of the comparative sample in Table 1. After the solution treatment, the matrix structure was austenite and a very small amount of micron-sized eutectic carbides distributed at the grain boundaries, the matrix was insufficiently strengthened, the work hardening rate was low, and the wear resistance was poor, and the wear was serious. Figure 5 It can be seen that after solution aging treatment, the wear surface of the high manganese steel sample also has peeling pits and furrows, and there are many plastic deformation areas. Compared with the control group, the furrow area is reduced and the furrow depth is shallow, indicating that the wear is reduced and the wear mass loss is less. After aging treatment, the matrix disperses and precipitates (Ti, Nb, V) (C, N) submicron precipitates, which improves the work hardening ability and surface hardness of the high manganese steel, and enhances the depth of the hardened layer under impact wear conditions, so that the high manganese steel exhibits good wear resistance.

[0055] The above content describes the technical principles, beneficial effects and features of the present invention. It should be pointed out that the above is only a preferred implementation mode of the present invention, but is not limited to the above embodiments. For technicians in the technical field to which the present invention belongs, some improvements and optimizations can be made without departing from the content of the present invention, which should be regarded as belonging to the protection scope of the present invention.

Claims

1. A method for improving the performance of high manganese steel by composite precipitation phase, characterized in that: The following steps are involved: (1) Preparing the ingredients according to the mass percentage of the alloyed high manganese steel for casting, smelting the metal in a medium frequency induction furnace, and casting to obtain a molded alloyed high manganese steel ingot; (2) Solution treatment: heat the alloyed high manganese steel ingot to 1050-1150℃, keep it warm for 1-2h and then quench it in water; the time from opening the furnace door to the high manganese steel entering the water is ≤60s; the water temperature before the high manganese steel enters the water is ≤30℃; the water temperature after entering the water is ≤50℃; the cooling time is ≥90min; the mass ratio of the casting to water is not greater than 1:10; (3) Aging treatment: heating the alloyed high manganese steel obtained in step 1 to 350°C to 450°C, keeping the temperature for 48 to 96 hours, and then air cooling to room temperature to allow the alloyed high manganese steel to fully precipitate submicron carbides; The chemical composition and mass percentage of cast alloyed high manganese steel are: C: 0.85~0.95, N: 0.17~0.18, Mn: 18.0~19.0, Si: 0.8~1.0, Cr: 1.8~1.9, Ti: 0.08~0.1, V: 0.35~0.4, Nb: 0.1~0.12, Mo: 0.4~0.5, Ni: 0.2~0.3, Cu: 0.4~0.6, P: <0.02, S: <0.02, and the rest are Fe and inevitable trace impurities.

2. The method for improving the performance of high manganese steel by composite precipitation phase according to claim 1, characterized in that: The heating device is a box-type resistance furnace.

3. The method for improving the performance of high manganese steel by composite precipitation phase according to claim 2, characterized in that: The heating rate in the solution treatment of step (1) is not greater than 10°C / min.

4. The method for improving the performance of high manganese steel by composite precipitation phase according to claim 1, characterized in that: In step (2) of the aging treatment, the heating rate is controlled at 0.2 to 0.3°C / s, and the holding time is 48 to 96 hours.

5. The method for improving the performance of high manganese steel by composite precipitation phase according to claim 1, characterized in that: In the air cooling process of step (2), after keeping warm, immediately place it in the air to cool.

Citation Information

Patent Citations

  • Process of manufacturing strips of sheet steel for fabricating metal packaging by stamping and the sheet steel so produced

    CA2246591A1

  • High-mn austenite stainless steel and metal part for clothing

    CN102333900A

  • Nanometer intermetallic compound-reinforced superhigh strength ferritic steel and manufacturing method thereof

    CN104046891A

  • Method for improving property of alloying high-manganese steel casting

    CN109487047A

  • Preparation method of cast high manganese steel with high wear resistance under low stress impact

    CN111154951A